Kitchen paper and production method thereof
The described method for producing kitchen paper uses high-concentration pulping and alloy knife technology to create low-grammage, high-stiffness paper with reduced long fiber use, addressing cost and efficiency issues in traditional production methods.
Patent Information
- Application Number
- CN202411262783.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-12-06
AI Technical Summary
Existing kitchen paper production methods require high gram weight and long fiber content to achieve stiffness, leading to high production costs and inefficiencies.
A method involving high-concentration pulping and alloy knife longitudinal grain technology to produce low-grammage, high-stiffness kitchen paper using a combination of long-fiber softwood and short-fiber hardwood pulps, with the addition of glyoxal polyacrylamide and environmentally friendly polyamide epoxy resins, and a crescent paper machine process.
The method reduces raw material costs and enhances tensile strength while maintaining stiffness, suitability for large-scale production, and improves water absorption performance.
Smart Images

Figure CN119083226A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of household paper manufacturing, and in particular to kitchen paper and a production method thereof. Background Art
[0002] Kitchen paper is a paper towel used exclusively in the kitchen. It is larger and thicker than ordinary paper towels, and has better water and oil absorption. It is a good helper for home cleaning and food oil absorption. Kitchen paper has two major functions: one is for home cleaning, and the other is to absorb moisture and oil from food. In the process of producing kitchen paper, the base paper has high requirements. The base paper must have a high stiffness so that it can retain a high stiffness in the post-processing embossing process, and the produced product has a thick feel. The stiffness of kitchen paper with a lower gram weight is more difficult to make. In order to achieve the use effect, the current mainstream kitchen paper is generally more than 25 grams to ensure the stiffness of the finished paper. The high gram weight of the finished paper is relatively low cost-effective for both the manufacturer and the consumer. In traditional processes, in order to achieve high tensile strength and high thickness of kitchen paper base paper, the stiffness of the base paper is often increased by increasing the proportion of long fibers, which has a high production cost. Summary of the invention
[0003] In view of the above problems, the present application provides a low-grammage, high-stiffness kitchen paper and a production method thereof.
[0004] The first aspect of the present application provides a method for producing kitchen paper base paper, comprising the following steps:
[0005] Slurry preparation:
[0006] Long-fiber softwood pulp: bleached softwood pulp is pulped at low concentration using a double-disc refiner with a pulping concentration of 4.5-5.5% and a beating degree of 28-30°SR.
[0007] Short-fiber hardwood pulp: Bleached commercial hardwood pulp is refined to high consistency.
[0008] Mixing slurry:
[0009] Blanket layer: 60% long-fiber softwood pulp and 40% short-fiber hardwood pulp;
[0010] Web layer: 100% short fiber hardwood pulp;
[0011] Copied:
[0012] A crescent paper machine is used, where the pulp flows into the layered screen through a double-layer headbox, and is pressed and dehydrated to obtain a wet paper web;
[0013] Drying wrinkles:
[0014] The paper is dried by a drying cylinder and corrugated with a corrugating alloy knife to obtain kitchen paper base paper.
[0015] Different from the prior art, the present application adopts high-concentration pulping technology and alloy knife longitudinal grain technology. The increase in high-concentration pulping specific energy consumption can improve the tensile strength of the finished paper. The alloy knife provides 3D three-dimensional grains for the base paper, further ensuring that the finished paper has high stiffness for the production of low-quantity high-stiffness new kitchen paper. The technology of the present application has a simple process, can reduce the use of long fibers, save raw material costs, and is suitable for large-scale promotion.
[0016] Furthermore, the double-disc refining concentration is controlled at 4.5-5.5%, and the beating degree is controlled at 28-30°SR.
[0017] Furthermore, the high-concentration pulp has a dryness of 25-28%, and a beating degree of 20-23°SR.
[0018] Furthermore, in the slurry preparation step, glyoxal polyacrylamide dry strength agent is added to the slurry in an amount of 0.2 to 0.8 kg / ton of paper, and environmentally friendly polyamide epoxy resin is added in an amount of 15 to 30 kg / ton of paper.
[0019] Furthermore, the pulping amount of the felt layer is 50%, and the pulping amount of the mesh layer is 50%.
[0020] Furthermore, in the high-concentration pulping, the high-concentration pulping machine is a CDI3pl model high-concentration pulping machine of Andritz, and the pulping specific energy consumption is controlled at 55-60 kwh / ton of pulp.
[0021] Furthermore, the speed of the crescent paper machine is 700-1900 m / min.
[0022] Furthermore, the blade edge of the corrugated alloy knife is corrugated.
[0023] A second aspect of the present application provides a kitchen paper base paper, which is produced by the production method provided by the first aspect of the present application.
[0024] Furthermore, the kitchen paper base paper has a width of 5650 mm and a gram weight of 12-30 g / m 2 .
[0025] The above-mentioned records related to the invention content are only an overview of the technical solution of the present application. In order to enable ordinary technicians in the field to more clearly understand the technical solution of the present application, and then implement it according to the written contents of the specification, and to make the above-mentioned purpose and other purposes, features and advantages of the present application easier to understand, the specific implementation mode and drawings of the present application are explained below. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The drawings are only used to illustrate the principles, implementation methods, applications, characteristics and effects of the specific embodiments of the present application and other related contents, and shall not be considered as limitations of the present application.
[0027] In the drawings of the specification:
[0028] Figure 1 This is the relationship diagram of specific energy consumption-beating degree / wet weight.
[0029] Figure 2 It is the relationship diagram between specific energy consumption and tensile index / bulk thickness;
[0030] Figure 3 It is the relationship diagram between specific energy consumption and average fiber length / average fiber width;
[0031] Figure 4 is the relationship diagram between specific energy consumption and average morphology factor / fine fiber ratio;
[0032] Figure 5 This is a flow chart of the slurry preparation process according to the implementation mode of this application;
[0033] Figure 6 This is a flow chart of the flow process of this embodiment;
[0034] Figure 7 Kitchen paper produced by traditional crafts;
[0035] Figure 8 Kitchen paper produced for the embodiment. DETAILED DESCRIPTION
[0036] In order to explain in detail the possible application scenarios, technical principles, specific schemes that can be implemented, and the purposes and effects that can be achieved, the following is a detailed description of the specific embodiments listed in conjunction with the accompanying drawings. The embodiments described herein are only used to more clearly illustrate the technical solutions of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.
[0037] Reference to "embodiment" herein means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The term "embodiment" appearing in various places in the specification does not necessarily refer to the same embodiment, nor does it particularly limit its independence or association with other embodiments. In principle, in the present application, as long as there is no technical contradiction or conflict, the various technical features mentioned in the embodiments can be combined in any way to form a corresponding implementable technical solution.
[0038] Unless otherwise defined, the technical terms used in this document have the same meanings as those generally understood by those skilled in the art to which this application belongs; the use of relevant terms in this document is only for describing specific embodiments and is not intended to limit this application.
[0039] In the description of this application, the term "and / or" is an expression used to describe the logical relationship between objects, indicating that three relationships may exist, for example, A and / or B, which means: A exists, B exists, and A and B exist at the same time. In addition, the character " / " in this article generally indicates that the objects before and after are in an "or" logical relationship.
[0040] In the present application, terms such as “first” and “second” are merely used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship of quantity, priority or sequence between these entities or operations.
[0041] Without further limitations, in this application, the words "include", "comprises", "has" or other similar expressions used in the sentences are intended to cover non-exclusive inclusion. These expressions do not exclude the presence of additional elements in the process, method or product including the elements, so that the process, method or product including a series of elements may include not only those limited elements, but also other elements not explicitly listed, or also include elements inherent to such process, method or product.
[0042] Similar to the understanding in the Examination Guidelines, in this application, expressions such as "greater than", "less than", "exceed" and the like are understood to exclude the number itself; expressions such as "above", "below", "within" and the like are understood to include the number itself. In addition, in the description of the embodiments of this application, "multiple" means more than two (including two), and similar expressions related to "multiple" are also understood in this way, such as "multiple groups", "multiple times", etc., unless otherwise clearly and specifically limited.
[0043] The beating degree mentioned in this application is the beating degree. After the reaction pulp passes through the refiner, the fibers are cut, split, swollen, and hydrated, which are the effects of the refinement. Beating is to use the mechanical action of the grinding disc teeth to treat the fibers in the pulp, so that they are loosened, appropriately cut, and separated; more importantly, the fibers absorb water and swell during beating, so that they have higher elasticity and plasticity, meet the requirements of paper machine production, so that the produced paper can reach the expected quality indicators. Beating degree indicates the water filtration performance of pulp. Take 2 grams of absolute dry pulp, dilute to 1000 ml, pass through an 80-mesh screen at 20°C, and the amount of water discharged from the side tube of the Shaw beating degree meter is the result of the measurement. Beating degree is an indicator of the properties of paper stock. According to the beating degree of paper stock, it is possible to grasp the water filtration speed of paper stock on the copper screen of the paper machine in the future, and it is also possible to summarize and predict the mechanical strength, tightness and manageability of the paper produced in the future. Therefore, mastering the beating degree of paper stock is an important technical control method in production.
[0044] The first aspect of the present application provides a method for producing kitchen paper base paper, comprising the following steps:
[0045] Slurry preparation:
[0046] Long-fiber softwood pulp: The bleached softwood pulp is pulped at low concentration and refined using a double-disc refiner. The fibers are then separated and cut appropriately.
[0047] Short-fiber hardwood pulp: Bleached commercial hardwood pulp is subjected to high-concentration pulping. Using high-concentration pulping to refine hardwood pulp can fully separate the fibers and retain the fiber length well, solving the problem that low-concentration pulping and heavy pulping easily cause cutting, thereby greatly improving the utilization rate of short-fiber raw materials and reducing the amount of long fibers. Compared with low-concentration pulping, it can better maintain the bulk.
[0048] Mixing slurry:
[0049] Felt layer: 60% long-fiber softwood pulp and 40% short-fiber hardwood pulp; long-fiber softwood pulp is used to support the stiffness of the finished paper;
[0050] Web layer: 100% short fiber hardwood pulp; gives the front side of the base paper a smooth feel.
[0051] Copied:
[0052] A crescent paper machine is used, with pulp flowing into the layered screen through a double-layer headbox, and the wet paper web is obtained by pressing and dehydrating. The double-channel headbox pulp spreading technology is adopted, and the layered forming provides the base paper with different properties on both sides, ensuring that the finished paper is stiff while the front side of the base paper feels smooth and delicate.
[0053] Drying wrinkles:
[0054] The paper is dried in a drying cylinder and corrugated with a corrugating alloy knife to obtain the base paper for kitchen paper. The corrugating alloy knife provides the base paper with 3D texture, further ensuring that the finished paper has high stiffness.
[0055] Different from the prior art, the present application adopts high-concentration pulping technology and alloy knife longitudinal grain technology. The increase in high-concentration pulping specific energy consumption can improve the tensile strength of the finished paper. The alloy knife provides 3D three-dimensional grains for the base paper, further ensuring that the finished paper has high stiffness for the production of low-quantity high-stiffness new kitchen paper. The technology of the present application has a simple process, can reduce the use of long fibers, save raw material costs, and is suitable for large-scale promotion.
[0056] Furthermore, the double-disc refining concentration is controlled at 4.5-5.5%, and the beating degree is controlled at 28-30°SR.
[0057] Furthermore, the high-concentration pulp has a dryness of 25-28%, and a beating degree of 20-23°SR.
[0058] Furthermore, in the slurry preparation step, glyoxal polyacrylamide dry strength agent is added to the slurry in an amount of 0.2 to 0.8 kg / ton of paper; and environmentally friendly polyamide epoxy resin is added in an amount of 15 to 30 kg / ton of paper.
[0059] Glyoxal polyacrylamide dry strength agent is used to improve the dry strength of base paper and remove system fine fibers, and environmentally friendly polyamide epoxy resin is used to improve the wet strength of base paper.
[0060] Furthermore, the pulping amount of the felt layer is 50%, and the pulping amount of the mesh layer is 50%.
[0061] Furthermore, in the high-concentration pulping, the equipment used is the high-concentration pulping machine, which is the CDI3pl model high-concentration pulping machine of Andritz, and the pulping specific energy consumption is controlled at 55-60 kwh / ton of pulp.
[0062] Furthermore, the speed of the crescent paper machine is 700-1900 m / min.
[0063] Furthermore, the blade edge of the corrugated alloy knife is corrugated.
[0064] A second aspect of the present application provides a kitchen paper base paper, which is produced by the production method provided by the first aspect of the present application.
[0065] Furthermore, the kitchen paper base paper has a width of 5650 mm and a gram weight of 12-30 g / m 2 .
[0066] The glyoxal polyacrylamide dry strength agent (GAPM) described in this embodiment is produced by cross-linking reaction of polyacrylamide and glyoxal. The glyoxal polyacrylamide dry strength agent can generate bonds and forces to improve the dry strength of paper and paperboard by reacting an aldehyde group on its molecular formula with a hydroxyl group on the fiber to form a covalent bond, thereby improving the temporary wet strength of paper.
[0067] The environmentally friendly polyamide epoxy resin PAE in this embodiment meets the national requirements for food contact paper products.
[0068] The corrugated alloy knife used in this embodiment is a BTG corrugated knife 75-TEXTURA T10.
[0069] In this embodiment, the high-concentration pulping system and auxiliary equipment are provided by Andritz, including the model of the pressing screw: SCP1006, the model of the plug screw: CFE3, and the model of the high-concentration pulping machine: CDI3pl.
[0070] The bleached commercial hardwood pulp was refined at high concentration. The specific energy consumption was adjusted to 25kwh / t, 40kwh / t, and 55kwh / t under the condition that other process parameters remained unchanged. The high concentration mill outlet was sampled at the corresponding specific energy consumption, the pulp beating degree was tested, the fiber analysis was performed, and the paper sample bulk and tensile index were tested after papermaking. The results are as follows: Figure 1-Figure 4 shown.
[0071] Depend on Figure 1 It can be seen that with the increase of specific energy consumption, the beating degree increases, and there is no obvious regularity in wet weight. Figure 2 It can be seen that: with the increase of specific energy consumption, the tensile index increases, showing a positive correlation trend; the bulk decreases, showing a negative correlation trend. Figure 3 It can be seen that: with the increase of specific energy consumption, the average fiber length changes irregularly; the average fiber width does not change significantly. Figure 4 It can be seen that: with the increase of specific energy consumption, the average morphology factor increases accordingly, showing a positive correlation trend; the fine fiber ratio decreases accordingly, showing a positive correlation trend.
[0072] In short, with the increase of high-concentration grinding specific energy consumption, the beating degree, tensile index, average morphological factor (degree of fiber deformation) and fine fiber ratio increase, showing a positive correlation trend; the bulk decreases with the increase of high-concentration grinding specific energy consumption, showing a negative correlation trend. Compared with the blank sample without refining, the tensile index of the copy sheet increased by 31% when the specific energy consumption was 25kwh / t, the tensile index of the copy sheet increased by 39% when the specific energy consumption was 40kwh / t, and the tensile index of the copy sheet increased by 44% when the specific energy consumption was 55kwh / t.
[0073] Therefore, increasing the refining power can be used to increase the tensile strength of the finished paper. In this embodiment, the specific energy consumption is set to 55-60 kwh / t.
[0074] Example 1 Preparation of Kitchen Paper Base Paper
[0075] The paper machine is a crescent paper machine with a width of 5650mm. It produces base paper for daily use. The paper weight is 12-30g / m 2 , vehicle speed is 700~1900m / min, and the pulp source is coniferous pulp board and broadleaf pulp board.
[0076] Slurry preparation:
[0077] Long-fiber softwood pulp: bleached softwood pulp is pulped at low concentration using a double-disc refiner with a pulping concentration of 5% and a beating degree of 28-30°SR.
[0078] Short-fiber hardwood pulp: The bleached commercial hardwood pulp is subjected to high-consistency pulping with a dryness of 26% and a beating degree of 20-23°SR. The CDI3pl high-consistency pulping machine of Andritz is used, and the specific energy consumption of pulping is controlled at 55-60 kwh / ton of pulp.
[0079] Slurry preparation: the slurry amount of the felt layer is 50%, and the slurry amount of the mesh layer is 50%;
[0080] Blanket layer: 60% long-fiber softwood pulp and 40% short-fiber hardwood pulp;
[0081] Web layer: 100% short fiber hardwood pulp;
[0082] Copied:
[0083] A crescent paper machine is used, where the pulp flows into the layered screen through a double-layer headbox, and is pressed and dehydrated to obtain a wet paper web;
[0084] Drying wrinkles:
[0085] Drying with a drying cylinder, and corrugating the paper with a corrugating alloy knife to obtain kitchen paper base paper; the surface of the corrugating alloy knife in contact with the paper is the blade surface. In Example 1, BTG corrugating knife 75-TEXTURA T10 is used. The difference between Comparative Example 1 and Example 1 is that a 0° steel knife is used to corrugate the paper in Comparative Example 1. The kitchen paper base paper made from Example 1 and Comparative Example 1 is subjected to the 4 sample tests listed in Table 1, and the performance test results of the kitchen paper are shown in Table 2:
[0086] Table 1
[0087]
[0088] Table 2
[0089]
[0090]
[0091] The significance and data analysis of each performance index in Table 2:
[0092] 1. Roughness is the mean square value of the depth of each point in the microscopic morphology, which affects the smoothness of the paper feel and processing performance.
[0093] 2. Wrinkle depth is the average value of the peak-to-valley depth of wrinkles, indicating the depth of wrinkles.
[0094] 3. The wrinkle width is the average width of the wrinkle peak root, that is, the width of the zero point, which represents the width of the wrinkle.
[0095] 4. Wrinkle length: The average length of independent wrinkles in the field of view, which affects the softness, roughness and stiffness of the finished paper.
[0096] 5. Number of wrinkles: The number of independent wrinkles in a unit field of view affects the softness, roughness and stiffness of the finished paper.
[0097] Wrinkle distribution The percentage of wrinkles in different width ranges is divided into four levels: fine wrinkles, ordinary wrinkles, coarse wrinkles and extra-large wrinkles. It can be seen from Table 2 that the proportion of coarse wrinkles is higher when using a corrugating knife, and the base paper forms a more three-dimensional 3D texture with obvious thickness and bulk, which greatly improves the water absorption performance of the base paper.
[0098] The wrinkling results of Comparative Example 1 are as follows Figure 7 The wrinkling results of Example 1 are as follows Figure 8 As shown. The kitchen paper of comparative example 1 has only transverse wrinkles, and has good transverse stiffness, but no longitudinal wrinkles, low longitudinal stiffness, and poor thickness. In example 1, due to the corrugation of the alloy layer at the wrinkled alloy blade, the base paper can form regular longitudinal textures when peeled off the cylinder surface, providing longitudinal stiffness for the base paper, forming 3D three-dimensional textures on the base paper, having obvious thickness and bulk, and greatly improving the water absorption performance of the base paper.
[0099] Example 2 Preparation of Kitchen Paper Base Paper
[0100] The paper machine is a crescent paper machine with a width of 5650mm. It produces base paper for daily use. The paper weight is 12-30g / m 2 , vehicle speed is 700~1900m / min, and the pulp source is coniferous pulp board and broadleaf pulp board.
[0101] Slurry preparation:
[0102] Long-fiber softwood pulp: bleached softwood pulp is pulped at low concentration using a double-disc refiner with a pulping concentration of 4.5% and a beating degree of 28-30°SR.
[0103] Short-fiber hardwood pulp: Bleached commercial hardwood pulp is subjected to high-consistency pulping with a dryness of 25% and a beating degree of 20-23°SR. A CDI3pl high-consistency pulping machine from Andritz is used, and the specific energy consumption of pulping is controlled at 55-60 kwh / ton of pulp.
[0104] Slurry preparation: the slurry amount of the felt layer is 50%, and the slurry amount of the mesh layer is 50%;
[0105] Blanket layer: 60% long-fiber softwood pulp and 40% short-fiber hardwood pulp;
[0106] Web layer: 100% short fiber hardwood pulp;
[0107] Copied:
[0108] A crescent paper machine is used, where the pulp flows into the layered screen through a double-layer headbox, and is pressed and dehydrated to obtain a wet paper web;
[0109] Drying wrinkles:
[0110] The paper is dried in a drying cylinder and corrugated with a corrugating alloy knife to obtain kitchen paper base paper; the surface of the corrugating alloy knife in contact with the paper is the blade surface. In Example 2, a BTG corrugating knife 75-TEXTURA T10 is used.
[0111] Example 2 Preparation of Kitchen Paper Base Paper
[0112] The paper machine is a crescent paper machine with a width of 5650mm. It produces base paper for daily use. The paper weight is 12-30g / m 2 , vehicle speed is 700~1900m / min, and the pulp source is coniferous pulp board and broadleaf pulp board.
[0113] Slurry preparation:
[0114] Long-fiber softwood pulp: bleached softwood pulp is pulped at low concentration using a double-disc refiner with a pulping concentration of 5.5% and a beating degree of 28-30°SR.
[0115] Short-fiber hardwood pulp: The bleached commercial hardwood pulp is subjected to high-consistency pulping with a dryness of 28% and a beating degree of 20-23°SR. The CDI3pl high-consistency pulping machine of Andritz is used, and the specific energy consumption of pulping is controlled at 55-60 kwh / ton of pulp.
[0116] Slurry preparation: the slurry amount of the felt layer is 50%, and the slurry amount of the mesh layer is 50%;
[0117] Blanket layer: 60% long-fiber softwood pulp and 40% short-fiber hardwood pulp;
[0118] Web layer: 100% short fiber hardwood pulp;
[0119] Copied:
[0120] A crescent paper machine is used, where the pulp flows into the layered screen through a double-layer headbox, and is pressed and dehydrated to obtain a wet paper web;
[0121] Drying wrinkles:
[0122] The paper is dried in a drying cylinder and corrugated with a corrugating alloy knife to obtain kitchen paper base paper; the surface of the corrugating alloy knife in contact with the paper is the blade surface. In Example 2, a BTG corrugating knife 75-TEXTURA T10 is used.
[0123] Finally, it should be noted that although the above embodiments have been described in the specification and drawings of this application, this does not limit the scope of patent protection of this application. All technical solutions generated by replacing or modifying equivalent structures or equivalent processes based on the essential concept of this application using the contents recorded in the specification and drawings of this application, as well as directly or indirectly implementing the technical solutions of the above embodiments in other related technical fields, are included in the scope of patent protection of this application.
Claims
1. A method for producing kitchen paper base paper, It is characterized in that The following steps are involved: Slurry preparation: Long-fiber softwood pulp: bleached softwood pulp is pulped at low consistency and refined using a double disc refiner; Short-fiber hardwood pulp: Bleached commercial hardwood pulp is refined to high consistency. Mixing slurry: Blanket layer: 60% long-fiber softwood pulp and 40% short-fiber hardwood pulp; Web layer: 100% short fiber hardwood pulp; Copied: A crescent paper machine is used, where the pulp flows into the layered screen through a double-layer headbox, and is pressed and dehydrated to obtain a wet paper web; Drying wrinkles: The paper is dried by a drying cylinder and corrugated with a corrugating alloy knife to obtain kitchen paper base paper; the surface of the corrugating alloy knife in contact with the paper is the blade surface.
2. The production method according to claim 1, It is characterized in that The double-disc refining concentration is controlled at 4.5-5.5%, and the beating degree is controlled at 28-30°SR.
3. The production method according to claim 1, It is characterized in that The high-concentration pulping has a dryness of 25-28%, and a beating degree of 20-23°SR.
4. The production method according to claim 1, It is characterized in that In the slurry preparation step, glyoxal polyacrylamide dry strength agent is added to the slurry in an amount of 0.2-0.8 kg / ton of paper; and environmentally friendly polyamide epoxy resin is added in an amount of 15-30 kg / ton of paper.
5. The production method according to claim 1, It is characterized in that The pulping amount of the felt layer is 50%, and the pulping amount of the mesh layer is 50%.
6. The production method according to claim 1, It is characterized in that The high-concentration refiner is a CDI3pl high-concentration refiner of Andritz, and the specific energy consumption of pulping is controlled at 55-60 kwh / ton of pulp.
7. The production method according to claim 1, It is characterized in that The speed of the crescent paper machine is 700-1900 m / min.
8. The production method according to claim 1, It is characterized in that The blade edge of the wrinkled alloy knife is corrugated.
9. A kitchen paper base, It is characterized in that The kitchen paper base paper is produced by the production method described in any one of claims 1 to 8.
10. The kitchen paper base according to claim 9, It is characterized in that The kitchen paper base paper has a width of 5650 mm and a gram weight of 12-30 g / m 2 .
Citation Information
Patent Citations
Flexible tissue paper and preparation process thereof
CN104060492A
Kitchen paper and preparation process thereof
CN109554959A
Preparation technology of high-water-absorption breathable tissue raw paper material for puerperae
CN110172856A
Preparation method of high-strength paper
CN117286746A
Biaxially undulatory tissue and creping process using undulatory blade
US5656134A