Nanofiber felt for wide-temperature-range microwave absorption and preparation method thereof

By forming a SiTiOC amorphous layer on the surface of SiC and TiC nanofibers, combining electrospinning and high-temperature pyrolysis technology, the problem of unstable performance of existing high-temperature microwave absorbing materials in a wide temperature range is solved, and the performance of high-temperature conditions is achieved The stable microwave absorption and antioxidant properties are suitable for modern military and industrial applications.

CN119083034APending Publication Date: 2024-12-06YANAN UNIV

Patent Information

Application Number
CN202411493660.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-24
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing high-temperature microwave absorbing materials are difficult to maintain stable absorption performance under severe temperature fluctuations, and the oxidation resistance of traditional single-component carbon-based ceramic materials is weak, which limits their application in a wide temperature range.

Method used

Using nanofiber felt, nanofibers are composed of SiC and TiC, and SiTiOC amorphous nanolayer is formed on their surface. The electromagnetic wave absorption capacity is enhanced through interface polarization and multiple scattering, and prepared by electrospinning and high-temperature pyrolysis processes to form Stable conductive network and antioxidant film.

Benefits of technology

Maintain stable microwave absorption performance over a wide temperature range of 293K to 873K, enhances oxidation resistance and thermal stability, is suitable for applications under high temperature conditions, and has a relatively simple process and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119083034A_ABST
    Figure CN119083034A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of microwave absorption, and particularly relates to a wide-temperature-range microwave absorption nanofiber felt and a preparation method thereof.The nanofiber felt comprises nanofibers, the nanofibers are composed of SiC and TiC nanocrystals, the nanofiber felt further comprises a SiTiOC layer, and the nanofibers are coated with the SiTiOC layer. The nanofiber felt keeps stable microwave absorption performance in a wide temperature range from 293 K to 873 K, the minimum reflection loss reaches-45.55 dB, the effective wave absorption bandwidth is 3.6 GHz, and the application requirement under the high-temperature condition is met. The SiTiOC amorphous layer formed on the surface of the nanofiber in situ effectively prevents oxygen from diffusing into the fiber, enhances the oxidation resistance of the material at high temperature, and ensures that the material has better thermal stability and longer service life in a high-temperature environment. In addition, the nanofiber felt is prepared through electrostatic spinning and a high-temperature pyrolysis process, the process is relatively simple, large-scale production is easy, and the nanofiber felt is suitable for large-scale industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of microwave absorption, and in particular relates to a nanofiber felt capable of absorbing microwaves over a wide temperature range and a preparation method thereof. Background Art

[0002] With the advent of the Internet of Things era, electromagnetic waves, as the key carrier of electronic information transmission, have become indispensable in modern life and technological progress. However, the rapid development of electronic information technology and the exponential growth of data have led to serious congestion and interference in various electromagnetic wave frequency bands. In addition, the miniaturization and high integration of information terminals have led to significant accumulation of thermal radiation, which has put forward higher requirements on the thermal management capabilities of materials. At the same time, the significant progress in radar detection technology in modern military applications has also put forward higher requirements on the survivability and stealth capabilities of weapons and equipment in harsh environments. These challenges urgently require an electromagnetic absorption material that has both excellent electromagnetic properties and can remain stable under extreme high temperature conditions.

[0003] In recent years, high-temperature microwave absorbing materials have received extensive attention due to their excellent performance under various harsh conditions. The performance of high-temperature absorbing materials depends not only on their own electromagnetic properties, but also on their thermal stability in high-temperature environments. Through reasonable material composition design and structural optimization, the electromagnetic parameters of the material can be effectively controlled, thereby improving the microwave absorption performance. For example, C f / SiC nanofiber materials show excellent microwave absorption performance in a high temperature range. However, the electromagnetic properties of existing materials are very sensitive to temperature changes, and it is difficult to maintain stable absorption performance under drastic temperature fluctuations. In particular, traditional single-component carbon-based ceramic materials, despite their good high-temperature stability and mechanical strength, have simple electromagnetic loss mechanisms and weak anti-oxidation properties, which easily lead to impedance mismatch, thus limiting their further application in a wide temperature range. Summary of the invention

[0004] To solve the above problems, the present invention provides a nanofiber felt for wide temperature range microwave absorption, wherein the nanofiber felt comprises nanofibers composed of SiC and TiC nanocrystals, and also comprises a SiTiOC amorphous nanolayer, wherein the SiTiOC amorphous nanolayer coats the nanofibers.

[0005] In the nanofiber mat of the present invention, SiC and TiC, as the main microwave loss units, significantly enhance the electromagnetic wave absorption capacity of the material by providing interface polarization, multiple scattering and conductive network. Specifically, the introduction of TiC not only prevents the agglomeration of SiC nanocrystals, but also increases the reflection and scattering opportunities of electromagnetic waves inside the material through interface polarization and multiple scattering effects. Such multiple scattering and interface polarization effects can effectively improve the microwave absorption capacity of the material. In a high temperature environment, SiTiOC, as an antioxidant unit, forms a layer of amorphous protective film. This layer of SiTiOC nanolayer can effectively prevent oxygen from diffusing into the fiber interior and prevent SiC and TiC from being oxidized under high temperature conditions, thereby ensuring the long-term stability of the material under high temperature. In addition, the material exhibits a stable dielectric constant (including real and imaginary parts) over a wide temperature range, which is attributed to the interaction between SiC, TiC and SiTiOC, especially the introduction of TiC, which can maintain a higher conductivity under high temperature conditions, thereby enhancing the dielectric loss of the material. At the same time, SiC and TiC nanocrystals are evenly distributed in the fibers to form a stable conductive network, which gives the material good microwave loss capability over a wide temperature range.

[0006] Furthermore, the diameter of the nanofibers is 300 nanometers to 800 nanometers.

[0007] Furthermore, the thickness of the SiTiOC layer is 2-4 nanometers.

[0008] On the other hand, the present invention provides a method for preparing a nanofiber felt for wide temperature range microwave absorption, comprising the following steps: Step 1, dissolving polycarbosilane and titanyl acetate acetonate in tetrahydrofuran, and stirring to obtain a uniform first precursor solution; dissolving polyvinyl pyrrolidone in ethanol, and stirring to obtain a uniform second precursor solution; Step 2, slowly pouring the first precursor solution and the second precursor solution into a three-necked flask, and stirring with magnetic force to obtain a stable precursor spinning solution; Step 3, sucking the precursor spinning solution into a syringe, connecting the syringe to a needle, and placing the syringe into an electrospinning device after expelling bubbles; Step 4: After spinning is completed, the obtained precursor fiber is peeled off from the drum collector and placed in an oven for heat preservation to obtain heat-cured fiber; Step 5: placing the heat-cured fiber in a tubular furnace for high-temperature pyrolysis to convert polycarbosilane and titanyl acetate acetonate into SiC and TiC, and simultaneously forming a SiTiOC layer in situ on the fiber surface.

[0009] Furthermore, in step 3, the propulsion speed of electrospinning is 0.002 mm / s.

[0010] Furthermore, in step 3, the distance between the spinning needle head and the drum collector is 15 cm.

[0011] Furthermore, in step 3, the needle is a stainless steel needle, and the diameter of the needle is 0.9 mm.

[0012] Furthermore, in step 4, heating is performed from room temperature to 1100°C at a heating rate of 3°C / min; heating is continued from 1100°C to the set heat treatment temperature at a heating rate of 2°C / min, maintained at the set heat treatment temperature for 2 hours, then cooled to 200°C at a rate of 2°C / min, and finally naturally cooled to room temperature.

[0013] Furthermore, in step 4, the pyrolysis process is performed under an argon atmosphere. Furthermore, in step 4, the fiber thickness is greater than 0.7 mm and less than 0.9 mm. Beneficial effects of the present invention: (1) The nanofiber felt of the present invention maintains stable microwave absorption performance in a wide temperature range of 293K to 873K, with a minimum reflection loss of -45.55dB and an effective absorption bandwidth of 3.6GHz, which meets the application requirements under high temperature conditions.

[0014] (2) The SiTiOC amorphous film layer formed on the surface of the nanofibers effectively prevents the diffusion of oxygen into the interior of the fibers, enhances the material's antioxidant ability at high temperatures, and ensures that the material has good thermal stability and service life in a high-temperature environment.

[0015] (3) In the present invention, by adjusting the content of TiC, the impedance matching performance of the material can be optimized, so that electromagnetic waves can better enter the interior of the material, reduce reflection, and improve microwave absorption efficiency.

[0016] (4) The nanofiber felt of the present invention is prepared by electrospinning and high-temperature pyrolysis process, which is relatively simple and easy to scale up for production and is suitable for large-scale industrial applications.

[0017] Based on the above beneficial effects, the present invention has good application prospects in the field of microwave absorption technology. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1SEM images of SiC / C nanofiber mats and SiC / TiC / SiTiOC hybrid nanofiber mats with different TiC contents: (a) SiC / C, (b) SiC / TiC / SiTiOC-1, (c) SiC / TiC / SiTiOC-2, (d) SiC / TiC / SiTiOC-3, (e) SiC / TiC / SiTiOC-4; (fh) TEM images of SiC / TiC / SiTiOC-3 hybrid nanofiber mats; (ij) SAED and EDS spectra of single SiC / TiC / SiTiOC-3 hybrid nanofibers.

[0019] Figure 2 Microwave absorption properties of (a) SiC / C, (b) SiC / TiC / SiTiOC-1, (c) SiC / TiC / SiTiOC-2, (d) SiC / TiC / SiTiOC-3, and (e) SiC / TiC / SiTiOC-4; (f) Three-dimensional reflection loss curves of SiC / TiC / SiTiOC-3 at different temperatures; (g, h) Bar graphs of effective absorption bandwidth and minimum reflection loss of SiC / TiC / SiTiOC-3 at different temperatures (293K and 873K) (compared with SiC / C); (i) High-temperature oxidation resistance and thermal insulation properties of SiC / TiC / SiTiOC hybrid nanofiber felt.

[0020] Figure 3 (a) Real part of dielectric constant of SiC / C and SiC / TiC / SiTiOC nanofibers at different temperatures; (b) Imaginary part of dielectric constant of SiC / C and SiC / TiC / SiTiOC nanofibers at different temperatures; (c) Electrical conductivity of SiC / C and SiC / TiC / SiTiOC nanofibers; (d, e) Change rate of real and imaginary parts of dielectric constant of SiC / TiC / SiTiOC hybrid nanofibers and SiC / C nanofibers at different temperatures; (f, g) Dielectric loss tangent of SiC / C and SiC / TiC / SiTiOC-3 nanofibers at different temperatures; (h) Curve of the ratio of real part of dielectric constant to imaginary part of dielectric constant of SiC / C and SiC / TiC / SiTiOC-3 nanofibers; (i) Attenuation constant of SiC / C and SiC / TiC / SiTiOC-3 nanofibers at 873K.

[0021] Figure 4Cyclic stability of dielectric properties and electromagnetic wave absorption performance: (a, b) Real and imaginary parts of dielectric constants of SiC / C and SiC / TiC / SiTiOC-3 before and after high temperature testing; (c, d) Change rate of real and imaginary parts of dielectric constants of SiC / C and SiC / TiC / SiTiOC-3 after high temperature testing; (e) SEM images of SiC / C and SiC / TiC / SiTiOC-3 after high temperature testing; (f, g) Reflection loss of SiC / C and SiC / TiC / SiTiOC-3 before and after high temperature testing at room temperature; (h) Radar chart comparison of SiC / TiC / SiTiOC-3 and typical high temperature microwave absorbing materials in five dimensions: effective absorbing bandwidth, minimum reflection loss, thickness, temperature stability and temperature resistance.

[0022] Figure 5 (a) CST simulation model of radar cross section (RCS); (b) radiation pattern of perfect electric conductor (PEC); (c) PEC radiation pattern of SiC / C nanofiber felt; (d) PEC radiation pattern of SiC / TiC / SiTiOC-3 hybrid nanofiber felt; (e) Radar cross section values ​​of materials at different angles (873K); (f) Radar cross section reduction values ​​of SiC / C nanofiber felt and SiC / TiC / SiTiOC-3 hybrid nanofiber felt (873K). DETAILED DESCRIPTION

[0023] In order to make the objectives, technical solutions and advantages of the present application more clearly understood, the present application is further described in detail below with reference to the accompanying drawings and examples.

[0024] The present invention provides a method for preparing a nanofiber felt for wide temperature range microwave absorption, which mainly includes five steps. To clearly illustrate the present invention, the five steps are described as follows: Step 1: Prepare the first precursor solution and the second precursor solution. Specifically, weigh 1.2 g of polycarbosilane (PCS) and different masses of titanium acetonide (TiO(acac)2), dissolve them in 8 mL of tetrahydrofuran (THF), and stir for 120 minutes until the solution is uniform to obtain the first precursor solution; weigh 0.5 g of polyvinyl pyrrolidone (PVP), dissolve it in 5 mL of ethanol, and stir for 30 minutes until it is uniform to obtain the second precursor solution.

[0025] Step 2: Prepare a precursor spinning solution. Specifically, slowly pour the first precursor solution and the second precursor solution into a three-necked flask and stir them magnetically for 12 hours to obtain a stable precursor spinning solution.

[0026] Step 3, electrospinning. Specifically, the obtained precursor spinning solution is sucked into a 5mL medical syringe, connected to a stainless steel needle with a diameter of 0.9mm, and the bubbles are discharged; the syringe is placed in the electrospinning equipment, and the spinning parameters are set: the spinning propulsion speed is 0.002mm / s, the distance between the spinning needle and the roller collector is 15cm, and the voltage is 17KV; then electrospinning is performed, and after the spinning process is completed, the obtained precursor fiber is peeled off from the roller collector.

[0027] Step 4: Thermal curing: Specifically, the peeled precursor fiber is placed in an oven and kept at 200° C. for 2 hours to complete the thermal curing process and obtain thermally cured fibers.

[0028] Step 5, high temperature pyrolysis. The heat-cured fiber is placed in a tubular furnace for high temperature pyrolysis. The pyrolysis process is carried out under an argon atmosphere: heating from room temperature to 1100°C at a heating rate of 3°C / min; continuing to heat from 1100°C to the set heat treatment temperature (1300°C, 1400°C, 1500°C) at a heating rate of 2°C / min, and maintaining at the set heat treatment temperature for 2 hours; after the pyrolysis is completed, cool to 200°C at a rate of 2°C / min, and finally cool naturally to room temperature. PCS and TiO(acac)2 are converted into SiC and TiC, and a SiTiOC layer is formed on the fiber surface. The thickness of the nanofiber felt after pyrolysis is controlled between 0.7mm and 0.9mm to ensure good mechanical properties and microwave absorption properties.

[0029] Figure 1 (ae) show the SEM images of SiC / C nanofiber mat and SiC / TiC / SiTiOC hybrid nanofiber mat. Compared with the single-component SiC / C fiber, the diameter of the hybrid nanofiber gradually decreases with the increase of TiC content. The average diameter of the SiC / C nanofiber mat is about 800nm, accompanied by a small amount of micron-sized fibers. When the TiC content increases, the fiber diameter gradually decreases. The diameter of the SiC / TiC / SiTiOC-1 (the amount of TiO(acac)2 during preparation is 0.05g) sample is 700nm, and the fiber diameters of SiC / TiC / SiTiOC-2 (the amount of TiO(acac)2 during preparation is 0.15g), SiC / TiC / SiTiOC-3 (the amount of TiO(acac)2 during preparation is 0.3g), and SiC / TiC / SiTiOC-4 (the amount of TiO(acac)2 during preparation is 0.5g) are 480nm, 360nm, and 300nm, respectively. Figure 1(fh) shows the TEM images of SiC / TiC / SiTiOC-3 hybrid nanofiber mats. SiC and TiC nanocrystals are evenly distributed inside the nanofibers, providing more microwave reflection and scattering opportunities. Among them, the size of SiC crystals is about 15nm, while the size of TiC nanocrystals is slightly smaller, about 10nm. The fiber surface is wrapped with an amorphous SiTiOC anti-oxidation layer of about 3nm. This structure can effectively enhance the anti-oxidation performance and thermal stability of the fiber. Figure 1 (i) shows the SAED image of SiC / TiC / SiTiOC-3 hybrid nanofibers, confirming the coexistence of SiC and TiC phases. After pyrolysis, the TiO(acac)2 in the precursor is completely converted into TiC phase and is evenly distributed in the SiC nanofibers. Figure 1 (j) shows the EDS element mapping results of SiC / TiC / SiTiOC-3 hybrid nanofibers, indicating that only four elements, silicon, titanium, carbon and oxygen, exist in the sample, and these elements are evenly distributed in the fiber, proving the high purity of the sample. The XPS test analyzed the chemical bond state of each element in the sample and further verified the existence of SiC, TiC and SiTiOC. The Si 2p, Ti 2p and C 1s spectra reveal the existence of chemical bonds such as Si-OC, Ti-O, Si-O and Ti-C, indicating that an amorphous SiTiOC layer with antioxidant function is formed on the fiber surface.

[0030] Figure 2 (ae) shows the microwave absorption performance of different nanofiber materials. The minimum reflection loss of the single-component SiC / C nanofiber at room temperature (293K) is -20.34dB, but as the temperature rises to 873K, its absorption performance decreases significantly, and the minimum reflection loss decreases to -12.56dB. In contrast, the SiC / TiC / SiTiOC-3 hybrid nanofiber exhibits more stable microwave absorption ability in the entire test temperature range, and its absorption performance is significantly better than that of SiC / C materials. The minimum reflection loss is -48.53 dB at 293K and -45.55 dB at 873K. Figure 2 (g) shows the comparison of the effective absorption bandwidth of SiC / TiC / SiTiOC-3 and SiC / C. The effective absorption bandwidth of SiC / C is reduced from 2.4 GHz at room temperature to 1.04 GHz at 873K, a decrease of 1.36 GHz. In contrast, the effective absorption bandwidth of SiC / TiC / SiTiOC-3 at room temperature is 4.0 GHz, and it can still maintain 3.6 GHz at 873K, only a decrease of 0.4 GHz. This shows that the material has excellent absorption bandwidth stability under high temperature conditions. Figure 2(f) shows the three-dimensional reflection loss curve of SiC / TiC / SiTiOC-3 nanofibers at different temperatures. The reflection loss curve of the material changes little over the entire temperature range, indicating that it can maintain stable microwave absorption performance in a wide temperature range of 293K to 873K. This stable performance at high temperatures is mainly attributed to the multiple scattering of the material, the interface polarization effect, and the introduction of TiC, which together improve the loss capacity of electromagnetic waves. Figure 2 (i) Digital photo showing the anti-oxidation and thermal insulation properties of SiC / TiC / SiTiOC hybrid nanofiber felt at high temperature. The experiment shows that the material still maintains good structural stability at high temperature, with no obvious damage on the surface, showing excellent resistance to high temperature oxidation.

[0031] Figure 3 (a) and Figure 3 (b) shows the real and imaginary parts of the dielectric constants of SiC / C and SiC / TiC / SiTiOC nanofibers at different temperatures. The real and imaginary parts of the dielectric constants of SiC / C fluctuate greatly with increasing temperature, while the dielectric constants of SiC / TiC / SiTiOC nanofibers show higher stability, especially the SiC / TiC / SiTiOC-3 sample. With the increase of TiC content, the dielectric constant of SiC / TiC / SiTiOC materials increases, showing higher dielectric loss capacity, which is beneficial to enhance microwave absorption performance. Figure 3 In (c), the conductivity of SiC / TiC / SiTiOC hybrid nanofibers increases with the increase of TiC content. The conductivity of SiC / TiC / SiTiOC-4 sample is the highest, which is 721×10 -2 S / cm, while the conductivity of SiC / TiC / SiTiOC-2 and SiC / TiC / SiTiOC-3 are 424.5×10 -2 S / cm and 505 × 10 -2 However, too high conductivity may lead to impedance mismatch, thus reducing the microwave absorption performance, so SiC / TiC / SiTiOC-3 achieves a good balance between conductivity and microwave absorption performance. Figure 3 (d) and Figure 3 (e) shows the change rate of the real and imaginary parts of the dielectric constant of SiC / TiC / SiTiOC and SiC / C nanofibers at different temperatures. The dielectric constant of SiC / TiC / SiTiOC material changes less, especially the SiC / TiC / SiTiOC-3 sample shows better temperature stability. In contrast, the dielectric constant of SiC / C material changes more. Figure 3Figures (f) and (g) show the dielectric loss tangent values ​​of SiC / C and SiC / TiC / SiTiOC-3 nanofibers at different temperatures. E The values ​​are higher than those of SiC / C in the entire temperature range, which means that SiC / TiC / SiTiOC-3 has better energy loss capability, thus enhancing the microwave absorption performance. Figure 3 (h) shows the relationship between the ratio of the real part of the dielectric constant to the imaginary part of the dielectric constant of SiC / C and SiC / TiC / SiTiOC-3 nanofibers. The SiC / TiC / SiTiOC-3 sample shows a good linear relationship, which indicates that the interface polarization effect in the system is enhanced, which helps to improve the electromagnetic wave absorption performance. Figure 3 (i) The attenuation constants of SiC / TiC / SiTiOC-3 and SiC / C nanofibers at 873 K are shown. The attenuation constant of SiC / TiC / SiTiOC-3 is significantly higher than that of SiC / C, indicating that it has stronger microwave attenuation ability at high temperatures, which helps to improve the microwave absorption performance of the material in a wide temperature range.

[0032] Figure 4 (a) and Figure 4 (b) shows the changes in the real and imaginary parts of the dielectric constants of SiC / C and SiC / TiC / SiTiOC-3 before and after the high temperature test. The dielectric constant of the SiC / C material showed a significant decrease after the high temperature test, with the real part of the dielectric constant decreasing by about 20%, and the imaginary part of the dielectric constant decreasing by a greater margin, showing poor cycle stability. In contrast, the dielectric constant of the SiC / TiC / SiTiOC-3 material changed little before and after the high temperature test, indicating that it has good cycle stability at high temperatures. This is attributed to the introduction of the TiC and SiTiOC layers, which enhances the thermal stability and oxidation resistance of the material and maintains good dielectric properties. Figure 4 (c) and Figure 4 (d) shows the change rate of the real and imaginary parts of the dielectric constants of SiC / C and SiC / TiC / SiTiOC-3 materials after high temperature testing. The change rate of SiC / C material is relatively large, especially the change rate of the imaginary part of the dielectric constant exceeds 30%, indicating that it is difficult for this material to maintain stable dielectric properties under high temperature environment. The change rate of the dielectric constant of SiC / TiC / SiTiOC-3 material is relatively small, and the change rate of the imaginary part of the dielectric constant is only about 5%, further proving its excellent stability under high temperature environment. Figure 4(e) shows the scanning electron microscope images of SiC / C and SiC / TiC / SiTiOC-3 after high temperature testing. The SiC / C material showed obvious cracks and particle agglomeration on the surface after high temperature, indicating that its structure deteriorated at high temperature, resulting in performance degradation. On the contrary, the SiC / TiC / SiTiOC-3 material still maintained a uniform fiber structure after high temperature testing, with no obvious damage or agglomeration on the surface, proving that it has good structural stability at high temperatures. Figure 4 (f) and Figure 4 (g) shows the reflection loss curves of SiC / C and SiC / TiC / SiTiOC-3 at room temperature before and after high temperature testing. The minimum reflection loss of SiC / C material dropped from -20.34dB to -12.56 dB after high temperature testing, and the absorption performance was significantly reduced. However, SiC / TiC / SiTiOC-3 material still maintained high absorption performance after high temperature testing, and the minimum reflection loss only slightly dropped from -48.53dB to -45.55dB, indicating that the material still has excellent microwave absorption ability after high temperature cycling. Figure 4 (h) is a radar chart comparing SiC / TiC / SiTiOC-3 with other typical high-temperature microwave absorbing materials in five dimensions (effective absorption bandwidth, minimum reflection loss, thickness, temperature stability and temperature resistance). SiC / TiC / SiTiOC-3 performs well in terms of minimum reflection loss, temperature stability and temperature resistance, surpassing several other typical materials. Although its thickness is slightly higher than some other materials, its comprehensive performance far exceeds that of traditional high-temperature microwave absorbing materials, showing a highly competitive application prospect. The excellent cycle stability and microwave absorption performance of SiC / TiC / SiTiOC-3 nanofibers at high temperatures are mainly attributed to the following points: (1) The introduction of TiC enhances the electrical conductivity and interfacial polarization effect of the material, improves the microwave absorption capacity, and the high conductivity of TiC helps to maintain the stability of the dielectric properties at high temperatures; (2) The presence of the SiTiOC amorphous anti-oxidation layer makes the material less prone to oxidation or structural degradation in a high-temperature environment, ensuring its service life under high-temperature conditions; (3) The integrity of the fiber structure, especially after high-temperature testing, the SiC / TiC / SiTiOC-3 fibers still maintain good structural integrity, which helps to maintain their microwave absorption performance.

[0033] Figure 5 (a) shows the CST simulation model of radar cross section (RCS), which is used to evaluate the electromagnetic wave stealth capabilities of different materials in high temperature environments. The simulation model is based on a perfect electric conductor (PEC) substrate, covered with SiC / C and SiC / TiC / SiTiOC-3 nanofiber mats, respectively, to test their RCS performance under different temperature conditions. Figure 5(b) shows the radiation pattern of a bare perfect electric conductor (PEC). The radar scattering cross section of PEC is large, indicating that it strongly reflects electromagnetic waves. Figure 5 (c) shows the PEC pattern of the SiC / C nanofiber mat covered. Although it is improved compared with the bare PEC, the microwave absorption capacity of SiC / C nanofibers is limited, and the RCS reduction is small. Figure 5 (d) shows the PEC pattern of the SiC / TiC / SiTiOC-3 hybrid nanofiber mat. Compared with SiC / C nanofibers, SiC / TiC / SiTiOC-3 nanofibers exhibit significantly better microwave absorption performance and a significant reduction in RCS. Figure 5 (e) shows the radar cross-section values ​​of the materials at different angles, and the test temperature is 873K. The results show that the RCS value of SiC / TiC / SiTiOC-3 hybrid nanofibers is significantly lower than that of SiC / C nanofibers at most angles, showing better electromagnetic stealth effect. Especially in the angle range of 30° to 60°, the RCS reduction effect of SiC / TiC / SiTiOC-3 is most obvious, which is attributed to the multiple scattering and interface polarization effects of the material, which enhances the absorption capacity of electromagnetic waves. Figure 5 (f) shows the comparison of RCS reduction values ​​of SiC / C nanofiber mat and SiC / TiC / SiTiOC-3 hybrid nanofiber mat at 873K. The RCS reduction value of SiC / C nanofiber mat is relatively limited, while the RCS reduction value of SiC / TiC / SiTiOC-3 nanofiber mat is greatly improved. This further shows that the introduction of TiC and the protective effect of SiTiOC anti-oxidation layer not only improve the high temperature stability of the material, but also significantly improve its electromagnetic wave stealth performance. SiC / TiC / SiTiOC-3 nanofiber mat exhibits excellent radar cross section reduction effect at high temperature, which is mainly attributed to: (1) multiple scattering effect: the multiple scattering effect between TiC nanocrystals and SiC nanocrystals significantly enhances the absorption of electromagnetic waves; (2) interface polarization and reflection: the interface polarization effect between TiC and SiTiOC anti-oxidation layer enhances the loss of microwaves, thereby reducing the intensity of reflected waves; (3) high temperature stability: the SiTiOC layer not only improves the anti-oxidation performance of the material, but also ensures that the material still maintains good structural integrity and microwave absorption capacity at 873K.

[0034] On the basis of the above scheme, further, other metal oxide or carbide nanoparticles, such as ZnO, Fe3O4 or NiO, are added to SiC / TiC / SiTiOC nanofibers to enhance the multiple scattering and interface polarization effects inside the material. These nanoparticles have high dielectric constants or magnetic loss characteristics, which can further enhance the reflection, scattering and absorption of electromagnetic waves inside the material. In particular, magnetic materials (such as Fe3O4) can enhance the magnetic loss effect and improve the absorption bandwidth and strength of the composite material.

[0035] Furthermore, the SiC / TiC / SiTiOC nanofibers are surface functionalized, such as introducing polar functional groups on the fiber surface, or changing the fiber porosity by adjusting the electrospinning parameters, to enhance the interaction between the absorption material and the electromagnetic wave. Surface functionalization can enhance the polarization effect on the fiber surface, thereby increasing the loss of electromagnetic waves. By optimizing the porosity of the fiber, the propagation path of the electromagnetic wave inside the fiber can be increased, further enhancing the absorption effect of the material. In addition, the increase in porosity can also increase the surface area of ​​the fiber, thereby increasing the absorption interface.

[0036] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.

Claims

1. A nanofiber mat for wide temperature range microwave absorption, the nanofiber mat comprising nanofibers, characterized in that: The nanofiber consists of SiC and TiC nanocrystals and also includes a SiTiOC amorphous nanolayer, and the SiTiOC layer covers the nanofiber.

2. The nanofiber felt for wide temperature range microwave absorption according to claim 1, characterized in that: The diameter of the nanofiber is 300 nanometers to 800 nanometers.

3. The nanofiber felt for wide temperature range microwave absorption according to claim 3, characterized in that: The thickness of the SiTiOC layer is 2-4 nanometers.

4. A method for preparing a nanofiber felt for wide temperature range microwave absorption, characterized in that: The steps include: Step 1, dissolving polycarbosilane and titanyl acetate acetonate in tetrahydrofuran, and stirring to obtain a uniform first precursor solution; dissolving polyvinyl pyrrolidone in ethanol, and stirring to obtain a uniform second precursor solution; Step 2, slowly pouring the first precursor solution and the second precursor solution into a three-necked flask, and stirring with magnetic force to obtain a stable precursor spinning solution; Step 3, sucking the precursor spinning solution into a syringe, connecting the syringe to a needle, and placing the syringe into an electrospinning device after expelling bubbles; Step 4: After spinning is completed, the obtained precursor fiber is peeled off from the drum collector and placed in an oven for heat preservation to obtain heat-cured fiber; Step 5: placing the heat-cured fiber in a tubular furnace for high-temperature pyrolysis to convert polycarbosilane and titanyl acetate acetonate into SiC and TiC, and simultaneously forming a SiTiOC layer in situ on the fiber surface.

5. The method for preparing a nanofiber felt for wide temperature range microwave absorption according to claim 4, characterized in that: In step 3, the propulsion speed of electrospinning was 0.002 mm / s.

6. The method for preparing a nanofiber felt for wide temperature range microwave absorption according to claim 5, characterized in that: In step 3, the distance between the spinning needle and the drum collector was 15 cm.

7. The method for preparing a nanofiber felt for wide temperature range microwave absorption according to claim 6, characterized in that: In step 3, the needle is a stainless steel needle, and the diameter of the needle is 0.9 mm.

8. The method for preparing a nanofiber felt for wide temperature range microwave absorption according to claim 7, characterized in that: In step 4, heat from room temperature to 1100°C at a heating rate of 3°C / min; continue heating from 1100°C to the set heat treatment temperature at a heating rate of 2°C / min, maintain at the set heat treatment temperature for 2 hours, then cool to 200°C at a rate of 2°C / min, and finally cool naturally to room temperature.

9. The method for preparing a nanofiber felt for wide temperature range microwave absorption according to claim 8, characterized in that: In step 4, the pyrolysis process is carried out under an argon atmosphere.

10. The method for preparing a nanofiber felt for wide temperature range microwave absorption according to claim 9, characterized in that: In step 4, the fiber thickness is greater than 0.7 mm and less than 0.9 mm.

Citation Information

Patent Citations

  • Preparation method of TiO2 nanorod / SiC composite fiber felt

    CN103451852A

  • Electromagnetic wave absorbers of silicon carbide fibers

    US4726980A

Cited By

  • Preparation and application method of asymmetric electromagnetic shielding nanofiber film

    CN119711051A