Formation method of semiconductor structure

By using a combination of hard mask structure and protective layer in semiconductor manufacturing, the problems of uneven thickness of hard mask layer and uneven step height in shallow trough isolation process are solved, and higher device performance and lower leakage are achieved risk.

CN119092460AActive Publication Date: 2024-12-06ZHEJIANG ICSPROUT SEMICONDUCTOR CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411179226.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-12-06
Estimated Expiration
2044-08-26

AI Technical Summary

Technical Problem

The existing shallow trough isolation process results in uneven thickness of the hard mask layer and uneven step height during the etching process, affecting device performance and increasing leakage probability.

Method used

Using a hard mask structure as a mask, trenches are formed in the substrate through the first etching process, and the protective layer is retained after the trench is formed, reducing etching damage of the hard mask layer and accurately controlling the thickness of the hard mask layer. , an isolation layer is formed to reduce line width roughness and leakage abnormalities.

Benefits of technology

Improve device performance, reduce the probability of leakage abnormality, and improve the overall performance of the semiconductor structure by uniformly controlling step height and trench side wall exposure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092460A_ABST
    Figure CN119092460A_ABST
Patent Text Reader

Abstract

A forming method of a semiconductor structure comprises the following steps: providing a substrate; a hard mask structure is formed on part of the surface of the substrate, the hard mask structure comprises a hard mask layer and a protective layer located on the hard mask layer, and the protective layer and the hard mask layer are made of different materials; the hard mask structure is used as a mask, a first etching process is adopted to etch the substrate, a groove is formed in the substrate, and after the groove is formed, the protective layer is still reserved, and the hard mask layer is not exposed; an isolation material layer is formed in the groove and on the surface of the protection layer, the top surface of the isolation material layer is higher than the top surface of the protection layer, and the material of the isolation material layer is different from that of the hard mask layer; planarizing the isolation material layer and the protection layer until the hard mask layer is exposed, and forming an isolation layer by using the isolation material layer; after the planarization process, the hard mask layer is removed, so that the probability of exposure of the substrate on the side wall of the groove is reduced, the line width roughness of the isolation layer is reduced, the performance of the finally formed device is improved, and the probability of electric leakage abnormity is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor manufacturing, and in particular to a method for forming a semiconductor structure. Background Art

[0002] The Shallow Trench Isolation (STI) process plays a vital role in isolation and leakage between devices.

[0003] The shallow trench isolation process usually involves first depositing a layer of silicon nitride (Si3N4) on the semiconductor substrate, patterning the silicon nitride layer to form a hard mask. Next, a shallow trench is etched in the substrate isolation area, and then an oxide layer (SiO2) is deposited, which is then planarized by a mechanical chemical polishing (CMP) process to remove excess oxide layers, and then the silicon nitride layer is removed by an acid wash process.

[0004] However, the existing shallow trench isolation process needs to be further improved. Summary of the invention

[0005] The technical problem solved by the present invention is to provide a method for forming a semiconductor structure to improve the performance of the formed semiconductor structure.

[0006] In order to solve the above technical problems, the technical solution of the present invention provides a method for forming a semiconductor structure, comprising: providing a substrate; forming a hard mask structure on a portion of the surface of the substrate, the hard mask structure comprising a hard mask layer and a protective layer located on the hard mask layer, the protective layer and the hard mask layer being made of different materials; using the hard mask structure as a mask, etching the substrate by a first etching process to form a groove in the substrate, and after the groove is formed, the protective layer is still retained and the hard mask layer is not exposed; forming an isolation material layer in the groove and on the surface of the protective layer, the top surface of the isolation material layer is higher than the top surface of the protective layer, and the material of the isolation material layer is different from that of the hard mask layer; planarizing the isolation material layer and the protective layer until the hard mask layer is exposed, and forming an isolation layer with the isolation material layer; after the planarization process, removing the hard mask layer.

[0007] Optionally, the method for forming the hard mask structure includes: forming a hard mask material layer and a protective material layer located on the surface of the hard mask material layer on the substrate; patterning the protective material layer and the hard mask material layer to form the protective layer with the patterned protective material layer, and forming the hard mask layer with the patterned hard mask material layer.

[0008] Optionally, the hard mask layer includes a buffer layer and an etch stop layer located on the buffer layer; the hard mask material layer includes a buffer material layer and an etch stop material layer located on the surface of the buffer material layer; the method for forming the hard mask layer also includes: forming the buffer layer with the buffer material layer, and forming the etch stop layer with the etch stop material layer.

[0009] Optionally, the material of the buffer layer includes silicon oxide; and the material of the etch stop layer includes silicon nitride.

[0010] Optionally, the method of patterning the protective material layer and the hard mask material layer includes: forming a photoresist material layer on the surface of the protective material layer; patterning the photoresist material layer to form a photoresist layer; and etching the protective material layer and the hard mask material layer using the photoresist layer as a mask.

[0011] Optionally, the thickness of the photoresist material layer is in the range of to

[0012] Optionally, before forming the photoresist material layer, the method further includes: forming a bottom anti-reflection layer on the surface of the protective material layer, and the photoresist material layer is located on the surface of the bottom anti-reflection layer.

[0013] Optionally, before etching the protective material layer and the hard mask material layer, the method further includes: etching the bottom anti-reflection layer using the photoresist layer as a mask.

[0014] Optionally, the thickness of the bottom anti-reflection layer is in the range of to

[0015] Optionally, before forming the protective material layer, the method further includes: determining a thickness of the protective material layer according to the first etching process.

[0016] Optionally, the substrate includes a central area and an edge area surrounding the central area; the first etching process has a first etching rate for the protective layer on the edge area and a second etching rate for the protective layer on the central area, and the first etching rate is different from the second etching rate; the first etching rate is greater than the second etching rate.

[0017] Optionally, an etching selectivity ratio of the first etching process to the protective layer and the substrate ranges from 1:3 to 1:8.

[0018] Optionally, the thickness of the hard mask layer is in the range of to

[0019] Optionally, the thickness of the protective layer is in the range of to

[0020] Optionally, the material of the protective layer includes a dielectric material, and the dielectric material includes a combination of one or more of silicon oxide, silicon nitride, silicon carbide, silicon oxycarbide, silicon oxynitride, aluminum oxide, aluminum nitride, silicon carbide nitride and silicon carbon nitride oxynitride.

[0021] Optionally, the material of the hard mask layer includes a dielectric material, and the dielectric material includes a combination of one or more of silicon oxide, silicon nitride, silicon carbide, silicon oxycarbide, silicon oxynitride, aluminum oxide, aluminum nitride, silicon carbide nitride and silicon carbon nitride oxynitride.

[0022] Compared with the prior art, the technical solution of the embodiment of the present invention has the following beneficial effects:

[0023] In the method for forming a semiconductor structure provided by the technical solution of the present invention, a hard mask structure is used as a mask, and a first etching process is adopted to etch a substrate to form a groove in the substrate. After the groove is formed, the protective layer is still retained and the hard mask layer is not exposed. Since the hard mask layer is protected by the protective layer, the etching damage to the hard mask layer caused by the first etching process and the uneven thickness of the hard mask layer introduced by the first etching process are reduced, which is conducive to accurately controlling the thickness of the hard mask layer, thereby facilitating control of the step height formed between the top surface of the isolation layer and the surface of the substrate and the uniformity of the step height, thereby facilitating reducing the probability of exposure of the substrate on the side wall of the groove, reducing the line width roughness of the isolation layer, improving the performance of the final device, and reducing the probability of leakage anomalies. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figures 1 to 4 It is a cross-sectional schematic diagram of the formation process of a semiconductor structure;

[0025] Figure 5 is a flow chart of steps of a method for forming a semiconductor structure according to an embodiment of the present invention;

[0026] Figures 6 to 12 It is a structural schematic diagram of each step of the method for forming a semiconductor structure according to an embodiment of the present invention. DETAILED DESCRIPTION

[0027] It should be noted that the terms “surface” and “on” in this specification are used to describe relative positional relationships in space and are not limited to direct contact.

[0028] As described in the background art, the existing shallow trench isolation process needs to be further improved. Now, a semiconductor structure formation process is described and analyzed.

[0029] Figures 1 to 4It is a cross-sectional schematic diagram of the formation process of a semiconductor structure.

[0030] Please refer to Figure 1 , providing a substrate 100; forming a hard mask layer on a portion of the surface of the substrate 100, the hard mask layer comprising an oxide layer 101 and a silicon nitride layer 102 located on the surface of the oxide layer 101; using the hard mask layer as a mask, etching the substrate 100 to form a groove 103 in the substrate 100.

[0031] Please refer to Figure 2 An isolation material layer 104 is formed in the trench 103 and on the surface of the hard mask layer, and the isolation material layer 104 is higher than the hard mask layer.

[0032] Please refer to Figure 3 , planarizing the isolation material layer 104 until the hard mask layer is exposed.

[0033] Please refer to Figure 4 , remove the hard mask layer, and form an isolation structure 105 with the isolation material layer 104 .

[0034] The above method is used in the shallow trench isolation process, and the substrate 100 between adjacent isolation structures 105 is an active area. After the planarization process, a butterfly defect (such as dishing defect) will be generated on the surface of the isolation material layer 104. Figure 3 In the process of removing the hard mask layer, the isolation material layer 104 will also be etched, and the edge of the butterfly defect is more easily etched than the center, so that the top surface of the isolation structure 105 forms a convexity (as shown in FIG. Figure 4 A step is formed between the top surface of the isolation structure 105 and the substrate surface. When the height h of the step is small, it is easy to cause the side wall of the active area to be exposed, and a groove (such as Figure 5 As shown in the middle area B), the groove B is easily filled with metal silicide material in the subsequent Salicide process, resulting in device leakage problems.

[0035] The height h of the step is achieved by controlling the thickness of the hard mask layer. However, in the etching process for forming the groove 103, since the gas concentration on the wafer surface shows an etching edge effect that increases from the center to the edge, after the groove 103 is formed, the thickness of the hard mask layer at the edge of the wafer is lower than the thickness of the hard mask layer at the center of the wafer, which is not conducive to controlling the uniformity of the height h of the step on the entire wafer, affecting the performance of the device finally formed.

[0036] In order to solve the above problems, in a method for forming a semiconductor structure provided by the present invention, a hard mask structure is used as a mask, and a first etching process is adopted to etch a substrate to form a groove in the substrate. After the groove is formed, the protective layer is still retained and the hard mask layer is not exposed. Since the hard mask layer is protected by the protective layer, the etching damage to the hard mask layer caused by the first etching process and the uneven thickness of the hard mask layer introduced by the first etching process are reduced, which is conducive to accurately controlling the thickness of the hard mask layer, thereby facilitating the control of the step height formed between the top surface of the isolation layer and the surface of the substrate and the uniformity of the step height, thereby facilitating reducing the probability of the substrate being exposed on the side wall of the groove, reducing the line width roughness of the isolation layer, improving the performance of the device finally formed, and reducing the probability of leakage anomalies.

[0037] In order to make the above-mentioned objects, features and beneficial effects of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0038] Figure 5 is a flow chart of the steps of a method for forming a semiconductor structure according to an embodiment of the present invention.

[0039] In this embodiment, the method for forming the semiconductor structure includes the following steps:

[0040] Step S201, providing a substrate.

[0041] Step S202, forming a hard mask structure on a portion of the substrate surface, wherein the hard mask structure includes a hard mask layer and a protection layer located on the hard mask layer, and the protection layer and the hard mask layer are made of different materials;

[0042] Step S203, using the hard mask structure as a mask, etching the substrate by a first etching process to form a groove in the substrate, and after the groove is formed, the protection layer is still retained and the hard mask layer is not exposed;

[0043] Step S204, forming an isolation material layer in the trench and on the surface of the protection layer, wherein the top surface of the isolation material layer is higher than the top surface of the protection layer, and the material of the isolation material layer is different from that of the hard mask layer;

[0044] Step S205, planarizing the isolation material layer and the protection layer until the hard mask layer is exposed, and forming an isolation layer with the isolation material layer;

[0045] Step S206 , after the planarization process, removing the hard mask layer.

[0046] The following is a detailed description with reference to the accompanying drawings.

[0047] Figures 6 to 12 It is a structural schematic diagram of each step of the method for forming a semiconductor structure according to an embodiment of the present invention.

[0048] Please refer to Figure 6 , providing a substrate 300.

[0049] In this embodiment, the material of the substrate 300 is silicon.

[0050] In other embodiments, the substrate material includes silicon carbide, silicon germanium, a multinary semiconductor material composed of group III-V elements, silicon on insulator (SOI) or germanium on insulator (GOI). Among them, the multinary semiconductor material composed of group III-V elements includes InP, GaAs, GaP, InAs, InSb, InGaAs or InGaAsP.

[0051] In this embodiment, the substrate 300 includes a central region (not shown in the figure) and an edge region (not shown in the figure) surrounding the central region.

[0052] Subsequently, a hard mask structure is formed on a portion of the surface of the substrate 300 , wherein the hard mask structure includes a hard mask layer and a protection layer located on the hard mask layer, and the protection layer and the hard mask layer are made of different materials.

[0053] In this embodiment, the method for forming the hard mask structure is described in detail. Figures 6 to 8 .

[0054] Please continue to refer to Figure 6 , a hard mask material layer 301 and a protective material layer 302 located on the surface of the hard mask material layer 301 are formed on the substrate 300 .

[0055] In this embodiment, before forming the protective material layer 302, the method further includes: determining the thickness of the protective material layer 302 according to the subsequent first etching process. The protective material layer 302 is used to form a protective layer, and a suitable thickness of the protective material layer 302 is selected to ensure that the protective layer is still retained after the first etching process.

[0056] In this embodiment, the thickness of the protective material layer 302 is in the range of to

[0057] The material of the protective material layer 302 includes a dielectric material, and the dielectric material includes one or more combinations of silicon oxide, silicon nitride, silicon carbide, silicon oxycarbide, silicon oxynitride, aluminum oxide, aluminum nitride, silicon carbide nitride, and silicon oxycarbide nitride.

[0058] In this embodiment, the material of the protective material layer 302 is silicon oxide.

[0059] In this embodiment, the thickness range of the hard mask material layer 301 is to

[0060] In this embodiment, the hard mask material layer 301 is a double-layer material layer. Specifically, the hard mask material layer includes a buffer material layer 301a and an etch stop material layer 301b located on the surface of the buffer material layer 301a. In another embodiment, the hard mask material layer can be a single-layer or multi-layer material layer.

[0061] Specifically, the thickness of the etching stop material layer 301b is in the range of to The thickness of the etching stop material layer 301b is in the range of to

[0062] The material of the hard mask material layer 301 includes a dielectric material, and the dielectric material includes one or more combinations of silicon oxide, silicon nitride, silicon carbide, silicon oxycarbide, silicon oxynitride, aluminum oxide, aluminum nitride, silicon carbide nitride, and silicon oxycarbon nitride. The hard mask material layer 301 is used to form a hard mask layer.

[0063] In this embodiment, the material of the buffer material layer 301 a is silicon oxide, and the material of the etch stop material layer 301 b is silicon nitride. The buffer material layer 301 a is used to reduce the stress between the etch stop material layer 301 b and the substrate 300 .

[0064] Subsequently, the protective material layer 302 and the hard mask material layer 301 are patterned to form the protective layer with the patterned protective material layer 302 and to form the hard mask layer with the patterned hard mask material layer.

[0065] In this embodiment, the method of patterning the protective material layer 302 and the hard mask material layer 301 can be found in Figures 7 and 8 .

[0066] Please refer to Figure 7 , forming a photoresist material layer (not shown in the figure) on the surface of the protective material layer 302 ; and patterning the photoresist material layer to form a photoresist layer 304 .

[0067] In this embodiment, the thickness of the photoresist material layer ranges from to Here, the thickness of the photoresist material layer is determined according to the thickness of the protective material layer 302 , so as to avoid the situation in which the photoresist layer 304 is consumed before the etching is completed during the subsequent etching of the protective material layer 302 .

[0068] In this embodiment, before forming the photoresist material layer, a bottom anti-reflection layer 303 is formed on the surface of the protective material layer, and the photoresist material layer is located on the surface of the bottom anti-reflection layer 303 .

[0069] In this embodiment, the thickness of the bottom anti-reflection layer 303 is in the range of to Here, the thickness of the bottom anti-reflection layer is determined according to the thickness of the photoresist material layer.

[0070] Please refer to Figure 8 , using the photoresist layer 304 as a mask, etching the protection material layer 302 and the hard mask material layer 301 to form the protection layer 305 and the hard mask layer 306 .

[0071] In this embodiment, the thickness range of the hard mask layer 306 is to

[0072] In this embodiment, the thickness range of the protective layer 305 is to

[0073] In this embodiment, the hard mask layer 306 includes a buffer layer 306 a and an etch stop layer 306 b located on the buffer layer 306 a .

[0074] In this embodiment, the method for forming the hard mask layer 306 further includes: forming the buffer layer 306 a using the buffer material layer 301 a , and forming the etch stop layer 306 b using the etch stop material layer 301 b .

[0075] In this embodiment, before etching the protection material layer 302 and the hard mask material layer 301 , the bottom anti-reflection layer 303 is etched using the photoresist layer 304 as a mask.

[0076] In this embodiment, after the hard mask layer 306 is formed, the photoresist layer 304 and the bottom anti-reflection layer 303 are also removed.

[0077] Please refer to Fig. 9 , using the hard mask structure as a mask, the substrate 300 is etched by a first etching process to form a groove 307 in the substrate 300, and after the groove 307 is formed, the protection layer 305 is still retained and the hard mask layer 306 is not exposed.

[0078] In the first etching process, the protection layer 305 protects the hard mask layer 306 , which helps to control the thickness uniformity of the hard mask layer 306 on the entire substrate 300 .

[0079] The first etching process has a first etching rate for the protection layer 305 on the edge region and a second etching rate for the protection layer 305 on the central region, and the first etching rate and the second etching rate are different.

[0080] In this embodiment, the first etching rate is greater than the second etching rate. Here, the difference between the first etching rate and the second etching rate is caused by the etching edge effect. In another embodiment, the first etching rate is less than the second etching rate.

[0081] In this embodiment, the first etching process includes a dry etching process.

[0082] In this embodiment, the etching selectivity ratio of the first etching process to the protection layer 305 and the substrate 300 ranges from 1:3 to 1:8.

[0083] Here, it should be noted that it is necessary to select a suitable thickness of the protection layer 305 (protection material layer 302 ) to ensure that the protection layer 305 is still retained after the first etching process.

[0084] Specifically, the first etching rate, the second etching rate, the etching selectivity of the first etching process to the protective layer and the substrate, and the setting range of the depth of the groove can be provided in advance; the thickness of the protective material layer 302 is determined according to the setting range of the first etching rate, the second etching rate, the etching selectivity and the depth of the groove; or according to the set thickness of the protective layer 305, a suitable first etching process is selected later.

[0085] Please refer to Fig.10 An isolation material layer 308 is formed in the groove 307 and on the surface of the protection layer 305 , the top surface of the isolation material layer 308 is higher than the top surface of the protection layer 305 , and the material of the isolation material layer 308 is different from that of the hard mask layer 306 .

[0086] The material of the isolation material layer 308 includes a dielectric material, and the dielectric material includes one or more combinations of silicon oxide, silicon nitride, silicon carbide, silicon oxycarbide, silicon oxynitride, aluminum oxide, aluminum nitride, silicon carbonitride, and silicon carbonitride oxynitride.

[0087] In this embodiment, the material of the isolation material layer 308 is silicon oxide.

[0088] The isolation material layer 308 is formed by a chemical vapor deposition (CVD) process.

[0089] In this embodiment, the isolation material layer 308 is formed by a high density plasma deposition process (HDP).

[0090] Please refer to Fig.11 , planarizing the isolation material layer 308 and the protection layer 305 until the hard mask layer 306 is exposed, and forming an isolation layer 309 with the isolation material layer 308 .

[0091] The planarization process includes a chemical mechanical polishing (CMP) process.

[0092] In the planarization process, the hard mask layer 306 serves as an etching stop. Based on the foregoing, the protective layer 305 improves the thickness uniformity of the hard mask layer 306 on the entire substrate 300, so the hard mask layer 306 (the hard mask material layer 301) can be set to a thinner thickness, which is beneficial to reducing the time of the planarization process, and further beneficial to reducing the depth of the butterfly defect D (dishing defect) on the surface of the isolation layer 309.

[0093] In this embodiment, the planarization process has a first grinding rate for the isolation material layer 308 , and the planarization process has a second grinding rate for the hard mask layer 306 . The ratio of the first grinding rate to the second grinding rate ranges from 10:1 to 100:1.

[0094] Please refer to Fig.12 After the planarization process, the hard mask layer 306 is removed.

[0095] Thus, since the hard mask layer is protected by the protective layer, the etching damage to the hard mask layer caused by the first etching process and the uneven thickness of the hard mask layer introduced by the first etching process are reduced, which is conducive to accurately controlling the thickness of the hard mask layer, thereby facilitating the control of the step height H formed between the top surface of the isolation layer 309 and the surface of the substrate 300 and the uniformity of the step height H, thereby facilitating the reduction of the exposure of the substrate 300 on the sidewall of the trench 307 ( Fig.12 The probability of the isolation layer 309 being as shown in the middle dotted line is beneficial to reducing the line width roughness of the isolation layer 309, improving the performance of the device finally formed, and reducing the probability of leakage anomaly.

[0096] Here, it should be noted that the substrate 300 between the trenches 307 is used to form an active region of a device.

[0097] The process for removing the hard mask layer 306 is a second etching process, and the second etching process includes one or both of a dry etching process and a wet etching process. In this embodiment, the second etching process is a wet etching process.

[0098] The etching selectivity ratio of the second etching process to the etching stop layer 306 b and the isolation material layer 308 is in a range of 10:1 to 200:1.

[0099] In this embodiment, during the second etching process, since the materials of the buffer layer 306a and the isolation material layer 308 are both silicon oxide, the isolation layer 309 will also be etched while the buffer layer 306a is removed. Since the butterfly defect D on the surface of the isolation layer 309 has a small depth, the surface of the isolation layer 309 formed is relatively flat, which reduces the exposure of the substrate 300 on the side wall of the trench 307 ( Fig.12 The probability of the device being formed is improved (as shown by the middle dotted line).

[0100] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.

Claims

1. A method for forming a semiconductor structure, characterized in that: include: providing a substrate; forming a hard mask structure on a portion of the substrate surface, wherein the hard mask structure comprises a hard mask layer and a protective layer located on the hard mask layer, wherein the protective layer and the hard mask layer are made of different materials; Using the hard mask structure as a mask, etching the substrate by a first etching process to form a groove in the substrate, and after the groove is formed, the protective layer is still retained and the hard mask layer is not exposed; forming an isolation material layer in the groove and on the surface of the protection layer, wherein the top surface of the isolation material layer is higher than the top surface of the protection layer, and the material of the isolation material layer is different from that of the hard mask layer; planarizing the isolation material layer and the protection layer until the hard mask layer is exposed, and forming an isolation layer with the isolation material layer; After the planarization process, the hard mask layer is removed.

2. The method for forming a semiconductor structure according to claim 1, wherein: The method for forming the hard mask structure includes: forming a hard mask material layer and a protective material layer located on the surface of the hard mask material layer on the substrate; patterning the protective material layer and the hard mask material layer to form the protective layer with the patterned protective material layer, and forming the hard mask layer with the patterned hard mask material layer.

3. The method for forming a semiconductor structure according to claim 2, wherein: The hard mask layer includes a buffer layer and an etch stop layer located on the buffer layer; the hard mask material layer includes a buffer material layer and an etch stop material layer located on the surface of the buffer material layer; the method for forming the hard mask layer also includes: forming the buffer layer with the buffer material layer, and forming the etch stop layer with the etch stop material layer.

4. The method for forming a semiconductor structure according to claim 3, wherein: The material of the buffer layer includes silicon oxide; the material of the etch stop layer includes silicon nitride.

5. The method for forming a semiconductor structure according to claim 2, wherein: The method for patterning the protective material layer and the hard mask material layer includes: forming a photoresist material layer on the surface of the protective material layer; patterning the photoresist material layer to form a photoresist layer; and etching the protective material layer and the hard mask material layer using the photoresist layer as a mask.

6. The method for forming a semiconductor structure according to claim 5, wherein: The thickness of the photoresist material layer is in the range of to 7. The method for forming a semiconductor structure according to claim 5, wherein: Before forming the photoresist material layer, the method further includes: forming a bottom anti-reflection layer on the surface of the protective material layer, wherein the photoresist material layer is located on the surface of the bottom anti-reflection layer.

8. The method for forming a semiconductor structure according to claim 7, wherein: Before etching the protective material layer and the hard mask material layer, the method further includes: etching the bottom anti-reflection layer using the photoresist layer as a mask.

9. The method for forming a semiconductor structure according to claim 7, wherein: The thickness of the bottom anti-reflection layer is in the range of to 10. The method for forming a semiconductor structure according to claim 2, wherein: Before forming the protective material layer, the method further includes: determining a thickness of the protective material layer according to the first etching process.

11. The method for forming a semiconductor structure according to claim 1, wherein: The substrate includes a central area and an edge area surrounding the central area; the first etching process has a first etching rate for the protective layer on the edge area and a second etching rate for the protective layer on the central area, and the first etching rate is different from the second etching rate; the first etching rate is greater than the second etching rate.

12. The method for forming a semiconductor structure according to claim 11, wherein: The etching selectivity ratio of the first etching process to the protection layer and the substrate ranges from 1:3 to 1:

8.

13. The method for forming a semiconductor structure according to claim 1, wherein: The thickness of the hard mask layer is in the range of to 14. The method for forming a semiconductor structure according to claim 1, wherein: The thickness of the protective layer is in the range of to 15. The method for forming a semiconductor structure according to claim 1, wherein: The material of the protective layer includes a dielectric material, and the dielectric material includes one or more combinations of silicon oxide, silicon nitride, silicon carbide, silicon oxycarbide, silicon oxynitride, aluminum oxide, aluminum nitride, silicon carbide nitride, and silicon oxycarbide nitride.

16. The method for forming a semiconductor structure according to claim 1, wherein:The material of the hard mask layer includes a dielectric material, and the dielectric material includes a combination of one or more of silicon oxide, silicon nitride, silicon carbide, silicon oxycarbide, silicon oxynitride, aluminum oxide, aluminum nitride, silicon carbide nitride, and silicon oxycarbide nitride.

Citation Information

Patent Citations

  • Shallow trench isolation structure and manufacturing method

    CN110931421A

  • Preparation method of STI structure

    CN114038791A

  • Formation method of shallow trench isolation structure and formation method of semiconductor device

    CN115775766A

  • Method for forming shallow trench isolation structure

    CN118156218A

  • Fabrication method for shallow trench isolation

    US20040005765A1