Continuous casting method and continuous casting machine for steel

By using a bending continuous casting machine during the continuous casting of steel, combined with appropriate pressure speed and belly control, the problems of center segregation and hydrogen-induced cracks of steel are solved, and a more stable steel quality is achieved.

CN119095679APending Publication Date: 2024-12-06JFE STEEL CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202380039253.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-26
Filing Date
2023-05-15
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The prior art is difficult to effectively reduce the central segregation grade and deviation in the width direction of the casting sheet during continuous casting of steel, especially in strict steel materials such as pipelines, which lead to macroscopic segregation and hydrogen-induced cracks.

Method used

By using a bending or vertical bending continuous casting machine, the deflection conditions of the fan section are satisfied by applying a pressing speed of 0.3 mm/min or more and 2.0 mm/min to the center of the thickness of the casting sheet (2×τ-A/( n-1)≤3.25×2×δ≤1.3), and gradually increase the roll opening of the cast sheet support roller in the intentional belly band to reduce the roll opening of the light pressing belt to control the belly bulge and Press the amount.

Benefits of technology

It effectively reduces the central segregation level and deviation in the width direction of the casting sheet, reduces the occurrence of hydrogen-induced cracks, and improves the quality stability of the steel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119095679A_ABST
    Figure CN119095679A_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing a continuous casting method and a continuous casting machine for steel with which it is possible to reduce the overall segregation level of center segregation in the width direction of a casting piece and to reduce variations in the degree of segregation in the width direction of the casting piece. A continuous casting method for steel, in which steel is continuously cast using a continuous casting machine (1), is characterized in that: the center solid fraction, which is the solid fraction at the center of the thickness of a continuously cast slab, is at least 0.2 to less than 1.0, and the slab is pressed at a pressing speed of 0.3 to 2.0 mm / min inclusive; the flexure [tau] of the segment (18), which is the flexure in the thickness direction of the segment frame of the segment (18) that is pressed to the casting piece, satisfies the equation (1): 2 * [tau]-A / (n-1) < = 3.25 * 2 * [delta] < = 1.3 (1) where [delta] is the measured belly amount (mm), [tau] is the flexure (mm) of the segment, A is the set amount (mm) of the press-down of the soft press-down, and n is the number of pairs of casting piece support rollers present in the soft press-down zone.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a continuous casting method and a continuous casting machine for steel. Background Art

[0002] During the solidification process of steel, solute elements such as carbon (C), phosphorus (P), sulfur (S), and manganese (Mn) are concentrated on the unsolidified liquid phase side due to redistribution during solidification. The concentrated solute elements become micro segregation formed between dendrite trees. In addition, during the continuous casting of steel in a continuous casting machine, due to the solidification shrinkage or thermal shrinkage of the cast piece, the bulging of the solidified shell generated between the rollers of the continuous casting machine, etc., when a gap is formed in the thickness center of the cast piece or a negative pressure is generated, the molten steel is absorbed by this part. However, since there is not enough molten steel in the unsolidified layer at the end of solidification, the concentrated molten steel flows due to the above-mentioned micro segregation, gathers in the center of the cast piece and solidifies. The concentration of the solute elements at the segregation point formed in this way becomes an exceptionally high concentration compared to the initial concentration of the molten steel. It is usually called macro segregation, and is also called center segregation according to its location.

[0003] The quality of pipes used to transport crude oil, natural gas, etc. deteriorates due to center segregation. If manganese sulfide or niobium carbide (NbC) is generated in the center segregation area, hydrogen that has penetrated into the steel due to corrosion reaction diffuses / aggregates around the manganese sulfide or niobium carbide in the steel, and cracks are generated due to the internal pressure of hydrogen. In addition, the center segregation area becomes hard, so the cracks propagate. This crack is called hydrogen-induced cracking (also called "HIC"), which is the main cause of the deterioration of the quality of pipes used in sour gas environments.

[0004] In order to deal with this problem, many measures have been proposed to reduce the center segregation of the cast piece or to render the center segregation of the cast piece harmless from the continuous casting process to the rolling process.

[0005] For example, Patent Documents 1 and 2 propose the following method: in a continuous casting machine, casting is performed while gradually pressing down a slab having an unsolidified layer in the final stage of solidification by a slab support roll at a reduction amount corresponding to the sum of the solidification shrinkage and the thermal shrinkage.

[0006] As in Patent Documents 1 and 2, the technique of gradually pressing down the cast piece during casting in a continuous casting machine by a reduction amount corresponding to the sum of the solidification shrinkage and the thermal shrinkage is called "soft reduction" or "soft reduction method". This soft reduction technique uses multiple pairs of rollers arranged in the casting direction to gradually press down the cast piece by a reduction amount corresponding to the sum of the solidification shrinkage and the thermal shrinkage to reduce the volume of the unsolidified layer. In this way, while preventing the formation of voids or negative pressure parts at the center of the cast piece, the flow of concentrated molten steel formed between the dendrite trees is prevented, thereby reducing the center segregation of the cast piece.

[0007] In addition, the continuous casting machine of recent years is mainly a segment type continuous casting machine composed of a segment having a plurality of pairs of rollers. In the case of the segment type continuous casting machine, the reduction roll group for performing light reduction (referred to as a "light reduction zone") is also composed of a plurality of segments. In the light reduction zone composed of the segments, the opening between the rollers relative to each other in the thickness direction of the cast piece is adjusted at the entry side and the exit side of the segment so that the opening at the entry side is larger than that at the exit side, thereby applying a predetermined reduction amount to the cast piece.

[0008] However, it is known that the shape of the solidification completion position of the cast sheet in the width direction of the cast sheet is closely related to the center segregation. For example, the following method is proposed in Patent Document 3: the solidification completion position in the width direction of the cast sheet is detected, and the flow of molten steel in the mold is adjusted or the width cutting amount of the secondary cooling is adjusted so that the difference between the shortest part and the longest part of the detected solidification completion position is within the reference. In the case where the solidification completion position is different in the width direction of the cast sheet, the reduction amount in the light reduction zone is different at each position in the width direction of the cast sheet. Therefore, at the position where the solidification completion position extends to the downstream side of the casting direction, the reduction amount becomes less, and a sufficient center segregation improvement effect cannot be obtained. However, according to the method of Patent Document 3, even in the case where the solidification completion position is different in the width direction of the cast sheet, the center segregation improvement effect can be obtained.

[0009] In addition, it is known that the bulging of the cast piece between the rolls will also affect the center segregation. For example, Patent Document 4 proposes the following continuous casting method: the bulging between the rolls of the cast piece in the light reduction zone is calculated by non-steady-state heat transfer solidification calculation, and the reduction speed applied to the cast piece is changed according to the calculated bulging between the rolls.

[0010] Prior art literature Patent Literature Patent Document 1: Japanese Patent Application Laid-Open No. 8-132203 Patent Document 2: Japanese Patent Application Laid-Open No. 8-192256 Patent Document 3: Japanese Patent Application Publication No. 2006-198644 Patent Document 4: Japanese Patent Application Publication No. 2012-45552 Summary of the invention

[0011] Problems to be solved by the invention

[0012] As described above, in order to improve the center segregation of the cast piece, measures have been taken for the rolling speed during light rolling, the shape of the solidification completion position in the width direction of the cast piece, and the bulging between the rolls. However, the quality requirements for the continuous casting cast piece have been further improved recently, and the deviation of the segregation degree in the width direction of the cast piece has also become a problem. In particular, in steel materials with severe segregation such as pipes and wires, even if there is only one large segregation portion in the width direction at the casting stage, it is difficult to use it as a pipe and wire material.

[0013] Furthermore, even when the above-mentioned conventional technology is applied, problems of center segregation may occur, such as deterioration of the overall segregation grade of center segregation in the slab width direction and increase in the dispersion of the segregation degree in the slab width direction. Therefore, a technology for reducing center segregation more stably is required.

[0014] Therefore, the present invention is completed in view of the above situation, and its purpose is to provide a continuous casting method and a continuous casting machine for steel, which can reduce the overall segregation level of center segregation in the width direction of the cast piece and can reduce the deviation of the segregation degree in the width direction of the cast piece.

[0015] Technical solutions to solve problems

[0016] (1) According to one embodiment of the present invention, there is provided a method for continuous casting of steel, wherein the steel is continuously cast using a continuous casting machine such as a curved continuous casting machine or a vertical curved continuous casting machine, wherein the cast piece is pressed down at a pressing speed of 0.3 mm / min to 2.0 mm / min within a range where the solid phase ratio at the thickness center of the continuously cast cast piece is at least 0.2 and less than 1.0, and the deflection in the thickness direction of the segment frame of the fan-shaped segment that presses down the cast piece, i.e., the deflection τ of the fan-shaped segment, satisfies the formula (1): 2×τ-A / (n-1)≤3.25×2×δ≤1.3…(1), in, δ: Actual bulge (mm), τ: deflection of the sector (mm), A: set reduction amount (mm) for soft reduction in a soft reduction zone where the solid phase ratio of the cast slab is 0.2 or more and less than 1.0, n: The number of pairs of cast slab support rolls present in the soft reduction zone where the solid phase fraction of the cast slab is 0.2 or more and less than 1.0.

[0017] (2) In the steel continuous casting method described in (1) above, the deflection deviation σ of the segment frame corresponding to the final solidification position is set to 0.2 mm or less, and the left and right displacement difference t of the segment frame is always set to 0.2 mm or less.

[0018] (3) In the continuous casting method of steel described in (1) or (2) above, in the intentional bulging belt of the above-mentioned continuous casting machine, the roll opening of multiple pairs of casting piece supporting rollers is gradually increased toward the downstream side in the casting direction, so that the long side surface of the above-mentioned casting piece is bulged with a total bulging amount of not less than 3 mm and not more than 20 mm, and in the light pressure belt on the downstream side in the casting direction than the above-mentioned intentional bulging belt, the roll opening of multiple pairs of casting piece supporting rollers is gradually reduced toward the downstream side in the above-mentioned casting direction, thereby applying the above-mentioned pressure reduction to the above-mentioned casting piece.

[0019] (4) According to one embodiment of the present invention, there is provided a continuous casting machine for steel, which is a curved continuous casting machine or a vertical curved continuous casting machine for continuously casting steel, wherein the continuous casting machine is provided with a light reduction belt, which presses the continuously casted slab in the thickness direction, and in the light reduction belt, within the range of the solid phase ratio at the thickness center of the slab, i.e., the center solid phase ratio, being at least 0.2 and less than 1.0, the slab is pressed down at a pressing speed of 0.3 mm / min to 2.0 mm / min, and the deflection in the thickness direction of the slab frame of the fan segment that presses down the slab in the light reduction belt, i.e., the deflection τ of the fan segment, satisfies formula (1).

[0020] Effects of the Invention

[0021] According to one embodiment of the present invention, a continuous casting method and a continuous casting machine for steel are provided, which can reduce the overall segregation level of center segregation in the width direction of a cast piece and can reduce the deviation of the segregation degree in the width direction of the cast piece. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a schematic side view showing a continuous casting machine in one embodiment of the present invention. Figure 2 This is a schematic front view showing the structure of a sector. Figure 3 It is a schematic side view showing the structure of a sector. Figure 4 This is a graph showing an example of a curve of the roll opening of the casting slab support roll. DETAILED DESCRIPTION

[0023] In the following detailed description, embodiments of the present invention are described with reference to the accompanying drawings. Each of the accompanying drawings is schematic and includes situations that are different from reality. In addition, the embodiments shown below illustrate devices and methods for concretizing the technical ideas of the present invention, and the technical ideas of the present invention do not specify the materials, structures, and configurations of the components to the following embodiments. The technical ideas of the present invention can be modified in various ways within the technical scope specified by the claims recorded in the claims.

[0024] In one embodiment of the present invention, a continuous casting machine 1 is a device for manufacturing a steel billet by continuously casting steel, wherein the steel billet is a cast piece having a cross section orthogonal to the long side direction, i.e., a rectangular cross-sectional shape, and the continuous casting machine 1 is a curved continuous casting machine or a vertical curved continuous casting machine. The continuous casting machine 1 involved in this embodiment is common in principle, and therefore can also be applied to any of the continuous casting machines of the curved continuous casting machine and the vertical curved continuous casting machine. In addition, in the following description of this embodiment, as an example, the continuous casting machine 1 is assumed to be a vertical curved continuous casting machine.

[0025] Figure 1 A side view schematically shows a continuous casting machine 1 as a vertical bending type steel billet continuous casting machine used in the implementation of the present invention. In addition, in this embodiment, the long side direction of the cast piece 3 and the moving direction of the cast piece 3 or the solidified shell 4 in the continuous casting machine 1 are referred to as the casting direction. In addition, the short side direction (in the cross section of the cross section of the cast piece 3 orthogonal to the long side direction) of the rectangle is referred to as the casting direction. Figure 1 The direction perpendicular to the casting direction in the cross section of the cast piece 3 is called the thickness direction, and the direction of the long side of the rectangle in the cross section of the cast piece 3 ( Figure 1 The front-to-back direction in the casting (in the front-to-back direction) is referred to as the width direction. Furthermore, the length of the casting slab 3 in the thickness direction is referred to as the thickness, and the length of the casting slab 3 in the width direction is referred to as the width. Furthermore, in the cross section of the casting slab 3, the sides opposite in the thickness direction are longer than the sides opposite in the width direction, and the sides opposite in the thickness direction are referred to as the long sides, and the sides opposite in the width direction are referred to as the short sides.

[0026] like Figure 1 As shown, a continuous steel billet casting machine 1 is provided with a casting mold 13 into which molten steel 2 is poured, and the molten steel 2 is cooled and solidified to form a shell shape of a cast piece 3 having a rectangular cross section. An intermediate container, i.e., a tundish 10, is provided at a predetermined position above the casting mold 13 for relaying the molten steel 2 supplied from a ladle (not shown) to the casting mold 13. A sliding nozzle 11 for adjusting the flow rate of the molten steel 2 is provided at the bottom of the tundish 10, and an immersion nozzle 12 is provided on the lower surface of the sliding nozzle 11.

[0027] A plurality of pairs of slab support rollers 14 composed of support rollers, guide rollers, and clamp rollers are arranged below the mold 13. Nozzles such as water nozzles or air mist nozzles (not shown) are arranged in the gaps between the slab support rollers 14 adjacent to each other in the casting direction, and a secondary cooling zone is formed in the range of the slab support rollers 14 from just below the mold to the end of the machine. The slab 3 is cooled by secondary cooling water sprayed from the nozzles of the secondary cooling zone while being pulled out.

[0028] A plurality of pairs of cast sheet support rollers 14 are arranged from a position about 1m to 4m away from the exit of the mold 13 in the casting direction toward the downstream side in the casting direction, forming an upper correction belt 173, which changes the direction of the support and / or guidance of the cast sheet 3 from the vertical direction to the bending direction. That is, the flat cast sheet 3 drawn from the mold 13 in the vertical direction is gradually bent into an arc shape in the upper correction belt 173, and is corrected into a curved portion with a constant radius. In the upper correction belt 173, tensile stress acts on the lower surface side of the cast sheet 3, and compressive stress acts on the upper surface side. Therefore, in the upper correction belt 173, surface cracks are easily generated on the lower surface side of the cast sheet 3, and surface cracks are generally not generated on the upper surface side. In this case, the radial inner side and outer side of the curved portion are defined as the upper surface side and the lower surface side, respectively, with the center position of the thickness direction of the cast sheet 3 as the boundary. In addition, regarding the long side surfaces (long side surfaces) of the cast piece 3, the surface on the radially inner side of the bent portion is referred to as an upper surface, and the surface on the radially outer side of the bent portion is referred to as a lower surface.

[0029] Similarly, a plurality of pairs of cast sheet support rollers 14 arranged near the position where the casting direction of the curved portion is parallel to the horizontal direction constitute a lower correction belt 174, which changes the direction of support / guiding the cast sheet 3 from the curved direction to the horizontal direction. That is, the arc-shaped cast sheet 3 is gradually bent back to a flat plate shape in the lower correction belt 174 and corrected toward the horizontal portion. In the lower correction belt 174, tensile stress acts on the upper surface side of the cast sheet 3, and compressive stress acts on the lower surface side. Therefore, in the lower correction belt 174, surface cracks are easily generated on the upper surface side of the cast sheet 3, and surface cracks are generally not generated on the lower surface side.

[0030] A plurality of conveying rollers 15 are provided on the downstream side of the casting slab support roller 14a, which is the most downstream side in the casting direction, and the plurality of conveying rollers 15 are used to convey the cast slab 3. In addition, a casting slab cutter 16 is arranged above the conveying rollers 15, and the casting slab cutter 16 is used to cut a casting slab 3a of a predetermined length from the cast slab 3.

[0031] A light reduction zone 171 is provided on the upstream and downstream sides of the solidification completion position 6 of the cast piece 3 in the casting direction. The light reduction zone 171 is composed of a plurality of pairs of cast piece support roller groups, and the plurality of pairs of cast piece support roller groups are set so that the interval (called "roller opening") between the two cast piece support rollers 14 that are opposite and paired in the thickness direction of the cast piece 3 gradually narrows toward the downstream side in the casting direction, that is, a reduction gradient is applied. In the light reduction zone 171, the cast piece 3 can be lightly reduced in its entire area or in a partially selected area. In addition, the so-called light reduction is a technology for gradually reducing the cast piece being cast in the continuous casting machine 1 by a reduction amount equivalent to the sum of the solidification shrinkage amount and the thermal shrinkage amount as described above. A nozzle for cooling the cast piece 3 is arranged between the cast piece support rollers 14 adjacent to each other in the casting direction of the light reduction zone 171. The cast piece support rollers 14 arranged in the light reduction zone 171 are also called reduction rollers 14b.

[0032] exist Figure 1 In the continuous casting machine 1 shown, the light reduction belt 171 is formed by connecting three segments 18 in the casting direction, and the segment 18 is composed of three pairs of reduction rolls. Figure 1 In the embodiment, the light pressure belt 171 is composed of three fan-shaped segments 18, but the number of fan-shaped segments 18 is not particularly limited and may be one, two, or more than four. Figure 1 In the figure, the number of reduction rolls 14b arranged in one segment 18 is three pairs, but the number is not limited to three pairs. The number of reduction rolls 14b arranged in one segment can be multiple pairs, and any number of pairs is acceptable as long as there are two or more pairs. Moreover, in the continuous casting machine 1, although not shown, the casting piece supporting rolls 14 other than the light reduction belt 171 are also of a segment structure, and in particular, the segment 18 of the light reduction belt 171 is also referred to as a light reduction segment 18a.

[0033] like Figure 2 and Figure 3 As shown, the lightly pressed sector segment 18a has an upper surface side frame 180, a lower surface side frame 181 and support struts 182. The upper surface side frame 180 supports a plurality of (three in this embodiment) casting sheet support rollers 14 on the upper surface side. The lower surface side frame 181 supports a plurality of (three in this embodiment) casting sheet support rollers 14 on the lower surface side. In addition, the upper surface side frame 180, the lower surface side frame 181 and the support struts 182 are also collectively referred to as sector frames. The support struts 182 are columns that connect and support the upper surface side frame 180 and the lower surface side frame 181. The support struts 182 are respectively provided at both ends in the width direction, and when a pair of support struts 182 arranged in the width direction are regarded as a group, a plurality of groups are provided along the casting direction. In this embodiment, as Figure 3As shown, a pair of support pillars 182 are provided at the two positions of the inlet end and the outlet end in the casting direction. In addition, the support pillars 182 have a mechanism for adjusting the roller opening by adjusting the interval in the thickness direction between the upper surface side frame 180 and the lower surface side frame 181 using hydraulic pressure or the like.

[0034] Generally, the reduction gradient in the light reduction zone 171 is expressed in units of "mm / m", which is the amount of reduction in the roll opening per meter in the casting direction. Therefore, the reduction speed (mm / min) of the cast piece 3 in the light reduction zone 171 is obtained by multiplying the reduction gradient (mm / m) by the cast piece drawing speed (m / min).

[0035] The casting piece support roller 14 disposed between the lower end of the mold 13 and the liquidus crater end position of the casting piece 3 is preferably formed as an intentional bulging belt 172. The so-called liquidus crater end position is the position in the casting direction of the continuous casting machine 1 where the center temperature of the casting piece 3 reaches the liquidus temperature of the steel to be cast, and is obtained by heat transfer solidification calculation (for example, the calculation method described in Patent Document 4) corresponding to the molten steel temperature and the cooling capacity of the continuous casting machine 1. In the intentional bulging belt 172, each casting piece support roller 14 is set so that the roller opening is sequentially expanded for each pair of rollers or each plurality of pairs of rollers toward the downstream side in the casting direction before the expansion amount of the roller opening reaches a predetermined value. The roller opening of the casting piece support roller 14 disposed on the downstream side of the intentional bulging belt 172 in the casting direction and on the upstream side of the light reduction belt 171 in the casting direction is constant or narrowed to a degree commensurate with the shrinkage amount of the casting piece 3 caused by the temperature drop.

[0036] Here, the bulging in the present embodiment means intentional bulging (intentional bulging), which is also referred to as "bulging" hereinafter. In addition, the intentional bulging preferably starts at the stage where the solid phase ratio in the center portion is 0, and ends after the total amount of bulging on the long side of the casting (the total amount of bulging on the upper surface and the lower surface) reaches 3m or more and 20mm or less. When the total amount of bulging of the intentional bulging is less than 3mm, there is a possibility that the short side of the casting 3 contacts the casting support roller 14 and sufficient light pressure cannot be applied. In addition, when bulging is performed intentionally, from the viewpoint of suppressing internal cracks, the total amount of bulging is preferably 15mm or less, and more preferably 10mm or less.

[0037] Figure 4 An example of a curve showing the roll opening of the slab support roll 14 in this embodiment is shown. Figure 4 In the curve of the roll opening shown in FIG. 1 , the long side of the cast piece is intentionally bulged by the static pressure of the molten steel in the intentionally bulging belt 172, thereby increasing the thickness of the central portion of the long side of the cast piece (area b). Figure 4In the curve of the roll opening shown in FIG. 1 , the roll opening is constant or narrowed to a degree commensurate with the shrinkage of the cast piece 3 as the temperature decreases, at the downstream side after passing the intentionally bulging belt 172 (region c). Figure 4 In the curve of the roll opening shown, the long side surface of the cast piece (area d) is pressed down by the light pressing belt 171. Figure 4 a and e in the figure are regions where the roll opening is narrowed to a degree commensurate with the shrinkage of the cast piece 3 as the temperature drops. a' in the figure is an example of the roll opening of a conventional method where the roll opening is narrowed to a degree commensurate with the shrinkage of the cast piece 3 as the temperature drops.

[0038] In the intentional bulging belt 172, the roll opening of the casting sheet support roller 14 is gradually expanded toward the downstream side in the casting direction, so that the long side surface of the casting sheet 3, except for the short side, is intentionally bulged by the static pressure of the molten steel in the unsolidified layer, imitating the casting sheet support roller 14. The long side surface near the short side of the casting sheet 3 is fixed and constrained by the short side surface of the casting sheet that has been solidified, so that the thickness at the time of starting the intentional bulging is maintained. Therefore, due to the intentional bulging, only the bulged part of the long side surface of the casting sheet 3 contacts the casting sheet support roller 14. In addition, in the light reduction belt 171, by making the total reduction amount less than the bulging total amount, only the bulged part of the long side surface of the casting sheet 3 is pressed down, and light reduction can be effectively performed. In addition, the so-called total reduction amount is the reduction amount of the casting sheet 3 from the start of reduction to the end of reduction in the light reduction belt 171, and the so-called bulging total amount is the bulging amount from the start of intentional bulging to the end of intentional bulging in the intentional bulging belt 172. The bulging amount is the maximum amount of bulging of the thickness of the slab 3 in the width direction, and is the length (mm) calculated as the difference between the maximum value of the thickness in the cross section of the slab 3 (basically the thickness in the center in the width direction) and the thickness on the short side.

[0039] In addition, when the casting 3 is intentionally bulged, it is preferred that the intentional bulging belt 172 is arranged between the lower end of the mold 13 and the end position of the liquidus ring pit of the casting 3. The reason is that, on the upstream side of the casting 3 in the casting direction relative to the end position of the liquidus ring pit, the entire center of the thickness of the casting is an unsolidified layer 5 (liquid phase), the temperature of the solidified shell 4 of the casting 3 is high, and the deformation resistance is small, so that it can be easily bulged. In addition, when the casting 3 is intentionally bulged, if it is bulged at a time point when there are fewer unsolidified layers 5 inside the casting 3, the center segregation will be worsened. However, when the casting 3 is bulged at the upstream side of the casting direction relative to the end position of the liquidus ring pit, at this time point, the molten steel with the initial concentration of the solute elements not concentrated is abundant inside the casting, and the molten steel flows easily. Even if the molten steel flows, it will not cause segregation, so the bulging at this time point will not become the cause of center segregation.

[0040] The liquidus of the casting 3 is a solidification start temperature determined by the chemical composition of the casting 3 and can be obtained, for example, by the following formula (2).

[0041] T L =1536-(78×[%C]+7.6×[%Si]+4.9×[%Mn] +34.4×[%P]+38×[%S]+4.7×[%Cu] +3.1×[%Ni]+1.3×[%Cr]+3.6×[%Al]…(2) In formula (2), T L is the liquidus temperature (°C), [%C] is the carbon concentration of molten steel (mass %), [%Si] is the silicon concentration of molten steel (mass %), [%Mn] is the manganese concentration of molten steel (mass %), [%P] is the phosphorus concentration of molten steel (mass %), [%S] is the sulfur concentration of molten steel (mass %), [%Cu] is the copper concentration of molten steel (mass %), [%Ni] is the nickel concentration of molten steel (mass %), [%Cr] is the chromium concentration of molten steel (mass %), and [%Al] is the aluminum concentration of molten steel (mass %). In addition, in the study of this embodiment, low-carbon aluminum-killed steel with C of 0.03 wt% or more and 0.2 wt% or less, Si of 0.05 wt% or more and 0.5 wt% or less, Mn of 0.8 wt% or more and 1.8 wt% or less, P less than 0.02 wt%, and S less than 0.005 wt% was used. However, the application range of the present invention is of course not limited to the above-mentioned component range.

[0042] The intentionally bulging belt 172 does not require any special mechanism and is constructed only by adjusting the roller opening. Therefore, it can be set at any position within the range from the lower end of the mold 13 to the end position of the liquidus annular pit of the casting 3.

[0043] In the billet continuous casting machine 1 of this structure, the molten steel 2 injected from the tundish 10 into the mold 13 via the immersion nozzle 12 is cooled by the mold 13 to form a solidified shell 4. The cast piece 3 having the solidified shell 4 as the outer shell and the unsolidified layer 5 inside is continuously pulled toward the bottom of the mold 13 while being supported by the cast piece support roller 14 provided below the mold 13. The cast piece 3 is cooled by the secondary cooling water of the secondary cooling zone while passing through the cast piece support roller 14, so that the thickness of the solidified shell 4 is increased. In addition, the thickness of the portion of the long side surface excluding the short side end of the cast piece 3 is increased in the intentional bulging zone 172, and the solidification is completed to the inside at the solidification completion position 6 while being lightly pressed in the light pressing zone 171. The cast piece 3 after solidification is cut by the cast piece cutter 16 to become a cast piece 3a. A mold slag (not shown) that functions as an insulating material, a lubricant, an antioxidant, etc. is added to the mold 13.

[0044] In addition, in the present embodiment, continuous casting is performed under the following casting conditions in the light reduction zone 171. In the light reduction zone 171, the cast piece 3 is reduced (lightly reduced) at a reduction rate of 0.3 mm / min to 2.0 mm / min, within the range where the solid phase ratio at the thickness center of the cast piece 3, i.e., the center solid phase ratio, is at least 0.2 and less than 1.0. In addition, the thickness center of the cast piece 3 in the present embodiment means the center in the thickness direction at the position in the width direction where the solid phase ratio of the thickness center portion in the cross section of the cast piece 3 is the lowest. When the reduction rate during light reduction when the center solid phase ratio is within the above range is less than 0.3 mm / min, the possibility of V-shaped segregation becomes high. On the other hand, when the reduction rate during light reduction when the center solid phase ratio is within the above range exceeds 2.0 mm / min, the possibility of inverted V-shaped segregation becomes high.

[0045] In the present embodiment, in the light-reduction belt having a center solid fraction within a range of at least 0.2 and less than 1.0, the deflection τ of the light-reduction segment 18a constituting the light-reduction belt satisfies the following formula (1): 2×τ-A / (n-1)≤3.25×2×δ≤1.3…(1), in, δ: Actual bulge (mm), τ: deflection of the sector (mm), A: Set amount of soft reduction in the soft reduction zone where the central solid fraction of the cast slab is 0.2 or more and less than 1.0 (mm), n: The number of pairs of slab support rolls present in the soft reduction zone having a central solid fraction of the slab of 0.2 or more and less than 1.0.

[0046] In formula (1), the deflection τ of the segment is the deflection in the thickness direction at the center of the width direction of the segment frame, and is obtained from the height in the thickness direction of the width direction ends and the width direction center of the segment frame. Specifically, Figure 2 As shown by the dashed line, the deflection τ is represented by the sum of the deflections τ1 and τ2 of the upper surface side frame 180 and the lower surface side frame 181 (τ=τ1+τ2). In addition, the deflection τ is preferably the maximum value of the deflections at multiple locations in the casting direction of the segment frame. For example, the deflection τ may also be the value of the maximum deflection in at least two locations, the exit side and the entry side, in the casting direction of the segment frame. In this case, as Figure 3As shown, the deflection τ of the segment can also be obtained by measuring the deflection at the casting direction position of the two parts where the support pillars 182 are provided. In addition, the deflection τ of the soft-pressed segment 18a can be a value measured when the cast piece 3 is actually continuously cast, or a value measured when the same steel grade is continuously cast using the continuous casting machine 1.

[0047] In addition, the measured bulging amount δ is the bulging amount after the time point when the central solid phase ratio of the casting 3 changes to more than 0.0. The measured bulging amount δ is the bulging amount of either the upper surface or the lower surface. From the perspective of ease of measurement, the measured value of the bulging amount of the upper surface is preferred. In addition, since the bulging amount is usually the same value on the upper surface and the lower surface, the total amount of bulging can be calculated by measuring the bulging amount of the long side of either side and doubling the measured bulging amount. In formula (1), the measured value of the total amount of bulging is shown by multiplying the measured bulging amount δ by 2 as a coefficient.

[0048] The set amount A of the soft reduction is the amount (set amount) of reduction that the slab 3 is reduced from a center solid fraction of 0.2 or more to complete solidification. The set amount of soft reduction is a set reduction determined only by the roll curve, that is, the set roll interval.

[0049] Here, the inventors of the present invention have confirmed that in actual soft reduction in a continuous casting machine, soft reduction may not be performed at the target reduction amount (reduction setting amount) due to the influence of deflection of the segment, etc. Furthermore, they have found that by using the segment 18 satisfying the relationship of formula (1) in the soft reduction zone 171 during continuous casting, the center segregation can be reduced more stably, thereby completing the present invention.

[0050] The load applied to the segment 18 constituting the light reduction zone 171, i.e., the light reduction segment 18a, is determined by the size of the slab 3, the reduction gradient in the light reduction zone 171, and the proportion of the unsolidified layer 5 of the slab 3 to be lightly reduced. In order to prevent the flow of molten steel at the end of solidification, which causes center segregation, it is necessary to apply a light reduction of an amount proportional to the solidification shrinkage or thermal shrinkage. However, when the set reduction gradient is large or the slab size is large, the load applied to the light reduction segment 18a becomes larger. When the load applied to the light reduction segment becomes larger, the roll opening in the light reduction segment 18a moves in the direction of expansion. Therefore, even if the slab size and the reduction gradient are set the same, the load applied to the light reduction segment 18a changes according to the shape of the solidification completion position 6 in the slab width direction, and the roll opening also changes according to the load. Therefore, the reduction speed actually applied to the slab 3 also changes from the set value.

[0051] However, by making the light reduction segment 18a of the light reduction belt 171 satisfy equation (1) within the above-mentioned range of the central solid phase ratio of the slab 3, the rigidity of the light reduction segment 18a can be sufficiently obtained, thereby making it possible to perform light reduction with a sufficient reduction amount, and further making it possible to reduce the central segregation more stably. In addition, since the set light reduction conditions can be uniformly applied to the width direction of the slab, the deviation of the segregation degree in the width direction caused by the central segregation can be reduced, and the segregation degree at all parts in the width direction can be reduced. On the other hand, when the light reduction segment 18a of the light reduction belt 171 does not satisfy equation (1), a sufficient reduction amount cannot be reliably obtained. Therefore, sometimes the overall segregation level of the central segregation of the slab 3 in the width direction of the slab is deteriorated, or the deviation of the segregation degree in the width direction of the slab is increased. Furthermore, when verifying the prior art such as Patent Documents 1 to 4, the major premise is that the set soft reduction conditions are directly applied to the cast piece, without considering the deviation from the soft reduction opening caused by the actually generated mechanical deflection of the fan-shaped segment or the mechanical elongation of the support.

[0052] Moreover, as the casting condition of the present embodiment, it is preferable that, for the segment 18 corresponding to the solidification completion position 6, the deflection deviation σ of the segment frame is 0.2 mm or less, and the displacement difference t of the left and right of the segment frame is always 0.2 mm or less. The deflection deviation σ is the deviation of the deflection of each of the upper surface side frame 180 and the lower surface side frame 181 of the segment 18, and is the difference between the maximum value and the minimum value of the deflection at multiple positions in the casting direction of each of the upper surface side frame 180 and the lower surface side frame 181. That is, the deflection deviation σ is 0.2 mm or less, which means that the deflection deviation in the casting direction of each of the upper surface side frame 180 and the lower surface side frame 181 is 0.2 mm or less. For example, the deflection deviation may also be the difference in deflection between the inlet end and the outlet end in the casting direction of each of the upper surface side frame 180 and the lower surface side frame 181. In this case, the position where the deflection is measured may also be the position where the support pillar 182 is provided. In addition, the difference between the maximum and minimum values ​​of the deflection at three or more casting direction positions can also be set as the deflection deviation σ. The left and right displacement difference t is the displacement difference between the two ends of the width direction of the sector frame. Usually, since the structure of the lower part of the sector 18 is fixed and does not move, the displacement difference between the two ends of the width direction of the upper surface side frame 180 of the sector 18 becomes the left and right displacement difference t. In addition, the displacement difference t can also be the difference in height between the upper ends of a pair of supporting pillars 182 connected to the two ends of the width direction of the upper surface side frame 180. Moreover, the left and right displacement difference t is preferably always less than 0.2 mm at different positions in the casting direction. By adopting such casting conditions, center segregation can be reduced more stably.

[0053] <Modification>

[0054] The present invention has been described above with reference to specific embodiments, but it is not intended to limit the present invention by these descriptions. By referring to the description of the present invention, other embodiments of the present invention including various modifications together with the disclosed embodiments are also clear to those skilled in the art. Therefore, it should be understood that the embodiments of the invention described in the claims also include embodiments including these modifications described in this specification alone or in combination.

[0055] For example, in the above embodiment, the support pillars 182 adjust the roll opening, but the present invention is not limited to this example. For example, the roll opening may be adjusted by extending or retracting the support member connecting the slab support rolls 14 and the segment frame by hydraulic pressure or the like.

[0056] Example

[0057] The present inventors will now describe an embodiment of the present invention. In the embodiment, in order to investigate the effect of casting conditions on the thickness center segregation of the cast slab 3, two types of segments 18 (frame 1 and frame 2) with different rigidities were experimentally set up, and continuous casting was performed under various casting conditions. Figure 1 The vertical bending type continuous casting machine 1 shown in the figure is a casting condition when continuous casting is performed by light reduction. In addition, the Mn segregation degree and hydrogen induced cracking resistance test (HIC test) are measured and evaluated for the cast slab 3. The detailed casting conditions are as follows.

[0058] In the embodiment, for the purpose of effectively lightly pressing the cast piece 3, the cast piece drawing speed is constant at 1.1m / min. The total amount of bulging in the intentional bulging belt 172 varies at each level within the range of more than 0.0mm and less than 15.0mm. The set pressing speed in the light pressing belt 171 varies at each level within the range of more than 0mm / min and less than 4.0mm / min. The size of the cast cast piece 3 is a steel billet cast piece of 2100mm wide and 250mm thick. Regarding the segment frame of the segment 18, the rigidity of frame 1 is made higher than that of frame 2. In addition, the secondary cooling water volume is adjusted so that it is the same at all levels. In addition, the final solidification position is calculated by the same heat transfer solidification as in patent document 4.

[0059] During the casting process, in the lightly pressed sector located at the solidification completion position 6 closest to the downstream side of the casting direction calculated in advance by heat transfer solidification calculation, the displacement of the center of the sector and the supporting struts of the sector frame is measured by a non-contact sensor as the displacement of the roll opening.

[0060] After casting, the cross section of the test piece collected from the casting (equivalent to the longitudinal section of the casting) was corroded with picric acid to investigate the relationship between the reduction rate actually applied to the casting 3 and the segregation of the casting 3, and to investigate the presence or absence of V-shaped segregation, inverted V-shaped segregation, and internal cracks. In addition, in the test piece collected from the casting 3, the segregation of Mn in the center of the thickness of the casting was analyzed by EPMA, and the Mn segregation degree at each position in the width direction of the casting was investigated. In addition, the hydrogen induced cracking test (HIC test) was carried out on the test piece collected from each position in the width direction of the casting.

[0061] The conditions and test results of each level in the embodiment are shown in Table 1. Levels 1 to 13 are the cases where fan segments with improved frame rigidity are applied, and levels 14 to 28 are the cases where fan segments with insufficient rigidity are applied. In the embodiment, the light-pressing belt 171 uses frames 1 and 2 with different rigidity, and the casting conditions other than this are implemented in the same manner. In addition, the number of light-pressing fan segments 18a provided in the light-pressing belt 171 is one. In addition, in Table 1, the measured bulge amount is the measured value of the bulge amount of the cast slab, the value α is the value obtained by the following formula (2), and the value β is the value obtained by the following formula (3). Moreover, the set pressure reduction amount A in formula (1) is obtained by the following formula (4), and the length L of the light-pressing belt 171 in the casting direction is set to 1.89 m according to the length of the light-pressing fan segment 18a, and the casting speed V is set to 1.89 m. c is set to 1.1 m / min. Moreover, according to the number of roller pairs provided in the light-pressing sector segment 18a, the number n of the cast sheet support roller pairs present in the light-pressing belt 171 is set to 8 groups. In addition, in Table 1, it is judged whether the value β is less than 1.3, and the case where the value β is less than 1.3 is set to "○", and the case where the value β exceeds 1.3 is set to "×". That is, the condition that the value β is greater than the value α and is judged to be "○" satisfies the formula (1). Moreover, in Table 1, the deflection deviation of the sector displacement is the deflection deviation σ in the sector at the final solidification position, which is the value obtained by adding the deflection deviation σ of the upper surface side frame 180 to the deflection deviation σ of the lower surface side frame 181. In addition, the "in" and "out" of the sector displacement represent the displacement of the end portions (positions where the support pillars 182 are provided) of the inlet and outlet sides of the sector at the final solidification position in the casting direction. In addition, the "south" and "north" of the segment displacement represent the displacement of the ends (positions where the support pillars 182 are provided) of one end (the south end in the actual machine) and the other end (the north end in the actual machine) in the width direction of the segment. Moreover, the "difference" of the segment displacement is the difference between the south and north displacements, which is the left and right displacement difference t. In this embodiment, the segment displacement represents how much the upper end position is displaced from the reference with the upper end position of the support pillar 182 in the state where the segment is not bent as the reference.

[0062] α=2×τ-A / (n-1)…(2) in, τ: deflection of the sector (mm), A: set reduction amount (mm) for soft reduction in a soft reduction zone where the solid phase ratio of the cast slab is 0.2 or more and less than 1.0, n: the number of pairs of cast slab support rolls present in the soft reduction zone where the solid phase fraction of the cast slab is 0.2 or more and less than 1.0, β = 3.25 × 2 × δ… (3) in, δ: Actual bulge (mm), A=V p ×L / V c … (4) in, V p : Set the pressing speed (mm / min), L: Length in the casting direction under light pressure (m), V c : Casting speed (m / min).

[0063] [Table 1]

[0064] As shown in Table 1, when comparing frame 1 and frame 2, the center deflection was reduced to 0.4 mm or less by increasing the frame rigidity, and the left-right displacement difference was suppressed to 0.2 mm or less, thereby improving the center segregation.

[0065] In addition, levels 1 to 6 are conditions within the scope of the present invention, and both the segregation degree and the deviation σ are good results. V-shaped segregation occurs when the reduction speed in the light reduction zone 171 of levels 9 to 11, 16 to 17, and 22 to 24 is less than 0.3 mm / min, and inverted V-shaped segregation occurs when the reduction speed exceeds 2.0 mm / min in levels 12, 13, 25, and 26.

[0066] In the case of V-shaped segregation and inverted V-shaped segregation in the center segregation, the Mn segregation degree deteriorates, and the crack segregation area ratio (%) = vehicle (collision area ratio) as the HIC score also deteriorates. In addition, as a criterion for judging the center segregation, 1.06 or less is considered good for the Mn segregation degree, and 2.0 or less is considered good for the HIC score. Therefore, it can be seen that the reduction speed in the light reduction zone 171 needs to be controlled to be above 0.3 mm / min and below 2.0 mm / min. In addition, the reduction speed actually applied to the casting 3 is calculated as the product of the reduction gradient calculated based on the displacement of the roll opening in the light reduction sector measured by the non-contact sensor and the drawing speed of the casting.

[0067] Description of symbols 1 Billet continuous casting machine 10 Tundish 11 Sliding nozzle 12 Dipping nozzle 13. Casting 14, 14a Casting support roller 14b Pressing roller 15 Conveyor roller 16 Casting Slab Cutting Machine 171 Lightly press down the belt 172 Intentional Bellyband 173 Upper Correction Belt 174 Lower Correction Belt 18 sectors 18a Gently press down the fan-shaped segment 180 Upper surface side frame 181 Lower surface side frame 182 Support pillars 2 Molten Steel 3.3a ​​Casting 4 Solidification shell 5 Unsolidified layer 6 Solidification completion position.

Claims

1. A method for continuously casting steel, wherein the steel is continuously cast using a continuous casting machine such as a curved continuous casting machine or a vertical curved continuous casting machine, wherein: The cast piece is pressed at a pressing speed of 0.3 mm / min to 2.0 mm / min, while the solid phase ratio at the center of the thickness of the continuously cast piece, i.e., the central solid phase ratio, is at least 0.2 or more and less than 1.

0. The deflection in the thickness direction of the segment frame of the segment that applies pressure to the cast sheet, that is, the deflection τ of the segment satisfies the formula (1): 2×τ-A / (n-1)≤3.25×2×δ≤1.3…(1), in, δ: Actual bulge (mm), τ: deflection of the sector (mm), A: Set amount of soft reduction in the soft reduction zone where the central solid fraction of the cast slab is 0.2 or more and less than 1.0 (mm), n: The number of pairs of slab support rolls present in the soft reduction zone having a central solid fraction of the slab of 0.2 or more and less than 1.

0.

2. The method for continuous casting of steel according to claim 1, wherein: The deflection deviation σ of the segment frame corresponding to the final solidification position is set to 0.2 mm or less, and the left-right displacement difference t of the segment frame is always set to 0.2 mm or less.

3. The method for continuous casting of steel according to claim 1 or 2, wherein: In the intentionally bulging belt of the continuous casting machine, the roller opening of the plurality of pairs of cast sheet support rollers is gradually increased toward the downstream side in the casting direction, so that the long side surface of the cast sheet is bulged with a total bulging amount of 3 mm or more and 20 mm or less. In the light reduction zone located downstream of the intentional bulging zone in the casting direction, the roll opening of a plurality of pairs of slab support rolls is gradually reduced toward the downstream side in the casting direction, thereby applying the reduction to the slab.

4. A continuous casting machine for steel, which is a continuous casting machine such as a curved continuous casting machine or a vertical curved continuous casting machine for continuously casting steel, wherein: A light reduction belt is provided, wherein the light reduction belt reduces the continuously cast slab in the thickness direction. In the soft reduction zone, the cast piece is pressed at a reduction rate of 0.3 mm / min to 2.0 mm / min, within a range where the solid phase ratio at the center of the thickness of the cast piece, i.e., the center solid phase ratio, is at least 0.2 to less than 1.

0. The deflection in the thickness direction of the segment frame of the segment that applies pressure to the cast piece in the soft reduction zone, that is, the deflection τ of the segment satisfies the formula (1): 2×τ-A / (n-1)≤3.25×2×δ≤1.3…(1), in, δ: Actual bulge (mm), τ: deflection of the sector (mm), A: Set amount of soft reduction in the soft reduction zone where the central solid fraction of the cast slab is 0.2 or more and less than 1.0 (mm), n: The number of pairs of slab support rolls present in the soft reduction zone having a central solid fraction of the slab of 0.2 or more and less than 1.0.

Citation Information

Patent Citations

  • Continuous casting method

    JP1996132203A

  • Continuous casting method

    JP1996192256A

  • Method of manufacturing continuously cast slab

    JP2006198644A

  • Continuous casting method of steel cast slab

    JP2012045552A