Preparation method of electrolyte and low-temperature aluminum shell battery

By adjusting the ratio of organic solvents and additives in the lithium battery electrolyte, the dissociation amount of lithium salt is improved, and the problems of increasing the viscosity of the electrolyte and slowing down the ion conduction speed of lithium batteries under low temperature conditions are solved, and efficient battery performance is achieved The performance, especially at -40°C, the discharge efficiency of 0.2C reaches more than 80%.

CN119092817APending Publication Date: 2024-12-06ANHUI LEOCH PENEWABLE ENERGY DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410394834.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-04-02
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The viscosity of the electrolyte becomes larger under low temperature conditions, and the ion conduction speed slows down, resulting in a decrease in the battery polarization and charge and discharge capacity.

Method used

By adjusting the composition and ratio of organic solvents and additives in the electrolyte, the dissociation amount of lithium salts is increased, the conductivity and ion conduction speed are increased, and the viscosity of the electrolyte is reduced.

Benefits of technology

Under -40°C, the battery's 0.2C discharge efficiency reaches more than 80%, the electrolyte's conductivity is improved, the viscosity is reduced, and the battery performance is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004773681570000091
    Figure BDA0004773681570000091
  • Figure BDA0004773681570000101
    Figure BDA0004773681570000101
  • Figure BDA0004773681570000111
    Figure BDA0004773681570000111
Patent Text Reader

Abstract

The invention discloses an electrolyte, a preparation method of the electrolyte and a low-temperature aluminum shell battery, the electrolyte comprises an organic solvent, a lithium salt and an additive, and the mass ratio of the organic solvent to the lithium salt to the additive is (70-85): (10-20): (5-10). According to the electrolyte prepared by the invention, the viscosity of the electrolyte is reduced at normal temperature, the conductivity is improved, and the 0.2 C discharge efficiency at-40 DEG C is greater than 80%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of electrolytes, and in particular to an electrolyte, a method for preparing the electrolyte, and a low-temperature aluminum shell battery having the electrolyte. Background Art

[0002] At present, lithium-ion batteries have the advantages of high specific energy, high voltage, many cycles and long storage time. They are not only widely used in portable electronic devices such as mobile phones, digital cameras and laptops, but also widely used in large and medium-sized electric equipment such as electric vehicles, energy storage, electric bicycles and power tools.

[0003] However, lithium batteries often have no power in winter and consume power quickly. This is because under low temperature conditions, the viscosity of the electrolyte in the battery will increase, and the ion conduction speed will slow down, causing a mismatch in the electron migration speed in the external circuit. As a result, the battery becomes severely polarized and the charge and discharge capacity drops sharply. Summary of the invention

[0004] In order to solve the above technical problems, the present application provides an electrolyte, a method for preparing the electrolyte and a low-temperature aluminum shell battery. The specific technical solutions are as follows.

[0005] On the one hand, the present application provides a method for preparing an electrolyte, comprising an organic solvent, a lithium salt and an additive, wherein the mass ratio of the organic solvent, the lithium salt and the additive is (70-85): (10-20): (5-10).

[0006] As a further technical solution of the present invention, the organic solvent includes ethylene carbonate, propylene carbonate and ethyl methyl carbonate, and the mass ratio of ethylene carbonate, propylene carbonate and ethyl methyl carbonate is (30-40): (5-15): (45-65).

[0007] As a further technical solution of the present invention, the additive includes vinylene carbonate, vinyl ethylene carbonate and propylene sulfite, and the mass ratio of vinylene carbonate, vinyl ethylene carbonate and propylene sulfite is (10-30): (10-20): (50-80).

[0008] As a further technical solution of the present invention, when the mass ratio of the organic solvent, the lithium salt and the additive is 80:15:5, the mass ratio of ethylene carbonate, propylene carbonate and ethyl methyl carbonate in the organic solvent is (32-38):(7-13):55, and the mass ratio of vinylene carbonate, ethylene carbonate and propylene sulfite in the additive is (18-22):(13-17):65.

[0009] As a further technical solution of the present invention, the lithium salt is one or more of lithium hexafluorophosphate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium tetrafluoroborate, and lithium difluorobisoxalatophosphate.

[0010] In a second aspect, the present application also provides a method for preparing an electrolyte, comprising the following steps:

[0011] S1, weigh the organic solvent and place it in an inert gas environment;

[0012] S2, weighing a lithium salt, and adding it into an organic solvent under an inert gas environment for mixing, to obtain a mixture of the organic solvent and the lithium salt;

[0013] S3, weighing the additive, adding it to the mixture of the organic solvent and the lithium salt, and mixing them evenly under an inert gas environment to obtain an electrolyte.

[0014] In a third aspect, the present application also provides a low-temperature aluminum shell battery, comprising the electrolyte described in any one of claims 1-5.

[0015] The beneficial effects of the present invention are as follows:

[0016] The electrolyte prepared in the present application has reduced viscosity and improved conductivity at room temperature, and the 0.2C discharge efficiency is greater than 80% at -40°C. DETAILED DESCRIPTION

[0017] The following examples further illustrate the present application in detail.

[0018] The present application provides an electrolyte, comprising an organic solvent, a lithium salt and an additive, wherein the mass ratio of the organic solvent, the lithium salt and the additive is (70-85):(10-20):(5-10); the organic solvent comprises ethylene carbonate, propylene carbonate and ethyl methyl carbonate, and the mass ratio of ethylene carbonate, propylene carbonate and ethyl methyl carbonate is (30-40):(5-15):(45-65); the additive comprises vinylene carbonate, vinyl ethylene carbonate and propylene sulfite, and the mass ratio of vinylene carbonate, vinyl ethylene carbonate and propylene sulfite is is (10-30): (10-20): (50-80); when the mass ratio of the organic solvent, the lithium salt and the additive is 80:15:5, the mass ratio of ethylene carbonate, propylene carbonate and ethyl methyl carbonate in the organic solvent is (32-38): (7-13): 55, and the mass ratio of vinylene carbonate, ethylene carbonate and propylene sulfite in the additive is (18-22): (13-17): 65; the lithium salt is one or more of lithium hexafluorophosphate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium tetrafluoroborate and lithium difluorobisoxalatophosphate.

[0019] Prior to this application, the viscosity of the electrolyte of the lithium battery would increase under low temperature conditions, and the ion conduction speed would slow down, resulting in a mismatch in the electron migration speed of the external circuit. As a result, the battery would become severely polarized and the charge and discharge capacity would drop sharply.

[0020] In response to the above technical problems, the present application increases the amount of lithium salt dissociation in the electrolyte by changing the composition and ratio of the organic solvent and additive in the electrolyte. The more lithium salt dissociates, the more migrations there are, and the higher the conductivity. The higher the conductivity, the faster the ion conduction rate, the smaller the polarization, and the better the performance of the battery at low temperatures. It can effectively reduce the viscosity of the electrolyte and increase the ion conduction speed.

[0021] Unless otherwise specified, the important components involved in this application are purchased from commercially available products, including:

[0022] Ethylene carbonate, propylene carbonate, ethyl methyl carbonate, vinylene carbonate, vinyl ethylene carbonate and propylene sulfite were all purchased from Wuhan Jixinyibang Biotechnology Co., Ltd.

[0023] Preparation Example 1 to Preparation Example 7 are preparation examples of organic solvents, and the details are as follows.

[0024] Preparation Example 1

[0025] The components of the organic solvent are weighed according to the mass ratio of ethylene carbonate, propylene carbonate and ethyl methyl carbonate of 30:5:65, and the components in the organic solvent are mixed under an inert gas environment to obtain a mixed organic solvent.

[0026] Preparation Example 2

[0027] The components of the organic solvent were weighed according to the mass ratio of ethylene carbonate, propylene carbonate and ethyl methyl carbonate of 35:10:55, and the components in the organic solvent were mixed under an inert gas environment to obtain a mixed organic solvent.

[0028] Preparation Example 3

[0029] The components of the organic solvent are weighed according to the mass ratio of ethylene carbonate, propylene carbonate and ethyl methyl carbonate of 40:15:45, and the components in the organic solvent are mixed under an inert gas environment to obtain a mixed organic solvent.

[0030] Preparation Example 4

[0031] The components of the organic solvent are weighed according to the mass ratio of ethylene carbonate, propylene carbonate and ethyl methyl carbonate of 30:15:55, and the components in the organic solvent are mixed under an inert gas environment to obtain a mixed organic solvent.

[0032] Preparation Example 5

[0033] The components of the organic solvent were weighed according to the mass ratio of ethylene carbonate, propylene carbonate and ethyl methyl carbonate of 32:13:55, and the components in the organic solvent were mixed under an inert gas environment to obtain a mixed organic solvent.

[0034] Preparation Example 6

[0035] The components of the organic solvent were weighed according to the mass ratio of ethylene carbonate, propylene carbonate and ethyl methyl carbonate of 38:7:55, and the components in the organic solvent were mixed under an inert gas environment to obtain a mixed organic solvent.

[0036] Preparation Example 7

[0037] The components of the organic solvent are weighed according to the mass ratio of ethylene carbonate, propylene carbonate and ethyl methyl carbonate of 40:5:55, and the components in the organic solvent are mixed under an inert gas environment to obtain a mixed organic solvent.

[0038] Table 1 shows the component data of the organic solvent in Preparation Examples 1 to 7, see Table 1 for details.

[0039] Table 1

[0040] Ethylene carbonate Propylene carbonate Ethyl methyl carbonate Preparation Example 1 30 5 65 Preparation Example 2 35 10 55 Preparation Example 3 40 15 45 Preparation Example 4 30 15 55 Preparation Example 5 32 13 55 Preparation Example 6 38 7 55 Preparation Example 7 40 5 55

[0041] Preparation Examples 8-14 are preparation examples of additives, and the details are as follows.

[0042] Preparation Example 8

[0043] The components of the additive are weighed according to the mass ratio of vinylene carbonate, ethylene carbonate and propylene sulfite of 10:10:80, and the components of the additive are mixed under an inert gas environment to obtain a mixed additive.

[0044] Preparation Example 9

[0045] The components of the additive are weighed according to the mass ratio of vinylene carbonate, ethylene carbonate and propylene sulfite of 20:15:65, and the components of the additive are mixed under an inert gas environment to obtain a mixed additive.

[0046] Preparation Example 10

[0047] The components of the additive are weighed according to a mass ratio of vinylene carbonate, ethylene carbonate and propylene sulfite of 30:20:50, and the components of the additive are mixed under an inert gas environment to obtain a mixed additive.

[0048] Preparation Example 11

[0049] The components of the additive are weighed according to the mass ratio of vinylene carbonate, ethylene carbonate and propylene sulfite of 25:10:65, and the components of the additive are mixed under an inert gas environment to obtain a mixed additive.

[0050] Preparation Example 12

[0051] The components of the additive are weighed according to a mass ratio of vinylene carbonate, ethylene carbonate and propylene sulfite of 22:13:65, and the components of the additive are mixed under an inert gas environment to obtain a mixed additive.

[0052] Preparation Example 13

[0053] The components of the additive are weighed according to the mass ratio of vinylene carbonate, ethylene carbonate and propylene sulfite of 18:17:65, and the components of the additive are mixed under an inert gas environment to obtain a mixed additive.

[0054] Preparation Example 14

[0055] The components of the additive are weighed according to the mass ratio of vinylene carbonate, ethylene carbonate and propylene sulfite of 15:20:65, and the components of the additive are mixed under an inert gas environment to obtain a mixed additive.

[0056] Table 2 shows the component data of the additives in Preparation Examples 8 to 14, see Table 2 for details.

[0057] Table 2

[0058] Vinylene carbonate Ethylene carbonate Propylene sulfite Preparation Example 8 10 10 80 Preparation Example 9 20 15 65 Preparation Example 10 30 20 50 Preparation Example 11 25 10 65 Preparation Example 12 22 13 65 Preparation Example 13 18 17 65 Preparation Example 14 15 20 65

[0059] Example 1

[0060] The preparation method of the electrolyte comprises the following specific steps:

[0061] S1, selecting the organic solvent in Preparation Example 1;

[0062] S2, weighing a lithium salt, and adding it into an organic solvent under an inert gas environment for mixing, to obtain a mixture of the organic solvent and the lithium salt;

[0063] S3, selecting the additive of Preparation Example 8, adding it to the organic solvent and the mixture of the organic solvent and the lithium salt, and mixing them evenly under an inert gas environment to obtain an electrolyte;

[0064] And the mass ratio of the organic solvent, the lithium salt and the additive in the electrolyte prepared above is 70:20:10.

[0065] Example 2

[0066] The preparation method of the electrolyte comprises the following specific steps:

[0067] S1, selecting the organic solvent in Preparation Example 2;

[0068] S2, weighing a lithium salt, and adding it into an organic solvent under an inert gas environment for mixing, to obtain a mixture of the organic solvent and the lithium salt;

[0069] S3, selecting the additive of Preparation Example 9, adding it to the organic solvent and the mixture of the organic solvent and the lithium salt, and mixing them evenly under an inert gas environment to obtain an electrolyte;

[0070] In addition, the mass ratio of the organic solvent, the lithium salt and the additive in the electrolyte prepared above is 80:15:5.

[0071] Example 3

[0072] The preparation method of the electrolyte comprises the following specific steps:

[0073] S1, selecting the organic solvent in Preparation Example 3;

[0074] S2, weighing a lithium salt, and adding it into an organic solvent under an inert gas environment for mixing, to obtain a mixture of the organic solvent and the lithium salt;

[0075] S3, selecting the additive of Preparation Example 10, adding it to the organic solvent and the mixture of the organic solvent and the lithium salt, and mixing them evenly under an inert gas environment to obtain an electrolyte;

[0076] In addition, the mass ratio of the organic solvent, the lithium salt and the additive in the prepared electrolyte is 85:10:5.

[0077] Comparative Example 1

[0078] The preparation method of the electrolyte comprises the following specific steps:

[0079] S1, selecting the organic solvent in Preparation Example 3;

[0080] S2, weighing a lithium salt, and adding it into an organic solvent under an inert gas environment for mixing, to obtain a mixture of the organic solvent and the lithium salt;

[0081] S3, selecting the additive of Preparation Example 10, adding it to the organic solvent and the mixture of the organic solvent and the lithium salt, and mixing them evenly under an inert gas environment to obtain an electrolyte;

[0082] In addition, the mass ratio of the organic solvent, the lithium salt and the additive in the electrolyte prepared above is 60:25:15.

[0083] In the present invention, in order to clearly understand the performance of the electrolyte provided by the present invention, the performance of the battery will be analyzed by conducting the following comparative examples and embodiments to compare and analyze the conductivity, viscosity and 0.2C discharge efficiency of the electrolyte of each embodiment at -40°C.

[0084] It should be noted that the battery used in the experiment has a positive electrode material of lithium cobalt oxide, a negative electrode material of modified artificial graphite MGMC, a 16um thick diaphragm, a 2mm wide tab, and is packaged in an aluminum-plastic packaging bag; it is assembled into a battery according to the manufacturing process of polymer batteries for performance testing.

[0085] The conductivity of the electrolytes of Examples 1-3 and Comparative Example 1 at 25° C. was tested respectively: Test equipment: AT-510 conductivity tester manufactured by KEM. Test method: The conductivity tester was calibrated to a standard state using a reference electrode, and the electrolytes of each example were taken out from a closed container. The displayed value was the conductivity of the electrolytes of each example. The test results are shown in Table 3.

[0086] The viscosity of the electrolytes of Examples 1-3 and Comparative Example 1 at 25°C was tested respectively: Testing equipment: DV-III ULTRAPROGRAMMABLERHEOMETER viscosity tester produced by Brookfield Engineering Laboratory INC. Testing method: A small amount of the electrolytes of each example was added to the tester, and the viscosity of the electrolytes of each example could be calculated by measuring the respective shear stresses.

[0087] Table 3

[0088]

[0089]

[0090] It can be seen from the test results of the above-mentioned Examples 1 to 3 and Comparative Example 1 that in the present application, at room temperature, the conductivity of the electrolyte prepared in Examples 1 to 3 is higher than the conductivity of the electrolyte prepared in Comparative Example 1, and the viscosity of the electrolyte is reduced, and the discharge efficiency at -40°C can reach more than 80%.

[0091] The present application found that the conductivity of the electrolyte in Example 2 is better than that in Example 1 and Example 3, and the viscosity of the electrolyte is significantly lower than that in Example 1 and Example 3. Therefore, the present application designs Examples 4 to 7 based on Example 2. In Examples 4 to 7, except for the changes in the ratio of each component in the organic solvent and the ratio of each component in the additive, that is, the changes in the preparation examples of the organic solvent selection and the additive selection, everything else remains unchanged, and the preparation method remains unchanged, as shown in Table 4 for details.

[0092] Table 4

[0093] Organic solvents additive Example 4 Preparation Example 4 Preparation Example 11 Example 5 Preparation Example 5 Preparation Example 12 Example 6 Preparation Example 6 Preparation Example 13 Example 7 Preparation Example 7 Preparation Example 14

[0094] The performance of the electrolytes prepared in Examples 4 to 7 was tested, and the test results are shown in Table 5.

[0095] Table 5

[0096]

[0097] It can be seen from the test results of Table 5 that the test results of Example 5 and Example 6 are better than those of Examples 1, 3, 4 and 7. Combined with Example 2, it can be seen that when the mass ratio of the organic solvent, the lithium salt and the additive is 80:15:5, the mass ratio of ethylene carbonate, propylene carbonate and ethyl methyl carbonate in the organic solvent is (32-38): (7-13): 55, and the mass ratio of vinylene carbonate, vinyl ethylene carbonate and propylene sulfite in the additive is (18-22): (13-17): 65, the performance of the electrolyte is better, and the battery can achieve a 0.2C discharge efficiency of more than 83% under a -40°C environment.

[0098] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. An electrolyte comprising an organic solvent, a lithium salt and an additive, characterized in that: The mass ratio of the organic solvent, the lithium salt and the additive is (70-85):(10-20):(5-10).

2. The electrolyte according to claim 1, characterized in that: The organic solvent includes ethylene carbonate, propylene carbonate and ethyl methyl carbonate, and the mass ratio of ethylene carbonate, propylene carbonate and ethyl methyl carbonate is (30-40): (5-15): (45-65).

3. The electrolyte according to claim 1, characterized in that: The additives include vinylene carbonate, vinyl ethylene carbonate and propylene sulfite, and the mass ratio of vinylene carbonate, vinyl ethylene carbonate and propylene sulfite is (10-30): (10-20): (50-80).

4. The electrolyte according to claim 1, characterized in that When the mass ratio of the organic solvent, the lithium salt and the additive is 80:15:5, the mass ratio of ethylene carbonate, propylene carbonate and ethyl methyl carbonate in the organic solvent is (32-38):(7-13):55, and the mass ratio of vinylene carbonate, vinyl ethylene carbonate and propylene sulfite in the additive is (18-22):(13-17):

65.

5. The electrolyte according to claim 4, characterized in that: The lithium salt is one or more of lithium hexafluorophosphate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium tetrafluoroborate, and lithium difluorobisoxalatophosphate.

6. The method for preparing an electrolyte according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1, weigh the organic solvent and place it in an inert gas environment; S2, weighing a lithium salt, and adding it into an organic solvent under an inert gas environment for mixing, to obtain a mixture of the organic solvent and the lithium salt; S3, weighing the additive, adding it to the mixture of the organic solvent and the lithium salt, and mixing them evenly under an inert gas environment to obtain an electrolyte.

7. Low temperature aluminum shell battery, characterized by: The electrolyte comprising the electrolyte according to any one of claims 1 to 5.