Preparation method of ceramic reinforced polyimide fiber membrane
By adding ceramic powder to the polyimide solution and preparing ceramic reinforced polyimide fiber membranes by electrospinning technology, the problem of poor thermal stability of separators in the prior art is solved, and the mechanics of high-performance lithium-ion batteries are realized Performance improvement and process simplification reduce costs.
Patent Information
- Application Number
- CN202411275626.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing polyolefin-based separators have poor thermal stability and are difficult to meet the needs of high-performance lithium-ion batteries. The existing polyimide film preparation process is complex and costly.
The ceramic powder is added to the polyimide solution by electrospinning technology to prepare ceramic reinforced polyimide fiber membranes. The ceramic reinforced polyimide fiber membranes are obtained through heat treatment and rolling press to improve their thermal stability and mechanical strength.
It significantly improves the mechanical properties and heat resistance of the fiber membrane, reduces the preparation cost, simplifies the process flow, is suitable for industrial production, and improves the safety performance of lithium-ion batteries.
Smart Images

Figure CN119083042A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of battery separators, and in particular to a method for preparing a polyimide fiber membrane, which is suitable for energy storage devices such as lithium-ion batteries and supercapacitors. Background Art
[0002] With the widespread application of lithium-ion batteries, the performance requirements for battery separators are getting higher and higher. As an important component of the battery, the separator is not only required to have good ion conductivity, but also good thermal stability, mechanical strength and chemical stability. The polyolefin-based separators in the prior art have the disadvantage of poor thermal stability and are difficult to meet the needs of high-performance batteries.
[0003] Polyimide fiber has become an ideal diaphragm material due to its excellent thermal stability, mechanical strength and chemical inertness. However, the existing polyimide membrane preparation process often uses dianhydride and diamine powders to cast into films in polar solvents, spin / cast coating, and cast stretching processes, which have the disadvantages of being complex and costly. Therefore, a simple and efficient method for preparing polyimide fiber membranes is urgently needed. Summary of the invention
[0004] The technical problem to be solved by the present invention is to overcome the shortcomings of the prior art and provide a method for preparing a ceramic reinforced polyimide fiber membrane. Ceramic powder is added to a polyimide solution and a ceramic reinforced polyimide fiber membrane is prepared by an electrospinning process, thereby further improving the thermal stability and mechanical strength of the composite fiber membrane.
[0005] In order to solve the above technical problems, the technical solution proposed by the present invention is:
[0006] A method for preparing a ceramic reinforced polyimide fiber membrane, characterized in that the ceramic reinforced polyimide fiber is composited from minerals and polyimide fibers; the ceramic reinforced polyimide fiber has an average diameter of 200 to 500 nm; and the fiber membrane has a thickness of 20 to 400 μm.
[0007] The above method comprises the following steps:
[0008] (1) Preparation of ceramic reinforced polyimide fiber membrane: polyimide powder is dissolved in N,N-dimethylformamide and mixed evenly to form a polyimide solution, mineral powder is ultrasonically dispersed in the polyimide solution to form a mixed solution A, and then the mixed solution A is electrospun to form a precursor fiber membrane, and then the precursor fiber membrane is placed in a nitrogen or argon atmosphere for heat treatment, and the ceramic reinforced polyimide fiber membrane is obtained after rolling on a roller press.
[0009] In the above preparation method, preferably, in step (1), the number average molecular weight of the polyimide powder is 1000 g / mol to 100000 g / mol; the solid content of the polyimide solution is 8% to 25 wt%; and the viscosity is 1.3 dL / g to 3.5 dL / g.
[0010] In the above preparation method, preferably, in step (1), the selected ceramics are all mineral powders, one or more of mullite, kaolin, halloysite, attapulgite, and cordierite; and the content of the ceramics in the mixed solution A is 5% to 25wt%.
[0011] In the above-mentioned preparation method, preferably, in the step (1), during the electrospinning process, the diameter of the syringe pump nozzle is 0.3-1.2 mm, the flow rate of the mixed solution A is 0.4-1.2 mL / hour, the distance between the syringe pump nozzle and the collecting roller is 10-20 cm, and the voltage between the syringe pump nozzle and the collecting roller is 15-25 kV.
[0012] In the above preparation method, preferably, in step (1), the heat treatment temperature is 150 to 350° C., and the heat treatment time is 1 to 4 hours.
[0013] In the above-mentioned preparation method, preferably, in the step (1), the roller gap pressure of the roller press is 6.5 to 9.5 MPa.
[0014] Compared with the prior art, the advantages of the present invention are:
[0015] (1) The present invention uses electrospinning technology to prepare ceramic-reinforced polyimide fiber membranes; mineral ceramics have excellent physical and chemical properties and can significantly improve the mechanical properties of polyimide fiber membranes. At the same time, mineral ceramics can also improve the heat resistance and chemical corrosion resistance of the fiber membrane, and can significantly improve the safety performance of lithium-ion batteries.
[0016] The present invention directly adopts polyimide powder dissolved in N,N-dimethylformamide solution to form electrospinning spinning solution. Compared with the traditional process of preparing polyamic acid solution from dianhydride and diamine and then thermally imidizing it into fiber membrane, the preparation method is simple, easy to control, low in cost and good in repeatability, and the equipment used is conventional equipment, so it is convenient for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Table 1 is the comparative data of mechanical strength, Young's modulus and decomposition temperature in the comparative examples and embodiments of the present invention.
[0018] Figure 1 This is a scanning electron microscope photograph of the polyimide fiber prepared in the comparative example of the present invention.
[0019] Figure 2This is a scanning electron microscope photograph of the mullite reinforced polyimide fiber membrane prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0020] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.
[0021] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0022] Unless otherwise specified, all reagents and raw materials used in the present invention are commercially available products or products that can be prepared by known methods.
[0023] Comparative Example:
[0024] In order to reflect the advantages of the present invention, the comparative example did not use the ceramic minerals of the present invention to prepare the polyimide fiber membrane, and the average diameter of the polyimide fiber was 150 nm; the thickness of the fiber membrane was 25 μm.
[0025] The preparation method of the polyimide fiber membrane of this comparative example comprises the following steps:
[0026] (1) 2 g of polyimide powder (PI, number average molecular weight 20000 g / mol) was dissolved in 8 g of N,N-dimethylformamide to prepare a PI solution with a mass fraction of 20% and a viscosity of 2.16 dL / g.
[0027] (2) The PI solution was transferred to a syringe pump for high-voltage electrospinning, wherein the syringe pump nozzle diameter was 0.6 mm, the flow rate was 0.6 mL / h, the distance between the nozzle and the collecting roller was 15 cm, and the voltage between the nozzle and the collecting roller was 18 kV to obtain a fiber precursor.
[0028] (3) The fiber precursor is heat treated at 250° C. in a nitrogen atmosphere for 2 hours to obtain polyimide fibers.
[0029] (4) The polyimide fiber obtained in step (3) is rolled on a roller press to obtain a polyimide fiber membrane, and the roller gap pressure of the roller press is 9.5 MPa.
[0030] like Figure 1 The scanning electron microscope photo of the polyimide fiber membrane prepared in step (4) of the comparative example is a smooth continuous fiber. Table 1 shows that the tensile strength of the polyimide fiber membrane prepared in step (4) of the comparative example is 12.3 MPa, the Young's modulus is 1.05 GPa, and the thermal decomposition temperature is 372°C.
[0031] Embodiment 1:
[0032] The invention discloses a ceramic-reinforced polyimide fiber membrane, wherein the ceramic mineral is mullite powder, the average diameter of the mullite-reinforced polyimide fiber is 250nm, and the fiber membrane thickness is 25μm.
[0033] The method for preparing the ceramic reinforced polyimide fiber membrane of this embodiment comprises the following steps:
[0034] (1) 2 g of polyimide powder (PI, number average molecular weight 20000 g / moL) was dissolved in 8 g of N,N-dimethylformamide to prepare a PI solution with a mass fraction of 20%; the viscosity was 2.16 dL / g; 1 g of mullite was ultrasonically dispersed into the PI solution to obtain a mixed solution A; the content of mullite in the mixed solution A was 9.1%.
[0035] (2) The mixed solution A is transferred to a syringe pump for high-voltage electrospinning, wherein the diameter of the syringe pump nozzle is 0.6 mm, the flow rate of the mixed solution A is 0.6 mL / hour, the distance between the nozzle and the collecting roller is 15 cm, and the voltage between the nozzle and the collecting roller is 18 kV to obtain a fiber precursor.
[0036] (3) The fiber precursor was heat treated at 250° C. in a nitrogen atmosphere for 2 hours to obtain mullite-reinforced polyimide fibers.
[0037] (4) The mullite-reinforced polyimide fiber obtained in step (3) is rolled on a roller press to obtain a mullite-reinforced polyimide fiber membrane, and the roller gap pressure of the roller press is 8.5 MPa.
[0038] like Figure 2 The scanning electron microscope photo of the mullite reinforced polyimide fiber membrane prepared in step (4) of this embodiment is in the form of continuous fibers, and the mullite is uniformly dispersed in the fibers. Table 1 shows the tensile strength of the mullite reinforced polyimide fiber membrane prepared in step (4) of this embodiment, which is 162.7 MPa, the Young's modulus is 13.1 GPa, and the thermal decomposition temperature is 437°C.
[0039] Embodiment 2:
[0040] The invention discloses a ceramic-reinforced polyimide fiber membrane, wherein the ceramic mineral is kaolinite powder, the average diameter of the kaolinite-reinforced polyimide fiber is 300nm, and the fiber membrane thickness is 50μm.
[0041] The method for preparing the ceramic reinforced polyimide fiber membrane of this embodiment comprises the following steps:
[0042] (1) 1 g of polyimide powder (PI, number average molecular weight 60000 g / moL) was dissolved in 9 g of N,N-dimethylformamide to prepare a PI solution with a mass fraction of 10%; the viscosity was 2.52 dL / g; 1 g of kaolin was ultrasonically dispersed in the PI solution to obtain a mixed solution A, in which the content of kaolin in the mixed solution A was 9.1%.
[0043] (2) The mixed solution A is transferred to a syringe pump for high-voltage electrospinning, wherein the diameter of the syringe pump nozzle is 1 mm, the flow rate of the mixed solution A is 1 mL / hour, the distance between the nozzle and the collecting roller is 18 cm, and the voltage between the nozzle and the collecting roller is 23 kV to obtain a fiber precursor.
[0044] (3) The fiber precursor was heat treated at 300° C. in a nitrogen atmosphere for 4 hours to obtain kaolin-reinforced polyimide fibers.
[0045] (4) The mullite-reinforced polyimide fiber obtained in step (3) is rolled on a roller press to obtain a mullite-reinforced polyimide fiber membrane, and the roller gap pressure of the roller press is 8.5 MPa.
[0046] Table 1 shows that the kaolinite reinforced polyimide fiber membrane prepared in step (4) of this embodiment has a tensile strength of 57.5 MPa, a Young's modulus of 7.62 GPa, and a thermal decomposition temperature of 423°C.
[0047] Embodiment 3:
[0048] The invention discloses a ceramic-reinforced polyimide fiber membrane, wherein the ceramic mineral is halloysite powder, the average diameter of the halloysite-reinforced polyimide fiber is 400nm, and the fiber membrane thickness is 150μm.
[0049] The method for preparing the ceramic reinforced polyimide fiber membrane of this embodiment comprises the following steps:
[0050] (1) 2 g of polyimide powder (PI, number average molecular weight 1000 g / mol) was dissolved in 3 g of N,N-dimethylformamide to prepare a PI solution with a mass fraction of 20%; the viscosity was 1.37 dL / g. 1.5 g of halloysite was ultrasonically dispersed into the PI solution to obtain a mixed solution A, in which the content of halloysite in the mixed solution A was 23.07%.
[0051] (2) The mixed solution A is transferred to a syringe pump for high-voltage electrospinning, wherein the diameter of the syringe pump nozzle is 1.2 mm, the flow rate of the mixed solution A is 0.8 mL / hour, the distance between the nozzle and the collecting roller is 15 cm, and the voltage between the nozzle and the collecting roller is 25 kV to obtain a fiber precursor.
[0052] (3) The fiber precursor was heat treated at 350° C. in a nitrogen atmosphere for 1 hour to obtain halloysite-reinforced polyimide fiber.
[0053] (4) The halloysite-reinforced polyimide fiber obtained in step (3) is rolled on a roller press to obtain a halloysite-reinforced polyimide fiber membrane, and the roller gap pressure of the roller press is 7 MPa.
[0054] Table 1 shows that the tensile strength of the halloysite reinforced polyimide fiber membrane prepared in step (4) of this embodiment is 47.3 MPa, the Young's modulus is 7.81 GPa, and the thermal decomposition temperature is 448°C.
[0055] Embodiment 4:
[0056] The invention discloses a ceramic-reinforced polyimide fiber membrane, wherein the ceramic mineral is attapulgite powder, and the average diameter of the attapulgite powder-reinforced polyimide fiber is 300nm; and the fiber membrane thickness is 300μm.
[0057] The method for preparing the ceramic reinforced polyimide fiber membrane of this embodiment comprises the following steps:
[0058] (1) 3 g of polyimide powder (PI, number average molecular weight 80,000 g / moL) was dissolved in 13.67 g of N,N-dimethylformamide to prepare a PI solution with a mass fraction of 18%; the viscosity was 3.42 dL / g; 2.5 g of attapulgite was ultrasonically dispersed into the PI solution to obtain a mixed solution A, in which the content of attapulgite in the mixed solution A was 13.04%.
[0059] (2) The mixed solution A is transferred to a syringe pump for high-voltage electrospinning, wherein the diameter of the syringe pump nozzle is 1 mm, the flow rate of the mixed solution A is 1 mL / hour, the distance between the nozzle and the collecting roller is 18 cm, and the voltage between the nozzle and the collecting roller is 18 kV to obtain a fiber precursor.
[0060] (3) The fiber precursor was heat treated at 250° C. in a nitrogen atmosphere for 3 hours to obtain attapulgite-reinforced polyimide fibers.
[0061] (4) The attapulgite-reinforced polyimide fiber obtained in step (3) is rolled on a roller press to obtain an attapulgite-reinforced polyimide fiber film, and the roller gap pressure of the roller press is 9.2 MPa.
[0062] Table 1 shows that the tensile strength of the attapulgite reinforced polyimide fiber membrane prepared in step (4) of this embodiment is 70.6 MPa, the Young's modulus is 9.23 GPa, and the thermal decomposition temperature is 420°C.
[0063] Embodiment 5:
[0064] The invention discloses a ceramic-reinforced polyimide fiber membrane, wherein the ceramic mineral is cordierite powder, and the average diameter of the cordierite powder-reinforced polyimide fiber is 500nm; and the fiber membrane thickness is 400μm.
[0065] The method for preparing the ceramic reinforced polyimide fiber membrane of this embodiment comprises the following steps:
[0066] (1) 1.5 g of polyimide powder (PI, number average molecular weight 60000 g / moL) was dissolved in 8.5 g of N,N-dimethylformamide to prepare a PI solution with a mass fraction of 15%; the viscosity was 2.81 dL / g; 3 g of cordierite powder was ultrasonically dispersed in the PI solution to obtain a mixed solution A, in which the content of cordierite powder in the mixed solution A was 23.07%.
[0067] (2) The mixed solution A is transferred to a syringe pump for high-voltage electrospinning, wherein the diameter of the syringe pump nozzle is 1.2 mm, the flow rate of the mixed solution A is 0.9 mL / hour, the distance between the nozzle and the collecting roller is 20 cm, and the voltage between the nozzle and the collecting roller is 20 kV to obtain a fiber precursor.
[0068] (3) The fiber precursor is placed in a nitrogen atmosphere at 300° C. for 2 hours to obtain cordierite powder reinforced polyimide fiber.
[0069] (4) The cordierite-reinforced polyimide fiber obtained in step (3) is rolled on a roller press to obtain a cordierite-reinforced polyimide fiber membrane, and the roller gap pressure of the roller press is 6.5 MPa.
[0070] Table 1 shows that the tensile strength of the attapulgite reinforced polyimide fiber membrane prepared in step (4) of this embodiment is 112.6 MPa, the Young's modulus is 12.62 GPa, and the thermal decomposition temperature is 446°C.
[0071] Embodiment 6:
[0072] The invention discloses a ceramic-reinforced polyimide fiber membrane, wherein the ceramic minerals are mullite powder, kaolinite powder and cordierite powder, and the ceramic-reinforced polyimide fiber has an average diameter of 350 nm; and the fiber membrane has a thickness of 70 μm.
[0073] The method for preparing the ceramic reinforced polyimide fiber membrane of this embodiment comprises the following steps:
[0074] (1) 0.5 g of polyimide powder (PI, number average molecular weight 100000 g / moL) was dissolved in 7.5 g of N,N-dimethylformamide to prepare a PI solution with a mass fraction of 12.5%; the viscosity was 3.17 dL / g; 0.5 g of mullite powder, 0.25 g of kaolinite powder and 0.5 g of cordierite powder were ultrasonically dispersed into the PI solution to obtain a mixed solution A, in which the content of ceramic powder in the mixed solution A was 13.51%.
[0075] (2) The mixed solution A is transferred to a syringe pump for high-voltage electrospinning, wherein the diameter of the syringe pump nozzle is 0.8 mm, the flow rate of the mixed solution A is 1.2 mL / hour, the distance between the nozzle and the collecting roller is 18 cm, and the voltage between the nozzle and the collecting roller is 17 kV to obtain a fiber precursor.
[0076] (3) The fiber precursor is placed in a nitrogen atmosphere at 300° C. for 2 hours to obtain a mixed ceramic powder reinforced polyimide fiber.
[0077] (4) The mixed ceramic reinforced polyimide fiber obtained in step (3) is rolled on a roller press to obtain a mixed ceramic reinforced polyimide fiber membrane, and the roller gap pressure of the roller press is 9 MPa.
[0078] Table 1 shows that the tensile strength of the hybrid reinforced polyimide fiber membrane prepared in step (4) of this embodiment is 183.2 MPa, the Young's modulus is 13.52 GPa, and the thermal decomposition temperature is 431°C.
[0079] The above analysis and results prove that the ceramic-reinforced polyimide fiber membrane of the present invention can effectively improve the mechanical properties and thermal stability of polyimide fibers.
[0080] Table 1 Mechanical strength, Young's modulus and decomposition temperature in comparative examples and embodiments
[0081]
Claims
1. A method for preparing a ceramic reinforced polyimide fiber membrane, characterized in that: The ceramic reinforced polyimide fiber is composited with minerals and polyimide fibers; the average diameter of the ceramic reinforced polyimide fiber is 200-500nm; and the thickness of the fiber membrane is 20-400μm. (1) Dissolving polyimide powder in N,N-dimethylformamide and mixing evenly to form a polyimide solution, ultrasonically dispersing mineral powder in the polyimide solution to form a mixed solution A, and then electrospinning the mixed solution A to form a precursor fiber membrane, and then placing the precursor fiber membrane in a nitrogen or argon atmosphere for heat treatment, and after a roller press, the ceramic reinforced polyimide fiber membrane is obtained.
2. The preparation method according to claim 1, characterized in that In the step (1), the number average molecular weight of the polyimide powder is 1000 g / mol to 100000 g / mol; the solid content of the polyimide solution is 3% to 25 wt%; and the viscosity is 1.3 dL / g to 3.5 dL / g.
3. The preparation method according to claim 1, characterized in that: In the step (1), the selected ceramics are all mineral powders, one or more of mullite, kaolin, halloysite, attapulgite, and cordierite; the content of the ceramics in the mixed solution A is 5% to 25wt%.
4. The preparation method according to claim 1, characterized in that: In the step (1), during the electrospinning process, the diameter of the syringe pump nozzle is 0.3-1.2 mm, the flow rate of the mixed solution A is 0.4-1.2 mL / hour, the distance between the syringe pump nozzle and the collecting roller is 10-20 cm, and the voltage between the syringe pump nozzle and the collecting roller is 15-25 kV.
5. The preparation method according to any one of claims 1 to 4, characterized in that: In the step (1), the heat treatment temperature is 150 to 350° C., and the heat treatment time is 1 to 4 hours.
6. The preparation method according to any one of claims 1 to 5, characterized in that: In the step (1), the roller gap pressure of the roller press is 6.5 to 9.5 MPa.