Metal-clad laminate, printed wiring board, semiconductor package, and method for manufacturing same
By setting the first and second resin layers on the fiber substrate and setting the prepreg and metal foil heating and pressing method of the unimpregnated area, the thickness accuracy and size of the metal laminated plate under the fiber substrate is solved by the solution of the thickness accuracy and size of the metal laminated plate under the fiber substrate with a thickness of more than 40 μm. The problem of uneven changes reduces the fluctuation of warping volume of semiconductor packaging and improves product quality.
Patent Information
- Application Number
- CN202380037005.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-12-07
- Filing Date
- 2023-12-06
- Publication Date
- 2024-12-06
AI Technical Summary
In the prior art, it is difficult to manufacture a metal-covered laminated plate with uniform thickness accuracy and dimensional variation when using a fiber substrate with a thickness of 40 μm or more, and it is difficult to reduce the warping fluctuation of the semiconductor package.
By using a stacking method of heating and pressurizing the prepreg and metal foil, the first and second resin layers are set on the fiber substrate, the ratio of thickness difference is controlled to be -9.0% to +9.0%, and the fiber substrate is used. Unimpregnated areas are provided in the material to uniformize the surface corrugation and ensure uniformity of thickness accuracy and dimensional changes.
When using a fiber base material with a thickness of 40 μm or more, it is possible to manufacture a metal-covered laminated plate with uniform thickness accuracy and dimensional variation, and reduce the warping fluctuation of the semiconductor package and improve the quality of the metal-covered laminated plate.
Smart Images

Figure CN119095722A_ABST
Abstract
Description
Technical Field
[0001] The present embodiment relates to a metal-clad laminate, a printed wiring board, a semiconductor package, and methods for manufacturing the same. Background Art
[0002] In recent years, electronic devices have been developing in the direction of miniaturization, lightness and high functionality, and the semiconductor devices installed in electronic devices are becoming more and more highly integrated. Along with this, the metal-clad laminates and semiconductor packages used in printed wiring boards are required to have higher quality than before.
[0003] For example, for metal-clad laminates, from the viewpoint of improving the productivity of the resulting printed wiring board, a higher thickness accuracy than in the past is required. In addition, sometimes the metal-clad laminates are subjected to various treatments such as heat treatment and liquid treatment, but the dimensional variation caused by these treatments is required not to be uneven between products.
[0004] Furthermore, semiconductor packages are required to reduce the variation in warpage between products compared to conventional methods.
[0005] Patent document 1 describes a method for manufacturing a prepreg, which is characterized in that in a method for manufacturing a prepreg by impregnating a substrate in a resin liquid and then drying it, convex resin protrusions generated on the surface of the prepreg are flattened by pressing the prepreg with a roller during the drying process or after the drying is completed, thereby improving the smoothness of the surface.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Laid-Open No. 01-272416 Summary of the invention
[0009] Problems to be solved by the invention
[0010] The technology of Patent Document 1 mechanically pressurizes the surface of the prepreg to improve the smoothness.
[0011] However, as described above, the high integration of semiconductor devices has been significantly developed, and it is difficult to achieve the thickness accuracy of the metal-clad laminate at the level required in recent years using the technology of Patent Document 1. In addition, the technology of Patent Document 1 does not solve the problem of uniformizing the dimensional variation of the metal-clad laminate and reducing the fluctuation of the warpage of the semiconductor package.
[0012] In particular, the inventors have found that when the thickness of the fiber substrate used in the prepreg is 40 μm or more, it becomes more difficult to improve the thickness accuracy and uniformity of the dimensional variation of the metal-clad laminate and reduce the fluctuation in the warpage of the semiconductor package.
[0013] In view of this situation, the present embodiment aims to provide a method for manufacturing a metal-clad laminate having excellent thickness accuracy and uniformity of dimensional variation when a fiber substrate with a thickness of 40 μm or more is used, a method for manufacturing a printed circuit board and a semiconductor package using the metal-clad laminate, a metal-clad laminate capable of reducing fluctuations in the warping amount of a semiconductor package when a fiber substrate with a thickness of 40 μm or more is used, and a printed circuit board and a semiconductor package having the metal-clad laminate.
[0014] Means for solving problems
[0015] The present inventors have conducted studies to solve the above-mentioned problems, and as a result, have found that the problems can be solved by the present embodiment described below.
[0016] That is, this embodiment relates to the following [1] to
[11] .
[0017] [1] A method for producing a metal-clad laminate, the method comprising laminating a prepreg and a metal foil by heating and pressurizing them.
[0018] The prepreg comprises a thermosetting resin composition and a fiber substrate having a thickness of 40 μm or more, and has:
[0019] a first resin layer provided on one surface of the fiber substrate and containing a thermosetting resin composition; and
[0020] a second resin layer provided on the other side of the fiber substrate and containing a thermosetting resin composition,
[0021] When the thickness of the first resin layer is d1 and the thickness of the second resin layer is d2,
[0022] The thickness difference ratio R represented by the following formula (1) is -9.0% to +9.0%.
[0023] R = (d1-d2) × 100 / (d1+d2) (1)
[0024] The surface waviness (Wa) of both surfaces of the prepreg is 6 μm or less.
[0025] [2] The method for producing a metal-clad laminate according to [1] above, wherein the prepreg has a region impregnated with the thermosetting resin composition and a region not impregnated with the thermosetting resin composition in the fiber base material.
[0026] [3] The method for producing a metal-clad laminate according to [1] or [2], wherein the thickness d1 of the first resin layer and the thickness d2 of the second resin layer are each 2 to 20 μm.
[0027] [4] The method for producing a metal-clad laminate according to any one of [1] to [3] above, wherein the fiber base material has a thickness of 40 to 120 μm.
[0028] [5] The method for producing a metal-clad laminate according to any one of [1] to [4] above, wherein the fiber substrate is glass cloth.
[0029] [6] A method for producing a printed wiring board, comprising producing a metal-clad laminate using the method for producing a metal-clad laminate described in any one of [1] to [5] above, and forming a wiring pattern on the metal-clad laminate.
[0030] [7] A method for manufacturing a semiconductor package, comprising manufacturing a printed wiring board using the method for manufacturing a printed wiring board described in [6] above, and mounting a semiconductor element on the printed wiring board.
[0031] [8] A metal-clad laminate comprising a cured product of a thermosetting resin composition, one or more fiber substrates, and a metal foil,
[0032] The thickness of the fiber substrate is 40 μm or more.
[0033] The value determined by the following method is 0.5% or less.
[0034] (method)
[0035] The area of 500 mm × 500 mm in the surface of the metal-clad laminate was divided into a grid pattern at intervals of 50 mm in the vertical and horizontal directions. Figure 4 At the positions shown in the plan view of the metal-clad laminate 30, 21 measurement unit areas 7 having a square shape of 50 mm in length and 50 mm in width in plan view are set.
[0036] In the measurement unit area 7, a point located inside the measurement unit area 7 and spaced 10 mm from the longitudinal and transverse sides, i.e. Figure 4 The thickness is measured at the positions of the four thickness measurement points 8 shown, the difference between the maximum and minimum thickness values at the four points is defined as the thickness difference V1 within the measurement unit area 7, and the average value of the thickness at the four points is defined as T1.
[0037] V1 and T1 are calculated for the 21 measurement unit areas 7, and the average value V ave and the average value of T1 ave , use the following formula to calculate the value.
[0038] V ave ×100 / T aVe
[0039] [9] The metal-clad laminate according to [8] above, wherein:
[0040] The metal-clad laminate has the metal foil on both sides and has:
[0041] a first resin cured product layer provided on a surface of the fiber base material, in contact with the metal foil on one surface of the metal-clad laminate, and containing a cured product of a thermosetting resin composition; and
[0042] The second resin cured product layer is provided on one surface of the fiber base material, is in contact with the metal foil on the other surface of the metal-clad laminate, and contains a cured product of a thermosetting resin composition.
[0043] When the thickness of the first cured resin layer is d'1 and the thickness of the second cured resin layer is d'2,
[0044] The ratio R' of the thickness difference represented by the following formula (1') is -9.0% to +9.0%.
[0045] R'=(d'1-d'2)×100 / (d'1+d'2) (1')
[0046]
[10] A printed wiring board comprising the metal-clad laminate according to [8] or [9] above.
[0047]
[11] A semiconductor package comprising the printed wiring board described in
[10] above and a semiconductor element.
[0048] Effects of the Invention
[0049] According to the present embodiment, there can be provided a method for manufacturing a metal-clad laminate having excellent thickness accuracy and uniformity of dimensional variation even when a fiber substrate having a thickness of 40 μm or more is used, a method for manufacturing a printed circuit board and a semiconductor package using the metal-clad laminate, a metal-clad laminate capable of reducing fluctuations in the warping amount of a semiconductor package even when a fiber substrate having a thickness of 40 μm or more is used, and a printed circuit board and a semiconductor package having the metal-clad laminate. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1This is a schematic cross-sectional view showing one form of the prepreg used in the production method of the present embodiment.
[0051] Figure 2 This is a schematic cross-sectional view showing one embodiment of a prepreg having intermittent unimpregnated regions in the plane direction.
[0052] Figure 3 This is an image used in calculating the abundance ratio of the impregnation region in the prepreg produced in Example 1.
[0053] Figure 4 It is a schematic plan view for explaining a method for measuring the thickness of a metal-clad laminate.
[0054] Figure 5 It is a schematic plan view for explaining a method for measuring fluctuations in the amount of dimensional change of a metal-clad laminate. DETAILED DESCRIPTION
[0055] In the present specification, a numerical range expressed using "to" indicates a range including the numerical values described before and after "to" as the minimum value and the maximum value, respectively.
[0056] For example, a numerical range such as "X to Y" (X and Y are real numbers) means a numerical range of more than X and less than Y. Furthermore, a description such as "more than X" in this specification means X and a numerical value greater than X. In addition, a description such as "less than Y" in this specification means Y and a numerical value less than Y.
[0057] The lower limit value and the upper limit value of the numerical range described in the present specification can be arbitrarily combined with the lower limit value or the upper limit value of other numerical ranges, respectively.
[0058] In the numerical range described in the present specification, the lower limit value or the upper limit value of the numerical range may be replaced with the value shown in the Examples.
[0059] Each component and material exemplified in the present specification may be used alone or in combination of two or more unless otherwise specified.
[0060] In the present specification, when a plurality of substances corresponding to each component are present in the resin composition, the content of each component in the resin composition means the total amount of the plurality of substances present in the resin composition unless otherwise specified.
[0061] The term "solid content" as used herein refers to components other than the solvent, and components that are liquid at room temperature are also considered solid components. Here, room temperature as used herein means 25°C.
[0062] The action mechanism described in this specification is a guess, and does not limit the mechanism by which the effects of the present embodiment are achieved.
[0063] The expression "containing" described in the present specification includes not only the case of simply containing "...", but also the case of containing in a state of reacting "..." when the substance described in "..." is a substance capable of reacting.
[0064] The present embodiment also includes any combination of the matters described in this specification.
[0065] [Method for producing metal-clad laminate]
[0066] The method for producing a metal-clad laminate of the present embodiment is a method for producing a metal-clad laminate by laminating a prepreg and a metal foil by heating and pressurizing.
[0067] The prepreg comprises a thermosetting resin composition and a fiber substrate having a thickness of 40 μm or more, and has:
[0068] a first resin layer provided on one surface of the fiber substrate and containing a thermosetting resin composition; and
[0069] a second resin layer provided on the other side of the fiber substrate and containing a thermosetting resin composition,
[0070] When the thickness of the first resin layer is d1 and the thickness of the second resin layer is d2,
[0071] The thickness difference ratio R represented by the following formula (1) is -9.0% to +9.0%.
[0072] R = (d1-d2) × 100 / (d1+d2) (1)
[0073] The surface waviness (Wa) of both surfaces of the prepreg is 6 μm or less.
[0074] It should be noted that in the following description, a prepreg having the above-mentioned structure, that is, a prepreg containing a thermosetting resin composition and a fiber base material with a thickness of more than 40 μm, having the above-mentioned first resin layer and the above-mentioned second resin layer, the ratio R of the above-mentioned thickness difference is -9.0% to +9.0%, and the surface waviness (Wa) of both surfaces is less than 6 μm, is sometimes referred to as "prepreg (P)".
[0075] The reason why the metal-clad laminate produced by the production method of the present embodiment is excellent in thickness accuracy and uniformity of dimensional variation is not certain, but can be inferred as follows.
[0076] The prepreg (P) used in the present embodiment has a thickness difference ratio R represented by the above formula (1) of -9.0% to +9.0%, and a surface waviness (Wa) of 6 μm or less on both sides. That is, the amount of the thermosetting resin composition attached to the front and back sides of the fiber substrate of the prepreg (P) used in the present embodiment is uniform, and the surface is smooth. As a result, the residual thickness fluctuation of the prepreg itself and the uniformity of the flow behavior of the thermosetting resin composition on the front and back sides of the prepreg when pressurized are improved, which is presumed to be one of the reasons for improving the thickness accuracy and uniformity of the dimensional change of the metal-clad laminate.
[0077] Hereinafter, each member used in the method for producing a metal-clad laminate according to the present embodiment will be described first, and then lamination conditions and the like of each member will be described.
[0078] <Prepreg (P)>
[0079] The prepreg (P) used in this embodiment contains a thermosetting resin composition and a fiber substrate with a thickness of more than 40 μm, and has: a first resin layer, which is arranged on one surface of the above-mentioned fiber substrate and contains the thermosetting resin composition; and a second resin layer, which is arranged on the other surface of the above-mentioned fiber substrate and contains the thermosetting resin composition.
[0080] Figure 1 A schematic cross-sectional view showing an example of the prepreg (P) used in this embodiment is shown in FIG.
[0081] Figure 1 The prepreg 10 shown comprises: a fiber substrate 1, a first resin layer 2 having a thickness d1 provided on one surface of the fiber substrate 1, and a second resin layer 3 having a thickness d2 provided on the other surface of the fiber substrate 1. It should be noted that the fiber substrate 1 preferably has an impregnation region with a thermosetting resin composition, and more preferably has an impregnation region with a thermosetting resin composition and a non-impregnation region.
[0082] In the prepreg 10 , the surface of the first resin layer 2 opposite to the fiber base material 1 constitutes one surface of the prepreg 10 , and the surface of the second resin layer 3 opposite to the fiber base material 1 constitutes the other surface of the prepreg 10 .
[0083] The thermosetting resin composition contained in the first resin layer and the thermosetting resin composition contained in the second resin layer may be the same or different, but are preferably the same.
[0084] When the thermosetting resin composition contained in the first resin layer is the same as the thermosetting resin composition contained in the second resin layer, these thermosetting resin compositions may be the same as or different from the thermosetting resin composition contained in the fiber base material, but are preferably the same.
[0085] It is preferred that the first resin layer and the second resin layer do not contain a fiber base material.
[0086] (Thickness difference ratio R)
[0087] In the prepreg (P) used in the present embodiment, when the thickness of the first resin layer is d1 and the thickness of the second resin layer is d2, the ratio R of the thickness difference represented by the following formula (1) is -9.0% to +9.0%.
[0088] R=(d1-d2)×100 / (d1+d2) (1)
[0089] Regarding the ratio R of the thickness difference represented by the above formula (1), from the viewpoint of further improving the thickness accuracy and uniformity of the dimensional change of the metal-clad laminate, it is preferably -8.0% to +8.0%, more preferably -7.0% to +7.0%, further preferably -6.0% to +6.0%, and particularly preferably -5.0% to +5.0%.
[0090] The thickness d1 of the first resin layer and the thickness d2 of the second resin layer used in calculating the thickness difference ratio R can be measured by the following method. In addition, more specific conditions can be set to the conditions described in the Examples.
[0091] [Method for measuring the thickness d1 of the first resin layer and the thickness d2 of the second resin layer]
[0092] A cross section of a prepreg subjected to a heat treatment as required is formed, and the cross section is observed using a metal microscope to obtain a cross-sectional image. In the obtained cross-sectional image, a fiber substrate having a thickness of 40 μm or more, a first resin layer, and a second resin layer are determined, and the minimum thickness of the first resin layer and the minimum thickness of the second resin layer in the field of view are respectively measured. The minimum thickness is measured in any 5 fields of view where the area does not overlap, and the value obtained by averaging the minimum thicknesses of the 5 fields of view in the first resin layer is set as the thickness d1 of the first resin layer, and the value obtained by averaging the minimum thicknesses of the 5 fields of view in the second resin layer is set as the thickness d2 of the second resin layer.
[0093] (Thickness d1 of the first resin layer and thickness d2 of the second resin layer)
[0094] The thickness d1 of the first resin layer and the thickness d2 of the second resin layer are not particularly limited, but are preferably 2 to 20 μm, more preferably 5 to 15 μm, further preferably 6 to 13 μm, and particularly preferably 7 to 10 μm from the viewpoint of further improving the ease of manufacturability and the thickness accuracy and uniformity of the dimensional change of the metal-clad laminate.
[0095] In addition, only one of the thickness d1 of the first resin layer and the thickness d2 of the second resin layer may be within the above range.
[0096] The method for measuring the thickness d1 of the first resin layer and the thickness d2 of the second resin layer is as described above.
[0097] (Surface waviness (Wa))
[0098] The surface waviness (Wa) of both surfaces of the prepreg (P) used in the present embodiment is 6 μm or less.
[0099] It should be noted that the "surface" of the prepreg (P) of the present embodiment refers to the surface that is overlapped when the prepregs (P) are stacked to produce a metal-clad laminate, or the surface on the opposite side thereof.
[0100] The surface waviness (Wa) of both surfaces of the prepreg (P) used in the present embodiment is preferably 5.5 μm or less, more preferably 5 μm or less, and even more preferably 4 μm or less, from the viewpoint of further improving the thickness accuracy and uniformity of the dimensional change of the metal-clad laminate.
[0101] The surface waviness (Wa) of both surfaces of the prepreg (P) used in the present embodiment is preferably as small as possible, but may be 0.5 μm or more, or 0.8 μm or more, from the viewpoint of easy manufacturability.
[0102] It should be noted that the surface waviness (Wa) of the present embodiment is the arithmetic mean height (Wa) that can be obtained from the waviness curve in accordance with ISO 4287 (1997). The surface waviness (Wa) can be measured by the method described in the examples.
[0103] (Impregnated area and non-impregnated area)
[0104] The prepreg (P) used in the present embodiment preferably has a fiber base material having a region impregnated with the thermosetting resin composition and a region not impregnated with the thermosetting resin composition.
[0105] If the thermosetting resin composition is completely impregnated in the fiber substrate, there is a tendency that the waviness of the fiber substrate is easily exposed on the surface of the prepreg (P). In particular, this tendency becomes significant when the thickness of the fiber substrate is 40 μm or more. On the other hand, by providing an unimpregnated area in the fiber substrate, the waviness of the fiber substrate is not easily exposed on the surface of the prepreg (P), and there is a tendency to easily adjust the surface waviness (Wa) of the prepreg (P) to less than 6 μm. It should be noted that the impregnation area and the unimpregnation area having the above-mentioned thermosetting resin composition in the fiber substrate ultimately refer to the prepreg, that is, the prepreg in the B-stage state, and do not involve the cured product of the prepreg.
[0106] The unimpregnated regions of the prepreg (P) used in the present embodiment are preferably present intermittently, and more preferably present intermittently in the plane direction.
[0107] By making the non-impregnated areas exist intermittently, it is easy to promote the penetration of the thermosetting resin composition into the non-impregnated areas during heating and pressurization when laminating the prepreg (P) and the metal foil, and the generation of tiny voids caused by the non-impregnated areas is suppressed, which tends to improve the insulation reliability.
[0108] Figure 2 2 shows a schematic cross-sectional view of a prepreg 20 as an example of a prepreg (P) in which unimpregnated regions exist intermittently in the surface direction.
[0109] Figure 2 The prepreg 20 shown has a thermosetting resin composition 5 on the front and back surfaces and inside of a fiber base material 1 , and includes a non-impregnated region 6 inside the fiber base material 1 .
[0110] It should be noted that the so-called "surface direction" of the prepreg refers to Figure 2 The direction along the surface of the fiber substrate is represented by X.
[0111] The existence ratio of the impregnation area in the prepreg (P) can be obtained as follows, that is, by observing the surface of the prepreg (P) using an optical microscope, for example, obtaining a surface observation image with a magnification of 50 times, determining the impregnation area and the non-impregnation area in the surface observation image, and thus obtaining it in the form of the area ratio of the impregnation area.
[0112] Specifically, in the observation under the above conditions, in the surface observation image captured at an appropriate brightness, the surface where the unimpregnated area of the thermosetting resin composition exists in the lower part of the observation surface is a void portion and is easy to reflect light, so it appears as a relatively bright area, and the other area, that is, the impregnated area, appears as a relatively dark area.
[0113] The surface observation image is binarized such that a relatively bright area representing a non-impregnated area is one value and a relatively dark area representing an impregnated area is another value. In the resulting binarized image, the area ratio of the impregnated area to the total area can be calculated.
[0114] Here, when capturing the surface observation image, it is preferable to adjust the exposure time for capturing the surface within the range of 60 to 100 ms, thereby capturing the image with appropriate brightness that can fully reflect the impregnated area and the non-impregnated area.
[0115] For the surface observation image of the prepreg (P), in order from strong to weak color, there are "areas where there is no fiber substrate in the resin layer", "areas where the thermosetting resin composition is fully impregnated into the fiber substrate", and "areas where the thermosetting resin composition is insufficiently impregnated into the fiber substrate". In this embodiment, the above-mentioned "areas where there is no fiber substrate in the resin layer" are also included in the impregnation area. If the surface observation image is too bright, not only the parts where the resin is insufficiently impregnated into the fiber substrate are easy to be brightly displayed, but even the parts where the resin is sufficiently impregnated into the fiber substrate are easy to be brightly displayed. In addition, when the image is bright, there is a tendency for the surface observation image after binarization to become brighter as a whole. On the other hand, if the surface observation image is too dark, the surface observation image becomes darker as a whole, and there is a tendency that it is difficult to reflect the existence of the non-impregnated area. Therefore, it is preferred to shoot with moderate brightness. Regarding the observation conditions, from the viewpoint of shooting with moderate brightness, the observation conditions described in detail in the embodiments are adopted.
[0116] An example of processing a surface observation image captured at a moderate brightness using the above method is shown in FIG. Figure 3 middle. Figure 3 This is an image obtained by binarizing the surface observation image of the prepreg produced in Example 1. Figure 3 In the image, it can be observed that impregnated areas (black) and non-impregnated areas (white) exist alternately in the surface direction. The exposure time when taking this surface observation image is 85 ms.
[0117] The abundance ratio of the impregnation region measured by the above method is not particularly limited, but is preferably 30 to 99%, more preferably 50 to 98%, and even more preferably 60 to 97%.
[0118] If the existence ratio of the impregnation region is greater than the above lower limit, the thickness accuracy and uniformity of the dimensional change of the metal-clad laminate tend to be further improved. In addition, if the existence ratio of the impregnation region is less than the above upper limit, the powder particles of the prepreg (P) are suppressed from falling off, and the handling property tends to be further improved.
[0119] (Fiber base material)
[0120] The fiber base material contained in the prepreg (P) used in the present embodiment is not particularly limited as long as it has a thickness of 40 μm or more.
[0121] The thickness of the fiber substrate can be appropriately adjusted in accordance with the desired thickness of the metal-clad laminate within a range of 40 μm or more, and is not particularly limited. However, from the viewpoint of further improving the thickness accuracy and uniformity of the dimensional change of the metal-clad laminate, and the productivity and operability of the prepreg (P), it is preferably 40 to 120 μm, more preferably 45 to 110 μm, more preferably 50 to 105 μm, further preferably 55 to 100 μm, further preferably 60 μm or more and less than 100 μm, further preferably 70 to 97 μm, and particularly preferably 80 to 95 μm. If the thickness of the fiber substrate is below the above upper limit, the impregnation of the fiber substrate with the thermosetting resin composition is improved, and there is a tendency that the heat resistance and insulation reliability of the cured product of the prepreg (P) are easily improved.
[0122] In the production method of the present embodiment, when a plurality of prepregs are stacked, the thicknesses of the fiber base materials contained in the respective prepregs may be the same as or different from each other.
[0123] The thickness of the fiber base material can be determined as an average value obtained by measuring five arbitrary locations of the fiber base material using a micrometer.
[0124] As the material of the fiber substrate, for example, natural fibers such as paper and cotton linters; inorganic fibers such as glass fibers and asbestos; organic fibers such as aramid, polyimide, polyvinyl alcohol, polyester, tetrafluoroethylene, acrylic fibers; mixtures thereof, etc. Among them, inorganic fibers are preferred, and glass fibers are more preferred from the viewpoint of flame retardancy.
[0125] Examples of the glass fiber include glass fibers made of E glass, C glass, D glass, S glass, and the like.
[0126] The material of the fiber base material may be one kind alone or two or more kinds may be combined.
[0127] Examples of the shape of the fiber substrate include woven fabric, nonwoven fabric, roving, chopped strand mat, and surface mat. Among these, woven fabric is preferred.
[0128] Among the above options, glass cloth is preferred as the fiber base material from the viewpoints of low thermal expansion, flame retardancy, versatility, and the like.
[0129] The fiber substrate may be a fiber substrate consisting of one layer or a fiber substrate consisting of multiple layers. In the case of a fiber substrate consisting of multiple layers, at least one layer contains a fiber substrate having a thickness of 40 μm or more. It should be noted that the so-called fiber substrate consisting of one layer means a fiber substrate consisting only of entangled fibers. In the case of a fiber substrate without entanglement, it is classified as a fiber substrate consisting of multiple layers. The material and shape of the fiber substrates of two or more layers may be the same or different.
[0130] The surface waviness (Wa) of the fiber substrate is not particularly limited, but may be greater than 6 μm and less than 40 μm, 6.5 to 35 μm, 7 to 30 μm, 10 to 25 μm, or 15 to 23 μm.
[0131] According to the manufacturing method of this embodiment, even if the surface waviness (Wa) of the fiber substrate is within the above range, a metal-clad laminate having excellent thickness accuracy and uniformity of dimensional change can be obtained by adjusting the surface waviness (Wa) of the prepreg (P) to a given range.
[0132] (Thermosetting resin composition)
[0133] The thermosetting resin composition is contained in the first resin layer and the second resin layer in the prepreg (P) used in the present embodiment, and can also be impregnated into at least a part of the fiber base material.
[0134] The thermosetting resin composition contained in the prepreg (P) used in the present embodiment contains at least a thermosetting resin.
[0135] The thermosetting resin composition preferably contains, in addition to the thermosetting resin, at least one selected from, for example, a curing agent, a curing accelerator, an inorganic filler, an organic filler, a coupling agent, a leveling agent, an antioxidant, a flame retardant, a flame retardant aid, a thixotropy imparting agent, a thickener, a flexible material, a surfactant and a photopolymerization initiator as needed.
[0136] Hereinafter, each component which the thermosetting resin composition may contain will be described.
[0137] In addition, each component may be used individually by 1 type, or may use 2 or more types together.
[0138] (Thermosetting resin)
[0139] Examples of thermosetting resins include epoxy resins, polyimide resins, maleimide resins, modified maleimide resins, phenolic resins, polyphenylene ether resins, bismaleimide triazine resins, cyanate resins, isocyanate resins, benzoxazine resins, oxetane resins, amino resins, unsaturated polyester resins, allyl resins, dicyclopentadiene resins, silicone resins, triazine resins, and melamine resins.
[0140] Among them, epoxy resins, polyimide resins, maleimide resins, modified maleimide resins, cyanate resins, polyphenylene ether resins, and bismaleimide triazine resins are preferred from the viewpoints of moldability and electrical insulation, and epoxy resins, maleimide resins, and modified maleimide resins are more preferred.
[0141] As the epoxy resin, an epoxy resin having two or more epoxy groups in one molecule is preferred. Here, the epoxy resin can be classified into a glycidyl ether type epoxy resin, a glycidyl amine type epoxy resin, a glycidyl ester type epoxy resin, etc. Among them, a glycidyl ether type epoxy resin is preferred.
[0142] Epoxy resins can also be classified into various epoxy resins according to the difference of the main skeleton. For example, among the above-mentioned various types of epoxy resins, they can be further classified into bisphenol epoxy resins; alicyclic epoxy resins; aliphatic chain epoxy resins; novolac epoxy resins; stilbene epoxy resins; naphthalene skeleton-containing epoxy resins; biphenyl epoxy resins; xylylene epoxy resins; dihydroanthracene epoxy resins, etc. Among them, phenol novolac epoxy resins and naphthalene skeleton-containing epoxy resins are preferred.
[0143] The maleimide resin is preferably a maleimide resin having one or more N-substituted maleimide groups, and more preferably a maleimide resin having two or more N-substituted maleimide groups.
[0144] The maleimide resin is preferably an aromatic maleimide resin having an N-substituted maleimide group directly bonded to an aromatic ring.
[0145] Examples of maleimide resins include bis(4-maleimidephenyl)methane, bis(4-maleimidephenyl)ether, bis(4-maleimidephenyl)sulfone, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethanebismaleimide, 4-methyl-1,3-phenylenebismaleimide, m-phenylenebismaleimide, 2,2-bis[4-(4-maleimidephenoxy)phenyl]propane, and the like. Aromatic bismaleimide resins having bonded N-substituted maleimide groups; aromatic polymaleimide resins having three or more N-substituted maleimide groups directly bonded to aromatic rings, such as polyphenylmethane maleimide and biphenyl aralkyl maleimide; maleimide resins having an indane ring skeleton; aliphatic maleimide resins such as 1,6-bismaleimide-(2,2,4-trimethyl)hexane and pyrophosphate binder type long-chain alkyl bismaleimide, etc.
[0146] Examples of the modified maleimide resin include aminomaleimide resins having a structural unit derived from a maleimide resin and a structural unit derived from a diamine compound.
[0147] As the diamine compound, a compound having two primary amino groups is preferred.
[0148] Moreover, as a diamine compound, the aromatic diamine compound which has two primary amino groups directly bonded to an aromatic ring is preferable.
[0149] Examples of the diamine compound include aromatic diamines having two primary amino groups directly bonded to an aromatic ring, such as m-phenylenediamine, p-phenylenediamine, 1,4-bis(4-aminophenoxy)benzene, 4,4'-diaminodiphenylmethane, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-diethyl-4,4'-diaminodiphenylmethane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-diaminobenzophenone, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, bis[4-(4-aminophenoxy)phenyl] sulfone, benzidine, 4,4'-bis(4-aminophenoxy)biphenyl, 4,4'-diaminodiphenyl sulfide, and 4,4'-diamino-3,3'-biphenol; and silicone compounds having two primary amino groups.
[0150] The aminomaleimide resin can be synthesized by subjecting a maleimide resin and a diamine compound to Michael addition reaction using a known method.
[0151] The equivalent ratio (Ta2 / Ta1) of the total equivalent weight (Ta2) of the groups derived from the -NH2 groups of the diamine compounds in the aminomaleimide resin to the total equivalent weight (Ta1) of the groups derived from the N-substituted maleimide groups of the maleimide resin is not particularly limited, but from the viewpoint of dielectric properties, heat resistance, flame retardancy and glass transition temperature, it is preferably 0.05 to 10, more preferably 1 to 8, and further preferably 3 to 7. It should be noted that the groups derived from the -NH2 groups of the above-mentioned diamine compounds also include -NH2 itself. In addition, the groups derived from the N-substituted maleimide groups of the above-mentioned maleimide resin also include the N-substituted maleimide groups themselves.
[0152] The content of the thermosetting resin in the thermosetting resin composition is not particularly limited, but from the viewpoint of heat resistance, formability, processability and conductor adhesion, it is preferably 10 to 70% by mass, more preferably 15 to 50% by mass, and further preferably 20 to 40% by mass relative to the total solid content (100% by mass) of the thermosetting resin composition.
[0153] 〔Curing agent〕
[0154] Examples of the curing agent include phenolic curing agents, cyanate curing agents, acid anhydride curing agents, amine curing agents, compounds containing active ester groups, etc. Among them, when epoxy resin is used as the thermosetting resin, a phenolic curing agent is preferred as the curing agent.
[0155] Preferred examples of the phenolic curing agent include cresol novolac-type phenolic resins, biphenyl aralkyl-type phenolic resins, phenol novolac-type phenolic resins, naphthylene ether-type phenolic resins, and triazine skeleton-containing phenolic resins.
[0156] When the thermosetting resin composition contains a curing agent, the content thereof is not particularly limited, but is preferably 20 to 200 parts by mass, more preferably 25 to 150 parts by mass, and even more preferably 30 to 100 parts by mass, relative to 100 parts by mass of the thermosetting resin, from the viewpoint of obtaining good curability.
[0157] When the thermosetting resin composition contains a curing agent, the equivalent ratio of the functional group of the thermosetting resin to the functional group of the curing agent [functional group of the thermosetting resin / functional group of the curing agent] is not particularly limited, but is preferably 0.8 to 1.2 when the functional group of the curing agent is a phenolic hydroxyl group, preferably 0.2 to 0.4 when it is an amino group, and preferably 0.3 to 0.6 when it is an active ester group.
[0158] 〔Curing accelerator〕
[0159] Examples of the curing accelerator include imidazole compounds, imidazole compound derivatives, and other imidazole-based curing accelerators; phosphorus-based compounds; tertiary amine compounds; quaternary ammonium compounds, etc. Among them, imidazole-based curing accelerators are preferred from the viewpoint of obtaining a sufficient curing acceleration effect.
[0160] Examples of the imidazole compound include imidazole compounds such as 2-methylimidazole, 2-ethylimidazole, 2-undecylimidazole, 2-phenylimidazole, 1,2-dimethylimidazole, and 2,4-diamino-6-[2'-methylimidazolyl-(1')]ethyl-s-triazine.
[0161] Examples of the derivatives of the imidazole compound include salts of an imidazole compound and trimellitic acid such as 1-cyanoethyl-2-phenylimidazolium trimellitic acid; salts of an imidazole compound and isocyanuric acid; and salts of an imidazole compound and hydrobromic acid.
[0162] When the thermosetting resin composition contains a curing accelerator, the content thereof is not particularly limited, but is preferably 0.01 to 20 parts by mass, more preferably 0.1 to 10 parts by mass, and further preferably 0.4 to 2 parts by mass, relative to 100 parts by mass of the thermosetting resin, from the viewpoint of the curing acceleration effect and storage stability.
[0163] 〔Inorganic filler materials〕
[0164] As inorganic fillers, for example, silica, alumina, titanium oxide, mica, beryllium oxide, barium titanate, potassium titanate, strontium titanate, calcium titanate, aluminum carbonate, magnesium hydroxide, aluminum hydroxide, aluminum silicate, calcium carbonate, calcium silicate, magnesium silicate, silicon nitride, boron nitride, clay, talc, aluminum borate, silicon carbide, etc. Among them, silica and alumina are preferred from the viewpoint of reducing the coefficient of thermal expansion, the relative dielectric constant and the dielectric loss tangent, and silica and aluminum hydroxide are preferred from the viewpoint of heat resistance.
[0165] The inorganic filler may be surface-treated with a surface treatment agent such as a silane coupling agent.
[0166] When the thermosetting resin composition contains an inorganic filler, the content thereof on a mass basis is not particularly limited, but is preferably 10 to 80 mass %, more preferably 20 to 75 mass %, further preferably 40 to 70 mass %, and particularly preferably 45 to 65 mass %, relative to the total solid content (100 mass %) of the thermosetting resin composition.
[0167] When the content of the inorganic filler is above the lower limit, low thermal expansion and heat resistance tend to be improved. When the content of the inorganic filler is below the upper limit, formability and conductor adhesion tend to be improved.
[0168] (Thickness of prepreg (P))
[0169] The thickness of the prepreg (P) used in the present embodiment is not particularly limited and can be appropriately adjusted according to the thickness of the fiber substrate used and the desired thickness of the metal-clad laminate. For example, from the perspective of the thickness accuracy and uniformity of the dimensional change of the metal-clad laminate and the productivity and operability of the prepreg (P), the thickness is preferably 50 to 160 μm, more preferably 70 to 140 μm, further preferably 80 to 125 μm, and particularly preferably 90 to 100 μm.
[0170] It should be noted that in the present embodiment, the thickness of the prepreg refers to the thickness of one sheet of prepreg.
[0171] In the present embodiment, the thickness of the prepreg can be determined by measuring five arbitrary points of the prepreg using a digital indicator and averaging the measured values.
[0172] (Method for producing prepreg (P))
[0173] The method for producing the prepreg (P) used in the present embodiment may be, for example, a method of laminating a film-like thermosetting resin composition (hereinafter also referred to as "resin film") on both sides of a fiber substrate having a thickness of 40 μm or more (hereinafter also referred to as "lamination method"), or a method of impregnating a fiber substrate having a thickness of 40 μm or more in a thermosetting resin composition diluted with an organic solvent (hereinafter also referred to as "resin varnish") and drying it (hereinafter also referred to as "immersion method"). Among them, from the viewpoint of facilitating the adjustment of the ratio R of the above-mentioned thickness difference to -9.0% to +9.0% and facilitating the adjustment of the surface waviness (Wa) to 6 μm or less, it is preferred to produce the prepreg (P) used in the present embodiment by laminating a film-like thermosetting resin composition on both sides of a fiber substrate having a thickness of 40 μm or more.
[0174] [Lamination method]
[0175] The resin film used in the lamination method can be produced by, for example, a method in which a resin varnish is applied on the surface of a support and then dried.
[0176] The resin varnish can be prepared by, for example, adding a thermosetting resin and other components used as necessary to an organic solvent, and then mixing and stirring the mixture using a known mixer.
[0177] Examples of the organic solvent used in the resin varnish include alcohol solvents such as methanol, ethanol, methyl cellosolve, butyl cellosolve, and propylene glycol monomethyl ether; ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, methyl ethyl ketone, cyclohexanone, and 4-methyl-2-pentanone; ester solvents such as ethyl acetate, butyl acetate, propylene glycol monomethyl ether acetate, and γ-butyrolactone; ether solvents such as tetrahydrofuran; aromatic solvents such as toluene, xylene, and mesitylene; nitrogen atom-containing solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methylpyrrolidone; sulfur atom-containing solvents such as dimethyl sulfoxide, and the like.
[0178] The solid content concentration of the resin varnish is not particularly limited, but is preferably 20 to 85% by mass, more preferably 40 to 80% by mass, and even more preferably 50 to 70% by mass.
[0179] Examples of the method for applying the resin varnish include a method using a known coating apparatus such as a comma-type knife coater, a bar coater, a kiss coater, a roll coater, a gravure coater, and a die coater.
[0180] The drying temperature and drying time after applying the resin varnish may be determined according to the type and amount of the organic solvent. For example, in the case of a resin varnish containing 30 to 70% by mass of an organic solvent, a resin film can be suitably formed by drying at 50 to 160° C. for 1 to 8 minutes.
[0181] Examples of the support include organic films such as polyethylene terephthalate (PET), biaxially oriented polypropylene (OPP), polyethylene, polyvinyl fluoride, and polyimide; and metal foils of metals such as copper and aluminum or alloys. The support may also be a release film whose surface has been subjected to a release agent.
[0182] The thickness of the resin film is not particularly limited and may be appropriately determined depending on the thickness of the fiber substrate, the desired thickness of the prepreg (P), etc. However, it is preferably 10 to 100 μm, more preferably 15 to 70 μm, and further preferably 18 to 50 μm.
[0183] It should be noted that the thickness of the resin film is set to the following value, that is, the total thickness of any five locations of the resin film with a support is measured, the thickness of the single support is measured after the resin film at the measured location is peeled off with an adhesive tape, and the thickness of the single support is subtracted from the total thickness, and the average value of the obtained values is set. A digital indicator can be used for the measurement of the thickness.
[0184] Next, a method of laminating resin films on both surfaces of a fiber base material will be described.
[0185] First, two resin films with supports are prepared and arranged on both sides of the fiber substrate so that the resin films are in contact with the fiber substrate. Then, the arranged resin films with supports are laminated on the fiber substrate, thereby impregnating the fiber substrate with the resin films.
[0186] When the prepreg (P) is produced by a lamination method, the ratio R of the thickness difference can be adjusted to -9.0% to +9.0% by reducing the difference in thickness between the resin film laminated on one side of the fiber substrate and the resin film laminated on the other side of the fiber substrate, for example. The absolute value of the difference in thickness between the resin film laminated on one side of the fiber substrate and the resin film laminated on the other side of the fiber substrate is not particularly limited, but is preferably 2.5 μm or less, more preferably 1.5 μm or less, and further preferably 0.5 μm or less.
[0187] The lamination method is not particularly limited, and for example, roll lamination or pressure lamination using a hot plate may be used.
[0188] The heating temperature during lamination is not particularly limited, but is preferably 50 to 180°C, more preferably 100 to 170°C, and further preferably 120 to 165°C from the viewpoint of easily adjusting the ratio R of the thickness difference of the prepreg (P) and the surface waviness (Wa) to the above ranges.
[0189] The pressurizing pressure during lamination is not particularly limited, but is preferably 0.05 to 1.5 MPa, more preferably 0.1 to 1.3 MPa, and even more preferably 0.3 to 1.2 MPa from the viewpoint of easily adjusting the ratio R of the thickness difference of the prepreg (P) and the surface waviness (Wa) to the above range.
[0190] Lamination can be carried out under reduced pressure. The vacuum degree in this case is not particularly limited. However, from the viewpoint of easily adjusting the ratio R of the thickness difference of the prepreg (P) and the surface waviness (Wa) to the above range, it is preferably 200 kPa or less, more preferably 150 kPa or less, and further preferably 120 kPa or less.
[0191] In the lamination method, as a method for discontinuously providing the unimpregnated regions in the fiber base material, for example, there is a method of adjusting the heating and pressurizing conditions when laminating the resin film with a support and the fiber base material.
[0192] Here, when the same lamination conditions are set when the fiber substrate is thin and when the fiber substrate is thick, there is a tendency that the resin film is not easily impregnated into the fiber substrate when the fiber substrate is thick. Therefore, even if the conditions for laminating a resin film on a thin fiber substrate in the past are the same as the lamination conditions of this embodiment, in this embodiment, it is possible to discontinuously provide a region not impregnated with the thermosetting resin composition in the fiber substrate.
[0193] As a specific method for adjusting the conditions for heating and pressurizing, for example, the following method can be cited. Initially, after a prepreg is produced under given heating and pressurizing conditions, the existence ratio of the impregnation area of the thermosetting resin composition in the fiber substrate based on the above calculation method is calculated. As a result, when the impregnation area is 100%, that is, when there is no unimpregnated area, the heating temperature or the pressurizing pressure is reduced, or both the heating temperature and the pressurizing pressure are reduced, and the prepreg is re-produced, and the existence ratio of the impregnation area is calculated again. The above operation is further repeated as needed, thereby making it easy to grasp the conditions for manufacturing a prepreg with an unimpregnated area.
[0194] In addition, if the existence ratio of the unimpregnated area is desired to be reduced, the prepreg can be remade by increasing the heating temperature or the pressing pressure, or by increasing both the heating temperature and the pressing pressure. The above operation can extract the conditions under which the waviness of the fiber base material is not easily revealed on the surface of the prepreg, and the surface waviness (Wa) of the prepreg can be adjusted to 6 μm or less.
[0195] After the fiber base material is impregnated with the resin film, the support is peeled off from the obtained prepreg (P) with a support, if necessary, to obtain the prepreg (P).
[0196] [Immersion method]
[0197] Examples of the resin varnish used in the impregnation method include the same resin varnish as that used in the production of the resin film in the above-mentioned lamination method.
[0198] The drying temperature and drying time after the fiber base material is immersed in the resin varnish are not particularly limited and may be appropriately determined in consideration of the type of organic solvent and the like.
[0199] <Metal Foil>
[0200] As the metal type of the metal foil used in the manufacturing method of this embodiment, for example, copper, gold, silver, nickel, platinum, molybdenum, ruthenium, aluminum, tungsten, iron, titanium, chromium, alloys containing one or more of these metal elements, etc. can be cited. As the alloy, for example, copper alloys, aluminum alloys, iron alloys, etc. can be cited. As the copper alloy, for example, copper-nickel alloys, etc. can be cited. As the iron alloy, for example, iron-nickel alloys, etc. can be cited.
[0201] Among them, copper, nickel, aluminum, and iron-nickel alloys are preferred from the viewpoint of conductivity and availability, copper and aluminum are more preferred, and copper is further preferred. It should be noted that when copper foil is used as the metal foil, the resulting metal-clad laminate is sometimes referred to as a copper-clad laminate.
[0202] The thickness of the metal foil is not particularly limited, but is preferably 1 to 200 μm, more preferably 2 to 100 μm, and further preferably 3 to 50 μm.
[0203] The number of metal foils used in the production method of the present embodiment is not particularly limited, and may be one, but is preferably two.
[0204] In the metal-clad laminate obtained by the production method of the present embodiment, the metal foil is preferably arranged on at least one surface of the metal-clad laminate, and more preferably arranged on both surfaces of the metal-clad laminate.
[0205] <Prepreg and Metal Foil Lamination Method>
[0206] The metal-clad laminate can be produced by placing a metal foil on one or both surfaces of a prepreg and then heating and pressing it.
[0207] When heating and pressurizing, only one prepreg may be used, or two or more prepregs may be used in a stacked manner, but at least one prepreg (P) is used. When two or more prepregs are used, preferably all prepregs are prepregs (P).
[0208] When two or more prepregs are used, the total number of prepregs may be, for example, 2 to 20, 5 to 18, or 8 to 16.
[0209] In addition, the method for producing a metal-clad laminate having metal foils on both surfaces is preferably the production method described in the section [Metal-clad laminate] to be described later.
[0210] Alternatively, the substrate on which the inner layer circuit has been processed may be heat-pressed in addition to the prepreg and the metal foil.
[0211] Heating and pressurizing can be performed using, for example, a multistage press, a multistage vacuum press, a continuous molding machine, an autoclave molding machine, or the like.
[0212] The heating temperature during heating and pressurization is not particularly limited, but is preferably 100 to 300°C, more preferably 150 to 260°C, and further preferably 170 to 230°C.
[0213] The heating and pressing time during heating and pressing is not particularly limited, but is preferably 10 to 300 minutes, more preferably 30 to 200 minutes, and even more preferably 60 to 150 minutes.
[0214] The pressure during heating and pressurization is not particularly limited, but is preferably 1.0 to 6 MPa, more preferably 1.5 to 3 MPa, and even more preferably 1.8 to 2.5 MPa.
[0215] Heating and pressurizing may be a method of increasing the temperature while applying pressure. In this case, the maximum temperature is within the above-mentioned range of appropriate heating temperatures, and the holding time at the maximum temperature is preferably within the above-mentioned range of appropriate heating and pressurizing time.
[0216] The temperature increase rate when increasing the temperature while applying pressure is not particularly limited, but is preferably 1 to 10° C. / min, more preferably 2 to 5° C. / min.
[0217] The pressurization period when the temperature is increased while pressurizing is not particularly limited, but the temperature may be increased after starting pressurization at room temperature.
[0218] The thickness of the metal-clad laminate produced by the production method of the present embodiment is not particularly limited, but may be 400 to 2500 μm, 450 to 2000 μm, 500 to 1800 μm, or 550 to 1600 μm.
[0219] The thickness of the metal-clad laminate can be determined by using the T ave The determination method is used to determine the
[0220] As described above, according to the manufacturing method of this embodiment, a metal-clad laminate having excellent thickness accuracy can be manufactured. Therefore, in the manufacturing method of this embodiment, the smoothing treatment performed on the cured prepreg in order to improve the thickness accuracy of the metal-clad laminate can be omitted. As the smoothing treatment, for example, a method of pressing the cured prepreg with a roller, a method of grinding the surface of the cured prepreg, etc.
[0221] In the case where the metal-clad laminate produced by the production method of the present embodiment and the metal-clad laminate of the present embodiment described later contain a plurality of fiber substrates, from the viewpoint of productivity, the thickness of the fiber substrate located outermost on at least one surface side of the metal-clad laminate may be in the range of 0.6 to 1.3 times the thickness of the fiber substrate adjacent to the fiber substrate, or in the range of 0.7 to 1.3 times, or in the range of 0.8 to 1.2 times, or in the range of 0.9 to 1.1 times. It is preferred that the thickness of the fiber substrate located outermost on both surface sides of the metal-clad laminate is in the above range relative to the thickness of the adjacent fiber substrate.
[0222] [Manufacturing method of printed wiring board]
[0223] The method for manufacturing a printed circuit board of the present embodiment is a method for manufacturing a metal-clad laminated plate using the method for manufacturing a metal-clad laminated plate of the present embodiment, and forming a wiring pattern on the metal-clad laminated plate. The wiring pattern can be formed using a known method. In addition, as needed, etching, hole processing, metal plating processing, etc. of the metal foil can be appropriately implemented using a known method.
[0224] [Method for manufacturing semiconductor package]
[0225] The method for manufacturing a semiconductor package of the present embodiment is a method for manufacturing a semiconductor package that manufactures a printed wiring board using the method for manufacturing a printed wiring board of the present embodiment and mounts a semiconductor element on the printed wiring board.
[0226] The method of mounting the semiconductor element is not particularly limited, and a conventionally known method may be applied. Specifically, for example, the electrodes of the printed circuit board are temporarily fixed after being aligned with the bump positions of the semiconductor chip, and the semiconductor chip is bonded to the printed circuit board by applying a reflow process, a TCB (thermal compression bonding) process, etc.
[0227] Thereafter, the gap between the printed wiring board and the semiconductor chip can be sealed using a liquid sealing material. In addition, a portion or the entire surface of the semiconductor chip can also be sealed using a semiconductor sealing material. The liquid sealing material and the semiconductor sealing material can use conventionally known materials.
[0228] [Metal-clad laminate]
[0229] The metal-clad laminate of the present embodiment comprises a cured product of a thermosetting resin composition, one or more fiber base materials, and a metal foil.
[0230] The thickness of the fiber substrate is 40 μm or more.
[0231] The value determined by the following method is 0.5% or less.
[0232] (method)
[0233] The surface of the metal-clad laminate was divided into grids at intervals of 50 mm in both the longitudinal and transverse directions. Figure 4 At the positions shown in the plan view of the metal-clad laminate 30, 21 measurement unit areas 7 having a square shape of 50 mm in length and 50 mm in width in plan view are set.
[0234] In the measurement unit area 7, a point located inside the measurement unit area 7 and spaced 10 mm from the longitudinal and transverse sides, i.e. Figure 4 The thickness is measured at the positions of the four thickness measurement points 8 shown, the difference between the maximum and minimum thickness values at the four points is defined as the thickness difference V1 within the measurement unit area 7, and the average value of the thickness at the four points is defined as T1.
[0235] V1 and T1 are calculated for the 21 measurement unit areas 7, and the average value V ave and the average value of T1 ave, use the following formula to calculate the value.
[0236] V ave ×100 / T aVe
[0237] More specifically, it can be measured by the method described in the Examples.
[0238] Regarding the semiconductor package using the metal-clad laminate of the present embodiment, the reason why the variation in the warpage amount of the semiconductor package is small is not certain, but it can be estimated as follows.
[0239] The metal-clad laminate of the present embodiment has an excellent thickness accuracy of 0.5% or less as determined by the above method, and this is presumed to be one reason why the amount of thermal expansion of a substrate included in a semiconductor package manufactured using the metal-clad laminate is uniform among products.
[0240] The metal-clad laminate of this embodiment has metal foil on both sides and has:
[0241] A first resin cured product layer, which is provided on a surface of the fiber base material, contacts the metal foil on one surface of the metal-clad laminate, and contains a cured product of a thermosetting resin composition; and
[0242] a second resin cured product layer provided on a surface of the fiber base material, in contact with the metal foil on the other surface of the metal-clad laminate, and containing a cured product of a thermosetting resin composition;
[0243] When the thickness of the first cured resin layer is d'1 and the thickness of the second cured resin layer is d'2,
[0244] The ratio R' of the thickness difference represented by the following formula (1') is preferably -9.0% to +9.0%.
[0245] R'=(d'1-d'2)×100 / (d'1+d'2)(1')
[0246] Regarding the ratio R' of the thickness difference represented by the above general formula (1'), from the viewpoint of further improving the thickness accuracy and uniformity of the dimensional change of the metal-clad laminate, it is preferably -8.0% to +8.0%, more preferably -7.0% to +7.0%, further preferably -6.0% to +6.0%, and particularly preferably -5.0% to +5.0%.
[0247] In addition, more detailed measurement conditions of the thickness difference ratio R' can be set to the conditions described in the Examples.
[0248] The cured product of the thermosetting resin composition contained in the first cured resin layer and the cured product of the thermosetting resin composition contained in the second cured resin layer may be the same or different, but are preferably the same.
[0249] In addition, when the cured product of the thermosetting resin composition contained in the first resin cured product layer is the same as the cured product of the thermosetting resin composition contained in the second resin cured product layer, the cured products of these thermosetting resin compositions and the cured product of the thermosetting resin composition contained in the fiber base material may be the same or different, but are preferably the same.
[0250] It is preferred that the first cured resin layer and the second cured resin layer do not contain a fiber base material.
[0251] The metal-clad laminate of the present embodiment is preferably manufactured using the manufacturing method described in the above-mentioned [Method for manufacturing metal-clad laminate]. That is, the metal-clad laminate of the present embodiment is preferably manufactured using a prepreg (P). Therefore, the suitable manner of the cured product of the thermosetting resin composition and the fiber substrate possessed by the metal-clad laminate of the present embodiment is the same as the suitable manner of the cured product of the thermosetting resin composition contained in the prepreg (P) and the fiber substrate contained in the prepreg (P). The suitable manner of the stacking structure of each component when manufacturing the metal-clad laminate using the prepreg (P), the manufacturing conditions, etc. is also as described in the above-mentioned [Method for manufacturing metal-clad laminate].
[0252] In the case of manufacturing a metal-clad laminate having metal foil on both sides, from the viewpoint of the thickness accuracy of the metal-clad laminate, when the metal foil and the prepreg are heated and pressurized, the prepreg preferably in contact with the metal foil of one face and the prepreg in contact with the metal foil of another face are both prepregs (P). Thus, the first resin cured product layer and the second resin cured product layer possessed by the metal-clad laminate become layers of cured products comprising the first resin layer or the second resin layer possessed by the prepreg (P). As a method of making the prepreg in contact with the metal foil of one face and the prepreg in contact with the metal foil of another face both be prepregs (P), for example, it can be a method of laminating metal foils on both sides of 1 prepreg (P). In addition, when using a plurality of prepregs including two or more prepregs (P), the plurality of prepregs may be stacked in such a manner that one prepreg (P) is exposed on one surface and another prepreg (P) is exposed on the other surface, and a metal foil is laminated on the prepreg (P) exposed on one surface and another metal foil is laminated on the prepreg (P) exposed on the other surface.
[0253] The thickness of the metal-clad laminate of the present embodiment may be 400 to 2500 μm, 450 to 2000 μm, 500 to 1800 μm, or 550 to 1600 μm.
[0254] The method for measuring the thickness of the metal-clad laminate is as described above.
[0255] [Printed circuit board]
[0256] The printed wiring board of this embodiment is a printed wiring board having the metal-clad laminate of this embodiment. The printed wiring board of this embodiment can be manufactured by the method described in the above [Manufacturing method of printed wiring board] using the metal-clad laminate of this embodiment as the metal-clad laminate.
[0257] [Semiconductor packaging]
[0258] The semiconductor package of this embodiment is a semiconductor package having the printed wiring board of this embodiment and a semiconductor element. The semiconductor package of this embodiment can be manufactured by the method described in the above [Method for Manufacturing Semiconductor Package] using the printed wiring board of this embodiment as a printed wiring board.
[0259] Example
[0260] Hereinafter, the present embodiment will be further described in detail using the following examples, however, these examples do not limit the present embodiment.
[0261] [Method for measuring the thickness d1 of the first resin layer, the thickness d2 of the second resin layer, and the ratio R of the thickness difference of the prepreg]
[0262] (1) Preparation of test pieces
[0263] The prepregs prepared in the examples and comparative examples were heat treated in air at 170°C for 1 hour and then at 200°C for 1 hour. The prepregs after the heat treatment were injection molded with epoxy resin, polished using a polisher (manufactured by RefineTech Co., Ltd., trade name "Refine Polisher"), and the cross-sections were cut out to obtain test pieces.
[0264] (2) Measurement of the thickness d1 of the first resin layer and the thickness d2 of the second resin layer
[0265] The cross section of the test piece obtained in (1) is observed using a metal microscope at any magnification of 20 to 200 times to obtain a cross-sectional image. In the obtained cross-sectional image, the fiber substrate, the first resin layer and the second resin layer having a thickness of 40 μm or more are determined, and the minimum thickness of the first resin layer and the minimum thickness of the second resin layer in the field of view are respectively measured. The minimum thickness is measured in any 5 fields of view in which the area does not overlap, and the minimum thicknesses of the 5 fields of view in the first resin layer are all averaged, and the obtained value is set as the thickness d1 of the first resin layer. The minimum thicknesses of the 5 fields of view in the second resin layer are all averaged, and the obtained value is set as the thickness d2 of the second resin layer.
[0266] From the thickness d1 of the first resin layer and the thickness d2 of the second resin layer obtained above, the ratio R of the thickness difference was calculated based on the following formula (1).
[0267] R=(d1-d2)×100 / (d1+d2) (1)
[0268] [Method for measuring the thickness d'1 of the first cured resin layer, the thickness d'2 of the second cured resin layer, and the ratio R' of the thickness difference of the metal-clad laminate]
[0269] (1) Preparation of test pieces
[0270] The metal-clad laminates produced in Examples and Comparative Examples were polished using a polisher (manufactured by RefineTech Co., Ltd., trade name "Refine Polisher"), and cross sections were cut out to obtain laminates as test pieces.
[0271] (2) Measurement of the Thickness d′1 of the First Resin Cured Material Layer and the Thickness d′2 of the Second Resin Cured Material Layer
[0272] The cross section of the test piece obtained in the above (1) was observed using a metal microscope at any magnification of 20 to 200 times to obtain a cross-sectional image.
[0273] In the obtained cross-sectional image, a first resin cured material layer provided on the surface of the fiber substrate and in contact with the metal foil (copper foil) on one surface of the metal-clad laminate, and a second resin cured material layer provided on the surface of the fiber substrate and in contact with the metal foil (copper foil) on the other surface of the metal-clad laminate are determined, and the minimum thickness of the first resin cured material layer and the minimum thickness of the second resin cured material layer are respectively measured. The minimum thickness is measured in any five fields of view in which the regions do not overlap, and the minimum thicknesses of the five fields of view in the first resin cured material layer are all averaged, and the obtained value is set as the thickness d'1 of the first resin cured material layer, and the minimum thicknesses of the five fields of view in the second resin cured material layer are all averaged, and the obtained value is set as the thickness d'2 of the second resin cured material layer.
[0274] From the thickness d'1 of the first resin cured material layer and the thickness d'2 of the second resin cured material layer obtained above, the ratio R' of the thickness difference was calculated based on the following formula (1').
[0275] R'=(d'1-d'2)×100 / (d'1+d'2) (1')
[0276] [Measurement method of surface waviness (Wa)]
[0277] The prepregs prepared in the examples and comparative examples were used as measurement objects, and the shape was measured by automatic measurement using a shape analysis laser microscope (manufactured by Keyence Co., Ltd., trade name "VK-X100") using an observation application, and a waviness curve in accordance with ISO 4287 (1997) was obtained. The obtained waviness curve was subjected to surface roughness analysis using an analysis application, and the surface waviness (Wa) was calculated.
[0278] Here, the waviness curve is a curve obtained by applying a phase compensation type high-pass filter λc (λc=80 μm) to the cross-sectional curve and removing wavelengths shorter than 80 μm from the cross-sectional curve. The analysis range is 1000 μm×1000 μm.
[0279] In addition, the surface waviness (Wa) was measured on both sides of the prepreg, and the larger value was described in Table 1.
[0280] [Method for measuring the existence ratio of the impregnation region]
[0281] The existence ratio of the impregnation region was measured by the following method.
[0282] (1) Acquisition of surface observation images
[0283] The surface of the prepreg was observed under the following conditions using an optical microscope (manufactured by Olympus Corporation, trade name: MX61L-F) to obtain a surface observation image.
[0284] <Observation conditions>
[0285] ■ Magnification: 50 times
[0286] ■Observation mode: dark field
[0287] ■Sensitivity: ISO400
[0288] ■Exposure time when shooting the surface: 60 to 100 ms
[0289] ■Brightness of the observation environment: Two 35W fluorescent lamps were installed 2m above the observation platform.
[0290] It should be noted that the exposure time was adjusted between 60 and 100 ms so as to achieve appropriate brightness that can fully reflect the impregnated area and the non-impregnated area.
[0291] (2) Image processing
[0292] The surface observation image obtained above was binarized using image editing software so that the impregnated area was black and the non-impregnated area was white, and saved in BMP (Microsoft Windows Bitmap Image) format. Then, the pixel value data of each pixel of the binarized surface observation image saved in BMP format was saved in CSV (comma-separated values) format using image conversion software.
[0293] It should be noted that "Microsoft Paint" (manufactured by Microsoft Corporation) was used as the image editing software, and "bmp2csv" which is free software was used as the image conversion software.
[0294] (3) Calculation of the Existence Ratio of the Impregnation Area
[0295] The pixel value data saved in CSV format was pasted into Microsoft Excel (manufactured by Microsoft Corporation), and the number of black portions (pixel value = 0) corresponding to the impregnated area and the number of white portions (pixel value = 1) corresponding to the non-impregnated area were counted. Based on these numbers, the ratio of the black portion to the total of the black portion and the white portion was calculated, and this ratio was defined as the existence ratio of the impregnated area.
[0296] In addition, since the area|region corresponding to the non-impregnation area|region could not be identified in the prepregs obtained in Comparative Examples 3-5, it was made into "unmeasurable".
[0297] [Measurement of Thickness of Metal-Clad Laminated Plate]
[0298] A plan view for explaining a method for measuring the thickness of a metal-clad laminate is shown in FIG. Figure 4 middle.
[0299] like Figure 4 As shown, the 500 mm×500 mm area within the surface of the metal-clad laminate 30 is divided into a grid shape at intervals of 50 mm in the longitudinal and lateral directions, and 21 measurement unit areas 7 ( Figure 4 (the slashed part in the figure).
[0300] Then, if Figure 4As shown in the enlarged view of FIG. 1 , at four points ( Figure 4 The thickness is measured at point 8) in the measurement unit area, the difference between the maximum and minimum thicknesses of the four points is set as the thickness difference V1 in the measurement unit area 7, and the average thickness of the four points is set as T1.
[0301] Using the same method, V1 and T1 are obtained for each of the 21 measurement unit areas 7. The average value V of the obtained V1 is calculated. ave and the average value of T1 ave , use the following formula to find the value.
[0302] V ave ×100 / T ave
[0303] The value (unit: %) obtained by the above formula was used as an index of thickness accuracy.
[0304] [Measurement of Fluctuation in Dimensional Change of Metal-Clad Laminated Plate]
[0305] From the metal-clad laminates produced in each example, Figure 5 Four pieces of 340 mm × 250 mm were cut out as shown, and the obtained metal-clad laminate was used as the evaluation substrate. A total of four reference holes were set at 1 cm in the vertical direction and 1 cm in the horizontal direction from the four corners of the four evaluation substrates, and the distance between adjacent holes was measured using a CNC image measuring machine (Mitutoyo Co., Ltd., trade name: QV-H606T1L-D), and this value was set as the "reference size".
[0306] The evaluation substrate thus obtained was immersed in a copper etching solution (type of chemical solution: ammonium persulfate, temperature: 40° C., treatment time: 5 minutes) to remove the copper foil of the evaluation substrate.
[0307] Next, the evaluation substrate from which the copper foil was removed by etching was heated in air at 180° C. for 1 hour, naturally cooled to 25° C., and heated in air again at 180° C. for 1 hour. Thereafter, the distance between adjacent holes was measured by the same method as above, and the value was defined as the “post-heating dimension”.
[0308] From the dimensions obtained above, the dimensional change rate after heating was calculated for the four evaluation substrates based on the following formula.
[0309] Dimension change rate (%) = (size after heating - reference size) × 100 / reference size
[0310] The dimensional change rates of four evaluation substrates were measured (two data points in the longitudinal direction and two data points in the lateral direction for each substrate), and the standard deviation was calculated and used as the value of the fluctuation in the dimensional change amount of the metal-clad laminate (unit: %).
[0311] [Evaluation method of heat resistance of metal-clad laminate]
[0312] An evaluation substrate was prepared by cutting the metal-clad laminate obtained in each example into a size of 25 mm square, and the evaluation substrate was floated in a solder bath at a temperature of 288° C. for 90 minutes to confirm whether swelling occurred. Regarding the evaluation results, the evaluation substrate in which swelling was not confirmed at the time of floating for 90 minutes was evaluated as "A", and the evaluation substrate in which swelling was confirmed was evaluated as "B".
[0313] [Method for measuring fluctuation in warpage of semiconductor package]
[0314] Using the metal-clad laminate obtained in each example as the core layer, a build-up material (manufactured by Ajinomoto Co., Ltd., trade name "GX92", thickness 30 μm) (hereinafter also referred to as "BU"), copper foil (manufactured by Mitsui Mining and Smelting Co., Ltd., trade name "3EC-M3-VLP", thickness 12 μm) and solder resist (manufactured by RESONAC Co., Ltd., trade name "SR-7300") (hereinafter also referred to as "SR") were used to produce a substrate (with a rectangular shape of 60 mm × 60 mm when viewed from above) having the following layer structure.
[0315] (Layer structure of substrate)
[0316] SR / copper foil (residual copper rate 65%) / BU / BU / copper foil (residual copper rate 100%) / BU / BU / copper foil (residual copper rate 100%) / BU / BU / core layer / BU / BU / copper foil (residual copper rate 100%) / BU / BU / copper foil (residual copper rate 100%) / BU / BU / copper foil (residual copper rate 65%) / SR
[0317] In the above substrate, the thickness of the SR is 20 μm, the solder resist opening radius is 100 μm, the pad diameter is 150 μm, and the pad pitch is 200 μm.
[0318] It should be noted that each layer was stacked according to the following steps (1) to (5).
[0319] (1) Two build-up materials were laminated on each side of the metal-clad laminate obtained in each example, and copper foils were overlapped on the exposed surfaces of the build-up materials on both sides, followed by heat curing at 180° C., 0.5 MPa, and 90 minutes.
[0320] (2) Two build-up materials are further laminated on both sides of the obtained laminate, and copper foils are overlapped on the exposed surfaces of the build-up materials on both sides, followed by heating and curing under the same conditions as above.
[0321] (3) The same operation as in (2) is performed, and two build-up layer materials and copper foils are further laminated on both surfaces.
[0322] (4) The copper foils on both sides of the laminate obtained in (3) above are etched so as to obtain a predetermined pattern.
[0323] (5) On both surfaces of the laminated board having passed the above (4), a solder resist layer having a predetermined opening is formed using the above solder resist.
[0324] Then, a semiconductor chip made of silicon is mounted in the center of one surface of the substrate obtained above. The semiconductor chip is mounted by bonding the bumps provided on the circuit surface side of the semiconductor chip to the pads of the substrate using a TCB (Thermal Compression Bonding) process. The structure of the semiconductor chip is as follows.
[0325] (Semiconductor chip structure)
[0326] ■Chip size: 25mm×25mm rectangle in top view, thickness 0.725mm
[0327] ■Bump pitch: 200μm
[0328] ■ Bump metal: Sn-Ag solder alloy mounted on Cu pillars
[0329] ■Bump height: Cu pillar: 45μm, Sn-Ag solder alloy: 15μm
[0330] ■Bump size: φ90μm
[0331] Thereafter, the gap between the semiconductor chip and the substrate was sealed using a liquid sealing material (manufactured by Resonac Corporation, trade name "CEL-C-3730 series") to obtain a semiconductor package.
[0332] Four semiconductor packages were made from the metal-clad laminate obtained in each example by the above method, and the maximum warpage of each of the four semiconductor packages at 25°C and 260°C was measured using a warpage measuring device (manufactured by Akrometrix, trade name "TherMoire") at a heating rate of 20°C per minute.
[0333] Then, the standard deviation (unit: μm) of the maximum warpage at 25°C was calculated from the maximum warpage at 25°C of each of the four semiconductor packages, and this was used as the value of the fluctuation of the warpage of the semiconductor package at 25°C. In addition, the standard deviation (unit: μm) of the maximum warpage at 260°C was calculated from the maximum warpage at 260°C of each of the four semiconductor packages, and this was used as the value of the fluctuation of the warpage of the semiconductor package at 260°C. It should be noted that the standard deviations recorded in Table 1 are values obtained by rounding off the first decimal place.
[0334] [Synthesis of modified maleimide resin]
[0335] Synthesis example 1
[0336] Into a 2L reaction vessel capable of heating and cooling and equipped with a thermometer, a stirrer, and a moisture meter with a reflux condenser, 595.8 g of bis(4-maleimidephenyl)methane, 54.2 g of 4,4'-diaminodiphenylmethane, and 350.0 g of propylene glycol monomethyl ether were added, and the mixture was reacted for 5 hours while reflux, thereby obtaining a solution of a modified maleimide resin.
[0337] [Manufacture of resin varnish]
[0338] Production Example 1
[0339] (Resin varnish A)
[0340] 60 parts by mass of phenol novolac epoxy resin "EPICLON (registered trademark) N-770" (manufactured by DIC Corporation, epoxy equivalent: 188 g / eq), 40 parts by mass of biphenyl aralkyl phenol resin (manufactured by Meiwa Chemicals Co., Ltd., trade name "MEH-7700"), 17.5 parts by mass of aluminum hydroxide, 86 parts by mass of fused silica, 0.5 parts by mass of 2-methylimidazole, and methyl isobutyl ketone and cyclohexanone as diluents were added and mixed to prepare a resin varnish A having a solid content concentration of 65% by mass.
[0341] Production Example 2
[0342] (Resin varnish B)
[0343] 107 parts by mass of the solution of the modified maleimide resin obtained in Synthesis Example 1, 30 parts by mass of a tetrafunctional naphthalene-type epoxy resin "EXA-4710" (manufactured by DIC Corporation), 17.5 parts by mass of aluminum hydroxide, 130 parts by mass of fused silica, 0.5 parts by mass of 2,4-diamino-6-[2'-undecylimidazolyl-(1)']-ethyl-S-triazine, and methyl isobutyl ketone and cyclohexanone as diluents were added and mixed to prepare a resin varnish B having a solid content concentration of 65% by mass.
[0344] Example 1
[0345] (1) Preparation of resin film
[0346] The resin varnish described in Table 1 was applied onto a PET film using a comma-type knife coater so that the thickness of the resin film after drying was 30 μm, and then heated and dried at 130° C. for 2 minutes to produce a resin film with a PET film.
[0347] (2) Preparation of prepreg
[0348] Then, the resin film surface of the resin film with PET film was placed on both sides of the fiber substrate described in Table 1 so as to contact the glass cloth, and laminated using a vacuum laminating device. It should be noted that the vacuum lamination conditions were set to a heating plate temperature of 130° C., a pressing pressure of 0.5 MPa, a heating and pressing time of 30 seconds, a vacuum degree of 100 kPa or less, and a vacuum time of 30 seconds.
[0349] (3) Fabrication of Metal-Clad Laminated Plates
[0350] The obtained prepregs were stacked in the number of sheets listed in Table 1, and copper foils (manufactured by Furukawa Electric Co., Ltd., trade name "GTS-12", thickness 12 μm) were placed above and below them. Then, they were pressed under the following conditions to produce a square metal-clad laminate with a plan view of 1000 mm in length and 1000 mm in width.
[0351] -Pressure conditions-
[0352] Heating conditions: heating from 25°C to 185°C at a heating rate of 3°C / min, maintaining at 185°C for 90 minutes, and cooling for 30 minutes.
[0353] Pressure conditions: 4 MPa from the start of heating to the end of cooling.
[0354] Example 2
[0355] A resin film, a prepreg, and a metal-clad laminate were produced in the same manner as in Example 1, except that the number of prepregs stacked in "(3) Production of metal-clad laminate" of Example 1 was changed to 8.
[0356] Example 3
[0357] A resin film, a prepreg and a metal-clad laminate were produced by performing the same operations as in Example 1, except that the vacuum lamination conditions in "(2) Production of prepreg" of Example 1 were changed to a heating plate temperature of 150°C, a crimping pressure of 0.7 MPa, a heating and pressing time of 60 seconds, a vacuum degree of less than 100 kPa, and a vacuum time of 60 seconds.
[0358] Example 4
[0359] (1) Preparation of resin film
[0360] A resin film was produced by performing the same operation as in Example 1 except that the thickness of the resin film after drying was changed to 30.5 μm and 29.5 μm.
[0361] (2) Preparation of prepreg
[0362] A prepreg was prepared by performing the same operations as in Example 1, except that the lamination was performed in a manner such that a resin film with a thickness of 30.5 μm was in contact with one surface of the fiber substrate and a resin film with a thickness of 29.5 μm was in contact with the other surface of the fiber substrate, and the vacuum lamination conditions were changed to a heating plate temperature of 150°C, a pressing pressure of 0.7 MPa, a heating and pressing time of 60 seconds, a vacuum degree of less than 100 kPa, and a vacuum time of 60 seconds.
[0363] (3) Fabrication of Metal-Clad Laminated Plates
[0364] A metal-clad laminate was produced in the same manner as in Example 1 except that the prepreg obtained above was used.
[0365] Example 5
[0366] (1) Preparation of resin film
[0367] A resin film was produced by performing the same operation as in Example 1 except that the thickness of the resin film after drying was changed to 20.5 μm and 19.5 μm.
[0368] (2) Preparation of prepreg
[0369] A prepreg was prepared by performing the same operations as in Example 1, except that the type of fiber substrate was changed to the type shown in Table 1, the resin film with a thickness of 20.5 μm was arranged to abut against one surface of the fiber substrate, and the resin film with a thickness of 19.5 μm was arranged to abut against the other surface of the fiber substrate for lamination, and the conditions for vacuum lamination were changed to a heating plate temperature of 150°C, a pressing pressure of 0.7 MPa, a heating and pressing time of 60 seconds, a vacuum degree of less than 100 kPa, and a vacuum time of 60 seconds.
[0370] (3) Fabrication of Metal-Clad Laminated Plates
[0371] A metal-clad laminate was produced in the same manner as in Example 1 except that the prepreg obtained above was used.
[0372] Example 6
[0373] (1) Preparation of resin film
[0374] A resin film was produced by performing the same operation as in Example 1 except that the thickness of the resin film after drying was changed to 31 μm and 29 μm.
[0375] (2) Preparation of prepreg
[0376] A prepreg was prepared by performing the same operations as in Example 1, except that the lamination was performed in a manner such that a resin film having a thickness of 31 μm was in contact with one surface of the fiber substrate and a resin film having a thickness of 29 μm was in contact with the other surface of the fiber substrate, and the vacuum lamination conditions were changed to a heating plate temperature of 160°C, a crimping pressure of 1.0 MPa, a heating and pressing time of 60 seconds, a vacuum degree of less than 100 kPa, and a vacuum time of 60 seconds.
[0377] (3) Fabrication of Metal-Clad Laminated Plates
[0378] A metal-clad laminate was produced in the same manner as in Example 1 except that the prepreg obtained above was used.
[0379] Example 7
[0380] A resin film, a prepreg, and a metal-clad laminate were produced in the same manner as in Example 6, except that the type of the resin varnish was changed to the type shown in Table 1 in "(1) Production of resin film" of Example 6.
[0381] Comparative Example 1
[0382] (1) Preparation of resin film
[0383] A resin film was produced by performing the same operation as in Example 1 except that the thickness of the resin film after drying was changed to 32 μm and 28 μm.
[0384] (2) Preparation of prepreg
[0385] A prepreg was prepared by performing the same operations as in Example 1, except that the resin film having a thickness of 32 μm was arranged in contact with one surface of the fiber substrate, and the resin film having a thickness of 28 μm was arranged in contact with the other surface of the fiber substrate, and the vacuum lamination conditions were changed to a heating plate temperature of 100°C, a pressing pressure of 0.2 MPa, a heating and pressing time of 30 seconds, a vacuum degree of less than 100 kPa, and a vacuum time of 30 seconds.
[0386] (3) Fabrication of Metal-Clad Laminated Plates
[0387] A metal-clad laminate was produced in the same manner as in Example 1 except that the prepreg obtained above was used.
[0388] Comparative Example 2
[0389] (1) Preparation of resin film
[0390] A resin film was produced by performing the same operation as in Example 1 except that the thickness of the resin film after drying was changed to 32 μm and 29 μm.
[0391] (2) Preparation of prepreg
[0392] A prepreg was prepared in the same manner as in Example 1 except that the resin film having a thickness of 32 μm was arranged and laminated so as to contact one surface of the fiber substrate and the resin film having a thickness of 29 μm was contacted on the other surface of the fiber substrate.
[0393] (3) Fabrication of Metal-Clad Laminated Plates
[0394] A metal-clad laminate was produced in the same manner as in Example 1 except that the prepreg obtained above was used.
[0395] Comparative Example 3
[0396] The fiber base material described in Table 1 was immersed in the resin varnish described in Table 1, and dried at 140° C. for 3.5 minutes to obtain a prepreg. Thereafter, the same operation as in Example 1 was carried out to produce a metal-clad laminate.
[0397] Comparative Example 4
[0398] The fiber base material described in Table 1 was immersed in the resin varnish described in Table 1, and dried at 140° C. for 3.5 minutes to obtain a prepreg. Thereafter, the same operation as in Example 1 was carried out to produce a metal-clad laminate.
[0399] Comparative Example 5
[0400] The fiber base material described in Table 1 was immersed in the resin varnish described in Table 1, and dried at 140° C. for 3.5 minutes to obtain a prepreg. Thereafter, the same operation as in Example 1 was carried out to produce a metal-clad laminate.
[0401] [Table 1]
[0402] Table 1
[0403]
[0404] *1; cannot be measured
[0405] In addition, the details of the fiber base materials described in Table 1 are as follows.
[0406] "2116": Glass cloth "IPC#2116" (manufactured by Nitto Bosho Co., Ltd., basis weight: 104 g / m 2 , thickness: 91μm, surface waviness (Wa): 21.9μm)
[0407] "1078": Glass cloth "IPC#1078" (manufactured by Nitto Bosho Co., Ltd., basis weight: 47 g / m 2 , thickness: 44am, surface waviness (Wa): 7.3μm)
[0408] According to Table 1, the metal-clad laminates manufactured in Examples 1 to 7 of the present embodiment have excellent thickness accuracy and uniformity of dimensional variation. In addition, the semiconductor packages manufactured using the metal-clad laminates manufactured in Examples 1 to 7 of the present embodiment have small variations in warpage.
[0409] Description of Reference Numerals
[0410] 10, 20, 30 metal-clad laminate, 1 fiber substrate, 2 first resin layer, 3 second resin layer, 5 thermosetting resin composition, 6 unimpregnated area, 7 measurement unit area, 8 thickness measurement point, X plane direction.
Claims
1. A method for producing a metal-clad laminate, the method comprising laminating a prepreg and a metal foil by heating and pressurizing them. The prepreg comprises a thermosetting resin composition and a fiber substrate having a thickness of 40 μm or more, and has: A first resin layer provided on one surface of the fiber substrate and containing a thermosetting resin composition; and a second resin layer, which is provided on the other side of the fiber substrate and contains a thermosetting resin composition, When the thickness of the first resin layer is d1 and the thickness of the second resin layer is d2, The thickness difference ratio R represented by the following formula (1) is -9.0% to +9.0%. R = (d1-d2) × 100 / (d1+d2) (1) The surface waviness Wa of both surfaces of the prepreg is 6 μm or less.
2. The method for producing a metal-clad laminate according to claim 1, wherein: The prepreg has a region impregnated with the thermosetting resin composition and a region not impregnated with the thermosetting resin composition in the fiber base material.
3. The method for producing a metal-clad laminate according to claim 1 or 2, wherein: The thickness d1 of the first resin layer and the thickness d2 of the second resin layer are respectively 2 μm to 20 μm.
4. The method for producing a metal-clad laminate according to claim 1 or 2, wherein: The fiber substrate has a thickness of 40 μm to 120 μm.
5. The method for producing a metal-clad laminate according to claim 1 or 2, wherein: The fiber substrate is glass cloth. 6 . A method for producing a printed wiring board, comprising producing a metal-clad laminate using the method for producing a metal-clad laminate according to claim 1 or 2, and forming a wiring pattern on the metal-clad laminate.
7. A method for manufacturing a semiconductor package, wherein: A printed wiring board is manufactured by the method for manufacturing a printed wiring board according to claim 6, and a semiconductor element is mounted on the printed wiring board.
8. A metal-clad laminate comprising a cured product of a thermosetting resin composition, one or more fiber substrates, and a metal foil, The thickness of the fiber substrate is 40 μm or more, The value calculated by the following method is less than 0.5%: (method) The 500 mm×500 mm area in the surface of the metal-clad laminate is divided into a grid shape at intervals of 50 mm in the longitudinal and lateral directions, and 21 measurement unit areas 7 having a square shape of 50 mm in length and 50 mm in width are set at the position shown in the top view of the metal-clad laminate 30 in FIG. 4 ; The thickness is measured at the points located inside the measurement unit area 7 and spaced 10 mm from the longitudinal and transverse sides, i.e., the positions of the four thickness measurement points 8 shown in FIG. 4 , and the difference between the maximum and minimum values of the thickness at the four points is set as the thickness difference V1 in the measurement unit area 7, and the average value of the thickness at the four points is set as T1; V1 and T1 are calculated for the 21 measurement unit areas 7, and the average value V ave and the average value of T1 ave , use the following formula to calculate the value: V ave ×100 / T ave 。 9. The metal-clad laminate according to claim 8, wherein: The metal-clad laminate has the metal foil on both sides and comprises: a first resin cured product layer provided on a surface of the fiber base material, in contact with the metal foil on one surface of the metal-clad laminate, and containing a cured product of a thermosetting resin composition; and a second resin cured product layer provided on a surface of the fiber base material, in contact with the metal foil on the other surface of the metal-clad laminate, and containing a cured product of a thermosetting resin composition; When the thickness of the first resin cured material layer is d'1 and the thickness of the second resin cured material layer is d'2, The thickness difference ratio R' represented by the following formula (1') is -9.0% to +9.0%, R'=(d'1-d'2)×100 / (d'1+d'2) (1').
10. A printed wiring board comprising the metal-clad laminate according to claim 8 or 9.
11. A semiconductor package comprising the printed wiring board according to claim 10 and a semiconductor element.
Citation Information
Patent Citations
Manufacture of prepreg
JP1989272416A