Air battery catalytic compound as well as preparation method and application thereof
Through the combination of precious metal Pt-Co nanoparticles and carbon support, the activity and specific surface area of the catalytic composite of aluminum-air battery are improved, the corrosion and polarization problems in aluminum-air batteries are solved, and the discharge performance and oxygen utilization rate of the battery are improved. .
Patent Information
- Application Number
- CN202411187651.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
Aluminum-air batteries have problems such as corrosion and hydrogen evolution of aluminum anode, serious polarization of air electrodes, low oxygen energy expansion ability, and low oxygen utilization rate of air electrodes.
The combination of precious metal Pt-Co nanoparticle catalyst and carbon support is used to prepare a composite support of carbon materials and graphene through graphite oxidation and ultrasonic treatment, which improves the specific surface area and discharge platform of the catalytic composite, and is used to prepare the catalytic of aluminum air batteries. layer.
The oxygen reduction activity and catalytic performance of the catalytic composite are significantly improved, the discharge performance of aluminum-air batteries is enhanced, and the key problems in the development of aluminum-air batteries are solved.
Smart Images

Figure CN119092730A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an air battery catalytic composite, a preparation method and application thereof, and belongs to the technical field of functional materials. Background Art
[0002] As a new type of high-energy green chemical power source, metal-air fuel cells have superior cost-effectiveness and have the potential to replace traditional lead-acid batteries. The basic structure and working principle of metal-air batteries are similar. Their negative electrodes all use cheap metals as active materials, while the active materials used in the air electrode are oxygen or pure oxygen from the air. Oxygen continuously diffuses through the air electrode to the interface of the electrochemical reaction and reacts chemically with the anode metal to release electrical energy. Metal-air batteries are usually classified according to the different types of metal anodes. At present, the types of metal-air batteries that are studied more are mainly zinc-air batteries, magnesium-air batteries, aluminum-air batteries, lithium-air batteries, etc. Aluminum-air batteries stand out among many metal-air batteries because of their high specific energy, rich sources of raw materials, safe use, and good stability. Aluminum-air batteries use pure aluminum or aluminum alloy as the negative electrode of aluminum-air batteries, and oxygen in the air as the positive electrode fuel of the battery. During the discharge process of the battery, the anode is continuously consumed to generate Al(OH)3. Oxygen enters the electrolyte through the air electrode and reaches the reaction interface to undergo oxygen reduction reaction, resulting in a discharge reaction. Applications include: electric vehicles, communication power supply, and submarine operations. Although aluminum-air batteries have many outstanding advantages, there are still some problems. For example, the corrosion and hydrogen evolution of the aluminum anode in the aluminum-air electrode, the serious polarization of the air electrode, the low oxygen expansion capacity, and the low oxygen utilization rate of the air electrode. Summary of the invention
[0003] In order to overcome the shortcomings of the prior art, the first object of the present invention is to provide an air battery catalytic composite, which improves the activity of the catalytic composite as a whole by combining precious metals and carbon carriers, and the obtained catalytic composite has a larger specific surface area and a higher discharge platform.
[0004] The second object of the present invention is to provide a method for preparing the above-mentioned air battery catalytic composite. By improving the preparation method, the catalyst and the carrier are better combined to achieve functional coordination, thereby enhancing the discharge performance of the battery.
[0005] The third object of the present invention is to provide an application of the above-mentioned air battery catalytic composite for preparing an air battery using a NaCl solution as an electrolyte.
[0006] The first object of the present invention can be achieved by adopting the following technical scheme: an air battery catalytic composite, comprising a catalyst and a carrier; the catalyst is loaded on the carrier; the catalyst is a Pt-Co nanoparticle catalyst, and the mass ratio of Pt to Co is 1-10:3; the carrier is a composite carrier of carbon material and graphene; the mass ratio of carbon material to graphene is 1:1-10; the carbon material is carbon black XC-72 and / or multi-walled carbon nanotubes.
[0007] Furthermore, the mass ratio of Pt to Co is 2:1.
[0008] Furthermore, the mass ratio of the carbon material to the graphene is 1:2.
[0009] Furthermore, the graphene is polyaniline-modified graphene.
[0010] The second object of the present invention can be achieved by adopting the following technical scheme: A method for preparing an air battery catalytic composite comprises:
[0011] Graphite oxidation step: pre-oxidize the graphite, place it in an ice bath for 0.2-5 hours, and then oxidize it at a temperature of 15-95° C. to obtain oxidized graphite;
[0012] The preparation steps of the carrier are as follows: mixing graphite oxide and carbon material, performing ultrasonic treatment, washing and drying to obtain the carrier; the carrier is a composite carrier of carbon material and graphene; the mass ratio of carbon material to graphene is 1:1-10; the carbon material is carbon black XC-72 and / or multi-walled carbon nanotubes;
[0013] The preparation steps of the catalytic complex are as follows: H2PtCl6 and Co(CH3COO)2 solution are added to the ethylene glycol and isopropanol suspension of the carrier, and microwave treatment is performed to obtain the catalytic complex; the mass ratio of Pt to Co in the catalytic complex is 1-10:3.
[0014] Furthermore, in the oxidation step of graphite, an ice bath is performed for 0.2-5 hours, a strong oxidant is slowly added under the condition of not exceeding 20°C, and then oxidation is carried out in sequence at a medium temperature of 30-50°C and a high temperature of 80-95°C to obtain oxidized graphite.
[0015] Furthermore, in the step of oxidizing graphite, the oxidized graphite is modified with polyaniline and then expanded.
[0016] Furthermore, in the step of preparing the catalytic complex, the microwave treatment is performed intermittently, the microwave time for each treatment is 0.3-3 minutes, and there is a pause of 0.3-1.5 minutes between each microwave treatment.
[0017] Furthermore, in the step of preparing the catalytic composite, the mass ratio of ethylene glycol to isopropanol is 3-12:1.
[0018] The third object of the present invention can be achieved by adopting the following technical scheme: an air battery, the air battery is an aluminum air battery, the air battery includes a catalytic layer; the catalytic layer carries an air battery catalytic complex; the air battery uses NaCl solution as an electrolyte; the air battery catalytic complex includes a catalyst and a carrier; the catalyst is loaded on the carrier; the catalyst is a Pt-Co nanoparticle catalyst, and the mass ratio of Pt to Co is 1-10:3; the carrier is a composite carrier of carbon material and graphene; the mass ratio of carbon material to graphene is 1:1-10; the carbon material is carbon black XC-72 and / or multi-walled carbon nanotubes.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1. The air battery catalytic composite of the present invention has a larger specific surface area and a higher discharge platform, and has a higher oxygen reduction activity;
[0021] 2. The air battery catalytic composite of the present invention combines the precious metal and the carbon carrier, the catalyst and the carrier have good binding properties, and they promote each other, and the whole has good catalytic performance;
[0022] 3. The preparation method of the air battery catalytic composite of the present invention is flexible and efficient, can be used for industrial production, and is beneficial to improving the bonding degree between the catalyst and the carrier. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1-3 To pre-treat graphite oxide XRD graph, infrared spectrum graph, Raman spectrum graph; Figure 4-5 SEM images of Pre-GO and N-GO; Figure 6-8 XRD diagram, infrared spectrum and Raman spectrum of ice bath sample; Figure 9-12 is the SEM image; Figure 13-15 XRD patterns, infrared spectra, and Raman spectra of flake graphite, graphite oxide, T-GNS, and PANI-GNS; Figure 16-19 is the SEM image; Figure 20-21 TEM images of T-GNS and PANI-GNS; Fig. 22 This is a diagram of the adsorption of the high-pressure part; Figure 23-26 The discharge curves are 10mA, 20mA, 30mA and 40mA; Fig. 27 is the XRD pattern of the catalytic composite; Figure 28-29 Cyclic voltammetry and linear scanning curves of the catalytic complex; Figure 30-32 XRD graph, CV graph, LSV graph; Figure 33-34 is the XRD pattern; Figure 35-38 Transmission electron microscopy of the catalytic complex; Figure 39-40CV curve and LSV curve of electrode; Figures 41-44 The discharge curves are 10mA, 20mA, 30mA and 40mA; Fig.45 is the XRD pattern of the carrier; Figures 46-51 is the TEM image of the carrier; Figure 52-53 CV curve and LSV graph of the carrier; Figure 54-57 The discharge curves are 10mA, 20mA, 30mA and 40mA; Figure 58-61 Transmission electron microscopy of the catalytic complex; Figure 62-63 CV curve and LSV graph of the catalytic complex; Figures 64-67 The discharge curves are 10mA, 20mA, 30mA and 40mA. DETAILED DESCRIPTION
[0024] Below, the present invention is further described in conjunction with the accompanying drawings and specific embodiments:
[0025] An air battery catalytic composite comprises a catalyst and a carrier; the catalyst is loaded on the carrier; the catalyst is characterized in that the catalyst is a Pt-Co nanoparticle catalyst, the mass ratio of Pt to Co is 1-10:3; the carrier is a composite carrier of carbon material and graphene; the graphene is polyaniline-modified graphene; the mass ratio of carbon material to graphene is 1:1-10; the carbon material is carbon black XC-72 and / or multi-walled carbon nanotubes.
[0026] The preparation method of the air battery catalytic composite is as follows:
[0027] Graphite oxidation steps: pre-oxidize the graphite, place it in an ice bath for 0.2-5h, slowly add a strong oxidant under the condition of not exceeding 20°C, and then oxidize it in sequence at a medium temperature of 30-50°C and a high temperature of 80-95°C to obtain oxidized graphite; modify the oxidized graphite with polyaniline, and then expand it;
[0028] The preparation steps of the carrier are as follows: mixing graphite oxide and carbon material, performing ultrasonic treatment, washing and drying to obtain the carrier; the carbon material is carbon black XC-72 and / or multi-walled carbon nanotubes;
[0029] The preparation steps of the catalytic complex are as follows: H2PtCl6 and Co(CH3COO)2 solution are added to the ethylene glycol and isopropanol suspension of the carrier, and the mass ratio of ethylene glycol to isopropanol is 3-12:1; then intermittent microwave treatment is performed, each microwave time is 0.3-3 minutes, and a pause of 0.3-1.5 minutes is made between each microwave treatment to obtain the catalytic complex.
[0030] The catalytic composite can be used to prepare aluminum-air batteries, and more specifically, loaded on the catalytic layer of the air battery: the air battery uses NaCl solution as the electrolyte.
[0031] Catalytic complexes are the core materials in air batteries. Developing highly active, long-life, and low-cost catalytic complexes is the key to improving the performance of air batteries and can solve many key issues that restrict the development of aluminum-air batteries.
[0032] The basic requirements for air electrode catalyst materials are as follows: the specific surface area must be large enough; it can accelerate the reduction / precipitation process of oxygen; it can catalyze the decomposition of the intermediate product H2O2; it has good corrosion resistance to electrolytes; and it has excellent electrical conductivity. For heterogeneous catalytic materials, the size of their specific surface area does not determine the level of their activity, but for the same catalyst material, the size of their specific surface area determines the number of catalytic active sites formed, thereby determining the size of the catalytic activity.
[0033] The particle size, uniformity, activity and type of the catalyst become direct factors affecting the performance of the air electrode. Current research focuses also include the preparation of different positive electrode catalysts, different configurations of air electrodes and the mechanism of catalyst reduction of oxygen.
[0034] The characterization and electrochemical performance testing methods of the following examples are as follows:
[0035] 1. Characterization methods
[0036] 1. Fourier transform infrared spectroscopy (FT-IR): Infrared absorption spectroscopy is to identify the structure of compounds and molecules by the characteristic absorption peaks of different substances to different wavelengths of infrared radiation. Mix and grind the dry sample (about 5 mg) with KBr (about 50 mg), press into tablets, and scan in the range of 4000-500 cm -1 , resolution 4cm -1 , scanning times 2. All samples in this test were tested for their infrared absorption spectra in the AVATAR360 Fourier transform infrared spectrometer produced by Nicolet, USA.
[0037] 2. X-ray diffraction test (XRD): X-ray diffraction test (X-Ray Diffraction) uses X-ray diffraction to detect crystal formation to determine the grain size and spatial structure arrangement of the sample. From a certain characteristic diffraction angle in its diffraction spectrum, it can be seen that the wider the half-peak width, the finer the grains and the better the distribution.
[0038] This analysis was conducted on a Shimadzu XRD-6000 X-ray diffractometer, with a CuKα target as the radiation source (λ = 0.154056 nm), a CuKα target as the diffraction source, a test angle of 5° to 90°, and a scanning speed of 2° / min. The particle size of the nanoparticles on the catalytic complex can be analyzed using the software MDI Jade 5.0. The interlayer spacing of graphene can be calculated using the Bragg formula: d 002 =λ / 2sinθ. λ is the characteristic wavelength of the incident ray, here it is 0.154056, θ is the diffraction angle. This method can detect and analyze the atoms inside the material. The space group, grain size, and lattice parameters of the crystal can be obtained, and the powder can be identified from the diffraction peak position and peak intensity.
[0039] 3. Scanning electron microscope (SEM) and energy spectrum (EDX): Scanning electron microscope (Scanning Electron Microscope) uses a focused electron beam to scan the sample surface point by point, collects the generated secondary electrons and some backscattered electrons, and converts them into electrical signals, showing an image synchronized with the electron beam. The morphology of the sample surface can be obtained through the scanning electron microscope. This paper uses a Japanese Hitachi S3700 scanning electron microscope.
[0040] Sample preparation: Take a small amount of sample and put it into a 50mL beaker, add 40mL of ethanol, place it on an ultrasonic cell crusher for ultrasonic dispersion for 5 minutes, and use a pipette tip to dip the sample and disperse it on the conductive glue.
[0041] 4. Transmission electron microscope (TEM), high-resolution transmission electron microscope (HRTEM): Transmission electron microscope (TEM), referred to as TEM, accelerates the electron beam to transmit to a very thin sample, produces a three-dimensional angle scattering, and obtains the microscopic shape, size, electron diffraction ring and energy spectrum of the sample through the different diffraction angles, the thickness and density of the sample. In order to better observe the microstructure of graphite oxide, graphene and metal-loaded catalytic complexes, they are dispersed and prepared into transmission electron microscope samples, and their micromorphology and particle microstructure are tested and analyzed under transmission electron microscope and high-resolution transmission electron microscope. The sample preparation method is: take a small amount of sample (about 1 mg) and grind it into fine powder, ultrasonically disperse it in anhydrous ethanol, treat it for 2 minutes, adjust it to a suitable concentration, take a drop of suspension with a pipette, carefully drop it on the micro grid coated with carbon film, and make the observation sample after natural drying.
[0042] 2. Electrochemical performance test and analysis
[0043] 1. Preparation of research electrodes: Preparation of research electrodes: Glassy carbon electrodes (0.071 cm 2 ) polished to a mirror surface, the treated electrodes were placed in acetone and double distilled water for 30 seconds, and then washed and set aside. Weigh 2 mg of the catalytic complex and disperse it in a mixed solution of 1 mL of double distilled water and 1 mL of anhydrous ethanol, ultrasonically oscillate for 15 minutes, then use a pipette to take 4 μL and carefully drop it on the glassy carbon electrode. After it is naturally dried in the air, cover the electrode surface with 4 μL of 0.5 wt% Nafion ethanol solution to obtain an electrode for use. The same steps were used to prepare other research electrodes.
[0044] 2. Preparation of oxygen reduction electrode and assembly of simulated battery: oxygen reduction electrode is the positive air electrode of aluminum-air battery, which is mainly composed of three parts: catalyst layer, current collector and diffusion layer. In order to increase the diffusion capacity of oxygen in the air and reduce the corrosion of the current collector, the structure of diffusion layer-current collector-diffusion layer-catalytic layer is adopted.
[0045] Preparation of diffusion layer: The diffusion layer has the functions of hydrophobicity and air permeability. On the one hand, it can prevent the leakage of electrolyte, and on the other hand, it can promote the better diffusion of oxygen in the air from the atmosphere to the reaction interface layer. Its preparation process is mainly as follows:
[0046] 1) Grind ammonium oxalate into fine powder, take 2.0g and add it to a 150mL beaker, then add 50mL of anhydrous ethanol, cover with plastic wrap, and stir for 3h;
[0047] 2) Add 1.0 g of acetylene black and continue to stir thoroughly for 9 h. Add 2.5 g of polytetrafluoroethylene (PTFE) dropwise to the mixture and continue to stir for 12 h to make it evenly dispersed. During this period, cover with plastic wrap to prevent ethanol from volatilizing after long-term stirring.
[0048] 3) Remove the plastic wrap, place in a 80°C water bath, stir and heat to remove ethanol, and when no obvious ethanol is present, roll it on both sides of a 2cm×3cm nickel foam, leaving 1.0cm at the top. Place in an oven and dry at 130°C for 12h.
[0049] Preparation of the catalytic layer: The main function of the catalytic layer is to catalyze the reduction reaction of oxygen in the air. The preparation process of the air electrode in this paper is made by manual coating method. The specific process is as follows: weigh 30 mg of the catalytic complex, put it in a small beaker, add a certain amount of n-2 methylpyrrolidone (NMP), ultrasonically disperse it for 30 minutes, add 0.1g of polyvinylidene fluoride (PVDF), stir it with a magnetic stirrer for 12 hours, until the catalytic complex is adjusted into a paste and evenly applied to one side of the diffusion layer, prepare two air electrodes, mark the catalytic layer, and then put it in a vacuum oven at 45°C for 12 hours, cool it down and take it out, use a tablet press at 4MPa for 5 minutes, press the electrode sheet tightly, and get the working electrode.
[0050] Leave 1.0 cm of nickel foam current collector on the upper side of the air electrode, mainly for the convenience of contact with the test electrode clamp during testing. When applying, be sure to divide the catalytic compound into two equal parts, and gently apply it on one layer of the catalytic layer. Wait until it is dry before pressing.
[0051] The negative electrode of the battery is an industrial aluminum sheet immersed in an electrolyte. The electrolyte is a 3.5wt% NaCl solution, and the air electrode is semi-immersed, with one side of the electrode in contact with the electrolyte and the other side connected to the atmosphere. A ventilation structure is designed on the layer connected to the atmosphere.
[0052] The aluminum-air batteries in this study all use 3.5wt% NaCl with a pH of 11 as the electrolyte.
[0053] 3. Linear Sweep Voltammetry: Linear Sweep Voltammetry is a method that controls the electrode potential to change at a constant rate while measuring the response current through the electrode. The measurement results are often expressed as an iE curve. When the electrode potential is scanned from a relatively positive potential where no reduction reaction occurs to a negative direction, the reduction current first gradually increases and then gradually decreases. By comparing the peak current, the catalytic oxygen reduction activity of the catalytic complex can be analyzed.
[0054] The operating conditions of this polarization curve are: electrode potential range: 0.8-0V; scanning speed: 0.0005V / s; static time: 5s; working electrode is glassy carbon (GC) electrode (d=3mm) loaded with the prepared catalytic complex; reference electrode: Ag / AgCl electrode; electrolyte: 0.5mol / L H2SO4; counter electrode: pure platinum electrode. Oxygen was passed into the electrolyte for 30min before the electrochemical test, and oxygen saturation was maintained during the test. All tests were carried out at 25°C.
[0055] 4. Cyclic voltammetry (CV) test: The cyclic voltammetry curve (Cyclic Voltammogram) uses a triangular wave signal as a potential control signal, scans negatively from a certain potential at a certain rate, and changes the scanning direction to scan back to the starting potential after reaching a certain electrode potential. The rate remains unchanged, and scans for multiple rounds to obtain the iE curve. The peak current of the cathode and anode can be obtained through the cyclic voltammetry curve. In this paper, it is mainly used to judge the cyclic stability of the catalytic complex.
[0056] The working electrode was a glassy carbon (GC) electrode (d = 3 mm) loaded with the prepared catalytic complex. Nitrogen was introduced into the electrolyte for 30 min to remove dissolved oxygen before the electrochemical test. The scanning speed was 0.5 V / s, the scanning range was -0.2 to 1.0 V, and 50 cycles were used. The other conditions were the same as those of the linear scanning test.
[0057] 5. Characterization of constant current discharge of aluminum-air battery: Constant current discharge curve is a common test method to measure the performance of electrodes. The discharge voltage of batteries composed of different electrodes under the same current conditions can be obtained through constant current discharge test, so as to judge the pros and cons of the activity of the catalytic complex during the use of the battery. Pure aluminum sheet is used as the negative electrode, air electrode is used as the positive electrode, the electrolyte is 3.5wt% NaCl, and the aluminum sheet specifications are: 99.986% high-purity aluminum, size 2.5cm×2.5cm. The whole battery is tested using the Xinwei BTS-5V / 100mA high-precision battery performance test system, and constant current discharge is performed at 10mA, 20mA, 30mA, and 40mA respectively. It is left to stand for 10min before discharge and discharged for 60min.
[0058] Embodiment 1:
[0059] Preparation of graphite oxide
[0060] The graphite uses natural flake graphite, and a mixed solution of P2O5, KMnO4, K2S2O8, and concentrated H2SO4 is used to pre-oxidize the graphite. NaNO and concentrated H2SO4 are added, and the mixture is stirred and mixed evenly in an ice bath (-2℃~4℃). A strong oxidant is slowly added under the condition that the temperature does not exceed 20℃, and then the graphite is oxidized through a process of medium temperature 35℃ and high temperature 90℃. A large amount of water is added to dilute it, and then hydrogen peroxide is added to reduce the remaining oxidant. The product is then washed with hydrochloric acid and distilled water, and vacuum dried to obtain oxidized graphite.
[0061] 1. Effect of pretreatment on the preparation of graphite oxide:
[0062] The ice bath (0℃) time was fixed at 4h, the medium temperature was 35℃ for 1h, and the high temperature was 90℃ for 30min. The graphite oxide was tested, and the XRD pattern was as follows: Figure 1As shown. Pre-GO is graphite oxide obtained after a pretreatment step, N-GO is graphite oxide obtained without a pretreatment step, and graphite is graphite without oxidation. Figure 1 As shown in the figure, the peak at the 2θ angle of 26.70° of flake graphite belongs to the typical graphite peak (002) diffraction peak, and has high intensity and sharp peak shape. 002 The value is about 0.3336nm. By comparing the diffraction pattern of the original flake graphite, it can be found that the peak at 26.70° disappears after the flake graphite is oxidized. For N-GO, the characteristic peak of (001) appears at 11.83°, and the interlayer spacing d 001 The value is about 0.7475nm. Under the same conditions, when the pretreatment step is adopted, the characteristic peak of the (001) of the obtained Pre-GO appears at 9.37°, and the interlayer spacing d 001 The value is about 0.9431nm. It is 0.1956nm larger than the interlayer spacing of N-GO without pretreatment. Compared with the original flake graphite, the interlayer spacing of oxidized graphite increases, which is due to the introduction of a large number of oxygen-containing groups. Comprehensive analysis shows that when the pre-oxidation step is adopted, the (001) characteristic peak of oxidized graphite shifts to a smaller angle and the interlayer spacing increases, which proves that the more oxygen-containing groups are inserted into the interlayer, the more completely the flake graphite is oxidized.
[0063] Figure 2 It is an infrared spectrum. As shown in the figure, at 3000~3700cm -1 The absorption peaks in the range are attributed to the deformation vibration peak of OH; 1734cm -1 The absorption peak at 1605cm -1 The peak at 1060cm corresponds to the deformation vibration absorption peak of the bound water molecules between samples; -1 The absorption peak that appears at belongs to the vibration absorption peak of COC. The existence of these oxygen-containing groups fully demonstrates that the graphite has been oxidized but not fully dried. From the spectrum analysis, it can be concluded that due to the presence of polar groups on the surface of graphite oxide, it is very easy to produce hydrogen bonds with water molecules in aqueous solution. This explains why graphite oxide has good hydrophilicity.
[0064] Raman spectroscopy Figure 3 As shown. Graphite sample at 1582cm -1 The peak is sharp, corresponding to all sp 2 The G peak is generated by the stretching motion of the atomic pair. -1 The D peak caused by the defective structure is smaller, which corresponds to the typical graphite structure characteristics. The increase in disorder and the presence of independent double bond fragments often lead to a blue shift of the G peak. The D peak enhancement obeys the TK relationship, I(D) / I (G) ∝1 / L a Among them, I (D) / I (G) Represents the intensity ratio of the D peak and the G peak, which is used to measure the degree of structural defects of the sample. a Represents the size of graphite crystallites in the sample. The more completely the graphite is oxidized, the more surface defects it will cause. (D) / I (G) By calculating the I of graphite, graphite oxide N-GO and Pre-GO (D) / I (G) The values of the G peak blue shift and the half-height width of the D peak are compared with the structural characteristics of the unoxidized graphite, as shown in Table 1. After the graphite is oxidized, the D peak is enhanced and broadened, the G peak is blue shifted and broadened, and the I (D) / I (G) The I of Pre-GO obtained after pretreatment is increased from 0.52 to 1.32 and 1.69. This is because the bonding mode of the carbon bonds on the surface of graphite is destroyed after oxidation, indicating that the disorder of the graphite structure increases after oxidation, resulting in the enhancement of the D band and the broadening of the G peak width. (D) / I (G) It is larger than that of N-GO obtained without pretreatment, and the half-peak width of the D band is also increased, indicating that the pretreatment step can make the graphite oxidation more complete.
[0065] Table 1 Raman spectroscopy analysis data
[0066] Sample type I(D) / I(G) <![CDATA[G peak offset (cm -1 )]]> <![CDATA[WF,D(cm- 1 )]]> graphite 0.52 0 35 N-GO 1.32 9 87 Pre-GO 1.69 6 164
[0067] The SEM morphologies of Pre-GO and N-GO are shown in Figure 4-5 As shown in the figure, both graphite oxides have wrinkled structures on their surfaces, but the wrinkles on the surface of graphite oxide Pre-GO obtained after the pretreatment step are more obvious, showing a larger surface area and being more fluffy. This indicates that the pretreatment step can make graphite oxidation more complete, which is consistent with the previous conclusion.
[0068] 2. Effect of ice bath time on graphite oxide:
[0069] Three groups of conditions with ice bath time of 0.5h, 2h and 4h were designed to prepare graphite oxide, which were represented by GO0.5, GO2 and GO4 respectively. Graphite was the untreated graphite. Figure 6 XRD patterns of three groups of samples.
[0070] The figure shows that the 2θ angle of the diffraction peak of flake graphite (002) is 26.70°, d 002The value is about 0.3336nm. By comparing the diffraction spectrum of the original flake graphite, it can be found that the peak at 26.70° disappears after the flake graphite is oxidized. For GO0.5, the characteristic peak (002) appears at 11.31°, d 002 The value is about 0.7817nm, and the characteristic peak of GO2 (002) appears at 9.98°, d 002 The value is about 0.8856nm. When the ice bath time is extended to 4h, the characteristic peak of GO4(002) appears at 9.37°, d 002 The value is about 0.9431nm. Compared with the original flake graphite, the interlayer spacing of oxidized graphite increases, which is due to the introduction of oxygen groups, which makes its interlayer spacing much larger than that of the original flake graphite. Comprehensive analysis shows that when the ice bath time is extended, the (002) characteristic peak of oxidized graphite shifts to a smaller angle and the interlayer spacing increases, which proves that the more oxygen-containing groups are inserted into the interlayer, the more completely the flake graphite is oxidized. The diffraction peak corresponding to the C hexagonal structure at a 2θ angle of 42.6°. The more obvious the peak, the fewer layers of oxidized graphite. As can be seen from the figure, as the ice bath time increases, the more obvious the peak here is, indicating that the flake graphite is more severely exfoliated.
[0071] Figure 7 This is the infrared spectrum of graphite oxide. As can be seen from the figure, after graphite is oxidized in different ice bath times, the -1 The absorption peak at 1628 cm is the vibration absorption peak of COC. -1 The peak is the deformation vibration absorption peak generated by the binding of water molecules, at 1732cm -1 The absorption peak at 3000-3700cm is attributed to the stretching vibration peak of C=O on the carboxyl group of graphite oxide; -1 The absorption peaks in the range are attributed to the deformation vibration peaks of OH; the presence of these oxygen-containing groups fully demonstrates that the graphite has been oxidized. From the peak shape and peak area, when the ice bath time is 4 hours, the oxidation is relatively complete.
[0072] Figure 8 is a Raman spectrum diagram. It can be seen from the figure that, relative to the original graphite, the D peak of the graphite oxide prepared under different ice bath times is enhanced and broadened, and the G peak is blue-shifted and broadened. The I (D) / I (G) , the blue shift of the G peak, and the half-peak width of the D band are shown in Table 2.
[0073] Table 2 Raman spectroscopy analysis data
[0074] Sample type I(D) / I(G) <![CDATA[G peak offset (cm -1 )]]> WF,D(cm-1) graphite 0.52 0 35 GO0.5 1.63 3 143 GO2 1.67 13 135 GO4 1.69 14 164
[0075] Compared with the original graphite, the G peak of the graphite oxide prepared under different ice bath time appears blue shift and broadening, and I(D) / I (G) The value increases, and the half-peak width of the D band increases. The I (D) / I (G) , G peak offset and D band half-peak width. As the ice bath time increases, the G peak offset increases, and I (D) / I (G) The value increases. This indicates that as the ice bath time increases, the disorder of the prepared graphite oxide increases and the oxidation becomes more complete.
[0076] Figure 9-12 The SEM images of graphite, GO0.5, GO2, and GO4 are shown in the figure. As shown in the figure, the interlayer spacing of the unoxidized flake graphite is very small, while the oxidized graphite prepared after deep oxidation has a typical oxidized graphite wrinkle morphology. As the ice bath time increases, the surface wrinkles of the oxidized graphite become more severe and the disorder increases. This is because the introduction of larger oxygen-containing groups increases the oxidation degree of the oxidized graphite.
[0077] Embodiment 2:
[0078] Preparation of graphene
[0079] Polyaniline (PANI)-modification method: Take 200 mg of graphite oxide (GO) fine powder prepared in Example 1, ultrasonicate in 400 mL of distilled water for 30 minutes, add concentrated HCl to make it into a 1 mol / L solution. After stirring for 30 minutes, add 100 mg of aniline monomer to the solution and continue stirring for 30 minutes. Then weigh 0.17 g of (NH4)S2O8 and dissolve it in 10 mL of 1 mol / L HCl, add it dropwise to the above mixture, and stir at room temperature for 24 hours. Wash with a large amount of distilled water, filter, and vacuum dry at 40 ° C to obtain PANI-GO powder. Grind the dried PANI-GO into powder, add it to a muffle furnace preheated to 1000 ° C, and expand it rapidly for 30 seconds to obtain peelable graphite. Add anhydrous ethanol and treat it in an ultrasonic bath for 30 minutes to obtain a black suspension. After washing and filtering with ethanol several times, vacuum dry it at 40 ° C for 24 hours to obtain PANI-graphene (GNS) powder.
[0080] For comparison, graphene was prepared by thermal expansion method: first, fine graphite oxide powder was placed in a muffle furnace preheated to 1000°C and rapidly expanded for 30 seconds to obtain exfoliable graphite. Anhydrous ethanol was added to the exfoliable graphite and treated in an ultrasonic bath for 30 minutes to obtain a black suspension. After washing and filtering with ethanol several times, T-graphene (GNS) powder was obtained by vacuum drying at 40°C for 24 hours.
[0081] The XRD patterns of graphite, graphite oxide (GO), T-GNS and PANI-GNS are shown in Figure 2. Fig.13As shown in the figure, the 2θ angle of the (002) diffraction peak of flake graphite is 26.70°, which is a typical graphite peak with sharp peak shape and high intensity. 002 The value is about 0.3336nm. By comparing the diffraction spectrum of the original flake graphite, it can be seen that the intensity of the (002) crystal plane diffraction peak at 26.70° is weakened, and the peak shape changes from sharp to a bun peak (GO, T-GNS and PANI-GNS), and shifts to a small angle. From the XRD of GO, it is known that the characteristic peak of (001) appears at 9.37°, d 001 The value is about 0.9431nm, which is due to the introduction of oxygen groups, making its interlayer spacing much larger than that of the original flake graphite. The diffraction peak corresponding to the C hexagonal structure at a 2θ angle of 42.6°. From the spectrum of T-GNS, since the product is thin-layer graphene, the diffraction peak corresponding to the (002) crystal plane disappears, a bun peak appears, and the structure becomes disordered, which explains from the lattice theory that the product meets the characteristics of thin-layer graphene. According to the position of the (002) diffraction peak, using the Bragg equation (2.1), it can be seen that the interplanar spacing of T-GNS has decreased by 0.5741nm compared to the original oxidized graphite of 0.9431nm, indicating that the thermal expansion has caused the oxygen-containing functional groups between the tight oxidized graphite layers to partially decompose into small molecules of water and carbon dioxide, thereby exfoliating the graphite sheets. The interlayer spacing of T-GNS after exfoliation is 0.3690nm, but it is still larger than the interlayer spacing of the original graphite of 0.3336nm, which indicates that there are still a small amount of incompletely reduced oxygen-containing functional groups between the stacking layers or on the surface of the obtained T-GNS sample. Relatively speaking, the diffraction peak intensity of PANI-GNS at (002) is weaker, and its disorder is greater, indicating that the exfoliation is more complete. According to the Bragg equation, the interplanar spacing of PANI-GNS is 0.3559nm, which is slightly smaller than the interplanar spacing of T-GNS, indicating that there are fewer residual oxygen-containing functional groups.
[0082] Infrared spectrum Fig.14 As shown in the figure, after strong oxidation by oxidant, the GO sample has a -1 An absorption peak appeared, which was attributed to OH stretching vibration. -1 The absorption peak at 1605cm is attributed to the stretching vibration of C=O at the edge of graphite oxide. -1 It is the absorption peak produced by the bound water molecules between samples. 1400cm -1 The absorption peaks at 1240 and 1060 cm are the vibration peaks of saturated tertiary hydroxyl groups. -1 The absorption peaks at 1240 and 1060 cm are generated by the asymmetric and symmetric stretching vibrations of the epoxy groups COC between graphene oxide layers. -1The peaks of the epoxy group stretching vibration between the layers are located at 1605 and 1400 cm -1 The vibration absorption peaks of interlayer bound water molecules and saturated tertiary hydroxyl groups at 1580 cm-1 of T-GNS are basically gone, which fully indicates that T-GNS and PANI-GNS have undergone reduction reaction. -1 and PANI-GNS at 1612cm -1 The absorption peak at is the absorption peak generated by the skeleton vibration of the graphene sheet. The absorption peak intensity of the sample T-GNS near this point is stronger than that of PANI-GNS, indicating that T-GNS has a higher degree of regularity, indicating that its degree of exfoliation and reduction is not as high as that of PANI-GNS. This is consistent with the previous XRD results.
[0083] Raman spectrum Fig.15 As shown, after graphite is oxidized, the surface carbon bond bonding mode changes. (D) / I (G) The increase in the graphite structure indicates that the disorder of the graphite oxide structure increases. Since the oxygen-containing groups destroy the symmetry of graphite and produce disorder, this leads to the enhancement of the D band and the increase in the peak width of the G peak. This further illustrates that after oxidation, the introduction of oxygen-containing groups leads to an increase in the disorder of the graphite interlayer structure. Compared with the Raman spectrum of graphite oxide, graphene I (D) / I (G) The value of further increases, which is mainly attributed to the further decrease in order degree during the transformation of graphene structure after the small molecules produced in the thermal expansion atmosphere are stripped off the graphite oxide. However, when the graphite oxide is reduced, the half-peak width of the D band decreases. This is because after the graphite oxide is reduced, the oxygen-containing groups on its surface are reduced, and the defects on the graphene surface are also relatively reduced, which is then reflected in the trend of the D band half-peak width to restore the graphite layer structure. However, from the I (D) / I (G) Compared with the values, the PANI-GNS modified by PANI has increased compared with T-GNS, indicating that its disorder degree has increased and the exfoliation is more thorough.
[0084] Table 3 Raman spectroscopy analysis data
[0085] Sample type I(D) / I(G) <![CDATA[G peak offset (cm -1 )]]> WF,D(cm-1) graphite 0.52 0 35 GO4 1.69 14 164 T-GNS 1.98 24 102 PANI-GNS 2.14 16 80
[0086] The SEM images of graphite, graphite oxide (GO), T-GNS and PANI-GNS are shown in Figure 2. Figure 16-19 shown.
[0087] It was found that the interlayer spacing of the unoxidized flake graphite was very small, while the GO prepared after deep oxidation showed a wrinkled silk structure. After high-temperature thermal expansion, the GO underwent obvious interlayer exfoliation, and the graphite layers were stretched open, expanding from the original tight layered structure to an accordion structure with a clear interlayer structure, which fully demonstrated the almost separated layered structure of the expandable graphite. The exfoliation degree of the expandable graphite doped with polyaniline was better, and most of the graphite sheets had been separated and the layer structure was very complete. This fully demonstrated that polyaniline played a good auxiliary role in the exfoliation process. Figure 20-21 TEM images of T-GNS and PANI-GNS. From the TEM image of T-GNS, we can see the gauze-like texture, which shows that the thin layer of graphene curls spontaneously, resulting in wrinkles on the intrinsic undulating surface. More nanopores and nanoholes are formed through these wrinkle structures, thereby increasing the specific surface area of graphene. In addition, some channels caused by thermal expansion can be observed on the graphene sheets. The sheet structure of PANI-GNS is relatively more complete, there are no damaged channels on the graphene sheets, and the surface is more wrinkled, showing a larger specific surface area.
[0088] The specific surface areas of PANI-GNS, T-GNS and commercial XC-72 were tested by nitrogen adsorption-desorption method. Fig. 22 As shown. By observing the adsorption-desorption hysteresis loop of the high-pressure part, it can be seen that all nitrogen adsorption-desorption curves obey the IV type curve classified by IUPAC. The BET areas between different materials are calculated as shown in Table 4. It can be seen that the BET values of PANI-GNS and T-GNS are more than twice that of commercial VulcanXC-72, and both reach 400m 2 / g, PANI-GNS is 66m higher than T-GNS 2 / g, with the largest specific surface area. In VulcanXC-72, PANI-GNS and T-GNS, the main mesoporous (2-50nm) structure appears. PANI-GNS has a larger specific surface area and a larger pore distribution, providing more adsorption sites during the oxygen reduction process.
[0089] Table 4 Specific surface area and pore size
[0090]
[0091] The T-GNS and PANI-GNS catalytic composites were used to prepare air electrodes and then assembled into aluminum-air batteries for constant current discharge tests. Fig.23 ), the discharge voltage platform of PANI-GNS electrode is 1.27V, which is more than 120mV higher than that of T-GNS electrode, and has an absolute advantage; when the current is 20mA( Fig.24 ), the discharge voltage of the PANI-GNS electrode is 0.85V, while the discharge voltage of the T-GNS electrode is reduced to about 0.46V; when the discharge current is 30mA ( Fig.25 ), the discharge voltage of PANI-GNS is stable at 0.84V, which is about 40mV higher than that of T-GNS electrode; when the discharge current is 40mA( Fig.26 ), the PANI-GNS electrode can still reach 0.81V, which is still about 40mV higher than the T-GNS electrode. And when the T-GNS electrode is discharged at a current of 10mA and 40mA, the discharge platform has a small fluctuation, and the battery stability is relatively not as good as that of the PANI-GNS electrode. In summary, it can be seen that the air electrode prepared by the PANI-GNS catalytic complex has better discharge performance.
[0092] Embodiment 3:
[0093] Preparation of Pt-Co / graphene (rGO) catalytic composite
[0094] Weigh 60 mg of PANI-graphene, add 60 mL of ethylene glycol and isopropanol, and disperse by ultrasound for 60 minutes to form a uniform graphene ethylene glycol suspension; drop 0.0386 mol / L H2PtCl6 and 0.1 mol / L Co(CH3COO)2 solution, and stir magnetically for 60 minutes; add 0.2 mol / L NaOH solution to adjust the pH value to 10, and stir for 10 minutes; put it in a microwave reactor (power 800 W), react at high temperature for 2 minutes, and then cool to room temperature; wash and filter with ethanol several times, dry at 60°C, and grind to powder; put the above-obtained sample into a tubular furnace, calcine at 300°C for 30 minutes under (5%) hydrogen / nitrogen atmosphere, collect the sample and put it into a dryer.
[0095] Due to the large viscosity coefficient of ethylene glycol, the ultrasonic time required to evenly disperse graphene in it increases, but at the same time, the energy between graphene sheets increases due to the prolonged ultrasonic time, thereby promoting the agglomeration of graphene. Based on this, an appropriate amount of isopropanol, a dispersant with a small viscosity coefficient and a low boiling point, is added to ethylene glycol. The effect of adding different amounts of dispersants on the graphene-based catalytic complex was investigated. 5mL, 10mL, and 15mL of isopropanol were added to 60mL of ethylene glycol as dispersants.
[0096] The XRD pattern of the prepared catalytic composite is shown in Fig. 27As shown. The mantou peak appearing at about 24.8° is the (002) diffraction peak of the carrier graphene. When the amount of the dispersant is 5mL and 10mL, the other four peaks except the graphene peak are attributed to the characteristic diffraction peaks of the face-centered cubic (fcc) of Pt (JCPDS-ICDD, Card No: 04-802), and the 2θ values are 39.9°, 48.0°, 67.4° and 81.2°, respectively corresponding to the (111), (200), (220) and (311) crystal plane diffraction peaks of Pt. It proves that all alloy catalytic complexes exist mainly in a single-phase disordered structure. Compared with the diffraction peaks of Pt in the PTF card (data from the Powder Diffraction Association (JCPDS-ICDD)), the diffraction peaks of the Pt-Co alloy shift to large angles, which is due to the incorporation of Co into the face-centered cubic Pt structure. No peaks of pure Co or Co oxide appear in the figure. When the amount of dispersant added reached 15 mL, no obvious characteristic peak of Pt appeared on XRD, indicating that the catalyst was not loaded or was not reduced.
[0097] Figure 28-29 The cyclic voltammetry and linear scanning curves of the catalytic composites prepared with different amounts of dispersants are shown in Figure 2. As can be seen from the figure, the catalytic composites prepared under the same reaction conditions with different amounts of dispersants have a 0.5 mol·L -1 The CV curve in the H2SO4 solution has a larger CV area when the amount of isopropanol is 10 mL. The relevant data calculated from the figure are shown in Table 5.
[0098] Table 5 Relevant data of each electrode
[0099] Dispersant(mL) <![CDATA[Loading amount of Pt, g·m -2 > <![CDATA[SECSA m 2 ·g -1 ]]> Half-wave potential V 5 0.225 80.6 0.55 10 0.226 85.0 0.58 15 0 - 0.11
[0100] When the amount of dispersant added was 10 mL, the catalytic composite had a higher activity. ECSA The value is 4.4m larger than that when the amount of dispersant added is 5mL 2 ·g -1 , indicating that the number of Pt particles at the electrode / solution interface of the catalytic composite prepared with 10mL of dispersant added is greater than that of the catalytic composite prepared with 5mL. The half-wave potential of the catalytic composite is 0.58V, which is about 30mV positively shifted compared to the catalytic composite (0.55V) at 5mL, which means a smaller electrochemical polarization. And compared with the catalytic composite prepared without the addition of dispersant, the catalytic composite prepared under the same other conditions has a larger electrochemically active specific surface area and half-wave potential. When the amount of dispersant is increased to 15mL, the performance decreases significantly, and the half-wave potential is only 0.11V. This may be because the metal is not loaded or reduced.
[0101] Four groups of different microwave time and stop control were designed. The specific parameters are shown in Table 6. The time in brackets is the microwave pause time.
[0102] Table 6 Microwave time parameters
[0103] Group Microwave time (min) a 2-(1)-1 b 1-(1)-1-(1)-1 c 2-(1)-0.5-(0.5)-0.5 d 1-(1)-1-(1)-0.5-(0.5)-0.5
[0104] XRD pattern Fig.30 Obvious Pt (111) diffraction peaks can be observed in the figure. The broadening of the peak is mainly due to the small particle size and the fact that Co is incorporated into the face-centered cubic Pt structure, causing the peak to shift toward the large angle direction. The CV curves of the Pt-Co / rGO catalytic composites prepared under different microwave times are shown in Figure 2. Fig.31 As shown, the LSV curve is as follows Fig.32 The data of electrochemical active specific surface area are shown in Table 7.
[0105] Table 7 Relevant data of each electrode
[0106] Group <![CDATA[The loading amount of Pt, g·m -2 > <![CDATA[SECSA m 2 ·g -1 ]]> Half-wave potential V a 0.225 115 0.59 b 0.230 109 0.51 c 0.226 81 0.55 d 0.224 105 0.55
[0107] When the microwave time program is selected as a, the electrochemically active specific surface area of Pt-Co / rGO is larger than that of other microwave times, indicating that the Pt-Co / rGO catalytic complex prepared under the microwave time program design of 2min microwave stop 1min, and then microwave 1min has a larger electrochemically active specific surface area and half-wave potential, and a high electrochemically active area is often more conducive to electrocatalytic oxidation, smaller electrochemical polarization, and the catalytic complex prepared under this microwave program has a smaller particle size and more uniform distribution. It can provide more electrocatalytic active sites, making it easier for oxygen to diffuse to the electrochemical reaction surface, reducing the impedance caused by electrochemical polarization, and showing better electrochemical activity. Therefore, on this basis, the subsequent method of conditional microwave 2min stop 1min, and then microwave 1min was selected.
[0108] Table 8 shows the catalytic composites with different metal ratios.
[0109] Table 8 Proportions of different metals
[0110]
[0111]
[0112] A commercial 40w% platinum-carbon (HPT040) catalyst (e) was used as a comparison. Fig.33 shown.
[0113] As can be seen from the figure, the four peaks with 2θ values of 39.8°, 46.5°, 67.8° and 81.2° belong to the characteristic diffraction peaks of face-centered cubic (fcc) of Pt (JCPDS-ICDD, Card No: 04-802). They correspond to the diffraction peaks of (111), (200), (220) and (311) crystal planes of Pt, respectively. It proves that all alloy catalytic complexes exist mainly in a single-phase disordered structure. Compared with the diffraction peaks of bulk Pt of the same crystal form (data from the Powder Diffraction Association (JCPDS-ICDD)), the diffraction peaks of the Pt-Co alloy shift to large angles. The shift of the Pt (111) diffraction peak reveals that the structure of the alloy is that Co is incorporated into the face-centered cubic Pt structure. Since XRD is sensitive to mass, even a very small amount of large particles in the sample will narrow the peak shape. Fig.34 The XRD diagram of each catalytic composite for the (111) crystal plane is enlarged. The broadening of several characteristic peaks of Pt in the diagram indicates that the prepared Pt-Co alloy catalytic composites exist in a relatively small particle size and a disordered form. No peaks of pure Co or Co oxide appear in the diagram.
[0114] Figure 35-38 The transmission electron microscope photos of each catalytic complex. The photos in the upper right corner of each transmission electron microscope photo are their high-power lattice diffraction patterns. As can be seen from the figure, when the Pt-Co mass ratio is 3:1 and 2:1, the particle size distribution of the prepared catalytic complex is wide and uneven, and the proportion of large-size catalytic complex particles is high, and the lattice spacing is relatively large, indicating that the alloy effect between Pt and Co is not strong, and the agglomeration is relatively strong, which is consistent with the data obtained by XRD. When the Pt-Co mass ratio is 1:1 and 1:2, the catalytic complex particles are evenly dispersed on the surface of graphene, and the particle size distribution is uniform and small. The lattice spacing is relatively small. This is because the introduction of Co atoms shortens the distance of the Pt-Pt bond, thereby shortening the lattice spacing. It shows that the alloy effect of Pt and Co in these two catalytic complexes is relatively complete and the distribution is relatively uniform. It can also be seen from the figure that when the Pt-Co mass ratio is 3:1 and 2:1, the particle size distribution of the catalytic composite particles is uneven, the agglomeration is relatively strong, and the graphene sheet is also thicker. This shows that the metal mass ratio has a certain relationship with the morphology of the carrier graphene.
[0115] Electrodes a, b, c, d, and e prepared from the catalytic composite were tested for electrochemical performance using HPT040 as a control. The CV curves and LSV curves are shown in Figure 2. Figure 39-40 The relevant data are shown in Table 9:
[0116] Table 9 Relevant data of each electrode
[0117] Catalytic complex <![CDATA[Loading amount of Pt, g·m -2 > <![CDATA[SECSA m 2 ·g -1 ]]> Half-wave potential V <![CDATA[Pt3-Co1 / rGO(a)]]> 0.342 81.5 0.51 <![CDATA[Pt1-Co1 / rGO(b)]]> 0.260 69.1 0.47 <![CDATA[Pt1-Co2 / rGO(c)]]> 0.153 179.4 0.58 <![CDATA[Pt2-Co1 / rGO(d)]]> 0.318 95.0 0.56 HPT040(e) 0.450 92.8 0.49
[0118] Figures 41-44 The electrodes prepared by each catalytic complex were discharged at constant current at 10mA, 20mA, 30mA, and 40mA to obtain discharge curves. When the current was 10mA, the c battery and the d battery had a higher discharge platform of about 1.25V, and the b discharge platform was somewhat unstable, mainly because the static time was too short and the passivation film on the aluminum surface had not yet formed, resulting in unstable current during discharge, which was also related to its smaller electrochemical active specific surface area and half-wave potential. The a battery had the smallest discharge platform, which was attributed to its relatively small electrochemical active specific surface area. When the current was 20mA, the b battery's discharge platform showed a significant decrease, which was attributed to its smaller electrochemical active specific surface area and half-wave potential. The d battery's discharge platform remained at about 1.2V. The c battery's discharge platform showed a slight tilt, and the a battery's discharge platform basically remained at about 1V. When the discharge current was 30mA and 40mA, the discharge platforms of each battery tended to be stable, which was related to the discharge time of the battery. The discharge voltage of each battery is between 0.43V-0.58V, and c>d>b>a (where a, b, c, and d represent aluminum-air batteries obtained by preparing air electrodes with Pt3-Co1 / rGO, Pt1-Co1 / rGO, Pt1-Co2 / rGO, and Pt2-Co1 / rGO as catalytic composites, respectively).
[0119] Comprehensively analyzing the discharge conditions of each battery, it can be seen that when the mass ratio of Pt to Co is 1:2, the obtained air battery has a higher discharge platform under the same discharge conditions. This is mainly because when the mass ratio of Pt to Co is 1:2, its particles are more uniform and fine, with a larger electrochemical active specific surface area and smaller electrochemical polarization, and excellent catalytic performance. This is consistent with the analysis conclusions obtained above.
[0120] Embodiment 4:
[0121] Preparation of Supports by Multi-walled Carbon Nanotubes (MWCNT) and Graphite Oxide
[0122] The MWCNTs were pretreated by acidification in concentrated nitric acid at 120°C for 12 hours and then dried. The acidified MWCNTs were then ultrasonicated in H2O2 for 30 minutes, washed and filtered, and vacuum dried for 4 hours before being taken out and mixed with the graphite oxide of Example 1 and then ultrasonicated for 20 minutes. Under the condition that the mass ratio of Pt-Co metal was 1:1, the ratio of MWCNT to graphene was changed to prepare catalytic composites of different proportions, and the loading method was the same as that of Example 3.
[0123] (a), (b), (c), (d), and (e) represent carriers with a mass ratio of graphene to MWCNT of 10:1, 4:1, 2:1, 1:1, and 0:1, respectively. The XRD patterns are shown in Fig.45As shown. The catalyst prepared by using only MWCNT as the catalyst carrier has relatively sharp characteristic peaks of Pt face-centered cube and obvious characteristic peaks of Co single substance. This shows that when using only MWCNT as the carrier, the particle size of the catalytic composite particles is very large and the alloy is incomplete. As the specific gravity of graphene increases, the (111) diffraction peak of Pt becomes broadened and shifts to a larger angle, and the diffraction peaks of the other crystal planes become less obvious, and no Co or Co oxide appears. This shows that the particle size of the catalyst particles becomes smaller and the alloy is more complete. TEM pictures are shown in Figure 46-51 As shown, (f) is the carrier with only graphene. From the transmission electron micrograph, it can be seen that when multi-walled carbon nanotubes are used as carriers alone, the nanotubes are strongly agglomerated and the metal particles are larger. After being composited with graphene, the nanotubes are more evenly dispersed and can connect different graphene fragments. The catalytic composite was used to prepare a working electrode and its electrochemical performance was tested. Fig.52 The CV curves of different carrier ratios are shown in Figure 1, and HPT040 is (g). Fig.53 The relevant data are shown in Table 10:
[0124] Table 10 Relevant data of each electrode
[0125] Catalytic complex <![CDATA[Loading amount of Pt, g·m -2 > <![CDATA[SECSA m 2 ·g -1 ]]> Half-wave potential V (a) 0.225 102.5 0.56 (b) 0.220 99.1 0.55 (c) 0.224 105.4 0.54 (d) 0.221 98.0 0.55 (e) 0.221 95.0 0.54 (f) 0.223 69.1 0.47 (g) 0.223 92.8 0.49
[0126] It can be seen from the data in the figure and table that when the mass ratio of graphene to MWCNT is 2:1, the prepared catalytic composite has the largest electrochemically active specific surface area and a higher half-wave potential. This means that the catalytic composite has the highest activity. When the mass ratio of graphene to MWCNT increases, its half-wave potential increases, but the electrochemically active specific surface area decreases. When the mass ratio of graphene to MWCNT decreases, both the half-wave potential and the electrochemically active specific surface area decrease, and the activity of the catalyst decreases. This is because when there are too few MWCNTs doped in the carrier, the carrier layer is thicker and the peeling is incomplete. When the amount of MWCNT increases, the MWCNT inserted between the graphene layers increases, and the longer MWCNT can connect multiple sheets of graphene to increase its electron transfer ability, but a larger proportion of MWCNT is added to it, which will reduce the specific surface area of the carrier as a whole, and the agglomeration between MWCNTs is more severe. The corresponding electrochemically active specific surface area also decreases.
[0127] The constant current discharge curves between the catalysts at currents of 10mA, 20mA, 30mA, and 40mA are as follows: Figure 54-57As shown in the figure, when the mass ratio of graphene to MWCNT is 2:1, the obtained air battery has a higher discharge platform under the same discharge conditions, and can reach 1.38V, 0.65V, 0.62V, and 0.58V under 10mA, 20mA, 30mA, and 40mA discharge conditions, respectively. This is attributed to its better catalytic performance. This is consistent with the analysis conclusions obtained above.
[0128] The composite with a mass ratio of graphene to MWCNT of 2:1 was selected, and the metal specific gravity was adjusted to prepare different catalytic composites. (a), (b), (c), and (d) are Pt:Co ratios of 3:1, 2:1, 1:1, and 1:3, respectively. The transmission electron microscopy morphologies of the catalytic composites are shown in Figure 2. Figure 58-61 As shown. It can be seen from the figure that when Pt:Co=3:1 and 1:1, the catalytic composites prepared have larger metal particles of different sizes and uneven distribution. The carrier graphene layer is also relatively thick, and the carbon nanotubes are completely wrapped in the graphene, and the agglomeration is relatively severe. When Pt:Co=2:1 and 1:3, the catalyst metal particles prepared are evenly distributed and small, the graphene layer is thin, the distribution of graphene and carbon nanotubes is relatively uniform, and the carbon nanotubes are evenly spread on the surface of the graphene. However, the particle size of Pt:Co=2:1 is smaller than that of Pt:Co=1:3, which is consistent with the results of XRD. It can be seen that the metal ratio has a great influence on the morphology of the catalyst. The CV curve is shown in the figure. Fig.62 As shown, HPT040 is (e), and the LSV curve is as follows Fig.63 The data is shown in Table 11:
[0129] Table 11 Relevant data of each electrode
[0130] Catalytic complex <![CDATA[Loading amount of Pt, g·m -2 > <![CDATA[SECSA m 2 ·g -1 ]]> Half-wave potential V (a) 0.225 87.9 0.57 (b) 0.220 111.3 0.58 (c) 0.224 103.5 0.54 (d) 0.221 64.3 0.55 (e) 0.223 92.8 0.49
[0131] As can be seen from the figure, under the premise that the mass ratio of the carrier graphene to MWCNT is 2:1, when the prepared Pt-Co mass ratio is 2:1, the catalyst has the maximum electrochemically active specific surface area and half-wave potential, which means that when the Pt-Co mass ratio is 2:1, the catalyst active specific surface area is the highest and the electrochemical polarization is the smallest. However, when the mass ratio of Pt-Co increases to 3:1, the activity of the catalyst decreases instead. This is because when the amount of base metal Co doped in the catalyst is too small, the area of Pt that can be exposed to the outside is reduced, the corresponding electrochemically active specific surface area is also reduced, and the electron transfer rate is also reduced accordingly, resulting in a decrease in catalytic activity. However, when the mass ratio of Pt-Co increases to 1:3, the electrochemically active specific surface area and half-wave potential of the catalyst are also reduced accordingly. This is because when too much base metal is doped, the proportion of Pt that can play a catalytic role is too low, which reduces the oxygen reduction activity of the catalyst. This is roughly consistent with the situation when graphene is used alone as a catalyst carrier. At currents of 10mA, 20mA, 30mA, and 40mA, the constant current discharge curves of different catalytic complexes are as follows: Figures 64-67 As shown in the figure, it can be seen from the curve that when the Pt-Co mass ratio is 2:1, the obtained air battery has a higher discharge platform under the same discharge conditions, which is attributed to its better catalytic performance. This is consistent with the previous analysis conclusion.
[0132] For those skilled in the art, various other corresponding changes and modifications can be made according to the technical solutions and concepts described above, and all of these changes and modifications should fall within the protection scope of the claims of the present invention.
Claims
1. An air battery catalytic composite, comprising a catalyst and a carrier; the catalyst is supported on the carrier; It is characterized in that The catalyst is a Pt-Co nanoparticle catalyst, the mass ratio of Pt to Co is 1-10:3; the carrier is a composite carrier of carbon material and graphene; the mass ratio of the carbon material to graphene is 1:1-10; the carbon material is carbon black XC-72 and / or multi-walled carbon nanotubes.
2. The air battery catalytic composite according to claim 1, It is characterized in that The mass ratio of Pt to Co is 2:
1.
3. The air battery catalytic composite according to claim 1, It is characterized in that The mass ratio of the carbon material to the graphene is 1:
2.
4. The air battery catalytic composite according to claim 1, It is characterized in that The graphene is polyaniline-modified graphene.
5. A method for preparing an air battery catalytic composite, Features include: Graphite oxidation step: pre-oxidize the graphite, place it in an ice bath for 0.2-5 hours, and then oxidize it at a temperature of 15-95° C. to obtain oxidized graphite; The preparation steps of the carrier are as follows: mixing graphite oxide and carbon material, performing ultrasonic treatment, washing and drying to obtain the carrier; the carrier is a composite carrier of carbon material and graphene; the mass ratio of the carbon material to graphene is 1:1-10; the carbon material is carbon black XC-72 and / or multi-walled carbon nanotubes; Preparation steps of the catalytic complex: Add H 2 PtCl 6 and Co(CH 3 COO 2 The solution is subjected to microwave treatment to obtain a catalytic composite; the mass ratio of Pt to Co in the catalytic composite is 1-10:
3.
6. The method for preparing the air battery catalytic composite according to claim 5, It is characterized in that In the oxidation step of graphite, an ice bath is performed for 0.2-5 hours, a strong oxidant is slowly added under the condition of not exceeding 20°C, and then oxidation is carried out in sequence at a medium temperature of 30-50°C and a high temperature of 80-95°C to obtain oxidized graphite.
7. The method for preparing the air battery catalytic composite according to claim 5, It is characterized in that In the graphite oxidation step, the graphite oxide is modified with polyaniline and then expanded.
8. The method for preparing the air battery catalytic composite according to claim 5, It is characterized in that In the step of preparing the catalytic complex, the microwave treatment is performed intermittently, each microwave treatment lasts for 0.3-3 minutes, and each microwave treatment is paused for 0.3-1.5 minutes.
9. The method for preparing the air battery catalytic composite according to claim 5, It is characterized in that In the step of preparing the catalytic composite, the mass ratio of ethylene glycol to isopropanol is 3-12:
1.
10. An air battery, It is characterized in that The air battery is an aluminum-air battery, comprising a catalytic layer; the catalytic layer carries an air battery catalytic complex; the air battery uses a NaCl solution as an electrolyte; the air battery catalytic complex comprises a catalyst and a carrier; the catalyst is carried on the carrier; the catalyst is a Pt-Co nanoparticle catalyst, and the mass ratio of Pt to Co is 1-10:3; the carrier is a composite carrier of carbon material and graphene; the mass ratio of the carbon material to graphene is 1:1-10; the carbon material is carbon black XC-72 and / or multi-walled carbon nanotubes.