Preparation method and application of diaphragm with mesoporous silica particle coating

By coating mesoporous silica particles on the lithium-ion battery separator, the problem of insufficient thermal stability and wettability of the separator is solved, the safety and performance of the battery are improved, and the preparation process is simplified, which is suitable for large-scale production.

CN119092937APending Publication Date: 2024-12-06HEBEI UNIV OF TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411458319.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-18
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The lithium-ion battery separator has insufficient thermal stability at high temperatures and has low wettability of the electrolyte, which affects the safety and performance of the battery.

Method used

Mesoporous silica particles were coated on polypropylene separators by sol-gel method, and high-synthesis was synthesized in alkaline solution using ethyl orthosilicate and cetyl trimethylammonium bromide as silicon source and soft template. Mesoporous silica with specific surface area and covers the polypropylene membrane with it, enhancing the thermal stability and wettability of the membrane.

Benefits of technology

It significantly improves the thermal stability and wettability of the diaphragm, enhances ionic conductivity, reduces battery impedance, improves battery safety and performance, and is simple in preparation and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119092937A_ABST
    Figure CN119092937A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method and application of a diaphragm with a mesoporous silica particle coating. According to the method, a sol-gel method is adopted, tetraethoxysilane (TEOS) is taken as a silicon source, cetyltrimethylammonium bromide (CTAB) is taken as a soft template, ethyl acetate is taken as a pore-enlarging agent, and mesoporous silica with high specific surface area is synthesized in an alkaline solution. And then coating the surface of a polypropylene diaphragm (PP) with the coating solution. The mesoporous silica coated polypropylene diaphragm obtained by the invention has higher thermal stability, thereby having better safety; the mesoporous silica has a stronger adsorption effect on the organic electrolyte, so that the modified diaphragm has better wettability and ionic conductivity; and the preparation method is simple, high in yield of a single-time prepared product and capable of realizing mass production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The technical solution of the present invention relates to a modification of a lithium-ion battery separator, in particular to a preparation method of a mesoporous silica coating-modified lithium-ion battery separator. Background Art

[0002] Over the past two decades, the demand for energy storage units for portable electronic devices has promoted the development of lithium-ion batteries (LIBs) science and industry. Recently, many researchers have focused on developing energy storage devices with medium-to-high capacity for electronic automotive energy storage devices and generators. In the process of increasing the energy capacity of LIBs, several issues must be considered, such as safety, energy density, power efficiency, and fast charge / discharge rate. So far, improvements in each component (cathode, anode, electrolyte, and separator) of high-performance LIBs have been widely studied. Although LIBs offer high energy density storage, they have been seriously plagued by safety issues. The safety performance of LIBs is closely related to the thermal behavior of the separator and the stability of the electrolyte, and is also one of the most important factors in these application areas.

[0003] In most current LIBs systems, porous olefin membranes are used as commercial separators due to their excellent electrochemical stability, effective blocking of dendrite growth, and cost-effectiveness. However, the main problem of high-performance LIBs is that the separators not only have low porosity and low wettability in organic electrolytes, but also have weak thermal stability. In order to overcome the above shortcomings, researchers have made many efforts to modify polyolefin separators, including surface grafting modified separators, self-assembled ceramic separators, and inorganic composite separators. Among these modification methods, coating inorganic particles on self-assembled ceramic separators has been proven to be a low-cost and effective method. The introduction of inorganic particle coatings with high heat resistance and mechanical strength can improve the mechanical strength and thermal stability of the separator. At the same time, inorganic particles can promote the absorption of electrolytes, allowing uniform distribution of Li throughput. Inorganic particles such as SiO 2 、TiO 2 、Al 2 O 3 It has been widely studied. 2 It is the focus of attention due to its advantages of simple preparation, easy availability of raw materials, low price, etc. Mesoporous silica is used in the research of the present invention because it has more pores than silicon dioxide and has less restriction on ion passage.

[0004] Patent CN202211323147 discloses a lithium-ion battery separator with high electrolyte wettability and high adhesion PVDF hollow porous nanoparticle coating slurry. Patent CN202211475642 discloses a microcapsule and a lithium-ion battery separator containing the microcapsule, which reduces the reactivity of the negative electrode material by loading the microcapsule with a deactivator to reduce the risk of battery short circuit. Patent CN202310261238 discloses a high-temperature resistant ceramic composite lithium battery separator and a preparation method thereof, which uses binders of different properties to enhance the bonding between the silane coupling agent, ceramic particles and the base film, thereby improving the density and heat resistance. Patent CN202310292188 discloses the preparation of a lithium-ion battery composite separator with a high migration number. The prepared separator has the characteristics of high migration number and low interface impedance, thereby reducing the polarization of the lithium battery during discharge and improving the battery electrical performance. However, the high-adhesion coating has poor high temperature resistance, which makes the coating uneven and affects the overall separator performance. The microcapsules loaded with inactivators reduce the risk of short circuits while also reducing the activity of the negative electrode material, thereby affecting the performance of the negative electrode material and the overall battery performance. The high-temperature resistant ceramic composite lithium battery separator is expensive in the preparation process and is not suitable for mass production. Summary of the invention

[0005] The present invention aims at the shortcomings of the current lithium-ion battery separator, such as weak thermal stability and low wettability in electrolyte, and provides a preparation method and application of a separator with a mesoporous silica particle coating. The method adopts a sol-gel method, tetraethyl orthosilicate (TEOS) as a silicon source, hexadecyltrimethylammonium bromide (CTAB) as a soft template, and ethyl acetate as a pore expander to synthesize high specific surface area mesoporous silica in an alkaline solution. Then it is coated on the surface of a polypropylene separator (PP). The mesoporous silica-coated polypropylene separator obtained by the present invention has higher thermal stability and thus better safety; due to the stronger adsorption of mesoporous silica on organic electrolyte, the modified separator has better wettability and ionic conductivity; and the preparation method is simple, the single preparation product yield is high, and it can be mass-produced.

[0006] The technical solution of the present invention is: A method for preparing a diaphragm having a mesoporous silica particle coating, the method comprising the following steps: Step 1: Dissolve CTAB in deionized water, stir, and then add ethanol, ammonia water, and ethyl acetate to obtain a mixed solution; For every 40-50 ml of deionized water, add 2-3 g of CTAB, 70-80 ml of ethanol, 15-20 ml of ammonia (25-28 wt%), and 1-2 ml of ethyl acetate; Step 2: Add TEOS to the mixed solution, then rapidly stir for 1.5-3 h, age for 16-24 h, filter and wash, and dry at 70-80 °C for 12 h to obtain silicon dioxide; Among them, 1-8 ml of TEOS was added to every 40-50 ml of the mixed solution obtained by deionized water; The rapid stirring rate is 1000-3000 r / min; Step 3: heating the dried silica to 500-600°C in a tube furnace at a heating rate of 1-5°C / min, keeping the temperature for 5-8 hours, removing the soft template, and obtaining mesoporous silica; Step 4: Grind and mix mesoporous silica and polyvinylidene fluoride (PVDF) in a mass ratio of 8~10:0.5~2, add N-methylpyrrolidone (NMP), grind evenly and use a scraper to evenly coat on the polypropylene diaphragm; the coating thickness is 10-90 μm.

[0007] Step 5: Dry the coated diaphragm in a drying oven at 60-70 °C for 8-12 h to obtain a modified diaphragm.

[0008] The diaphragm with mesoporous silica particle coating obtained by the method is used as a lithium ion battery diaphragm.

[0009] The lithium-ion battery specifically comprises a graphite positive electrode and a lithium sheet negative electrode, and an electrolyte of 1 M LiPF 6 Ethylene carbonate (EC) and diethyl carbonate (DMC) to which 10 wt% of fluorinated ethylene carbonate (FEC) was added.

[0010] The beneficial effects of the present invention are: The specific manifestations are as follows: 1. The present invention creatively proposes to use mesoporous silica loaded on a polypropylene diaphragm to improve the thermal stability of the diaphragm. The shrinkage rate is only 42.5% when treated at a high temperature of 140°C for 30 minutes (see Appendix Figure 4 ) and increase the wettability of the diaphragm to the electrolyte on the basis of enhancing the thermal stability of the diaphragm. The specific surface area is as high as 948.7m 2 g ﹣1 (Attached Figure 3 ) thereby increasing the ionic conductivity of the diaphragm. Since hexadecyltrimethylammonium bromide is used as a soft template, a large number of mesopores are present in the silica, so the prepared mesoporous silica has a high specific surface area. And since there are a large number of hydroxyl groups on the surface and in the pores of the mesoporous silica, it has a strong adsorption effect on the organic electrolyte. After coating the diaphragm, it shows high wettability and the contact angle with the lithium-ion battery electrolyte is only 10.34° (attached Figure 6Therefore, coating the mesoporous silica on the polypropylene separator not only significantly enhances the thermal stability of the separator, but also reduces the battery impedance due to its higher wettability, improves the physical and chemical properties of the material, and the comprehensive effects are significantly stronger than those of ordinary commercial polypropylene separators and Al 2 O 3 Coated polypropylene diaphragm.

[0011] 2. The present invention uses a sol-gel method to prepare mesoporous silica and a scraper to coat the diaphragm. The preparation method is simple, and the yield of the product prepared in a single time is high, and mass production is possible. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 is a scanning electron microscope image of the modified diaphragm obtained in Example 1; Figure 2 is a transmission electron microscope photograph of the mesoporous silica obtained in Example 1; Figure 3 The adsorption-desorption isotherm and pore size distribution diagram of the mesoporous silica obtained in Example 1; Figure 4 This is a comparison chart of thermal stability of the mesoporous silica modified polypropylene diaphragm obtained in Example 1, the alumina modified polypropylene diaphragm and the commercial polypropylene diaphragm; Figure 5 This is a comparison chart of the impedance of the mesoporous silica modified polypropylene diaphragm, the alumina modified polypropylene diaphragm and the commercial polypropylene diaphragm obtained in Example 1; Figure 6 A comparison diagram of the organic electrolyte contact angles of the mesoporous silica-modified polypropylene diaphragm obtained in Example 1, the alumina-modified polypropylene diaphragm, and the commercial polypropylene diaphragm; DETAILED DESCRIPTION

[0013] The method of the present invention is further described below in conjunction with examples. These examples further describe and illustrate embodiments within the scope of the present invention. The examples provided are for illustrative purposes only, but are not limited thereto, and should not constitute any limitation to the present invention, and various changes may be made thereto without departing from the spirit and scope of the present invention.

[0014] Embodiment 1: Step 1: Dissolve 2.5 g CTAB in 46.3 ml deionized water and stir until the solution becomes colorless.

[0015] Step 2: Measure 76 ml of ethanol and add it to the above mixed solution. After stirring for 15 min, add 15 ml of ammonia water (25-28 wt%) and 1 ml of ethyl acetate and stir for 25 min. Add 5 ml of TEOS (99.9 wt%), stir (1000 r / min) for 2 h, and age for 16 h. Filter, wash, and dry to obtain the product silica.

[0016] Step 3: Heat all the products to 550 °C in a tube furnace at a heating rate of 2 °C / min, keep it at this temperature for 5 h, and then cool it naturally in air.

[0017] Step 4: Weigh the obtained mesoporous silica, mix it with polyvinylidene fluoride in a mass ratio of 8:1, grind it in a mortar for 35 min, add NMP (the mass ratio of mesoporous silica to NMP is 1:1.5) and grind it evenly.

[0018] Step 5: The scraper thickness was adjusted to 10 μm, and the ground slurry was evenly coated on a single surface of the cleaned polypropylene diaphragm using a scraper. The coated diaphragm was dried in an oven at 70 °C for 12 h.

[0019] Step 6: Use a contact angle meter to test the electrolyte wettability of the modified diaphragm, polypropylene diaphragm, and commercial ceramic diaphragm. At the same time, cut the three diaphragms into 10*10 cm 2 After being sized, they were treated in an oven at constant temperatures of 80℃, 100℃, 120℃, and 140℃ for 30 min, and the shrinkage rates were calculated.

[0020] Step 7: The dried diaphragm is cut into a circular diaphragm using a φ=18 mm mold. The positive and negative electrodes are graphite and lithium sheets respectively, and the electrolyte is 1 M LiPF with a volume ratio of 1:1. 6 Ethylene carbonate (EC) and diethyl carbonate (DMC), to which fluorinated ethylene carbonate (FEC) was added with 10 wt% of the total mass of the electrolyte, CR2025 batteries were assembled and the CHI660e instrument was used at 1*10 ﹣2 Hz-10*10 4 Electrochemical impedance spectroscopy was performed with an amplitude of 5 mV in the frequency range of Hz.

[0021] Figure 1 This is a scanning electron microscope photo of the modified diaphragm prepared in this example. From the photo, we can see that the mesoporous silica is evenly dispersed on the diaphragm.

[0022] Figure 2This is a transmission electron microscope image of the mesoporous silica prepared in this example. From the image, we can see that MSNs have a large number of pores and are dendritic, indicating that they have high electrolyte wettability and strong ability to bear stress.

[0023] Figure 3 The adsorption-desorption isotherm and pore size distribution of the mesoporous silica prepared in this example. The BET specific surface area of ​​the prepared mesoporous silica calculated from the adsorption-desorption isotherm is 948.72 m² g ﹣1 The prepared mesoporous silica has a large specific surface area and a large number of pore structures.

[0024] Figure 4 This is a comparison chart of the thermal stability of the mesoporous silica modified polypropylene membrane, alumina modified polypropylene membrane and commercial polypropylene membrane prepared in this example. It can be seen from the figure that the thermal stability of the modified membrane is always higher than that of the commercial ceramic membrane and polypropylene membrane. Compared with the shrinkage rate of the commercial ceramic membrane (90%) and the polypropylene membrane (83.3%) at 140 ℃, the shrinkage rate of the modified membrane in this example (42.5%) is lower and has a more stable structure.

[0025] Figure 5 The impedance comparison chart of the mesoporous silica modified polypropylene diaphragm, alumina modified polypropylene diaphragm and commercial polypropylene diaphragm prepared in this example shows that the impedance of the modified diaphragm in the battery (43.1 Ω) is 20.2 Ω and 8.8 Ω smaller than that of the polypropylene diaphragm (63.3 Ω) and the commercial ceramic diaphragm (51.9 Ω), respectively. This proves that coating the diaphragm does not increase its impedance due to the addition of material. On the contrary, the impedance is reduced due to the higher electrolyte wettability of the coating.

[0026] Figure 6 The following is a comparison of the contact angles of the mesoporous silica modified polypropylene membrane, alumina modified polypropylene membrane and commercial polypropylene membrane with organic electrolyte. It can be seen from the figure that the contact angle of the electrolyte with the modified membrane of this example is only 10.34°, while the contact angles with the commercial polypropylene membrane and alumina modified polypropylene membrane are 45.60° and 42.02° respectively, indicating that its uniform mesoporous structure enhances the adsorption capacity of the modified membrane to the electrolyte, making the membrane have a smaller impedance.

[0027] Embodiment 2: The preparation steps of the mesoporous silica-loaded polypropylene diaphragm are the same as those in Example 1, except that the amount of TEOS added in step 2 is 1 ml.

[0028] Embodiment 3: The preparation steps of the mesoporous silica-loaded polypropylene diaphragm are the same as those in Example 1, except that the reaction temperature after adding TEOS in step 2 is 80°C.

[0029] Embodiment 4: The preparation steps of the mesoporous silica-loaded polypropylene diaphragm are the same as those in Example 1, except that the aging time after adding TEOS in step 2 is 20 h.

[0030] Embodiment 5: The preparation steps of the mesoporous silica-loaded polypropylene diaphragm are the same as those in Example 1, except that the heating rate of the tubular furnace in step 3 is 1° C. / min.

[0031] Embodiment 6: The preparation steps of the mesoporous silica-loaded polypropylene diaphragm are the same as those in Example 1, except that the mass ratio of mesoporous silica to polyvinylidene fluoride in step 4 is 9:1.

[0032] From the above examples, it can be seen that the mesoporous silica submicron particles used in the case of the high viscosity binder used in the present invention are monodispersed and have good uniformity, so that the coating is uniformly maintained during the coating process and the high temperature process. Similarly, the distribution of mesoporous silica particles not only enhances the high temperature resistance of the diaphragm material, but also shares the stress caused by the dendrite growth of the diaphragm material due to the isotropic nature of the spherical structure of the mesopores. The preparation of mesoporous silica is through a simple sol-gel method, which is not only simple to prepare, low-cost and suitable for mass preparation, but also provides a solid material basis for the mass preparation of the composite diaphragm material of the present invention. Similarly, due to the presence of a large number of hydroxyl functional groups and a large specific surface area in mesoporous silica, it has high wettability with the electrolyte, providing more high-speed channels for the passage of particles and reducing the impedance of the interface.

[0033] Matters not covered by the present invention are known technologies.

Claims

1. A method for preparing a diaphragm having a mesoporous silica particle coating, characterized in that the method comprises the following steps: Step 1: Dissolve CTAB in deionized water, stir, and then add ethanol, ammonia water, and ethyl acetate to obtain a mixed solution; in, Add 2-3 g of CTAB, 70-80 ml of ethanol, 15-20 ml of ammonia, and 1-2 ml of ethyl acetate to every 40-50 ml of deionized water; Step 2: Add TEOS to the mixed solution, then rapidly stir for 1.5-3 h, age for 16-24 h, filter and wash, and dry at 70-80 °C for 12 h to obtain silicon dioxide; Among them, 1-8 ml of TEOS was added to every 40-50 ml of the mixed solution obtained by deionized water; Step 3: heating the dried silica to 500-600°C in a tube furnace at a heating rate of 1-5°C / min, keeping the temperature for 5-8 hours, removing the soft template, and obtaining mesoporous silica; Step 4: Grind and mix mesoporous silica and polyvinylidene fluoride (PVDF) in a mass ratio of 8-10:0.5-2, add N-methylpyrrolidone (NMP), and coat them on a polypropylene diaphragm after grinding; the coating thickness is 10-90 μm; Step 5: Dry the coated diaphragm in a drying oven at 60-70 °C for 8-12 h to obtain a modified diaphragm.

2. The method for preparing a diaphragm having a mesoporous silica particle coating as claimed in claim 1, characterized in that the concentration of the ammonia water in step 1 is 25-28 wt%.

3. The method for preparing a diaphragm having a mesoporous silica particle coating as claimed in claim 1, Its characteristics are The rapid stirring rate described in step 2 is 1000~3000 r / min.

4. Application of the diaphragm having a mesoporous silica particle coating obtained by the method as claimed in claim 1, characterized in that it is used as a lithium-ion battery diaphragm.

5. The use as claimed in claim 1, characterized in that the lithium-ion battery is specifically: graphite is the positive electrode, lithium sheet is the negative electrode, and the electrolyte is 1 M LiPF 6 Ethylene carbonate (EC) and diethyl carbonate (DMC), as well as fluorinated ethylene carbonate (FEC) at 10 wt% of the total mass of the electrolyte.

Citation Information

Cited By

  • Isolating membrane for sodium-ion battery and preparation method of isolating membrane

    CN120432813A