Preparation method of double-side grounding type thin film resistor

The described method enhances the precision and efficiency of double-sided grounded thin film resistor production by laser trimming and slotting, enabling accurate resistance values of less than ±1%.

CN119092239AActive Publication Date: 2024-12-06GUANGZHOU AURORA TECHNOLOGIES CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411270001.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-12-06
Estimated Expiration
2044-09-11

AI Technical Summary

Technical Problem

The existing manufacturing process of double-sided grounded thin film resistors lacks precision, with poor alignment accuracy and low efficiency in laser resistance adjustment, making it difficult to produce high-precision resistors with resistance values less than ±1%.

Method used

A method involving sequential depositions and electroplatings on both sides of an insulating substrate, followed by laser trimming and slotting, to form a double-sided grounded thin film resistor, allowing for accurate resistance measurement and adjustment before final assembly.

Benefits of technology

The method achieves high-precision double-sided grounded thin film resistors with resistance accuracy of less than ±1%, improving alignment accuracy and laser resistance adjustment efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092239A_ABST
    Figure CN119092239A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of thin film circuit manufacturing, and particularly relates to a preparation method of a double-side grounding type thin film resistor. The method comprises the following steps: preparing a front functional layer and a front resistive layer on the front of an insulating substrate to obtain a front resistor semi-finished product, performing laser resistance trimming on the front resistor semi-finished product, and grooving the insulating substrate of the front resistor semi-finished product to obtain the front resistor. According to the invention, through the step of adjusting the slotting, after the preparation of the front independent semi-product of the product is completed, on the premise of accurate measurement, laser resistance trimming is preferentially carried out, then the slotting of the insulating substrate is carried out, and finally the side wall and the back metallization grounding conduction are manufactured. The resistance precision of the double-side grounding type thin film resistor product obtained by the preparation method provided by the invention is less than + / -1%, and the alignment precision and the laser resistance trimming efficiency of the double-side grounding type thin film resistor are greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thin film circuit manufacturing, and in particular relates to a method for preparing a double-side grounded thin film resistor. Background Art

[0002] The classification of thin film circuits includes power dividers, attenuators, resistors, etc. Among them, resistors are an important classification of thin film circuits. There are usually four types according to the structure: double-sided metal thin film resistors (the structural diagram is as follows Figure 1 and Figure 2 As shown), single-side grounded thin film resistor (structural diagram as shown Figure 3 and Figure 4 As shown), double-side grounded thin film resistor (structural diagram as shown Figure 5 and Figure 6 As shown), single-sided metal film resistor (structural diagram as shown Figure 7 and Figure 8 Among them, the manufacturing process of double-side grounded thin film resistors is the most difficult.

[0003] At present, the manufacturing process of conventional double-sided grounded thin film resistors is as follows: first, the ceramic substrate is grooved according to the specifications of the design drawings, and then the resistance layer, adhesion layer, barrier layer and seed layer are sputtered, and finally formed by electroplating thickening, photolithography and etching. The grooves are cut by using a diamond cutter to cut through the ceramic at equal intervals. The metal film layer will cover the position where the ceramic is cut during sputtering to form a conduction, and electroplating will cause metal growth in the groove. The front side of the grounding resistor of the double-sided grounded thin film resistor is an independent resistance unit, but the conduction of the side wall makes the independent resistance units on the front side connected in parallel. Therefore, the disadvantage of the manufacturing process of the above-mentioned double-sided grounded thin film resistor is that the resistance value cannot be accurately tested after the entire piece is patterned. The resistance value can only be tested after the independent resistance units are cut and the front resistance is connected in series. However, at this time, laser adjustment of the resistance one by one is not only difficult to align, but also has extremely low resistance adjustment efficiency and poor accuracy.

[0004] Therefore, due to the above-mentioned current manufacturing process limitations, double-side grounded thin film resistors cannot be accurately laser-trimmed during the manufacturing process, that is, high-precision (less than ±1%) double-side grounded thin film resistors cannot be produced.

[0005] In summary, although the existing manufacturing process of the double-side grounded thin film resistor can ensure the grounding conduction effect of the sidewall metal, the disadvantage is that the precision is poor. Summary of the invention

[0006] The object of the present invention is to provide a method for preparing a double-sided grounded thin film resistor. The preparation method provided by the present invention can greatly improve the alignment accuracy and laser resistance adjustment efficiency of the double-sided grounded thin film resistor, thereby obtaining a high-precision double-sided grounded thin film resistor.

[0007] In order to achieve the above object, the present invention provides the following technical solutions:

[0008] The present invention provides a method for preparing a double-side grounded thin film resistor, comprising the following steps:

[0009] (1) performing a first deposition on the front surface of the insulating substrate to obtain a first semi-finished product, wherein the first deposition includes sequentially depositing a front resistance film, a front adhesion film, a front barrier film, and a front seed film;

[0010] (2) coating a photoresist on the front side of the first semi-finished product, and then transferring the pattern of the front functional layer to the front side of the first semi-finished product using a mask, and forming a patterned surface of the front functional layer after development to obtain a first patterned semi-finished product;

[0011] (3) performing a first electroplating on the first patterned semi-finished product, then removing the photoresist to obtain a front electroplating layer, etching the front seed film, the front barrier film and the front adhesion film outside the front electroplating layer area to obtain a front adhesion layer, a front barrier layer and a front seed layer, wherein the front seed layer and the front electroplating layer form a front functional layer to obtain a second semi-finished product;

[0012] (4) coating a photoresist on the front side of the second semi-finished product, and then transferring the front resistance layer pattern to the front side of the second semi-finished product using a mask, and forming a patterned surface of the front resistance layer after development to obtain a second patterned semi-finished product;

[0013] (5) etching the patterned surface of the resistor layer of the second patterned semi-finished product, and then removing the photoresist to form a front resistor layer on the front side of the insulating substrate to obtain a front resistor semi-finished product;

[0014] (6) laser trimming the resistance of the front resistor semi-finished product, and then slotting the insulating substrate, wherein the slotting position contacts the edge of the front functional layer, to obtain a semi-finished product with a through slot;

[0015] (7) performing a second deposition on the back side of the semi-finished product having the through groove and on the side wall of the through groove to obtain a third semi-finished product; the second deposition comprises sequentially depositing a back adhesive film and a side wall adhesive layer, a back barrier film and a side wall barrier layer, a back seed film and a side wall seed layer;

[0016] (8) performing a second electroplating on the third semi-finished product to obtain a fourth semi-finished product;

[0017] (9) After obtaining the fourth semi-finished product, or coating the back side of the fourth semi-finished product with photoresist, then using a mask to transfer the back functional layer pattern to the back side of the fourth semi-finished product, etching after development, and removing the photoresist, a back adhesive layer, a back barrier layer, a back seed layer and a back electroplating layer are obtained on the back side of the insulating substrate, and the back seed layer and the back electroplating layer form a back functional layer; and then removing the electroplated film formed during the second electroplating on the surface of the front resistance layer of the fourth semi-finished product, to obtain the double-side grounded thin film resistor;

[0018] Alternatively, the electroplated film formed during the second electroplating on the surface of the front resistor layer of the fourth semi-finished product is removed; then, a photoresist is coated on the back of the fourth semi-finished product, and a mask is used to transfer the back functional layer pattern to the back of the fourth semi-finished product, and etching is performed after development. After removing the photoresist, a back adhesion layer, a back barrier layer, a back seed layer and a back electroplating layer are obtained on the back of the insulating substrate. The back seed layer and the back electroplating layer form a back functional layer to obtain the double-sided grounded thin film resistor.

[0019] Preferably, in step (3): the material of the front electroplating layer is gold, and the thickness of the front electroplating layer is 1 to 4 μm.

[0020] Preferably, in step (8): the second electroplating forms an electroplated film on the front, side walls and back of the third semi-finished product, the material of the electroplated film formed by the second electroplating is gold, and the thickness of the electroplated film obtained by the second electroplating on the back of the third semi-finished product is 3 to 10 μm.

[0021] Preferably, the material of the front resistance layer is tantalum nitride; the thickness of the front resistance layer is 0.01-0.1 μm.

[0022] Preferably, the material of the front adhesive layer, the side wall adhesive layer and the back adhesive layer is titanium-tungsten alloy; the thickness of the front adhesive layer and the back adhesive layer is independently 0.1-0.5 μm.

[0023] Preferably, the material of the front barrier layer, the sidewall barrier layer and the back barrier layer is nickel; the thickness of the front barrier layer and the back barrier layer are independently 0.1-0.5 μm.

[0024] Preferably, the material of the front seed layer, the sidewall seed layer and the back seed layer is gold; the thickness of the front seed layer and the back seed layer is independently 1 to 3 μm.

[0025] Preferably, the insulating substrate is a ceramic substrate.

[0026] Preferably, the first deposition and the second deposition are performed by magnetron sputtering.

[0027] The magnetron sputtering is completed by a tunnel inline magnetron sputtering device transported by a carrier plate.

[0028] Preferably, in step (3), the etching method of the front seed film outside the front electroplating layer area is dry etching; the etching method of the front barrier film and the front adhesion film outside the front electroplating layer area is wet etching;

[0029] In step (5), the etching method for the patterned surface of the resistor layer of the second patterned semi-finished product is wet etching;

[0030] In step (9), the etching method of the back side of the fourth semi-finished product after development is as follows: the etching method of the back electroplating film is wet etching, the etching method of the back seed film is wet etching, and the etching method of the back barrier film and the back adhesion film is wet etching.

[0031] The present invention provides a method for preparing a double-side grounded thin-film resistor, comprising the following steps: (1) performing a first deposition on the front side of an insulating substrate to obtain a first semi-finished product, wherein the first deposition comprises sequentially depositing a front resistance film, a front adhesion film, a front barrier film and a front seed film; (2) coating a photoresist on the front side of the first semi-finished product, and then using a mask to transfer the pattern of the front functional layer to the front side of the first semi-finished product, and forming a patterned surface of the front functional layer after development to obtain a first patterned semi-finished product; (3) performing a first electroplating on the first patterned semi-finished product, and then removing the photoresist to obtain a front electroplated layer, and performing a first electroplating on the front seed film, the front barrier film and the front adhesion film outside the front electroplated layer area; (4) coating the front surface of the second semi-finished product with photoresist, and then using a mask to transfer the front resistance layer pattern to the front surface of the second semi-finished product, and forming a patterned surface of the front resistance layer after development, thereby obtaining a second patterned semi-finished product; (5) etching the patterned surface of the resistance layer of the second patterned semi-finished product, and then removing the photoresist, forming a front resistance layer on the front surface of the insulating substrate, and obtaining a front resistor semi-finished product; (6) laser trimming the resistance of the front resistor semi-finished product, and then slotting the insulating substrate, wherein the slotted position contacts the insulating substrate. The edge of the front functional layer is formed to obtain a semi-finished product with a through groove; (7) a second deposition is performed on the back side of the semi-finished product with the through groove and the side wall of the through groove to obtain a third semi-finished product; the second deposition includes sequentially depositing a back adhesive film and a side wall adhesive layer, a back barrier film and a side wall barrier layer, a back seed film and a side wall seed layer; (8) the third semi-finished product is subjected to a second electroplating to obtain a fourth semi-finished product; (9) after obtaining the fourth semi-finished product, the back side of the fourth semi-finished product is coated with photoresist, and then the back functional layer pattern is transferred to the back side of the fourth semi-finished product using a mask, and then etching is performed after development. After removing the photoresist, a back adhesive layer, a back barrier layer, and a back seed layer are obtained on the back side of the insulating substrate. layer and a back electroplating layer, the back seed layer and the back electroplating layer form a back functional layer; after removing the electroplated film formed during the second electroplating on the surface of the front resistor layer of the fourth semi-finished product, the double-sided grounded thin film resistor is obtained; or the electroplated film formed during the second electroplating on the surface of the front resistor layer of the fourth semi-finished product is removed; then the back side of the fourth semi-finished product is coated with photoresist, the back functional layer pattern is transferred to the back side of the fourth semi-finished product using a mask, and etching is performed after development. After removing the photoresist, a back adhesion layer, a back barrier layer, a back seed layer and a back electroplating layer are obtained on the back side of the insulating substrate, the back seed layer and the back electroplating layer form a back functional layer, and the double-sided grounded thin film resistor is obtained.The preparation method provided by the present invention abandons the method in the prior art of first grooving a ceramic substrate according to the specifications of the drawing and then sputtering a resistor film layer, an adhesion layer, a barrier layer and a seed layer. The present invention first prepares a front functional layer and a resistor layer on the front side of an insulating substrate, obtains a front resistor semi-finished product, performs laser resistance adjustment on the front resistor semi-finished product, and then grooves the insulating substrate of the front resistor semi-finished product. The present invention achieves that after the product is completed as an independent front series semi-product, laser resistance adjustment is performed first on the premise of accurate measurement, and then the insulating substrate is grooved, and finally the side wall and the back metallization grounding connection are made, thereby providing a high-precision double-sided grounded thin film resistor preparation method capable of laser resistance adjustment. The resistance accuracy of the double-sided grounded thin film resistor product obtained by the preparation method provided by the present invention is less than ±1%, which greatly improves the alignment accuracy and laser resistance adjustment efficiency of the double-sided grounded thin film resistor. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It is a cross-sectional view of a double-sided metal film resistor;

[0033] Figure 2 It is a top view of a double-sided metal film resistor;

[0034] Figure 3 It is a cross-sectional view of a single-side grounded thin film resistor;

[0035] Figure 4 It is a top view of a single-side grounded thin film resistor;

[0036] Figure 5 It is a cross-sectional view of a double-side grounded thin film resistor;

[0037] Figure 6 It is a top view of a double-side grounded thin film resistor;

[0038] Figure 7 It is a cross-sectional view of a single-sided metal film resistor;

[0039] Figure 8 It is a top view of a single-sided metal film resistor;

[0040] In the figure: 1 is a ceramic substrate; 2 is a front resistance layer; 3 is a front adhesion layer; 4 is a front barrier layer; 5 is a front functional layer; 6 is a side wall adhesion layer; 7 is a side wall barrier layer; 8 is a side wall functional layer; 9 is a back adhesion layer; 10 is a back barrier layer; 11 is a back functional layer. DETAILED DESCRIPTION

[0041] The present invention provides a method for preparing a double-side grounded thin film resistor, comprising the following steps:

[0042] (1) performing a first deposition on the front surface of the insulating substrate to obtain a first semi-finished product, wherein the first deposition includes sequentially depositing a front resistance film, a front adhesion film, a front barrier film, and a front seed film;

[0043] (2) coating a photoresist on the front side of the first semi-finished product, and then transferring the pattern of the front functional layer to the front side of the first semi-finished product using a mask, and forming a patterned surface of the front functional layer after development to obtain a first patterned semi-finished product;

[0044] (3) performing a first electroplating on the first patterned semi-finished product, then removing the photoresist to obtain a front electroplating layer, etching the front seed film, the front barrier film and the front adhesion film outside the front electroplating layer area to obtain a front adhesion layer, a front barrier layer and a front seed layer, wherein the front seed layer and the front electroplating layer form a front functional layer to obtain a second semi-finished product;

[0045] (4) coating a photoresist on the front side of the second semi-finished product, and then transferring the front resistance layer pattern to the front side of the second semi-finished product using a mask, and forming a patterned surface of the front resistance layer after development to obtain a second patterned semi-finished product;

[0046] (5) etching the patterned surface of the resistor layer of the second patterned semi-finished product, and then removing the photoresist to form a front resistor layer on the front side of the insulating substrate to obtain a front resistor semi-finished product;

[0047] (6) laser trimming the resistance of the front resistor semi-finished product, and then slotting the insulating substrate, wherein the slotting position contacts the edge of the front functional layer, to obtain a semi-finished product with a through slot;

[0048] (7) performing a second deposition on the back side of the semi-finished product having the through groove and on the side wall of the through groove to obtain a third semi-finished product; the second deposition comprises sequentially depositing a back adhesive film and a side wall adhesive layer, a back barrier film and a side wall barrier layer, a back seed film and a side wall seed layer;

[0049] (8) performing a second electroplating on the third semi-finished product to obtain a fourth semi-finished product;

[0050] (9) After obtaining the fourth semi-finished product, or coating the back side of the fourth semi-finished product with photoresist, then using a mask to transfer the back functional layer pattern to the back side of the fourth semi-finished product, etching after development, and removing the photoresist, a back adhesive layer, a back barrier layer, a back seed layer and a back electroplating layer are obtained on the back side of the insulating substrate, and the back seed layer and the back electroplating layer form a back functional layer; and then removing the electroplated film formed during the second electroplating on the surface of the front resistance layer of the fourth semi-finished product, to obtain the double-side grounded thin film resistor;

[0051] Alternatively, the electroplated film formed during the second electroplating on the surface of the front resistor layer of the fourth semi-finished product is removed; then, a photoresist is coated on the back of the fourth semi-finished product, and a mask is used to transfer the back functional layer pattern to the back of the fourth semi-finished product, and etching is performed after development. After removing the photoresist, a back adhesion layer, a back barrier layer, a back seed layer and a back electroplating layer are obtained on the back of the insulating substrate. The back seed layer and the back electroplating layer form a back functional layer to obtain the double-sided grounded thin film resistor.

[0052] The present invention performs a first deposition on the front side of an insulating substrate to obtain a first semi-finished product, wherein the first deposition includes sequentially depositing a front resistance film, a front adhesion film, a front barrier film, and a front seed film. In the present invention, the insulating substrate is preferably a ceramic substrate. In the present invention, the thickness of the insulating substrate is preferably 0.1 to 0.6 mm, and is particularly preferably 0.127 mm, 0.254 mm, 0.381 mm, or 0.508 mm. Before the deposition, the present invention sequentially cleans and dries the insulating substrate. The present invention has no special requirements for the specific implementation of the cleaning and drying. The first deposition method is preferably magnetron sputtering. The magnetron sputtering is performed by a tunnel-line magnetron sputtering device transported by a carrier.

[0053] After obtaining the first semi-finished product, a photoresist is coated on the front side of the first semi-finished product, and then a mask is used to transfer the pattern of the front functional layer to the front side of the first semi-finished product, and after development, a patterned surface of the front functional layer is formed to obtain the first patterned semi-finished product. The present invention has no special requirements for the specific implementation methods of the coating of the photoresist, the transfer of the pattern of the front functional layer, and the development.

[0054] After obtaining the first patterned semi-finished product, the present invention performs a first electroplating on the first patterned semi-finished product, and then removes the photoresist to obtain a front electroplating layer, etches the front seed film, the front barrier film and the front adhesion film outside the front electroplating layer area to obtain a front adhesion layer, a front barrier layer and a front seed layer, the front seed layer and the front electroplating layer form a front functional layer to obtain a second semi-finished product.

[0055] The present invention has no special requirements for the specific implementation of the first electroplating. The material of the front electroplating layer obtained by the first electroplating is preferably gold, and the thickness of the front electroplating layer is preferably 1 to 4 μm. The thickness of the front electroplating layer is greater than the thickness of the front seed film. The etching method of the front seed film outside the front electroplating layer area is dry etching, specifically argon ion etching. In the present invention, the dry etching etches the front electroplating layer and the front seed film outside the front electroplating layer area at the same time. Since the thickness of the front electroplating layer obtained by the first electroplating is greater than the thickness of the front seed film, after the front seed film outside the front electroplating layer area is etched, there is still a remaining front electroplating layer, and the front functional layer is composed of the remaining front electroplating layer after the front electroplating layer is etched and the front seed layer thereunder. The etching method of the front barrier layer and the front adhesion layer is preferably wet etching. The present invention has no special requirements for the specific implementation of the wet etching.

[0056] In the present invention, the material of the front adhesion layer is preferably titanium-tungsten alloy; the thickness of the front adhesion layer is preferably 0.1-0.5 μm. The material of the front barrier layer is preferably nickel; the thickness of the front barrier layer is preferably 0.1-0.5 μm. The material of the front seed layer is preferably gold; the thickness of the front seed layer is preferably 1-3 μm.

[0057] After obtaining the second semi-finished product, the present invention coats a photoresist on the front side of the second semi-finished product, and then uses a mask to transfer the front resistance layer pattern to the front side of the second semi-finished product, and after development, a front resistance layer patterned surface is formed to obtain the second patterned semi-finished product. The present invention has no special requirements for the specific implementation methods of the coating of the photoresist, the transfer of the resistance layer pattern, and the development.

[0058] After obtaining the second patterned semi-finished product, the present invention etches the patterned surface of the resistor layer of the second patterned semi-finished product, then removes the photoresist, forms a front resistor layer on the front side of the insulating substrate, and obtains a front resistor semi-finished product. In the present invention, the etching method of the patterned surface of the resistor layer of the second patterned semi-finished product is preferably wet etching. The present invention has no special requirements for the specific implementation of the wet etching shown.

[0059] In the present invention, the material of the front resistance layer is preferably tantalum nitride; the thickness of the front resistance layer is preferably 0.01-0.1 μm.

[0060] In the present invention, a plurality of front resistor semi-finished products are formed on the front surface of the insulating substrate, and the plurality of front resistor semi-finished products on the front surface of the insulating substrate are arranged in an array.

[0061] After obtaining the semi-finished front resistor, the present invention performs laser resistance trimming on the semi-finished front resistor, and then grooves the insulating substrate, where the grooves are in contact with the edge of the functional layer, to obtain a semi-finished product with a through groove. The grooves in the present invention are in contact with the edge of the functional layer, so that after the subsequent second deposition on the back side, the front functional layer, the sidewall seed layer and the back seed film are connected, and thickened during the second electroplating.

[0062] The present invention has no special requirements for the specific implementation of the excitation adjustment group. After obtaining the front resistor semi-finished product, that is, after completing the front independent series connection product of the double-sided grounded thin film resistor, the present invention performs laser resistance adjustment. The laser resistance adjustment can realize accurate laser resistance adjustment of multiple front resistor semi-finished products on the insulating substrate, thereby obtaining a method for preparing a high-precision double-sided grounded thin film resistor that can be laser adjusted. The resistance accuracy of the double-sided grounded thin film resistor product obtained by the present invention is less than ±1%. In the present invention, part of the insulating substrate of the fixed strip is retained at both ends of the slot. The slotting is performed by equipment slotting.

[0063] After obtaining the semi-finished product with the through groove, the present invention performs a second deposition on the back side of the semi-finished product with the through groove and the side wall of the through groove to obtain a third semi-finished product; the second deposition includes sequentially depositing a back adhesion film and a side wall adhesion layer, a back barrier film and a side wall barrier layer, a back seed film and a side wall seed layer. In the present invention, the material of the back adhesion film is preferably a titanium-tungsten alloy; the thickness of the back adhesion film is preferably 0.1 to 0.5 μm. The material of the back barrier film is preferably nickel; the thickness of the back barrier film is preferably 0.1 to 0.5 μm. The material of the back seed film is preferably gold; the thickness of the back seed film is preferably 1 to 3 μm. The second deposition method is preferably magnetron sputtering. The present invention has no special requirements for the specific implementation of the magnetron sputtering.

[0064] After obtaining the third semi-finished product, the present invention performs a second electroplating on the third semi-finished product to obtain a fourth semi-finished product. The present invention has no special requirements for the specific implementation of the second electroplating. In the present invention, the second electroplating forms an electroplated film on the front, sidewall and back of the third semi-finished product, the material of the electroplated film formed by the second electroplating is gold, and the thickness of the electroplated film obtained by the second electroplating on the back of the third semi-finished product is 3 to 10 μm.

[0065] In the present invention, the second electroplating forms a second electroplated film on the front resistor layer, the front functional layer, the sidewall seed layer and the back seed film surface of the third semi-finished product. The front functional layer of the front resistor semi-finished product (and the third semi-finished product) and the second electroplated film formed by the second electroplating on the front functional layer together serve as the front functional layer of the double-side grounded thin film resistor. The second electroplated film formed by the second electroplating on the surface of the sidewall seed layer together constitutes the sidewall functional layer.

[0066] After obtaining the fourth semi-finished product, the present invention either coats the back of the fourth semi-finished product with photoresist, then uses a mask to transfer the back functional layer pattern to the back of the fourth semi-finished product, performs etching after development, and removes the photoresist to obtain a back adhesion layer, a back barrier layer, a back seed layer, and a back electroplating layer on the back of the insulating substrate, wherein the back seed layer and the back electroplating layer form a back functional layer; and then removes the electroplated film formed during the second electroplating on the surface of the front resistance layer of the fourth semi-finished product to obtain the double-sided grounded thin film resistor. In the present invention, after obtaining the back functional layer, the present invention preferably applies UV glue to the back of the semi-finished product obtained at this time for protection, and finally removes the electroplated film formed during the second electroplating on the surface of the front resistance layer of the fourth semi-finished product. The specific implementation method of the removal is preferably removal by dipping in glue.

[0067] After obtaining the fourth semi-finished product, the present invention removes the electroplated film formed during the second electroplating on the surface of the front resistor layer of the fourth semi-finished product; then the back of the fourth semi-finished product is coated with photoresist, and then the back functional layer pattern is transferred to the back of the fourth semi-finished product using a mask, and after development, etching is performed, and after removing the photoresist, a back adhesion layer, a back barrier layer, a back seed layer and a back electroplating layer are obtained on the back of the insulating substrate, and the back seed layer and the back electroplating layer form a back functional layer to obtain the double-sided grounded thin film resistor. In the present invention, the specific implementation of removing the electroplated film formed during the second electroplating on the surface of the front resistor layer of the fourth semi-finished product is preferably removal by dipping.

[0068] In the present invention, the etching method after the back side of the fourth semi-finished product is developed is preferably: the etching method for the back electroplating film is wet etching, the etching method for the back seed film is wet etching, and the etching method for the back barrier film and the back adhesion film is wet etching.

[0069] In the present invention, after obtaining the back functional layer and removing the electroplated film formed during the second electroplating on the surface of the front resistance layer of the fourth semi-finished product, the present invention preferably obtains a single double-side grounded thin film resistor by scribing. In the present invention, when scribing, the present invention preferably expands a suitable spacing on the blue film.

[0070] In the present invention, the insulating substrate is cut to obtain a single rough product of a double-sided grounded thin film resistor. The present invention preferably trims the excess grounding metal burrs on the back and side walls of the single rough product of the double-sided grounded thin film resistor to obtain a single finished product of the double-sided grounded thin film resistor.

[0071] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0072] Example 1

[0073] This embodiment uses a ceramic substrate with a thickness of 0.127 mm. The ceramic substrate is first cleaned and dried, and then a tantalum nitride film (front resistance film, 0.01 μm), a titanium tungsten alloy film (front adhesion film, 0.1 μm), a nickel film (front barrier film, 0.1 μm), and a gold film (front seed film, 1.0 μm) are sputtered on the front of the ceramic substrate in sequence; after the sputtering, a photoresist is coated on the surface of the front seed film on the front of the ceramic substrate, and a mask is used to transfer the pattern of the front functional layer to the front seed film of the ceramic substrate, and the front The front functional layer pattern is formed; then the first electroplating is performed, and the thickness of the gold film obtained by the first electroplating is 1 to 4 μm (for example: 2 μm, 3 μm, 4 μm, and the thickness of the gold film obtained by electroplating is greater than the thickness of the front seed layer); the photoresist is stripped to obtain the front electroplating layer; the front electroplating layer and the front seed layer are dry-etched (argon ion etching) on ​​the front side of the ceramic to obtain the front seed layer, the front electroplating layer and the front seed layer form a front functional layer, and the nickel film and the titanium-tungsten alloy film at the bottom of the front seed layer are wet-etched once to obtain the front barrier layer and the front adhesion layer, exposing the front tantalum nitride film.

[0074] Photoresist is coated on the surface of the front functional layer and the surface of the front tantalum nitride film, and the pattern of the front resistor layer is transferred to the tantalum nitride film of the ceramic substrate using a mask plate to develop the front resistor layer pattern; the resistor layer pattern is etched, and then the photoresist is removed to form a front resistor layer and a front functional layer on the front side of the ceramic substrate to obtain a front resistor semi-finished product.

[0075] The semi-finished product of the front resistor is laser trimmed, with an initial resistance of 8.24±10%Ω and a final resistance of 12.50±1%Ω; the dicing equipment is used to make grooves, and part of the ceramic of the fixed strip is retained at both ends; the groove position contacts the edge of the front functional layer to obtain a penetrating groove.

[0076] Then, a titanium-tungsten alloy film (0.1 μm back adhesion film and side wall adhesion layer), a nickel film (0.1 μm back barrier film and side wall barrier layer), and a gold film (1.0 μm back seed film and side wall seed layer) are sequentially sputtered on the back side of the ceramic substrate and the side wall obtained by the grooves to obtain a third semi-finished product;

[0077] After the sputtering is completed, the third finished product is electroplated for the second time. The thickness of the gold film obtained by the second electroplating on the surface of the back seed film on the back side is 3 to 10 μm (for example: 3 μm, 4 μm, 6 μm, 8 μm). Then, the surface of the back electroplated film obtained by the second electroplating on the back side is coated with photoresist, and the pattern of the back functional layer is transferred to the back electroplated film using a mask plate, and the back functional layer pattern is developed; then, wet etching is performed in sequence to obtain the back electroplated layer and the back seed layer. The back electroplated layer and the back seed layer form the back functional layer, and the back nickel film and the titanium tungsten alloy film are wet-etched once to obtain the back barrier layer and the back adhesion layer. Then, UV glue is applied to the back side, and the front side is dipped in glue to remove the excess gold film on the front resistor layer (formed by the second electroplating); a single finished product is cut, and the excess metal burrs of the side wall grounding are trimmed to obtain a single double-sided grounded thin film resistor.

[0078] Example 2

[0079] This embodiment uses a ceramic substrate with a thickness of 0.254 mm. The ceramic substrate is first cleaned and dried, and then a tantalum nitride film (front resistance film, 0.01 μm), a titanium tungsten alloy film (front adhesion film, 0.1 μm), a nickel film (front barrier film, 0.1 μm), and a gold film (front seed film, 1.0 μm) are sputtered on the front of the ceramic substrate in sequence; after the sputtering, a photoresist is coated on the surface of the front seed film on the front of the ceramic substrate, and a mask is used to transfer the pattern of the front functional layer to the front seed film of the ceramic substrate, and the front The front functional layer pattern is formed; then the first electroplating is performed, and the thickness of the gold film obtained by the first electroplating is 1 to 4 μm (for example: 2 μm, 3 μm, 4 μm, and the thickness of the gold film obtained by electroplating is greater than the thickness of the front seed layer); the photoresist is stripped to obtain the front electroplating layer; the front electroplating layer and the front seed layer are dry-etched (argon ion etching) on ​​the front side of the ceramic to obtain the front seed layer, the front electroplating layer and the front seed layer form a front functional layer, and the nickel film and the titanium-tungsten alloy film at the bottom of the front seed layer are wet-etched once to obtain the front barrier layer and the front adhesion layer, exposing the front tantalum nitride film.

[0080] Photoresist is coated on the surface of the front functional layer and the surface of the front tantalum nitride film, and the pattern of the front resistor layer is transferred to the tantalum nitride film of the ceramic substrate using a mask plate to develop the front resistor layer pattern; the resistor layer pattern is etched, and then the photoresist is removed to form a front resistor layer and a front functional layer on the front side of the ceramic substrate to obtain a front resistor semi-finished product.

[0081] The semi-finished front resistor is laser trimmed, with an initial resistance of 11.65±10%Ω and a final resistance of 25.00±1%Ω; the dicing equipment is used to make grooves, and part of the ceramic of the fixed strip is retained at both ends; the groove position contacts the edge of the front functional layer to obtain a penetrating groove.

[0082] Then, a titanium-tungsten alloy film (0.1 μm back adhesion film and side wall adhesion layer), a nickel film (0.1 μm back barrier film and side wall barrier layer), and a gold film (1.0 μm back seed film and side wall seed layer) are sequentially sputtered on the back side of the ceramic substrate and the side wall obtained by the grooves to obtain a third semi-finished product;

[0083] After the sputtering is completed, the third finished product is electroplated for the second time. The thickness of the gold film obtained by the second electroplating on the surface of the back seed film on the back side is 3 to 10 μm (for example: 3 μm, 4 μm, 6 μm, 8 μm). Then, the surface of the back electroplated film obtained by the second electroplating on the back side is coated with photoresist, and the pattern of the back functional layer is transferred to the back electroplated film using a mask plate, and the back functional layer pattern is developed; then, wet etching is performed in sequence to obtain the back electroplated layer and the back seed layer. The back electroplated layer and the back seed layer form the back functional layer, and the back nickel film and the titanium tungsten alloy film are wet-etched once to obtain the back barrier layer and the back adhesion layer. Then, UV glue is applied to the back side, and the front side is dipped in glue to remove the excess gold film on the front resistor layer (formed by the second electroplating); a single finished product is cut, and the excess metal burrs of the side wall grounding are trimmed to obtain a single double-sided grounded thin film resistor.

[0084] Example 3

[0085] In this embodiment, a ceramic substrate with a thickness of 0.381 mm is used. The ceramic substrate is first cleaned and dried, and then a tantalum nitride film (front resistance film, 0.01 μm), a titanium tungsten alloy film (front adhesion film, 0.1 μm), a nickel film (front barrier film, 0.1 μm), and a gold film (front seed film, 1.0 μm) are sputtered on the front of the ceramic substrate in sequence; after the sputtering, a photoresist is coated on the surface of the front seed film on the front of the ceramic substrate, and a mask is used to transfer the pattern of the front functional layer to the front seed film of the ceramic substrate, and a positive The front functional layer pattern is formed; then the first electroplating is performed, and the thickness of the gold film obtained by the first electroplating is 1 to 4 μm (for example: 2 μm, 3 μm, 4 μm, and the thickness of the gold film obtained by electroplating is greater than the thickness of the front seed layer); the photoresist is stripped to obtain the front electroplating layer; the front electroplating layer and the front seed layer are dry-etched (argon ion etching) on ​​the front side of the ceramic to obtain the front seed layer, the front electroplating layer and the front seed layer form a front functional layer, and the nickel film and the titanium-tungsten alloy film at the bottom of the front seed layer are wet-etched once to obtain the front barrier layer and the front adhesion layer, exposing the front tantalum nitride film.

[0086] Photoresist is coated on the surface of the front functional layer and the surface of the front tantalum nitride film, and the pattern of the front resistor layer is transferred to the tantalum nitride film of the ceramic substrate using a mask plate to develop the front resistor layer pattern; the resistor layer pattern is etched, and then the photoresist is removed to form a front resistor layer and a front functional layer on the front side of the ceramic substrate to obtain a front resistor semi-finished product.

[0087] The semi-finished front resistor is laser trimmed, with an initial resistance of 27.21±10%Ω and a final resistance of 50.00±1%Ω; the dicing equipment is used to make grooves, and part of the ceramic of the fixed strip is retained at both ends; the groove position contacts the edge of the front functional layer to obtain a penetrating groove.

[0088] Then, a titanium-tungsten alloy film (0.1 μm back adhesion film and side wall adhesion layer), a nickel film (0.1 μm back barrier film and side wall barrier layer), and a gold film (1.0 μm back seed film and side wall seed layer) are sequentially sputtered on the back side of the ceramic substrate and the side wall obtained by the grooves to obtain a third semi-finished product;

[0089] After the sputtering is completed, the third finished product is electroplated for the second time. The thickness of the gold film obtained by the second electroplating on the surface of the back seed film on the back side is 3 to 10 μm (for example: 3 μm, 4 μm, 6 μm, 8 μm). Then, the surface of the back electroplated film obtained by the second electroplating on the back side is coated with photoresist, and the pattern of the back functional layer is transferred to the back electroplated film using a mask plate, and the back functional layer pattern is developed; then, wet etching is performed in sequence to obtain the back electroplated layer and the back seed layer. The back electroplated layer and the back seed layer form the back functional layer, and the back nickel film and the titanium tungsten alloy film are wet-etched once to obtain the back barrier layer and the back adhesion layer. Then, UV glue is applied to the back side, and the front side is dipped in glue to remove the excess gold film on the front resistor layer (formed by the second electroplating); a single finished product is cut, and the excess metal burrs of the side wall grounding are trimmed to obtain a single double-sided grounded thin film resistor.

[0090] Example 4

[0091] This embodiment uses a ceramic substrate with a thickness of 0.508 mm. The ceramic substrate is first cleaned and dried, and then a tantalum nitride film (front resistance film, 0.01 μm), a titanium tungsten alloy film (front adhesion film, 0.1 μm), a nickel film (front barrier film, 0.1 μm), and a gold film (front seed film, 1.0 μm) are sputtered on the front of the ceramic substrate in sequence; after the sputtering, a photoresist is coated on the surface of the front seed film on the front of the ceramic substrate, and a mask is used to transfer the pattern of the front functional layer to the front seed film of the ceramic substrate, and the front The front functional layer pattern is formed; then the first electroplating is performed, and the thickness of the gold film obtained by the first electroplating is 1 to 4 μm (for example: 2 μm, 3 μm, 4 μm, and the thickness of the gold film obtained by electroplating is greater than the thickness of the front seed layer); the photoresist is stripped to obtain the front electroplating layer; the front electroplating layer and the front seed layer are dry-etched (argon ion etching) on ​​the front side of the ceramic to obtain the front seed layer, the front electroplating layer and the front seed layer form a front functional layer, and the nickel film and the titanium-tungsten alloy film at the bottom of the front seed layer are wet-etched once to obtain the front barrier layer and the front adhesion layer, exposing the front tantalum nitride film.

[0092] Photoresist is coated on the surface of the front functional layer and the surface of the front tantalum nitride film, and the pattern of the front resistor layer is transferred to the tantalum nitride film of the ceramic substrate using a mask plate to develop the front resistor layer pattern; the resistor layer pattern is etched, and then the photoresist is removed to form a front resistor layer and a front functional layer on the front side of the ceramic substrate to obtain a front resistor semi-finished product.

[0093] The semi-finished front resistor was laser trimmed, with an initial resistance of 67.54±10%Ω and a final resistance of 100.00±1%Ω; the dicing equipment was used to make grooves, and part of the ceramic of the fixed strips was retained at both ends; the groove position contacted the edge of the front functional layer to obtain a penetrating groove.

[0094] Then, a titanium-tungsten alloy film (0.1 μm back adhesion film and side wall adhesion layer), a nickel film (0.1 μm back barrier film and side wall barrier layer), and a gold film (1.0 μm back seed film and side wall seed layer) are sequentially sputtered on the back side of the ceramic substrate and the side wall obtained by the grooves to obtain a third semi-finished product;

[0095] After the sputtering is completed, the third finished product is electroplated for the second time. The thickness of the gold film obtained by the second electroplating on the surface of the back seed film on the back side is 3 to 10 μm (for example: 3 μm, 4 μm, 6 μm, 8 μm). Then, the surface of the back electroplated film obtained by the second electroplating on the back side is coated with photoresist, and the pattern of the back functional layer is transferred to the back electroplated film using a mask plate, and the back functional layer pattern is developed; then, wet etching is performed in sequence to obtain the back electroplated layer and the back seed layer. The back electroplated layer and the back seed layer form the back functional layer, and the back nickel film and the titanium tungsten alloy film are wet-etched once to obtain the back barrier layer and the back adhesion layer. Then, UV glue is applied to the back side, and the front side is dipped in glue to remove the excess gold film on the front resistor layer (formed by the second electroplating); a single finished product is cut, and the excess metal burrs of the side wall grounding are trimmed to obtain a single double-sided grounded thin film resistor.

[0096] It can be seen from the above embodiments that the preparation method provided by the present invention abandons the method in the prior art of first grooving the ceramic substrate according to the specifications of the drawing and then sputtering the resistor film layer, the adhesion layer, the barrier layer and the seed layer. The present invention first prepares the front functional layer and the front resistor layer on the front side of the insulating substrate, obtains the front resistor semi-finished product, performs laser resistance adjustment on the front resistor semi-finished product, and then grooves the insulating substrate of the front resistor semi-finished product. The present invention adjusts the grooving steps to achieve that after the product completes the front independent series semi-product, laser resistance adjustment is performed first, and then the insulating substrate is grooved, and finally the side wall and the back metallization grounding connection are made, thereby providing a high-precision double-sided grounded thin film resistor preparation method that can be laser-adjusted. The resistance accuracy of the double-sided grounded thin film resistor product obtained by the preparation method provided by the present invention is less than ±1%, which greatly improves the alignment accuracy and laser resistance adjustment efficiency of the double-sided grounded thin film resistor.

[0097] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for preparing a double-side grounded thin film resistor, characterized in that: The following steps are involved: (1) performing a first deposition on the front surface of the insulating substrate to obtain a first semi-finished product, wherein the first deposition includes sequentially depositing a front resistance film, a front adhesion film, a front barrier film, and a front seed film; (2) coating a photoresist on the front side of the first semi-finished product, and then transferring the pattern of the front functional layer to the front side of the first semi-finished product using a mask, and forming a patterned surface of the front functional layer after development to obtain a first patterned semi-finished product; (3) performing a first electroplating on the first patterned semi-finished product, then removing the photoresist to obtain a front electroplating layer, etching the front seed film, the front barrier film and the front adhesion film outside the front electroplating layer area to obtain a front adhesion layer, a front barrier layer and a front seed layer, wherein the front seed layer and the front electroplating layer form a front functional layer to obtain a second semi-finished product; (4) coating a photoresist on the front side of the second semi-finished product, and then transferring the front resistance layer pattern to the front side of the second semi-finished product using a mask, and forming a patterned surface of the front resistance layer after development to obtain a second patterned semi-finished product; (5) etching the patterned surface of the resistor layer of the second patterned semi-finished product, and then removing the photoresist to form a front resistor layer on the front side of the insulating substrate to obtain a front resistor semi-finished product; (6) laser trimming the resistance of the front resistor semi-finished product, and then slotting the insulating substrate, wherein the slotting position contacts the edge of the front functional layer, to obtain a semi-finished product with a through slot; (7) performing a second deposition on the back side of the semi-finished product having the through groove and on the side wall of the through groove to obtain a third semi-finished product; the second deposition comprises sequentially depositing a back adhesive film and a side wall adhesive layer, a back barrier film and a side wall barrier layer, a back seed film and a side wall seed layer; (8) performing a second electroplating on the third semi-finished product to obtain a fourth semi-finished product; (9) After obtaining the fourth semi-finished product, or coating the back side of the fourth semi-finished product with photoresist, then transferring the back side functional layer pattern to the back side of the fourth semi-finished product using a mask, performing etching after development, and removing the photoresist to obtain a back side adhesion layer, a back side barrier layer, a back side seed layer and a back side electroplating layer on the back side of the insulating substrate, wherein the back side seed layer and the back side electroplating layer form a back side functional layer; After removing the electroplated film formed during the second electroplating on the surface of the front resistance layer of the fourth semi-finished product, the double-side grounded thin film resistor is obtained; or removing the electroplated film formed during the second electroplating on the surface of the front resistance layer of the fourth semi-finished product; Then, the back side of the fourth semi-finished product is coated with photoresist, and the back functional layer pattern is transferred to the back side of the fourth semi-finished product using a mask. After development, etching is performed. After removing the photoresist, a back adhesion layer, a back barrier layer, a back seed layer and a back electroplating layer are obtained on the back side of the insulating substrate. The back seed layer and the back electroplating layer form a back functional layer to obtain the double-sided grounded thin film resistor.

2. The preparation method according to claim 1, characterized in that: In step (3): the material of the front electroplating layer is gold, and the thickness of the front electroplating layer is 1 to 4 μm.

3. The preparation method according to claim 1, characterized in that: In step (8): the second electroplating forms an electroplated film on the front, side walls and back of the third semi-finished product, the material of the electroplated film formed by the second electroplating is gold, and the thickness of the electroplated film obtained by the second electroplating on the back of the third semi-finished product is 3 to 10 μm.

4. The preparation method according to any one of claims 1 to 3, characterized in that: The material of the front resistance layer is tantalum nitride; the thickness of the front resistance layer is 0.01-0.1 μm.

5. The preparation method according to any one of claims 1 to 3, characterized in that: The materials of the front adhesive layer, the side wall adhesive layer and the back adhesive layer are titanium-tungsten alloy; the thickness of the front adhesive layer and the back adhesive layer are independently 0.1-0.5 μm.

6. The preparation method according to any one of claims 1 to 3, characterized in that: The material of the front barrier layer, the sidewall barrier layer and the back barrier layer is nickel; the thickness of the front barrier layer and the back barrier layer is independently 0.1-0.5 μm.

7. The preparation method according to any one of claims 1 to 3, characterized in that: The material of the front seed layer, the sidewall seed layer and the back seed layer is gold; the thickness of the front seed layer and the back seed layer is independently 1 to 3 μm.

8. The preparation method according to any one of claims 1 to 3, characterized in that: The insulating substrate is a ceramic substrate.

9. The preparation method according to claim 1, characterized in that: The first deposition and the second deposition are performed by magnetron sputtering. The magnetron sputtering is completed by a tunnel inline magnetron sputtering device transported by a carrier plate.

10. The preparation method according to claim 1, characterized in that: In step (3), the etching method of the front seed film outside the front electroplating layer area is dry etching; the etching method of the front barrier film and the front adhesion film outside the front electroplating layer area is wet etching; In step (5), the etching method for the patterned surface of the resistor layer of the second patterned semi-finished product is wet etching; In step (9), the etching method of the back side of the fourth semi-finished product after development is as follows: the etching method of the back electroplating film is wet etching, the etching method of the back seed film is wet etching, and the etching method of the back barrier film and the back adhesion film is wet etching.

Citation Information

Patent Citations

  • High-power chip whole-film fixed resistor and production method thereof

    CN105374480A

  • Glass-based surface-mounted ignition resistor and manufacturing method thereof

    CN115547597A

  • Film platinum resistor and preparation method thereof