Preparation method of anticoagulant coating on surface of polyester fiber fabric

By undergoing aldehyde modification of heparin and copolymerization with aminomalonitrile p-toluenesulfonate, combined with oscillation reaction and introduction of zinc sulfate, an anticoagulation coating on the surface of polyester fiber fabric was constructed, and the prior art was solved The problems of limited effects and short lifespan of anticoagulant coatings have achieved effective inhibition of thrombosis and improved antibacterial effects.

CN119083178AActive Publication Date: 2024-12-06ZHEJIANG SCI-TECH UNIV +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411004393.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-12-06
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

The existing anticoagulation coating technology has problems such as limited mechanism of action, inability to effectively prevent plasma protein adsorption and coagulation reaction, and short life of antithrombotic materials in long-term applications, making it difficult to play a role in both hemocompatibility and coagulation processes.

Method used

By undergoing aldehyde modification on heparin, it is given the ability to copolymerize with aminomalonitrile p-toluenesulfonate, and is mixed with aminomalonitrile p-toluenesulfonate under alkaline conditions and deposited on polyester by oscillation reaction The fiber fabric surface is constructed with anticoagulant coating and zinc sulfate is introduced in the secondary oscillation reaction to enhance antibacterial ability.

Benefits of technology

It has expanded the application field of anticoagulant coatings, significantly reduced thrombosis, enhanced antibacterial and anti-infection ability, promoted the secretion of vascular endothelial growth factors, and extended the effectiveness of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119083178A_ABST
    Figure CN119083178A_ABST
Patent Text Reader

Abstract

The invention relates to the field of coatings, and discloses a preparation method of a polyester fiber fabric surface anticoagulant coating, which comprises the following steps: S1, modifying heparin to introduce aldehyde group to obtain heparin with aldehyde group; s2, dissolving aminomalononitrile tosilate and heparin with an aldehyde group in a tris (hydroxymethyl) methyl aminomethane hydrochloride buffer solution, and mixing to obtain an anticoagulant coating solution; s3, immersing the polyester fiber fabric into the anticoagulant coating solution, taking out the polyester fiber fabric after oscillation incubation, cleaning and drying to obtain the polyester fiber fabric with the anticoagulant coating uniformly deposited on the surface. The preparation method comprises the following steps: firstly, carrying out formylation modification on heparin to endow heparin with the capability of copolymerizing with aminomalononitrile tosilate, then mixing heparin with aminomalononitrile tosilate under an alkaline condition, and depositing on the surface of a polyester fiber fabric through an oscillating reaction to prepare the anticoagulant coating.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of coatings, and in particular to a method for preparing an anti-coagulation coating on the surface of a polyester fiber fabric. Background Art

[0002] Factors such as the aging population, changes in social lifestyles, and environmental pollution have led to an increasing incidence of chronic diseases in humans. The treatment of many diseases such as heart disease, diabetes, and arthritis requires the use of implanted or invasive devices. Medical devices that are in long-term contact with blood will stimulate the host's immune defense mechanism, thereby causing thrombosis. When the device comes into contact with blood, the proteins in the blood (albumin, fibrinogen, etc.) will quickly adsorb to the surface of the material, and platelets will adhere and aggregate on the surface of the protein membrane, leading to the activation of coagulation factors, thereby producing thrombin. Thrombin combines with macromolecules such as fibrinogen and platelets, causing blood cells to adhere to the blood vessel wall, and eventually forming a thrombus.

[0003] In order to improve the blood compatibility of materials and reduce the risk of thrombosis, researchers have developed a variety of anticoagulant coating technologies. These technologies include bioinert surfaces, release of antithrombotic compounds, and the construction of fixed anticoagulant coatings. Although these technologies have certain prospects in clinical applications of blood compatibility, there are still some disadvantages that limit their long-term application. The disadvantages of fixed anticoagulants include their limited mechanism of action, and their disruption of the coagulation cascade does not prevent the adsorption of plasma proteins, which may bind to anticoagulants to promote coagulation reactions. Although the construction of bioinert surfaces can reduce the adhesion of blood components, it cannot inhibit the coagulation process and the anticoagulant effect is very limited. In addition, the life of antithrombotic release materials is limited to their load capacity and is easily exhausted by burst release.

[0004] Therefore, we constructed an aminomalononitrile / heparin / zinc composite coating, in which heparin can resist thrombosis, zinc ions can resist bacteria, increase the secretion of vascular endothelial growth factor, and promote angiogenesis. This composite coating can play a role in different stages of the coagulation process, reducing thrombosis by combining the fixation of anticoagulants and promoting the construction of a cell growth surface. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a method for preparing an anti-coagulation coating on the surface of a polyester fiber fabric. The present invention first performs aldehyde modification on heparin to give it the ability to copolymerize with aminomalononitrile p-toluenesulfonate, then mixes it with aminomalononitrile p-toluenesulfonate under alkaline conditions, and oscillates and reacts to deposit on the surface of the polyester fiber fabric to prepare an anti-coagulation coating, which greatly expands the application field.

[0006] The specific technical solution of the present invention is: a method for preparing an anti-coagulation coating on the surface of a polyester fiber fabric, comprising the following steps:

[0007] S1: Modifying heparin to introduce an aldehyde group to obtain heparin with an aldehyde group.

[0008] S2: dissolving aminomalononitrile p-toluenesulfonate and aldehyde heparin in a tris(hydroxymethyl)aminomethane hydrochloride buffer solution at pH=8.0-8.8, and adjusting the pH of the system to 8-9 with alkali to obtain an anticoagulant coating solution.

[0009] Wherein, the concentration of aminomalononitrile p-toluenesulfonate in the anticoagulant coating solution is 10-50 g / mL, and the concentration of aldehyde heparin is 0.5-2 mg / mL;

[0010] S3: immersing the polyester fiber fabric in the anticoagulant coating solution, taking it out after shaking and incubating, washing and removing the residual unpolymerized precipitate or its derivatives on the surface of the polyester fiber fabric, and drying to obtain the polyester fiber fabric with the anticoagulant coating uniformly deposited on the surface.

[0011] Heparin has an anticoagulant function, so if it is introduced into a coating of aminomalononitrile self-polymerization, the coating can be endowed with an anticoagulant effect. However, the heparin molecule itself does not have a group that can polymerize with aminomalononitrile. Therefore, in S1, the present invention first performs aldehyde modification on heparin, and introduces heparin into the coating through a Schiff base reaction between an aldehyde group and an amino group.

[0012] The modification of heparin by the present invention not only can endow it with the ability to copolymerize with aminomalononitrile p-toluenesulfonate, but the modification process will not destroy the functional active structure of heparin, so that the original activity can be almost maintained.

[0013] In S2, heparin with an aldehyde group is mixed with aminomalononitrile p-toluenesulfonate under alkaline conditions to obtain an anticoagulant coating solution; in S3, a dipping + oscillation incubation method is used to copolymerize on the surface of a polyester fiber fabric to construct a coating with anticoagulant function.

[0014] Preferably, in S1, the method for modifying the heparin with aldehyde groups is as follows: dissolving 10-20 mg / mL heparin in water, adjusting the pH to 1.5-3, adding 0.4-0.8 mg / mL sodium nitrite to lyse the heparin at 1-10°C for 2-4 hours; adjusting the pH to 6.0-7.0 with alkali to terminate the reaction; dialyzing in NH4HCO3 solution to obtain a heparin solution with aldehyde groups, and freeze-drying it for later use.

[0015] The principle of the above modification is to produce heparin oligomers with active aldehyde groups by nitric acid depolymerization. Heparin is composed of disaccharides containing L-iduronic acid and d-glucosamine residues. However, there is heterogeneity throughout the heparin polymer because the disaccharides are subjected to various chemical modifications to produce a series of residues. These sites are sensitive to nitrous acid at room temperature and low pH (1.5-3). When heparin is treated with nitrous acid, heparin is depolymerized by nitrous acid (HNO2) and heparin aldehyde is formed at the terminal position of the oligomer.

[0016] Preferably, in S3, the shaking incubation temperature is 20-30°C and the time is 8-12h.

[0017] Preferably, the method further comprises S4: immersing the polyester fiber fabric with the anticoagulant coating uniformly deposited on the surface obtained in S3 into an antibacterial modification liquid containing zinc sulfate, performing a secondary oscillation reaction, and obtaining a secondary modified anticoagulant coating after ultrasonic cleaning and drying; the number of amino groups in the aminomalononitrile toluenesulfonate is in excess compared to the aldehyde groups in the aldehyde heparin.

[0018] In order to further impart antibacterial function to the anticoagulant coating, antibacterial elements can be introduced into the anticoagulant coating by the method of immersion + oscillation reaction (the amino group in aminomalononitrile p-toluenesulfonate can chelate with the metal by coordination). In addition, in order to ensure that there are still redundant active groups in the anticoagulant coating that can react with zinc sulfate, it is necessary to control the amino group on aminomalononitrile p-toluenesulfonate in S2 to be excessive compared to the aldehyde group in the heparin with aldehyde group, and the preferred molar ratio of amino group to aldehyde group is (30-200):1.

[0019] More preferably, the temperature of the secondary oscillation reaction is 20-30° C. and the time is 12-24 h.

[0020] Further preferably, the total concentration of zinc sulfate in the antibacterial modified liquid is 60-80 μM.

[0021] Preferably, in S3, the cleaning is ultrasonic cleaning: ultrasonic cleaning is performed using deionized water for at least 15 minutes, with an ultrasonic frequency of 20-35 kHz and a power of 100-150 W. This step is used to remove polymers with weak bonding strength on the surface of the material.

[0022] Compared with the prior art, the beneficial effects of the present invention are:

[0023] (1) The present invention first performs aldehyde modification on heparin to give it the ability to copolymerize with aminomalononitrile p-toluenesulfonate, then mixes it with aminomalononitrile p-toluenesulfonate under alkaline conditions, and deposits it on the surface of polyester fiber fabric through an oscillating reaction, thereby obtaining a polyester fiber fabric with anti-coagulation function, which can greatly expand its application field.

[0024] (2) The present invention further combines zinc ions on the surface of the anticoagulant coating, which can further endow the anticoagulant coating with antibacterial and anti-infection capabilities, increase the secretion of vascular endothelial growth factor, and promote angiogenesis. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a scanning electron microscope image of polyester fiber fabric;

[0026] Figure 2 This is a scanning electron microscope image of the polyaminomalononitrile coating deposited on the polyester fiber fabric in Example 1;

[0027] Figure 3 This is a scanning electron microscope image of the anti-coagulation coating of the polyester fiber fabric in Example 2;

[0028] Figure 4 This is a test chart of the anticoagulant performance of polyester fiber fabric;

[0029] Figure 5 This is a photo of the antibacterial zone of polyester fabric; DETAILED DESCRIPTION

[0030] The present invention will be further described below in conjunction with the embodiments.

[0031] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0032] Hereinafter, examples are given to illustrate the specific embodiments of the present invention, but the embodiments of the present invention are not limited by the following examples, and any selection and change can be made within the scope that does not affect the technical effects to be achieved by the present invention. If no specific conditions are specified in the embodiments and test examples, the conventional conditions or the conditions recommended by the manufacturer are followed, and the reagents or instruments used without indicating the manufacturer are all conventional products that can be obtained commercially.

[0033] Example 1

[0034] A method for preparing a polyaminomalononitrile coating on a polyester fiber fabric comprises the following steps:

[0035] Step 1: Prepare buffer: prepare Tris buffer with a pH of 8.5 and a concentration of 0.1 M.

[0036] Step 2: Pretreatment of polyester fiber fabric: The prepared polyester fiber fabric (PET, 20D / 12F) was treated with acetone, anhydrous ethanol, and ultrasound for 3 times, each time for 30 minutes; then ultrasonically cleaned with deionized water for 3 times, each time for 20 minutes; the ultrasonic frequency was 35kHz and the power was 150W; during the treatment, the temperature of the mixed solution was kept at 25°C by ice water bath. Finally, the polyester fiber fabric was placed in normal pressure ventilation conditions at 65°C for 4 hours.

[0037] Step 3: Prepare polyaminomalononitrile coating: add 1g of aminomalononitrile p-toluenesulfonate to Tris buffer solution (50ml, pH=8.5) to prepare an AMN solution with a concentration of 20mg / mL; after sufficient dissolution, use 2M sodium hydroxide to adjust the pH of the aminomalononitrile solution to 8.5; immerse the cleaned polyester fiber fabric in the aminomalononitrile solution, place it in a water bath constant temperature oscillator for deposition for 10h, take it out after the deposition is completed, and ultrasonically clean it with deionized water for 50min (ultrasonic frequency is 35kHz, power is 150W), and dry it for use.

[0038] Figure 2 This is a scanning electron microscope image of the polyaminomalononitrile coating deposited on polyester fiber fabric.

[0039] Example 2

[0040] Step 1: Prepare buffer: prepare Tris buffer with a pH of 8.5 and a concentration of 0.1 M.

[0041] Step 2: Pretreatment of polyester fiber fabric: The prepared polyester fiber fabric (PET, 20D / 12F) was treated with acetone, anhydrous ethanol, and ultrasound for 3 times, each time for 30 minutes; then ultrasonically cleaned with deionized water for 3 times, each time for 20 minutes; the ultrasonic frequency was 35kHz and the power was 150W; during the treatment, the temperature of the mixed solution was kept at 25°C by ice water bath. Finally, the polyester fiber fabric was placed in normal pressure ventilation conditions at 65°C for 4 hours.

[0042] Step 3: Preparation of aldehyde heparin: Dissolve heparin in deionized water at 15 mg / mL and add glacial acetic acid to the solution to adjust the pH to 3. Then add 0.6 mg / ml sodium nitrite to the solution to lyse the heparin at 5°C for 3 h. Then adjust the pH of the solution to 6.5 with sodium hydroxide to terminate the reaction. Dialyze in 0.15 mol / L NH4HCO3 solution to obtain a pure aldehyde heparin (Hep-CHO) solution, which is freeze-dried for later use.

[0043] Step 4: Preparation of anticoagulant coating: Add 1g of aminomalononitrile p-toluenesulfonate and 50mg of aldehyde heparin to a Tris buffer solution (50mL, pH=8.5), the final concentrations of aminomalononitrile p-toluenesulfonate and aldehyde heparin are 20mg / mL and 1mg / mL respectively, and after the two are evenly mixed, the pH is adjusted to 8.5 using 2M sodium hydroxide. Then, the cleaned polyester fiber fabric is immersed in the impregnation solution, placed in a 25°C water bath constant temperature oscillator for reaction for 10h, and then ultrasonically cleaned with deionized water for 60min (ultrasonic frequency is 35kHz, power is 150W), and then taken out and dried for use.

[0044] Example 3

[0045] Step 1: Prepare buffer: prepare Tris buffer with a pH of 8.5 and a concentration of 0.1 M.

[0046] Step 2: Pretreatment of polyester fiber fabric: The prepared polyester fiber fabric (PET, 20D / 12F) was treated with acetone, anhydrous ethanol, and ultrasound for 3 times, each time for 30 minutes; then ultrasonically cleaned with deionized water for 3 times, each time for 20 minutes; the ultrasonic frequency was 35kHz and the power was 150W; during the treatment, the temperature of the mixed solution was kept at 25°C by ice water bath. Finally, the polyester fiber fabric was placed in normal pressure ventilation conditions at 65°C for 4 hours.

[0047] Step 3: Preparation of aldehyde heparin: Dissolve heparin in deionized water at 15 mg / mL and add glacial acetic acid to the solution to adjust the pH to 3. Then add 0.6 mg / ml sodium nitrite to the solution to lyse the heparin at 5°C for 3 h. Then adjust the pH of the solution to 6.5 with sodium hydroxide to terminate the reaction. Dialyze in 0.15 mol / L NH4HCO3 solution to obtain a pure aldehyde heparin (Hep-CHO) solution, which is freeze-dried for later use.

[0048] Step 4: Preparation of anticoagulant coating: Add 1g of aminomalononitrile p-toluenesulfonate and 50mg of aldehyde heparin to a Tris buffer solution (50mL, pH=8.5), the final concentrations of aminomalononitrile p-toluenesulfonate and aldehyde heparin are 20mg / mL and 1mg / mL respectively, and after the two are evenly mixed, the pH is adjusted to 8.5 using 2M sodium hydroxide. Then, the cleaned polyester fiber fabric is immersed in the impregnation solution, placed in a 25°C water bath constant temperature oscillator for reaction for 10h, and then ultrasonically cleaned with deionized water for 60min (ultrasonic frequency is 35kHz, power is 150W), and then taken out and dried for use.

[0049] Step 5: Preparation of antibacterial and anticoagulant coating: First, prepare a 70 μM zinc sulfate solution in dark conditions, then immerse the polyester fiber fabric with the anticoagulant coating in zinc sulfate and incubate for 24 hours. After obtaining the antibacterial and anticoagulant coating, use deionized water to ultrasonically clean and dry it for use.

[0050] Example 4

[0051] Step 1: Prepare buffer: prepare Tris buffer with a pH of 8.5 and a concentration of 0.1 M.

[0052] Step 2: Pretreatment of polyester fiber fabric: The prepared polyester fiber fabric (PET, 20D / 12F) was treated with acetone, anhydrous ethanol, and ultrasound for 3 times, each time for 30 minutes; then ultrasonically cleaned with deionized water for 3 times, each time for 20 minutes; the ultrasonic frequency was 35kHz and the power was 150W; during the treatment, the temperature of the mixed solution was kept at 25°C by ice water bath. Finally, the polyester fiber fabric was placed in normal pressure ventilation conditions at 65°C for 4 hours.

[0053] Step 3: Preparation of aldehyde heparin: Dissolve heparin in deionized water at 15 mg / mL and add glacial acetic acid to the solution to adjust the pH to 3. Then add 0.6 mg / ml sodium nitrite to the solution to lyse the heparin at 5°C for 3 h. Then adjust the pH of the solution to 6.5 with sodium hydroxide to terminate the reaction. Dialyze in 0.15 mol / L NH4HCO3 solution to obtain a pure aldehyde heparin (Hep-CHO) solution, which is freeze-dried for later use.

[0054] Step 4: Preparation of anticoagulant coating: Add 1g of aminomalononitrile p-toluenesulfonate and 100mg of aldehyde heparin to a Tris buffer solution (50mL, pH=8.5), the final concentrations of aminomalononitrile p-toluenesulfonate and aldehyde heparin are 20mg / mL and 2mg / mL respectively, and the two are mixed evenly and the pH is adjusted to 8.5 using 2M sodium hydroxide. Then, the cleaned polyester fiber fabric is immersed in the impregnation solution, placed in a 25°C water bath constant temperature oscillator for reaction for 10h, and then ultrasonically cleaned with deionized water for 60min (ultrasonic frequency is 35kHz, power is 150W), and then taken out and dried for use.

[0055] Step 5: Preparation of antibacterial and anticoagulant coating: First, prepare a 70 μM zinc sulfate solution in dark conditions, then immerse the polyester fiber fabric with the anticoagulant coating in zinc sulfate and incubate for 24 hours. After obtaining the antibacterial and anticoagulant coating, use deionized water to ultrasonically clean and dry it for use.

[0056] Example 5

[0057] Step 1: Prepare buffer: prepare Tris buffer with a pH of 8.5 and a concentration of 0.1 M.

[0058] Step 2: Pretreatment of polyester fiber fabric: The prepared polyester fiber fabric (PET, 20D / 12F) was treated with acetone, anhydrous ethanol, and ultrasound for 3 times, each time for 30 minutes; then ultrasonically cleaned with deionized water for 3 times, each time for 20 minutes; the ultrasonic frequency was 35kHz and the power was 150W; during the treatment, the temperature of the mixed solution was kept at 25°C by ice water bath. Finally, the polyester fiber fabric was placed in normal pressure ventilation conditions at 65°C for 4 hours.

[0059] Step 3: Preparation of aldehyde heparin: Dissolve heparin in deionized water at 15 mg / mL and add glacial acetic acid to the solution to adjust the pH to 3. Then add 0.6 mg / ml sodium nitrite to the solution to lyse the heparin at 5°C for 3 h. Then adjust the pH of the solution to 6.5 with sodium hydroxide to terminate the reaction. Dialyze in 0.15 mol / L NH4HCO3 solution to obtain a pure aldehyde heparin (Hep-CHO) solution, which is freeze-dried for later use.

[0060] Step 4: Preparation of anticoagulant coating: Add 2g of aminomalononitrile p-toluenesulfonate and 100mg of aldehyde heparin to a Tris buffer solution (50mL, pH=8.5), the final concentrations of aminomalononitrile p-toluenesulfonate and aldehyde heparin are 40mg / mL and 2mg / mL respectively, and the two are mixed evenly and the pH is adjusted to 8.5 using 2M sodium hydroxide. Then, the cleaned polyester fiber fabric is immersed in the impregnation solution, placed in a 25°C water bath constant temperature oscillator for reaction for 10h, and then ultrasonically cleaned with deionized water for 60min (ultrasonic frequency is 35kHz, power is 150W), and then taken out and dried for use.

[0061] Step 5: Preparation of antibacterial and anticoagulant coating: First, prepare a 70 μM zinc sulfate solution in dark conditions, then immerse the polyester fiber fabric with the anticoagulant coating in zinc sulfate and incubate for 24 hours. After obtaining the antibacterial and anticoagulant coating, use deionized water to ultrasonically clean and dry it for use.

[0062] Example 6

[0063] Step 1: Prepare buffer: prepare Tris buffer with a pH of 8.5 and a concentration of 0.1 M.

[0064] Step 2: Pretreatment of polyester fiber fabric: The prepared polyester fiber fabric (PET, 20D / 12F) was treated with acetone, anhydrous ethanol, and ultrasound for 3 times, each time for 30 minutes; then ultrasonically cleaned with deionized water for 3 times, each time for 20 minutes; the ultrasonic frequency was 35kHz and the power was 150W; during the treatment, the temperature of the mixed solution was kept at 25°C by ice water bath. Finally, the polyester fiber fabric was placed in normal pressure ventilation conditions at 65°C for 4 hours.

[0065] Step 3: Preparation of aldehyde heparin: Dissolve heparin in deionized water at 15 mg / mL and add glacial acetic acid to the solution to adjust the pH to 3. Then add 0.6 mg / ml sodium nitrite to the solution to lyse the heparin at 5°C for 3 h. Then adjust the pH of the solution to 6.5 with sodium hydroxide to terminate the reaction. Dialyze in 0.15 mol / L NH4HCO3 solution to obtain a pure aldehyde heparin (Hep-CHO) solution, which is freeze-dried for later use.

[0066] Step 4: Preparation of anticoagulant coating: Add 2.5g of aminomalononitrile p-toluenesulfonate and 100mg of aldehyde heparin to a Tris buffer solution (50mL, pH=8.5), the final concentrations of aminomalononitrile p-toluenesulfonate and aldehyde heparin are 50mg / mL and 2mg / mL respectively, and after the two are evenly mixed, the pH is adjusted to 8.5 using 2M sodium hydroxide. Then, the cleaned polyester fiber fabric is immersed in the impregnation solution, placed in a 25°C water bath constant temperature oscillator for reaction for 10h, and then ultrasonically cleaned with deionized water for 60min (ultrasonic frequency is 35kHz, power is 150W), and then taken out and dried for use.

[0067] Step 5: Preparation of antibacterial and anticoagulant coating: First, prepare a zinc sulfate solution with a concentration of 80 μM under dark conditions, and then immerse the polyester fiber fabric with the anticoagulant coating in zinc sulfate and incubate for 24 hours. After obtaining the antibacterial and anticoagulant coating, use deionized water to ultrasonically clean and dry it for use.

[0068] Example 7

[0069] Step 1: Prepare buffer: prepare Tris buffer with a pH of 8.5 and a concentration of 0.1 M.

[0070] Step 2: Pretreatment of polyester fiber fabric: The prepared polyester fiber fabric (PET, 20D / 12F) was treated with acetone, anhydrous ethanol, and ultrasound for 3 times, each time for 30 minutes; then ultrasonically cleaned with deionized water for 3 times, each time for 20 minutes; the ultrasonic frequency was 35kHz and the power was 150W; during the treatment, the temperature of the mixed solution was kept at 25°C by ice water bath. Finally, the polyester fiber fabric was placed in normal pressure ventilation conditions at 65°C for 4 hours.

[0071] Step 3: Preparation of aldehyde heparin: Dissolve heparin in deionized water at 15 mg / mL and add glacial acetic acid to the solution to adjust the pH to 3. Then add 0.6 mg / ml sodium nitrite to the solution to lyse the heparin at 5°C for 3 h. Then adjust the pH of the solution to 6.5 with sodium hydroxide to terminate the reaction. Dialyze in 0.15 mol / L NH4HCO3 solution to obtain a pure aldehyde heparin (Hep-CHO) solution, which is freeze-dried for later use.

[0072] Step 4: Preparation of anticoagulant coating: Add 1g of aminomalononitrile p-toluenesulfonate and 50mg of aldehyde heparin to a Tris buffer solution (50mL, pH=8.5), the final concentrations of aminomalononitrile p-toluenesulfonate and aldehyde heparin are 20mg / mL and 1mg / mL respectively, and after the two are evenly mixed, the pH is adjusted to 8.5 using 2M sodium hydroxide. Then, the cleaned polyester fiber fabric is immersed in the impregnation solution, placed in a 25°C water bath constant temperature oscillator for reaction for 10h, and then ultrasonically cleaned with deionized water for 60min (ultrasonic frequency is 35kHz, power is 150W), and then taken out and dried for use.

[0073] Step 5: Preparation of antibacterial and anticoagulant coating: First, prepare a zinc sulfate solution with a concentration of 80 μM under dark conditions, and then immerse the polyester fiber fabric with the anticoagulant coating in zinc sulfate and incubate for 24 hours. After obtaining the antibacterial and anticoagulant coating, use deionized water to ultrasonically clean and dry it for use.

[0074] Performance Testing

[0075] (1) Morphology observation: Figure 1 , 2 3 are scanning electron microscope images of the polyester fiber fabric, the polyaminomalononitrile coating deposited on the polyester fiber fabric in Example 1, and the anticoagulant coating deposited on the surface of the polyester fiber fabric in Example 2, respectively.

[0076] (2) Hemolysis rate test: Take 8 mL of fresh human whole blood containing 10.9 mM sodium citrate solution and dilute it with 10 mL of normal saline. Immerse the PET-AMN (Example 1), PET-AMN-Hep (Example 2), and PET-AMN-Hep-Zn (Example 3) specimens (10 mm × 10 mm) in 0.5 mL of diluted blood and incubate at 37°C for 1 h. Take out the specimens, add 9 mL of normal saline, centrifuge the diluted blood at 3000 rpm for 5 min, and measure the absorbance of the supernatant at 545 nm using a UV spectrophotometer, which is recorded as M1. Add 9 mL of deionized water to 0.5 mL of diluted blood, centrifuge the composite solution at 3000 rpm for 5 min, use the supernatant as the positive reference, and measure the absorbance at 545 nm, which is recorded as M2. Then, 9 mL of saline was added to the diluted 0.5 mL of blood, and the composite solution was centrifuged at 3000 rpm for 5 min. The supernatant was used as a negative reference, and the absorbance was measured at 545 nm and recorded as X3. The hemolysis rate can be calculated as:

[0077]

[0078] (3) APTT test: Fresh human whole blood and 10.9 mM sodium citrate solution were centrifuged at 3000 rpm for 10 min to obtain platelet-free plasma (PPP). PET-AMN (Example 1), PET-AMN-Hep (Example 2), and PET-AMN-Hep-Zn (Example 3) samples (10 mm × 10 mm) were incubated with 500 μL PPP at 37°C for 1 h. Then, after taking the sample, the APTT of PPP was measured using an APTT kit.

[0079] Figure 4 : is the hemolysis rate and APTT test graph of the polyester fiber fabric obtained in Example 1, Example 2 and Example 3; Figure 4 As shown in (a), the coating containing heparin can reduce the hemolysis rate to below 0.5%. According to the ISO10993-4 standard, if the hemolysis index is <2%, the material is classified as non-hemolytic. Therefore, the coating containing heparin is non-hemolytic. The APTT value is measured to evaluate the anticoagulant effect of the PET surface with different coatings, such as Figure 4 As shown in (b), the composite coating containing heparin can prolong the APTT value to more than 15s.

[0080] (4) Antibacterial zone test: Polyester fiber fabric (PET), PET-AMN-Hep (Example 2), and PET-AMN-Hep-Zn (Example 3) were cut and set aside. The polyester fiber fabrics were attached to the E. coli (10 7 CFU / mL) and coated with Staphylococcus aureus (S. aureus) (107 CFU / mL) in a culture dish, with 3 parallel samples in each group, and then placed in an incubator at 37°C and 95% humidity for 24 hours. After the experiment, the samples were taken out and the diameter of the inhibition zone was measured with a vernier caliper and photographed. Figure 5 As shown, the PET-AMN-Hep-Zn (Example 3) coating material prepared by the present invention has excellent antibacterial effect.

[0081] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.

[0082] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing an anti-coagulation coating on the surface of a polyester fiber fabric, characterized in that The steps include: S1: modifying heparin to introduce aldehyde groups to obtain heparin with aldehyde groups; S2: dissolving aminomalononitrile p-toluenesulfonate and heparin with an aldehyde group in a tris(hydroxymethyl)aminomethane hydrochloride buffer solution at pH=8.0-8.8, and adjusting the pH of the system to 8-9 with an alkali to obtain an anticoagulant coating solution; The concentration of aminomalononitrile p-toluenesulfonate in the anticoagulant coating solution is 10-50 mg / mL, and the concentration of heparin with an aldehyde group is 0.5-2 mg / mL; S3: immersing the polyester fiber fabric in the anticoagulant coating solution, taking it out after shaking and incubating, washing and removing the residual unpolymerized precipitate or its derivatives on the surface of the polyester fiber fabric, and drying to obtain the polyester fiber fabric with the anticoagulant coating uniformly deposited on the surface.

2. The preparation method according to claim 1, characterized in that: In S1, the method for modifying the heparin with an aldehyde group is as follows: dissolving 10-20 mg / mL heparin in water, adjusting the pH to 1.5-3, adding 0.4-0.8 mg / mL sodium nitrite to lyse the heparin at 1-10°C for 2-4 hours; adjusting the pH to 6.0-7.0 with alkali to terminate the reaction; dialyzing in NH4HCO3 solution to obtain a heparin solution with an aldehyde group, and freeze-drying it for later use.

3. The preparation method according to claim 1, characterized in that: In S3, the shaking incubation temperature is 20-30°C and the time is 8-12h.

4. The preparation method according to claim 1, characterized in that: The method further comprises S4: immersing the polyester fiber fabric with the anticoagulant coating uniformly deposited on the surface obtained in S3 into an antibacterial modification liquid containing zinc sulfate, performing a secondary oscillation reaction, ultrasonically cleaning and drying to obtain a secondary modified anticoagulant coating; the number of amino groups in the aminomalononitrile p-toluenesulfonate is in excess compared to the aldehyde groups in the heparin with aldehyde groups.

5. The preparation method according to claim 4, characterized in that: The temperature of the secondary oscillation reaction is 20-30°C and the time is 12-24h.

6. The preparation method according to claim 4, characterized in that: The total concentration of zinc sulfate in the antibacterial modified solution is 60-80 μM.

7. The preparation method according to claim 6, characterized in that: In S3, the cleaning is ultrasonic cleaning: ultrasonic cleaning is performed using deionized water for at least 15 minutes, with an ultrasonic frequency of 20-35 kHz and a power of 100-150 W.

Citation Information

Patent Citations

  • Medical material and method for preparing anticoagulation coating layer on surface of medical material

    CN111012959A

  • Anticoagulant antimicroorganism coating and preparation method and use thereof

    CN113209394A

  • Preparation method of heparin coating applied to medical equipment

    CN113350580A

  • Dopamine-heparin composite anticoagulant coating and preparation method thereof

    CN114984332A

  • Anticoagulant coating as well as preparation method and application thereof

    CN115998963A