Graphite negative electrode material and preparation method thereof, negative electrode plate and battery

By mixing the carbon particles prepared by the raw coke raw materials and cooked coke raw materials at different degrees of graphitization, the graphite negative electrode material formed solves the volume expansion problem in lithium-ion batteries, improves cycle stability and fast charging performance, and is suitable for large-scale applications.

CN119092638APending Publication Date: 2024-12-06SHENZHEN HIGHPOWER TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411340805.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing graphite negative electrode materials limit the increase in energy density due to volume expansion problems in lithium-ion batteries, and the production process is complex, resulting in low cycle life and fast charging capacity retention rate.

Method used

Carbon particles with low graphitization and high graphitization degree prepared from raw coke raw materials and cooked coke raw materials are used to mix and bond carbon particles with different graphitization degrees to form graphite negative electrodes with rich amorphous structure and stable structure. Material, reduce expansion rate and improve cycle stability.

Benefits of technology

It effectively reduces the expansion rate of graphite negative electrode material, improves the cycle stability and fast charging performance of the battery, extends the battery life, and reduces production costs and difficulty, making it suitable for large-scale applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092638A_ABST
    Figure CN119092638A_ABST
Patent Text Reader

Abstract

The invention relates to a graphite negative electrode material and a preparation method thereof, a negative electrode plate and a battery. The graphite negative electrode material comprises first carbon-containing particles and second carbon-containing particles, wherein the second carbon-containing particles are adhered to the surfaces of the first carbon-containing particles; the graphitization degree of the first carbon-containing particles is smaller than 93%, the graphitization degree of the second carbon-containing particles is larger than 94%, and the median particle size of the first carbon-containing particles is larger than or equal to the median particle size of the second carbon-containing particles. According to the scheme provided by the invention, the expansion rate of the material can be effectively reduced, the graphite capacity and the cycle capacity retention rate are relatively high, meanwhile, the production difficulty is low, and large-scale popularization and application are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of battery material preparation, and in particular to a graphite negative electrode material and a preparation method thereof, a negative electrode sheet and a battery. Background Art

[0002] Graphite negative electrode materials, as a key component in lithium-ion batteries, are widely used in batteries for power, energy storage and consumer electronics. With the growing demand for higher energy density in terminal devices, improving the energy density of graphite negative electrode materials has become particularly critical. During the application of graphite negative electrode materials, the volume expansion of graphite negative electrode materials limits the further improvement of battery energy density, especially in the initial half-charge and full-charge states of the battery, as well as in the subsequent cycle process. The expansion problem of the graphite negative electrode is likely to affect the performance and life of the battery.

[0003] In the related art, the graphite granulation process is mainly used to improve the isotropy of carbon-containing particles and disperse the volume expansion, so as to reduce the expansion rate of the negative electrode material. However, the graphite granulation production process for making graphite negative electrode materials in the related art is generally more complicated and difficult to produce. In addition, the capacity retention rate of the obtained negative electrode material is low during the fast charging cycle and the cycle life performance is poor. Summary of the invention

[0004] In order to solve or partially solve the problems existing in the related art, the present application provides a graphite negative electrode material and a preparation method thereof, a negative electrode sheet and a battery, which can effectively reduce the expansion rate of the material, have a higher graphite capacity and cycle capacity retention rate, and at the same time reduce the production difficulty to meet the requirements of large-scale promotion and application.

[0005] In a first aspect, the present application provides a graphite negative electrode material, comprising: first carbon-containing particles and second carbon-containing particles, wherein the second carbon-containing particles are bonded to the surface of the first carbon-containing particles; The graphitization degree of the first carbon-containing particles is less than 93%, the graphitization degree of the second carbon-containing particles is greater than 94%, and the median particle size of the first carbon-containing particles is greater than or equal to the median particle size of the second carbon-containing particles.

[0006] In some embodiments, the first carbon-containing particles are produced by graphitizing a green coke raw material, and the second carbon-containing particles are produced by graphitizing a cooked coke raw material.

[0007] In some embodiments, the mass ratio of the first carbon-containing particles to the second carbon-containing particles is (3:7) to (9:1).

[0008] In some embodiments, the degree of graphitization of the first carbon-containing particles is 85% to 93%; and / or the degree of graphitization of the second carbon-containing particles is 94% to 98%.

[0009] The second aspect of the present application provides a method for preparing the graphite negative electrode material described in the first aspect of the present application, comprising crushing the raw coke material into particles, and then subjecting the particles to graphitization treatment to prepare first carbonaceous particles having a graphitization degree of less than 93%; After the cooked coke raw material is crushed into particles, the second carbon-containing particles having a graphitization degree greater than 94% are prepared by graphitization treatment; The first carbon-containing particles and the second carbon-containing particles are mixed in a preset mass ratio, a binder is added, and granulation carbonization treatment is performed to obtain a graphite negative electrode material; wherein the second carbon-containing particles in the graphite negative electrode material are bonded to the surface of the first carbon-containing particles, and the median particle size of the first carbon-containing particles is greater than or equal to the median particle size of the second carbon-containing particles.

[0010] In some embodiments, the median particle size of the first carbon-containing particles is 7 μm to 15 μm; and / or the median particle size of the second carbon-containing particles is 4 μm to 7 μm.

[0011] In some embodiments, the raw coke material is one or more of petroleum coke, coal-based coke, oil-based needle coke, and coal-based needle coke; and / or the cooked coke material is obtained by calcining one or more of petroleum coke, coal-based coke, oil-based needle coke, and coal-based needle coke.

[0012] In some embodiments, the content of the binder in the graphite negative electrode material is 5wt%~50wt%; In some embodiments, the adhesive is selected from one or more of petroleum asphalt, coal tar asphalt, phenolic resin, epoxy resin, etc.

[0013] In some embodiments, the temperature of the raw coke material during graphitization treatment is 2500°C~2800°C, and the duration is 24~72 hours; and / or the temperature of the cooked coke material during graphitization treatment is 2900°C~3500°C, and the duration is 24~72 hours; and / or the temperature of the granulation carbonization is 500°C~2000°C, and the duration is 3~10 hours.

[0014] The third aspect of the present application provides a negative electrode sheet, comprising a negative electrode current collector and a negative electrode active material, wherein the negative electrode active material is arranged on the surface of the negative electrode current collector, and the negative electrode active material comprises the graphite negative electrode material described in any one of the first aspect of the present application or the graphite negative electrode material prepared by the method described in the second aspect of the present application.

[0015] The fourth aspect of the present application provides a battery, comprising the negative electrode sheet described in the third aspect of the present application.

[0016] The technical solution provided by this application may have the following beneficial effects: The technical solution of the present application is to produce a graphite negative electrode material by bonding the larger median particle size of the first carbon-containing particles to the second carbon-containing particles. The first carbon-containing particles with a low degree of graphitization (less than 93%) have a rich amorphous structure, which can effectively enhance the ability of lithium ions to be inserted and removed, and effectively reduce the volume expansion during the lithium insertion process. The second carbon-containing particles with a high degree of graphitization (greater than 94%) have a stable structure and a low resistivity. When bonded to the first carbon-containing particles, the graphite capacity can be effectively increased and a compaction effect can be played. Therefore, when the above-mentioned graphite negative electrode material is applied to the battery, it has low expansion performance, and effectively improves the cycle stability and cycle capacity retention rate of the battery, extends the battery life and improves the battery fast charging performance.

[0017] Furthermore, the first carbon-containing particles and the second carbon-containing particles are respectively prepared from raw coke raw materials to cooked coke, which effectively reduces the production cost of the graphite negative electrode material of the present application and effectively reduces the production difficulty, so that the graphite negative electrode material can meet the requirements of large-scale promotion and application.

[0018] It should be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The above and other objects, features and advantages of the present application will become more apparent by describing in more detail exemplary embodiments of the present application in conjunction with the accompanying drawings, wherein the same reference numerals generally represent the same components in the exemplary embodiments of the present application.

[0020] Figure 1 is a SEM image of a graphite negative electrode material shown in an embodiment of the present application; Figure 2 It is a schematic diagram of the process of preparing the graphite negative electrode material shown in the embodiment of the present application. DETAILED DESCRIPTION

[0021] The embodiments of the present application will be described in more detail below with reference to the accompanying drawings. Although the embodiments of the present application are shown in the accompanying drawings, it should be understood that the present application can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided to make the present application more thorough and complete, and to fully convey the scope of the present application to those skilled in the art.

[0022] The terms used in this application are for the purpose of describing specific embodiments only and are not intended to limit this application. The singular forms of "a", "said" and "the" used in this application and the appended claims are also intended to include plural forms unless the context clearly indicates other meanings. It should also be understood that the term "and / or" used herein refers to and includes any or all possible combinations of one or more associated listed items.

[0023] It should be understood that although the terms "first", "second", "third", etc. may be used in this application to describe various information, this information should not be limited to these terms. These terms are only used to distinguish the same type of information from each other. For example, without departing from the scope of this application, the first information may also be referred to as the second information, and similarly, the second information may also be referred to as the first information. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.

[0024] In the related art, the graphite granulation process is mainly used to improve the isotropy of carbon-containing particles and disperse the volume expansion, so as to reduce the expansion rate of the negative electrode material. However, the graphite granulation production process for making graphite negative electrode materials in the related art is generally more complicated and difficult to produce. In addition, the capacity retention rate of the obtained negative electrode material is low during the fast charging cycle and the cycle life performance is poor.

[0025] In response to the above problems, the embodiments of the present application provide a graphite negative electrode material that can effectively reduce the expansion rate of the material, has a high graphite capacity and cycle capacity retention rate, and at the same time has low production difficulty and meets the requirements of large-scale promotion and application.

[0026] The technical solution of the embodiments of the present application is described in detail below with reference to the accompanying drawings.

[0027] Figure 1 is a SEM image of a graphite negative electrode material shown in an embodiment of the present application.

[0028] See also Figure 1 , the graphite negative electrode material of the present application includes a first carbon-containing particle and a second carbon-containing particle. Among them, the second carbon-containing particle is bonded to the surface of the first carbon-containing particle. It should be understood that the first carbon-containing particle and the second carbon-containing particle can be prepared by high-temperature graphitization treatment of carbon-containing materials. Specifically, the degree of graphitization of the first carbon-containing particle is less than 93%, the degree of graphitization of the second carbon-containing particle is greater than 94%, and the median particle size of the first carbon-containing particle is greater than or equal to the median particle size of the second carbon-containing particle. It can be understood that the first carbon-containing particle with a degree of graphitization of less than 93% is a low graphitization material, the second carbon-containing particle with a degree of graphitization of greater than 94% is a high graphitization material, the median particle size of the first carbon-containing particle is greater than or equal to the median particle size of the second carbon-containing particle, and the second carbon-containing particle is bonded to the surface of the first carbon-containing particle. That is, the first carbon-containing particle is used as the main particle, and the second carbon-containing particle is bonded to the first carbon-containing particle as the surface particle, thereby forming the graphite negative electrode material of the present application.

[0029] The graphite negative electrode material of the present application is made into a graphite negative electrode material by bonding the larger median particle size of the first carbon-containing particles to the second carbon-containing particles. The first carbon-containing particles with a low degree of graphitization (less than 93%) have a rich amorphous structure, which can effectively enhance the ability of lithium ions to be embedded and released, and effectively reduce the volume expansion during the lithium embedding process, while ensuring the fast charging performance of the graphite negative electrode material. The second carbon-containing particles with a high degree of graphitization (greater than 94%) have a stable structure and a low resistivity. When bonded to the first carbon-containing particles, the graphite capacity can be effectively increased and a compaction effect can be played. Therefore, when the above-mentioned graphite negative electrode material is applied to a battery, it has low expansion performance, and effectively improves the cycle stability and cycle capacity retention rate of the battery, extends the battery life and improves the fast charging performance of the battery.

[0030] In some embodiments, the first carbon-containing particles can be prepared by graphitizing raw coke materials, and the second carbon-containing particles can be prepared by graphitizing cooked coke materials. The first carbon-containing particles and the second carbon-containing particles are made of different raw materials, wherein the first carbon-containing particles can be prepared by high-temperature graphitization of one or more raw coke materials, and the second carbon-containing particles can be prepared by high-temperature graphitization of one or more cooked coke materials. It can be understood that raw coke materials are generally coke materials that have not been subjected to high-temperature calcination treatment during the coking process, and cooked coke materials are generally coke materials formed after high-temperature calcination treatment during the coking process. The first carbon-containing particles and the second carbon-containing particles are respectively prepared from raw coke materials and cooked coke materials, which effectively reduces the production cost of the graphite negative electrode material of the present application, and effectively reduces the production difficulty, so that the graphite negative electrode material can meet large-scale promotion and application.

[0031] Furthermore, the raw material for raw coke can be one or more of petroleum coke, coal-based coke, oil-based needle coke, and coal-based needle coke; the raw material for cooked coke can be obtained by calcining one or more of petroleum coke, coal-based coke, oil-based needle coke, and coal-based needle coke. Still further, the raw material for raw coke and the raw material for cooked coke in the present application can be made from the same or different raw materials. For example, the raw material for raw coke is obtained by calcining petroleum coke, while the raw material for cooked coke is obtained by calcining coal-based coke; for another example, the raw material for raw coke is oil-based needle coke, while the raw material for cooked coke is obtained by calcining oil-based needle coke.

[0032] In some embodiments, the mass ratio of the first carbon-containing particles to the second carbon-containing particles may be (3:7) to (9:1). For example, the mass ratio of the first carbon-containing particles to the second carbon-containing particles may be 3:7. For another example, the mass ratio of the first carbon-containing particles to the second carbon-containing particles may be 8:2.

[0033] In some embodiments, the graphitization degree of the first carbon-containing particles can be 85% to 93%; the graphitization degree of the second carbon-containing particles can be 94% to 98%. Through the above-mentioned graphitization degree control, the first carbon-containing particles are effectively provided with suitable low graphitization performance and the second carbon-containing particles are effectively provided with suitable high graphitization performance, thereby improving the performance stability of the prepared graphite negative electrode material.

[0034] Figure 2 It is a schematic diagram of the process of preparing the graphite negative electrode material shown in the embodiment of the present application.

[0035] See also Figure 2 The present application also provides a method for preparing a graphite negative electrode material, which is used to prepare the graphite negative electrode material described above in the present application. The method for preparing the graphite negative electrode material of the present application comprises: S110, crushing the raw coke material into particles, and then subjecting the particles to graphitization to prepare first carbonaceous particles having a graphitization degree of less than 93%.

[0036] The raw coke material is crushed and subjected to high temperature graphitization treatment to obtain first carbonaceous particles with a graphitization degree of less than 93%. In some embodiments, the raw coke material can be one or more of petroleum coke, coal-based coke, oil-based needle coke, and coal-based needle coke. Preferably, the raw coke material can be oil-based needle coke.

[0037] In some embodiments, the median particle size of the first carbonaceous particles may be 7 μm to 15 μm. It is understood that the raw coke material may be first crushed into particles with a median particle size of 7 μm to 15 μm before graphitization. The median particle size of the first carbonaceous particles is maintained at 7 μm to 15 μm, so that the first carbonaceous particles prepared from the raw coke material can maintain a larger particle size and serve as the main particles in the graphite negative electrode material.

[0038] In some embodiments, the temperature of the raw coke material during graphitization treatment is 2500°C to 2800°C, and the duration is 24 to 72 hours. For example, the temperature of the raw coke material during graphitization treatment can be one of 2500°C, 2550°C, 2600°C, 2650°C, 2700°C, 2750°C and 2800°C, and the duration can be one of 24 hours, 36 hours, and 72 hours.

[0039] S120, crushing the cooked coke raw material into particles, and then subjecting the particles to graphitization to prepare second carbonaceous particles having a graphitization degree greater than 94%.

[0040] The cooked coke raw material is crushed and subjected to high-temperature graphitization treatment to obtain second carbon-containing particles with a graphitization degree greater than 94%. In some embodiments, the cooked coke raw material can be obtained by calcining one or more of petroleum coke, coal-based coke, oil-based needle coke, and coal-based needle coke. Among them, the raw coke raw material and the cooked coke raw material can be made of the same or different raw materials. For example, the raw coke raw material is obtained by calcining petroleum coke, while the cooked coke raw material is obtained by calcining coal-based coke; for another example, the raw coke raw material is oil-based needle coke, and the cooked coke raw material is obtained by calcining oil-based needle coke. Preferably, the cooked coke raw material can be obtained by calcining oil-based needle coke.

[0041] In some embodiments, the median particle size of the second carbon-containing particles may be 4 μm to 7 μm. It is understood that the cooked coke raw material may be first crushed into particles with a median particle size of 4 μm to 7 μm before graphitization. The median particle size of the second carbon-containing particles may be 4 μm to 7 μm, so that the second carbon-containing particles maintain a smaller particle size, and the second carbon-containing particles may be bonded to the surface of the first carbon-containing particles during the composite bonding process with the first carbon-containing particles.

[0042] The present application can effectively ensure that the median particle size of the first carbon-containing particles is greater than or equal to the second carbon-containing particles by having the first carbon-containing particles and the second carbon-containing particles located in different preset median particle size ranges, and that the median particle size of the prepared graphite negative electrode material is not too large or too small.

[0043] In some embodiments, the temperature of the cooked coke raw material during graphitization treatment may be 2900°C to 3500°C, and the duration may be 24 to 72 hours. For example, the temperature of the cooked coke raw material during graphitization treatment may be one of 2900°C, 2950°C, 3000°C, 3150°C, 3250°C, 3350°C, and 3500°C, and the duration may be one of 24 hours, 36 hours, and 72 hours.

[0044] S130, mixing the first carbon-containing particles and the second carbon-containing particles in a preset mass ratio, adding a binder, and performing granulation carbonization treatment to obtain a graphite negative electrode material; wherein the second carbon-containing particles in the graphite negative electrode material are bonded to the surface of the first carbon-containing particles, and the median particle size of the first carbon-containing particles is greater than or equal to the median particle size of the second carbon-containing particles.

[0045] After the obtained first carbon-containing particles and the second carbon-containing particles are mixed and stirred, granulation and carbonization treatment are carried out to obtain a graphite negative electrode material. The binder is mainly used to enhance the bonding effect between the first carbon-containing particles and the second carbon-containing particles. It can be understood that screening treatment can be carried out after the granulation and carbonization treatment to screen out particles that do not meet the particle size requirements. Among them, the particle size of the graphite negative electrode material has an important influence on the performance of the lithium-ion battery. The median particle size of the graphite negative electrode material in the present application can be 15μm~16μm, so that the median particle size of the graphite negative electrode material of the present application can effectively balance the insertion and deinsertion speed and path length of lithium ions, so that the battery using the graphite negative electrode material of the present application has high rate performance and good cycle stability.

[0046] In some embodiments, the mass ratio of the first carbon-containing particles to the second carbon-containing particles may be (3:7) to (9:1). For example, the mass ratio of the first carbon-containing particles to the second carbon-containing particles may be 3:7. For another example, the mass ratio of the first carbon-containing particles to the second carbon-containing particles may be 8:2.

[0047] In some embodiments, the temperature of granulation carbonization is 500°C to 2000°C, and the duration is 3 h to 10 h. It can be understood that the first graphitization treatment is to prepare the first carbon-containing particles and the second carbon-containing particles according to the raw coke raw material and the cooked coke raw material, and the first carbon-containing particles and the second carbon-containing particles are granulated and carbonized, which requires a second graphitization treatment. The first graphitization treatment uses a higher temperature and a longer duration to effectively ensure the carbonization effect of the material, and the second graphitization treatment uses a lower temperature and a shorter duration to ensure the bonding effect of the two particles while preventing the low temperature from affecting the original performance of the particles, effectively ensuring the stability of product performance.

[0048] In some embodiments, the content of the binder in the graphite negative electrode material is 5wt% to 50wt%. For example, the content of the binder in the graphite negative electrode material is one of 5wt%, 15wt%, 25wt%, 35wt%, and 50wt%. Furthermore, the binder is selected from one or more of petroleum asphalt, coal tar asphalt, phenolic resin, epoxy resin, etc.

[0049] The preparation method of the graphite negative electrode material of the present application is to make the graphite negative electrode material by bonding the larger median particle size of the first carbon-containing particles with the second carbon-containing particles. The first carbon-containing particles with a low degree of graphitization (less than 93%) have a rich amorphous structure, which can effectively enhance the ability of lithium ion insertion and extraction, and effectively reduce the volume expansion during the lithium insertion process. The second carbon-containing particles with a high degree of graphitization (greater than 94%) have a stable structure and a low resistivity. When bonded to the first carbon-containing particles, the graphite capacity can be effectively increased and a compaction effect can be played. Therefore, when the above-mentioned graphite negative electrode material is applied to the battery, it has low expansion performance, and effectively improves the cycle stability and cycle capacity retention rate of the battery, prolongs the battery life and improves the battery fast charging performance.

[0050] An embodiment of the present application also provides a negative electrode sheet, which includes a negative electrode collector and a negative electrode active material. The negative electrode active material is arranged on the surface of the negative electrode collector. The negative electrode active material includes the graphite negative electrode material described in any of the above embodiments or a graphite negative electrode material prepared by the preparation method of the graphite negative electrode material described in any of the above embodiments.

[0051] An embodiment of the present application further provides a battery, comprising the negative electrode sheet described in any of the above embodiments.

[0052] In order to make the present invention easier to understand, the present invention will be further described in detail below in conjunction with examples, which are merely illustrative and are not intended to limit the scope of application of the present invention. The raw materials or components used in the present invention can be obtained by commercial routes or conventional methods unless otherwise specified.

[0053] Example 1 1) Preparation of the first carbonaceous particle The oil-based needle coke raw material that has not been subjected to high-temperature calcination is crushed to D50 (ie, median particle size) = 13 μm, and then graphitized at 2600° C. for 48 hours to obtain first carbon-containing particles with a graphitization degree of 90%.

[0054] 2) Preparation of the second carbonaceous particle The oil-based needle coke calcined at high temperature was crushed to D50=6μm, and then graphitized at 3200°C for 48h to obtain second carbonaceous particles with a graphitization degree of 96%.

[0055] 3) Preparation of graphite negative electrode materials The first carbon-containing particles and the second carbon-containing particles were mixed and stirred in a mass ratio of 5:5, and then 20 wt% of a petroleum asphalt adhesive was added to carry out a granulation carbonization process. The temperature was controlled at 1000°C for 6 hours, and finally a screening process was performed to obtain a graphite negative electrode material.

[0056] Example 2 The difference with respect to Example 1 is that the mass ratio of the first carbon-containing particles to the second carbon-containing particles is 6:1.

[0057] Example 3 The difference with respect to Example 1 is that the mass ratio of the first carbon-containing particles to the second carbon-containing particles is 9:1.

[0058] Example 4 The difference with respect to Example 1 is that the mass ratio of the first carbon-containing particles to the second carbon-containing particles is 2:7.

[0059] Example 5 The difference with respect to Example 1 is that the mass ratio of the first carbon-containing particles to the second carbon-containing particles is 8:2.

[0060] Example 6 The difference with respect to Example 1 is that the mass ratio of the first carbon-containing particles to the second carbon-containing particles is 3:7.

[0061] Example 7 The difference with respect to Example 1 is that the oil-based needle coke raw material that has not been subjected to high-temperature calcination is crushed to D50=13 μm, and then graphitized at 2200° C. for 48 hours to obtain first carbon-containing particles with a graphitization degree of 83%.

[0062] Example 8 The difference with respect to Example 1 is that the oil-based needle coke raw material that has not been subjected to high-temperature calcination is crushed to D50=13 μm, and then graphitized at 2400° C. for 48 hours to obtain first carbon-containing particles with a graphitization degree of 85%.

[0063] Example 9 The difference with respect to Example 1 is that the oil-based needle coke raw material that has not been subjected to high-temperature calcination is crushed to D50=13 μm, and then graphitized at 2800° C. for 48 hours to obtain first carbon-containing particles with a graphitization degree of 93%.

[0064] Example 10 The difference with respect to Example 1 is that the oil-based needle coke raw material that has not been subjected to high-temperature calcination is crushed to D50=13 μm, and then graphitized at 3000° C. for 48 hours to obtain first carbon-containing particles with a graphitization degree of 95%.

[0065] Embodiment 11 The difference with respect to Example 1 is that the oil-based needle coke calcined at high temperature is crushed to D50=6 μm, and then graphitized at 3400° C. for 48 hours to obtain second carbon-containing particles with a graphitization degree of 98%.

[0066] Example 12 The difference with respect to Example 1 is that the oil-based needle coke calcined at high temperature is crushed to D50=6 μm, and then graphitized at 3000° C. for 48 hours to obtain second carbon-containing particles with a graphitization degree of 94%.

[0067] Embodiment 13 The difference with respect to Example 1 is that the oil-based needle coke calcined at high temperature is crushed to D50=6 μm, and then graphitized at 2800° C. for 48 hours to obtain second carbonaceous particles with a graphitization degree of 92%.

[0068] Embodiment 14 The difference with respect to Example 1 is that the oil-based needle coke calcined at high temperature is crushed to D50=6 μm, and then graphitized at 2600° C. for 48 hours to obtain second carbon-containing particles with a graphitization degree of 90%.

[0069] Embodiment 15 The difference with respect to Example 1 is that the oil-based needle coke raw material that has not been subjected to high-temperature calcination is crushed to D50=5 μm, and then graphitized at 2600° C. for 48 hours to obtain first carbon-containing particles with a graphitization degree of 90%.

[0070] Example 16 The difference with respect to Example 1 is that the oil-based needle coke raw material that has not been subjected to high-temperature calcination is crushed to D50=7 μm, and then graphitized at 2600° C. for 48 hours to obtain first carbon-containing particles with a graphitization degree of 90%.

[0071] Embodiment 17 The difference with respect to Example 1 is that the oil-based needle coke raw material that has not been subjected to high-temperature calcination is crushed to D50=14 μm, and then graphitized at 2600° C. for 48 hours to obtain first carbon-containing particles with a graphitization degree of 90%.

[0072] Embodiment 18 The difference with respect to Example 1 is that the oil-based needle coke raw material that has not been subjected to high-temperature calcination is crushed to D50=15 μm, and then graphitized at 2600° C. for 48 hours to obtain first carbon-containing particles with a graphitization degree of 90%.

[0073] Embodiment 19 The difference with respect to Example 1 is that the oil-based needle coke raw material that has not been subjected to high-temperature calcination is crushed to D50=20 μm, and then graphitized at 2600° C. for 48 hours to obtain first carbon-containing particles with a graphitization degree of 90%.

[0074] Embodiment 20 The difference with respect to Example 1 is that the oil-based needle coke calcined at high temperature is crushed to D50=2 μm, and then graphitized at 3200° C. for 48 hours to obtain second carbon-containing particles with a graphitization degree of 96%.

[0075] Embodiment 21 The difference with respect to Example 1 is that the oil-based needle coke calcined at high temperature is crushed to D50=4 μm, and then graphitized at 3200° C. for 48 hours to obtain second carbon-containing particles with a graphitization degree of 96%.

[0076] Embodiment 22 The difference with respect to Example 1 is that the oil-based needle coke calcined at high temperature is crushed to D50=7 μm, and then graphitized at 3200° C. for 48 hours to obtain second carbonaceous particles with a graphitization degree of 96%.

[0077] Embodiment 23 The oil-based needle coke calcined at high temperature was crushed to D50=10 μm, and then graphitized at 3200° C. for 48 hours to obtain second carbonaceous particles with a graphitization degree of 96%.

[0078] Comparative Example 1 Preparation of comparative graphite negative electrode materials The oil-based needle coke raw material that has not been calcined at high temperature was crushed to D50=12μm, and then graphitized at 2600℃ for 48h to obtain the first carbon-containing particles with a graphitization degree of 90%. Then 20 wt% of petroleum asphalt adhesive was added to carry out a granulation carbonization process with the temperature controlled at 1000℃ for 6h. Finally, it was screened to obtain a comparative graphite negative electrode material.

[0079] Comparative Example 2 Preparation of comparative graphite negative electrode materials The oil-based needle coke calcined at high temperature was crushed to D50=12μm, and then graphitized at 3200℃ for 48h to obtain the second carbon-containing particles with a graphitization degree of 96%. Then 20 wt% of petroleum asphalt adhesive was added to carry out a granulation carbonization process with the temperature controlled at 1000℃ for 6h. Finally, the comparative graphite negative electrode material was obtained by screening.

[0080] The graphite negative electrode materials of the above embodiments and comparative examples were made into batteries for cyclic charge and discharge tests, wherein the batteries were charged to 4.5V at 3C constant current and constant voltage, cut off at 0.05C, and discharged at 0.5C, and the 0.1C gram capacity, negative electrode sheet half-electric rebound, cycle expansion rate, and cycle capacity retention of each battery after 600 cycles of charge and discharge were tested. The relevant test data results of the batteries of each embodiment and comparative example are shown in Table 1 below.

[0081]

[0082] Table 1 It can be seen from the test data in Table 1 above that in Comparative Examples 1 and 2, both of which use a single raw coke raw material or a cooked coke raw material to prepare graphite negative electrode materials, the expansion rate of the battery is significantly increased, especially in Comparative Example 2 which uses a single cooked coke raw material. The gram capacity is high, but the overall expansion is the largest among all the embodiments and comparative examples, and the cycle performance is also significantly reduced. Although the cycle performance retention rate in Comparative Example 1 is relatively good, the gram capacity in Comparative Example 1 is low and the expansion rate is also high. Compared with Comparative Example 1, Comparative Example 2 and Example 1, Example 1 has significantly low expansion performance and cycle capacity retention rate while maintaining a relatively high gram capacity. Compared with Comparative Examples 1 and Comparative Example 2 which use a single raw coke raw material or a cooked coke raw material to prepare graphite negative electrode materials, Example 1 prepares the graphite negative electrode material by using a first carbon-containing particle prepared from a raw coke raw material and having a low graphitization and a second carbon-containing particle prepared from a highly cooked coke raw material and having a high graphitization, which effectively reduces the negative electrode half-electric rebound and cycle expansion of the battery, and at the same time ensures that the gram capacity and cycle performance of the graphite negative electrode material are not affected.

[0083] In Examples 2 to 6, relative to Example 1, Examples 2 to 6 use a different mass ratio for mixing two types of particles from that in Example 1. It can be seen that when the mass ratio of the first carbon-containing particles to the second carbon-containing particles is moderate, such as when the mass ratio in Example 1 is 5:5, it can be effectively ensured that the second carbon-containing particles are bonded to the surface of the first carbon-containing particles after granulation, so that the prepared graphite negative electrode material can be applied to the battery, and the battery can have a better cycle capacity retention rate and a lower cycle expansion rate; among them, it can be seen that the use of large-particle-size and low-graphitization first carbon-containing particles can improve the battery's cycle capacity retention rate and reduce expansion, and the use of small-particle-size and highly graphitized second carbon-containing particles can improve the battery's gram capacity and isotropy; in addition, when the proportion of the first carbon-containing particles in the mass ratio is low, the corresponding battery has a lower negative electrode half-electric rebound.

[0084] In Examples 7 to 10, relative to Example 1, the first carbon-containing particles in Examples 7 and 8 have a lower degree of graphitization, and the first carbon-containing particles in Examples 9 and 10 have a higher degree of graphitization. The graphite negative electrode material prepared from the first carbon-containing particles with a lower or higher degree of graphitization affects the cycle expansion rate and cycle capacity retention rate of the battery. For example, the degree of graphitization of the first carbon-containing particles in Example 7 is 83%, i.e., less than 85%, and the degree of graphitization of the first carbon-containing particles in Example 10 is 95, i.e., greater than 93%. The cycle expansion rate of the battery corresponding to Examples 7 and 10 increases and the cycle capacity retention rate decreases, especially the cycle expansion rate of the battery corresponding to Example 10 increases to a greater extent and the cycle capacity retention rate decreases to a greater extent; in addition, the higher the degree of graphitization of the first carbon-containing particles, the higher the negative electrode half-electric rebound of the corresponding battery.

[0085] In Examples 11 to 14, relative to Example 1, the second carbon-containing particles of Example 11 have a higher degree of graphitization, and the second carbon-containing particles of Examples 12 to 14 have a lower degree of graphitization, wherein the graphite negative electrode material prepared from the second carbon-containing particles with a lower or higher degree of graphitization affects the cycle expansion rate and cycle capacity retention rate of the battery, wherein the graphite negative electrode material prepared from the second carbon-containing particles with a higher degree of graphitization, the corresponding gram capacity of the battery is improved, but the cycle expansion rate and the cycle capacity retention rate will be reduced, such as the graphitization degree of the second carbon-containing particles in Example 11 is 98%, but the graphite negative electrode material prepared from the second carbon-containing particles with too low a degree of graphitization, the corresponding battery has a poor cycle expansion rate and a cycle capacity retention rate, such as the graphitization degree of the second carbon-containing particles in Example 14 is 90%, that is, less than 94%, and the corresponding battery has a greater increase in cycle expansion rate and a greater decrease in cycle capacity retention rate; in addition, the higher or lower the degree of graphitization of the second carbon-containing particles, the higher the negative electrode half-electric rebound of the corresponding battery.

[0086] In Example 15 to Example 19, relative to Example 1, Example 15 and Example 16 reduce the particle size of the crushed raw coke material (i.e., reduce the particle size of the first carbon-containing particles), and Example 17 to Example 19 increase the particle size of the crushed raw coke material (i.e., increase the particle size of the first carbon-containing particles); it can be seen that as the particle size of the raw coke material is smaller, the gram capacity of the battery becomes smaller, but the cycle expansion rate also increases, and the cycle power retention rate decreases, and as the particle size of the raw coke material is larger, the gram capacity of the battery becomes larger, but the cycle expansion rate also increases, and the cycle power retention rate also decreases; In Example 20 to Example 23, relative to Example 1, Example 20 and Example 21 reduce the particle size of the crushed coke raw material (i.e., reduce the particle size of the second carbon-containing particles), and Example 22 and Example 23 increase the particle size of the crushed coke raw material (i.e., increase the particle size of the second carbon-containing particles); it can be seen that as the particle size of the coke raw material is smaller, the gram capacity of the battery becomes smaller, the cycle expansion rate also increases, and the cycle power retention rate decreases, and as the particle size of the raw coke raw material is larger, the gram capacity of the battery becomes larger, the cycle expansion rate also increases, and the cycle power retention rate also decreases; In summary, the graphite negative electrode material of the present application or the graphite negative electrode material prepared by the preparation method of the present application, after being applied to batteries (such as lithium-ion batteries), can enable the battery to maintain a low expansion rate during a long cycle, while having a higher graphite gram capacity and cycle capacity retention rate, thereby extending the battery life and improving the battery fast charging performance.

[0087] The embodiments of the present application have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or improvements to the technology in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.

Claims

1. A graphite negative electrode material, characterized in that: include: A first carbon-containing particle and a second carbon-containing particle, wherein the second carbon-containing particle is bonded to a surface of the first carbon-containing particle; The graphitization degree of the first carbon-containing particles is less than 93%, the graphitization degree of the second carbon-containing particles is greater than 94%, and the median particle size of the first carbon-containing particles is greater than or equal to the median particle size of the second carbon-containing particles.

2. The graphite negative electrode material according to claim 1, characterized in that: The first carbon-containing particles are prepared by graphitizing a raw coke material, and the second carbon-containing particles are prepared by graphitizing a cooked coke material; Preferably, the mass ratio of the first carbon-containing particles to the second carbon-containing particles is (3:7) to (9:1).

3. The graphite negative electrode material according to claim 1, characterized in that: The degree of graphitization of the first carbonaceous particles is 85% to 93%; and / or The degree of graphitization of the second carbonaceous particles is 94% to 98%.

4. A method for preparing the graphite negative electrode material according to any one of claims 1 to 3, characterized in that: include: After the raw coke material is crushed into particles, the first carbon-containing particles having a graphitization degree of less than 93% are prepared by graphitization treatment; After the cooked coke raw material is crushed into particles, the second carbon-containing particles having a graphitization degree greater than 94% are prepared by graphitization treatment; The first carbon-containing particles and the second carbon-containing particles are mixed in a preset mass ratio, a binder is added, and granulation carbonization treatment is performed to obtain a graphite negative electrode material; wherein the second carbon-containing particles in the graphite negative electrode material are bonded to the surface of the first carbon-containing particles, and the median particle size of the first carbon-containing particles is greater than or equal to the median particle size of the second carbon-containing particles.

5. The preparation method according to claim 4, characterized in that: The median particle size of the first carbonaceous particles is 7 μm to 15 μm; and / or The median particle size of the second carbonaceous particles is 4 μm to 7 μm.

6. The preparation method according to claim 4, characterized in that: The raw coke material is one or more of petroleum coke, coal-based coke, oil-based needle coke, and coal-based needle coke; and / or The cooked coke raw material is obtained by calcining one or more of petroleum coke, coal-based coke, oil-based needle coke and coal-based needle coke.

7. The preparation method according to claim 4, characterized in that: The temperature of the raw coke material during graphitization treatment is 2500° C. to 2800° C. for 24 to 72 hours; and / or The temperature of the cooked coke raw material during graphitization treatment is 2900° C. to 3500° C. and the duration is 24 to 72 hours; and / or The granulation carbonization temperature is 500° C. to 2000° C., and the duration is 3 to 10 hours.

8. The preparation method according to claim 4, characterized in that: The method further comprises: The content of the binder in the graphite negative electrode material is 5wt%~50wt%; Preferably, the adhesive is selected from one or more of petroleum asphalt, coal tar asphalt, phenolic resin, epoxy resin and the like.

9. A negative electrode sheet, characterized in that: The invention comprises a negative electrode current collector and a negative electrode active material, wherein the negative electrode active material is arranged on the surface of the negative electrode current collector, and the negative electrode active material comprises the graphite negative electrode material according to any one of claims 1 to 3 or the graphite negative electrode material prepared by the method according to any one of claims 4 to 8.

10. A battery, characterized in that: Including the negative electrode sheet as claimed in claim 9.