Ferrihydrite material for treating radioactive waste liquid as well as preparation and application of ferrihydrite material

By simplifying the preparation process, iron ore and chitosan are combined to form spherical iron ore materials, the problem of difficulty in separation after adsorption is solved, the effect of efficient adsorption and easy separation is achieved, and the safety of handling radioactive waste liquid is improved. .

CN119092173APending Publication Date: 2024-12-06CENT SOUTH SAFETY & ENVIRONMENTAL TECH RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411223639.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing adsorbent preparation methods are complex, and the separation effect after adsorption is poor, which makes it difficult to separate powdered iron ore materials from the solution, which may lead to safety accidents.

Method used

Iron hydroglyite is added to the acetic acid solution containing chitosan, adjust the pH value, and add surfactant to the NaOH solution to form a spherical iron hydroglyite material. The preparation process is simplified and the separation is improved through freeze-drying treatment.

Benefits of technology

The obtained iron ore material has good adsorption properties, high adsorption amounts to Co2+ and Sr2+, removal rates are as high as 94.7% and 82.5%, and is easy to separate from the solution, reducing safety risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092173A_ABST
    Figure CN119092173A_ABST
Patent Text Reader

Abstract

The invention discloses a ferrihydrite material for treating radioactive waste liquid and preparation and application thereof.The method comprises the steps that ferrihydrite is added into an acetic acid solution containing chitosan and stirred to be uniform, and a mixture is obtained; sucking the mixture by using an injector with a needle, adding a surfactant into the NaOH solution, and slowly dripping the mixture in the injector into the NaOH solution at a constant speed above the NaOH liquid level when the NaOH solution is continuously stirred; after dripping, the mixture is spherical, standing, curing, cleaning and freeze-drying to obtain the ferrihydrite material for treating the radioactive waste liquid. The problems that an existing adsorbent is complex in preparation method and poor in separation effect after adsorption are solved, the material prepared from the ammonia water, the acetic acid and the sodium hydroxide has good adsorption performance, the removal rate of Co < 2 + > reaches up to 94.7%, the removal rate of Sr < 2 + > reaches up to 82.5%, and the material can be easily separated from a solution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a ferrihydrite material, and in particular to a ferrihydrite material for treating radioactive waste liquid and a preparation method and application thereof. Background Art

[0002] As nuclear energy has become more widely used in recent years, it will produce radioactive waste during its use. If these wastes enter the water environment, they will pose a great threat to human health and the natural environment. The adsorption method can treat radioactive substances generated by nuclear power plants and nuclear power platforms throughout their life cycle. The adsorption method for treating radioactive waste liquid is to enrich the radioactive substances in the water using porous materials (adsorbents) so that one or more elements in the waste liquid are adsorbed on the surface or in the pores of the adsorbent. At present, the adsorption materials for treating radioactive waste liquid are mainly composite adsorption materials prepared from natural materials or silicon-based and graphene oxide. The initial state of the prepared materials is powder. The composite adsorption material has a good treatment effect on radioactive waste liquid, but when it is actually applied to waste liquid or in related equipment, it is easy to have problems such as difficulty in recovery and powder clogging pipelines, which may even lead to safety accidents.

[0003] The key to the adsorption process of effective treatment of radioactive waste liquid is to select an adsorbent with high adsorption efficiency and excellent selectivity. Adsorbents can be classified according to their sources into two types: naturally occurring and artificially synthesized adsorbents. Studies have shown that ferrihydrite is a commonly used natural inorganic adsorbent. It is the natural iron (hydroxide) with the largest specific surface area. It has good surface activity and a large number of functional groups. It is a weakly crystalline (hydroxide) iron with a small particle size, usually around 2 to 100 nm. It has strong reusability. After 5 times of adsorption-desorption, the adsorption effect can still reach 84.5% of the initial adsorption capacity. It is an effective pollutant adsorbent. Existing literature 1 (Meng Kaiyue. Preparation of ferrihydrite-based composite materials and study of their adsorption performance for Cd(III) and As(V) [D]. Beijing: China University of Geosciences, 2020) When studying ferrihydrite-based composite materials, it was found that Cd 2+ and As 4+ When the initial concentration of ferrihydrite increased from 5 mg / g to 50 mg / g, the 2+ The adsorption rate of As was 91.8% to 76.6%. 4+ The adsorption rate is 98.0% to 90.1%.

[0004] Although ferrihydrite is widely distributed in the environment, it has many surface active functional groups, strong charge variability, large specific surface area, and strong adsorption to heavy metal pollutant element ions, but ferrihydrite is often in powder form and is difficult to separate from the solution after adsorption, which may clog the pipeline and require secondary disposal, and even lead to safety accidents in serious cases. In order to solve the problem of being difficult to separate from the solution, the existing technology uses magnetic materials for loading or modifies ferrihydrite or chitosan materials through more complex chemical reactions to improve the adsorption performance and separability of the materials, but the preparation cost of the materials is relatively high, the preparation method is relatively complex, and the final separation effect is not good. Summary of the invention

[0005] The purpose of the present invention is to provide a ferrihydrite material for treating radioactive waste liquid and its preparation and application, which solves the problems of complex preparation methods of existing adsorbents and poor separation effect after adsorption. The prepared material not only has good adsorption performance, but is also easy to separate from the solution.

[0006] In order to achieve the above object, the present invention provides a method for preparing a ferrihydrite material for treating radioactive waste liquid, the method comprising:

[0007] (1) adding ferrihydrite to an acetic acid solution containing chitosan, stirring uniformly to obtain a mixture;

[0008] The ferrihydrite is obtained by adding concentrated ammonia water to a Fe(NO3)3·9H2O solution, adjusting the pH value of the solution to 7.5-8, stirring, standing, removing the upper clear liquid, and performing subsequent treatment on the lower suspension;

[0009] (2) using a syringe with a needle to absorb the mixture obtained in step (1), adding a surfactant to the NaOH solution (to reduce the surface tension of the solution), and while continuously stirring the NaOH solution, slowly and evenly dripping the mixture in the syringe into the NaOH solution above the NaOH liquid surface (in order to solve the problem of the mixture sticking to the bottom of the cup before solidification and the low drop ball rate, when dripping the mixture, a magnetic stirrer is used to stir the NaOH solution to extend the distance for the dripping balls to fall to the bottom of the cup, thereby reducing the falling speed of the mixture);

[0010] (3) After the addition, the mixture is in a spherical shape, and is allowed to solidify by standing, and then washed and freeze-dried to obtain a ferrihydrite material for treating radioactive waste liquid.

[0011] Preferably, in step (1), the concentration of chitosan in the acetic acid solution containing chitosan is 40 g / L, and the concentration of acetic acid is 4%; the mass ratio of chitosan to ferrihydrite in the acetic acid solution containing chitosan is 1:4.

[0012] Preferably, in step (1), the subsequent processing is:

[0013] The lower suspension was repeatedly washed and allowed to stand until the conductivity of the supernatant of the suspension dropped to 250 μS / cm after standing. The supernatant was removed, and the remaining suspension was centrifuged and freeze-dried in vacuum.

[0014] Preferably, in step (2), the pore size of the needle is 0.1 mm; the concentration of the NaOH solution is 0.2 mol / L; and the vertical distance above the NaOH liquid surface is 25 to 35 cm, which reduces the falling speed of the mixture and solves the problem of low drop ball formation rate.

[0015] Preferably, in step (2), the surfactant is C 20 Polyoxyethylene ether; the concentration of the surfactant in the NaOH solution is 0.1 mol / L.

[0016] Preferably, in step (2), the slow and uniform speed is 10 drops / minute.

[0017] Preferably, in step (3), the probability that the mixture is spherical is greater than 90%.

[0018] The invention provides a novel ferrihydrite adsorbent prepared by the preparation method.

[0019] Preferably, the material is spherical and has an average particle size of 0.8 mm.

[0020] The present invention provides an application of the ferrihydrite material for treating radioactive waste liquid in the field of adsorption.

[0021] The ferrihydrite material for treating radioactive waste liquid of the present invention and its preparation and application solve the problems of complicated preparation method of existing adsorbents and poor separation effect after adsorption, and have the following advantages:

[0022] The invention utilizes the advantages of good surface activity of ferrihydrite and combines the characteristics of good compatibility and multiple adsorption sites of chitosan. On the premise of ensuring the adsorption effect, the homemade ferrihydrite is dissolved in a chitosan solution, dripped into a NaOH solution to form balls, and the wet balls are freeze-dried to prepare a new ferrihydrite material.

[0023] Compared with the prior art, the present invention uses low-cost raw materials such as ammonia water, acetic acid and sodium hydroxide, and uses a simple preparation method. The prepared material not only has better adsorption performance (for Co 2+ The maximum adsorption capacity reached 35.274 mg·g -1 The removal rate is as high as 94.7%. 2+ The adsorption capacity reached 28.532 mg·g-1 , removal rate up to 82.5%), and it is easy to separate from the solution. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a flow chart of preparing ferrihydrite material for treating radioactive waste liquid in Example 1 of the present invention.

[0025] Figure 2 This is a physical picture of the ferrihydrite material for treating radioactive waste liquid prepared in Example 1 of the present invention.

[0026] Figure 3 The ferrihydrite material prepared in Examples 1 to 2 of the present invention has a 2+ and Sr 2+ The adsorption results are shown in Figure 2.

[0027] Figure 4 This is the infrared spectrum of the ferrihydrite material of Example 1 of the present invention. DETAILED DESCRIPTION

[0028] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] The sources of the reagents involved in the following examples are as follows:

[0030] Table 1 Sources of reagents involved in the examples

[0031]

[0032]

[0033] Example 1

[0034] A method for preparing a ferrihydrite material for treating radioactive waste liquid, such as Figure 1 As shown, the flow chart of Example 1 of the present invention for preparing a ferrihydrite material for treating radioactive waste liquid comprises:

[0035] 1. Synthetic ferrihydrite

[0036] Weigh 25.0g Fe(NO3)3·9H2O and dissolve it in 1000mL deionized water. Add concentrated ammonia water to adjust the pH. After the solution is neutral, add it drop by drop to adjust the pH value of the solution to 7.5-8. Use a magnetic stirrer to stir for 3 hours to fully mix it. Let it stand for 30 minutes, remove the upper clear liquid, and wash the lower suspension repeatedly with ultrapure water for at least 3 times. Let it stand for 20 minutes to remove impurities in the solution until the conductivity of the supernatant after standing drops to 250μS / cm. Then remove the supernatant, transfer the remaining suspension to a centrifuge tube, and centrifuge it at a speed of 4000rpm for 10 minutes to obtain a sample. Use a freeze vacuum dryer to freeze-dry the sample for 24 hours, and grind it to obtain a reddish-brown ferrihydrite powder.

[0037] 2. Preparation of ferrihydrite materials for treating radioactive waste liquid

[0038] The steps of preparing the ferrihydrite material for treating radioactive waste liquid using chitosan as the material skeleton are as follows:

[0039] (1) 20 g of chitosan was dissolved in 500 mL of 4% acetic acid to obtain a chitosan solution, and 100 mL of the chitosan solution (5 g of chitosan) was added to a 250 mL beaker; at room temperature, 20 g of ferrihydrite was added to the beaker containing the chitosan solution so that the mass ratio of chitosan to ferrihydrite was 1:4, and the mixture was stirred with a magnetic stirrer to be completely mixed to obtain a mixture.

[0040] (2) Add 1 mL of C20 polyoxyethylene ether surfactant to 100 mL of 0.2 mol / L NaOH solution, draw up the mixture with a syringe with a 0.1 mm needle, and while stirring the 0.2 mol / L NaOH solution with a magnetic stirrer, place the needle 25 to 35 cm above the NaOH liquid surface and slowly and evenly drip the mixture in the syringe into the NaOH solution at a rate of 10 drops / min. Stir the NaOH solution with a magnetic stirrer during the dripping to prevent the prepared pellets from sticking to the bottom of the cup.

[0041] (3) After the addition, the wet mixture was spherical (the wet sphere particle size was 1 cm, and the sphericity rate could reach 92.2%), and was allowed to stand for 20 minutes to solidify (only standing without other operations), and the solidified spherical wet mixture was washed with deionized water for 3 times, and the spherical wet mixture was placed in a vacuum freeze dryer and dried for 24 hours to obtain a spherical ferrihydrite material with an average particle size of 0.8 mm for treating radioactive waste liquid.

[0042] like Figure 2 As shown, the physical picture of the ferrihydrite material for treating radioactive waste liquid prepared in Example 1 of the present invention, wherein A is a physical picture of the wet mixture; B is a physical picture of the ferrihydrite material for treating radioactive waste liquid. Figure 2It can be seen that the ferrihydrite powder is evenly distributed in the wet mixture pellets, there are no bubbles on the spheres, and the spheres are round and have no tails; after freeze-drying, the actual ferrihydrite material is still spherical particles, and its volume becomes smaller than that of the wet mixture pellets due to dehydration.

[0043] Example 2

[0044] A method for preparing a ferrihydrite material for treating radioactive waste liquid is substantially the same as that in Example 1, except that:

[0045] In step (1) of preparing the ferrihydrite material for treating radioactive waste liquid, the mass ratio of chitosan to ferrihydrite is adjusted from 1:4 to 2:1, 1:1 or 1:2.

[0046] Experimental Example 1 Verification of the adsorption performance of the material prepared in Example 1

[0047] The specific operation to verify the adsorption performance of the material obtained in Example 1 is as follows:

[0048] (1) Prepare Co with concentrations of 1 mg / L, 2 mg / L, 3 mg / L, 4 mg / L, and 5 mg / L respectively. 2+ and Sr. 2+ The standard solution is used to measure and determine the atomic absorption spectrometry standard curve and prepare Co with an original concentration of 10 mg / L. 2+ and Sr. 2+ The solution is used as the object of material adsorption

[0049] (2) Take 14 150 mL conical flasks and divide them into two groups, 7 in each group, numbered as group 01 and group 02. Add 100 mL of Co to each conical flask in group 01. 2+ Solution, add 100mL of Sr to each conical flask in group 02 for future use 2+ solution, and add 0.2g of the prepared material into each conical flask.

[0050] (3) The temperature of the constant temperature oscillating box was set to 30°C, the oscillation frequency was set to 100 rpm, and the oscillation time was set to 24 hours. The 14 conical flasks in (2) were placed in the oscillating box. One conical flask of group 01 or group 02 in the oscillating box was taken out after the adsorption was carried out for 10 minutes, 30 minutes, 60 minutes, 3 hours, 6 hours, 12 hours, and 24 hours, and the Co content of the sample to be tested was determined by flame-graphite furnace atomic absorption spectrometry. 2+ , Sr 2+ Concentration

[0051] (4) Based on the results of (3), draw the adsorption curve and determine the adsorption equilibrium time (t q ), solution equilibrium concentration (C e ) and the maximum adsorption capacity (qmax ).

[0052] The adsorption capacity is calculated as follows:

[0053]

[0054] Where: C0——Co 2+ , Sr 2+ Initial values ​​of the concentrations of the two ion solutions (mg·L -1 );

[0055] C e ——Co 2+ , Sr 2+ The concentration of the solution when the adsorption of the two ions reaches equilibrium (mg·L -1 );

[0056] V——volume of solution (L);

[0057] qe——adsorption amount when adsorption reaches equilibrium (mg·g -1 );

[0058] m——mass of adsorbent added (g).

[0059] The static adsorption performance experiment shows that the ferrihydrite material for treating radioactive waste liquid prepared in Example 1 of the present invention has a good adsorption effect on cobalt and strontium. The appearance of the prepared material after treating the radioactive waste liquid does not change. The prepared material has a good adsorption effect on Co 2+ and Sr 2+ The adsorption process of Co 2+ The maximum adsorption capacity reached 35.274 mg·g -1 The removal rate is as high as 94.7%. 2+ The adsorption capacity reached 28.532 mg·g -1 , the removal rate is as high as 82.5%, and it is easy to separate from the solution.

[0060] Specific separation operation: There are two methods for separating the prepared material from the adsorption solution: filtration and magnetic separation. The filtration method is simple to operate and can be directly filtered using a filtration device (sand filter or membrane filter). The material recovery rate of the filtration method can reach 100%; the magnetic separation method uses the effect of the magnetic field to achieve separation. A magnetic seed material is added to the solution, and the prepared material is attached to the magnetic seed by stirring to form a magnetic aggregate. The high gradient magnetic separator (HGMS) equipment is then used to separate the magnetic aggregates. The material recovery rate of the magnetic separation method can generally reach 90%. Both recovery methods do not affect the appearance of the original material.

[0061] Experimental Example 2 Investigating the effect of the mass ratio of chitosan to ferrihydrite on the adsorption of the prepared material

[0062] 0.02 g of ferrihydrite material with a mass ratio of chitosan to ferrihydrite of 2:1, 1:1, 1:2 and 1:4 in the acetic acid solution containing chitosan prepared in Example 1 and Example 2 was taken respectively, and 6 repeated experiments were set for each mass ratio, and Co 2+ and Sr 2+ In the six solutions with different concentration gradients of the two ions, Co 2+ The six gradient concentrations were 1.0 mg·L -1 , 2.0mg·L -1 , 5.0mg·L -1 、10.0mg·L -1 , 20.0mg·L -1 and 40mg·L -1 , Sr. 2+ The six gradient concentrations were 0.8 mg·L -1 、1.6mg·L -1 , 4.0mg·L -1 , 8.0mg·L -1 、16.0mg·L -1 and 32.0mg·L -1 , the pH value was controlled at 7.5, the adsorption time was 3 hours, and the adsorption control temperature was 30°C.

[0063] like Figure 3 As shown, the ferrihydrite materials prepared in Examples 1 to 2 of the present invention have a 2+ and Sr 2+ The adsorption results of the ferrihydrite materials with different proportions are shown in Figure 2, where A is the adsorption of Co 2+ The isotherm adsorption curves of ferrihydrite materials with different proportions are shown in Figure 2. 2+ The adsorption isotherm of Figure 3 It can be seen that compared with ferrihydrite materials in other proportions, the ferrihydrite material in which the mass ratio of chitosan to ferrihydrite in the acetic acid solution containing chitosan prepared in Example 1 is 1:4 has the largest adsorption amount and the best adsorption effect. The reason may be that the ferrihydrite content is higher at this ratio and the porosity of the material is higher. Infrared characterization shows that the hydroxyl radical content of the material is very high, which is conducive to adsorption.

[0064] Experimental Example 3 Characterization of the adsorption of the material obtained in Example 1 using an infrared spectrometer

[0065] The ferrihydrite material in the acetic acid solution containing chitosan in Example 1 with a mass ratio of chitosan to ferrihydrite of 1:4 was tested using an infrared spectrometer, specifically: the sample was characterized by Fourier infrared on an infrared spectrometer. Test conditions: After background testing of the blank, 5 mg of ferrihydrite material with a ratio of 1:4 and 100 mg of potassium bromide were placed in a mortar, and after sufficient grinding, a small amount of the mixed sample was taken for tableting. During tableting, the tablet press pressure was gradually increased to 15 MPa, and the pressing time was 2 minutes. The prepared sample was placed in an infrared spectrometer for testing, with a scanning range of 400 to 4000 cm -1 , resolution 2cm -1 .

[0066] like Figure 4 As shown, the infrared spectrum of the ferrihydrite material of Example 1 of the present invention. Figure 4 It can be seen that the ferrihydrite material sample is between 3200 and 3400 cm -1 The absorption peak at 3300cm can be attributed to the stretching vibration of hydroxyl groups. The hydroxyl groups in the ferrihydrite material associate between molecules, and the polymers formed have connected hydrogen bonds. Therefore, the infrared absorption position moves to a lower wave number, and the peak shape becomes wider and blunter. -1 There are two weaker absorption peaks nearby, which can be attributed to the stretching vibration of amino groups. -1 There are two obvious absorption peaks, which can be attributed to the failure to completely deduct the background absorption of carbon dioxide in the air. -1 There are two obvious absorption peaks, which can be attributed to the stretching vibration of methyl. The sample is at 1060~1150cm -1 There are two weaker absorption peaks, which can be attributed to the stretching vibration of aliphatic ether. -1 The absorption peaks near the ferrihydrite are attributed to the absorption peaks of iron oxides. The results of infrared spectrum analysis show that the ferrihydrite material synthesized in Example 1 of the present invention has characteristic absorption peaks of both chitosan functional groups and iron oxides.

[0067] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.

Claims

1. A method for preparing a ferrihydrite material for treating radioactive waste liquid, characterized in that: The method includes: (1) adding ferrihydrite to an acetic acid solution containing chitosan, stirring uniformly to obtain a mixture; The ferrihydrite is obtained by adding concentrated ammonia water to a Fe(NO3)3·9H2O solution, adjusting the pH value of the solution to 7.5-8, stirring, standing, removing the upper clear liquid, and performing subsequent treatment on the lower suspension; (2) using a syringe with a needle to absorb the mixture obtained in step (1), adding a surfactant to the NaOH solution, and while continuously stirring the NaOH solution, slowly and evenly dripping the mixture in the syringe into the NaOH solution above the NaOH liquid surface; (3) After the addition, the mixture is in a spherical shape, and is allowed to solidify by standing, and then washed and freeze-dried to obtain a ferrihydrite material for treating radioactive waste liquid.

2. The preparation method according to claim 1, characterized in that: In step (1), the concentration of chitosan in the acetic acid solution containing chitosan is 40 g / L, and the concentration of acetic acid is 4%; the mass ratio of chitosan to ferrihydrite in the acetic acid solution containing chitosan is 1:

4.

3. The preparation method according to claim 1, characterized in that: In step (1), the subsequent processing is: The lower suspension was repeatedly washed and allowed to stand until the conductivity of the supernatant of the suspension dropped to 250 μS / cm after standing. The supernatant was removed, and the remaining suspension was centrifuged and freeze-dried in vacuum.

4. The preparation method according to claim 1, characterized in that: In step (2), the pore diameter of the needle is 0.1 mm; the concentration of the NaOH solution is 0.2 mol / L; and the vertical distance above the NaOH liquid surface is 25 to 35 cm.

5. The preparation method according to claim 1, characterized in that: In step (2), the surfactant is C 20 Polyoxyethylene ether; the concentration of the surfactant in the NaOH solution is 0.1 mol / L.

6. The preparation method according to claim 1, characterized in that: In step (2), the slow and uniform speed is 10 drops / minute.

7. The preparation method according to claim 1, characterized in that: In step (3), the probability that the mixture is spherical is greater than 90%.

8. A ferrihydrite material for treating radioactive waste liquid obtained by the preparation method according to any one of claims 1 to 7.

9. The ferrihydrite material for treating radioactive waste liquid according to claim 8, characterized in that: The material is spherical and its average particle size is 0.8 mm.

10. Use of the ferrihydrite material for treating radioactive waste liquid as claimed in claim 8 in the field of adsorption.