Laminated glass pane for head-up display
By using a combination of pure substoichiometric or doped tungsten oxide layer and metal functional layer in laminated assembly glass, the combination of "sunlight control" and heating functions in head-up displays is solved, and high light transmittance and low surface are achieved Increased reflectivity of resistance and p-polarized electromagnetic radiation, suitable for head-up displays and heating applications.
Patent Information
- Application Number
- CN202380036606.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-28
- Filing Date
- 2023-04-26
- Publication Date
- 2024-12-06
AI Technical Summary
Existing laminated assembled glass is difficult to simultaneously realize the "sunlight control" properties and heating functions in head-up display applications, and it is necessary to meet low solar factors, high light transmittance, color neutrality in reflection and transmission, p-polarization electromagnetic in visible spectrum High reflection and low surface resistance of radiation.
The laminated assembly glass structure is adopted with a dielectric module composed of pure substoichiometric or doped tungsten oxide layer combined with a metal functional layer. The tungsten oxide layer is doped by cesium to optimize optical characteristics, and the metal functional layer is used to reflect infrared radiation. And achieve low surface resistance through a specific thin-layer stack design.
The high light transmittance, low surface resistance and color neutrality are achieved while improving the reflectivity of p-polarized electromagnetic radiation in the visible spectrum, suitable for head-up displays and heating applications.
Smart Images

Figure CN119095810A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to laminated glazing for a head-up display. Technical Background
[0002] Modern vehicles are currently equipped with heads-up displays (HUDs).
[0003] These systems or devices include a projector, usually located near the vehicle dashboard, configured to project an image into the area of the vehicle's windshield. The projected image appears to the vehicle driver as a virtual image behind the windshield, displaying information such as vehicle speed, navigation, and or warnings directly in the driver's field of view. The driver no longer has to take his eyes off the road to view this information and remains alert to events occurring outside the vehicle. HUD systems or devices thus help improve road safety.
[0004] Most HUD devices are based on emitting polarized electromagnetic radiation with s-type polarization and an angle of incidence of about 65° to the windshield normal. This angle is close to the Brewster angle of the glass-air interface, which is about 56.5° for soda-lime glass. The projected image is then reflected by the two main outer surfaces of the windshield. In addition to the main image, a secondary image appears, which is more or less offset and more or less partially covers the main image. This secondary image is called a "phantom image" or "ghost image".
[0005] To reduce the ghost image effect, the main surfaces of the windscreen are arranged at different angles, usually by inserting a laminate interlayer of variable thickness, so that the ghost image and the main image overlap. This type of glazing is often called wedge glazing or wedge windscreen.
[0006] For example, EP0420228 A2 [HUGHES AIRCRAFT CO [US]] 04.03.1991 describes a windshield comprising a laminated interlayer whose thickness tapers between the first and second windshield sides so that the two glass sheets in bonding contact with the interlayer have two different inclination angles relative to the projector.
[0007] However, this type of glazing is expensive to manufacture, is limited to certain viewing angles of the projected image, and does not prevent the formation of ghost images when the glazing includes a functional coating.
[0008] Alternatively, it is common practice to use HUD devices whose implementation is based on emitting electromagnetic radiation polarized according to p-type polarization and emitted onto a windshield comprising a functional coating suitable for forming a new reflective interface for this type of radiation inside said windshield.
[0009] Since p-type polarized electromagnetic radiation is emitted toward the windshield at an incident angle close to the Brewster angle, it is not reflected by the glass-air interface. Reflection occurs only at the reflective interface formed by the functional coating. Various types of functional coatings can be used.
[0010] WO 2005 / 017600 A1 [3M INNOVATIVE PROPERTIES CO [US]] 02.24.2005 describes a polarizing optical film comprising a plurality of individual layers having different optical refractive indices. The film is intended to be laminated into a laminated glazing to form a head-up display windshield and comprises a region that reflects mainly visible light polarized according to p-polarization. The film may also reflect infrared radiation to reduce the greenhouse effect phenomenon in vehicles.
[0011] DE 102014220189 A1 [CONTINENTAL AUTOMOTIVE GMBH [DE]] 04.07.2016 describes a laminated glazing unit comprising a silver or aluminum-based metal layer having a thickness of 5 nm to 9 nm. The metal layer is capable of reflecting p-polarized visible light.
[0012] WO 2016 / 058474 A2 [FUYAO GLASS IND GROUP CO LTD [CN]] 04.21.2016, WO 2021 / 104800 A1 [SAINT GOBAIN [FR]] 06.03.2021, WO 2019 / 046157 A1 [VITRO FLAT GLASSLLC [US]] 03.07.2019, WO 2020 / 094422 A1 [SAINT GOBAIN [FR]] 05.14.2020 describe laminated glazing for head-up displays, which is provided with a functional coating comprising one or more metallic functional layers, in particular silver-based functional layers, allowing reflection of visible light polarized according to p-polarization. The functional coating may also include a dielectric layer, which dielectric layer, possibly in combination with the metallic functional layer, imparts other properties, such as solar control and / or color neutralization of the coating in transmission and / or reflection.
[0013] Laminated and non-laminated "solar control" glazings also include glazings with a thin film stack but without a functional metal layer to ensure a certain transparency to radio frequencies used for onboard telecommunication systems. Functional layers that absorb infrared radiation are often used instead of the functional metal layer. They can be based on oxides and / or nitrides.
[0014] JP H0812378A [NISSAN MOTOR] 01 / 16 / 1996 describes a functional "solar control" stack comprising a tungsten oxide layer arranged between two dielectric layers. This stack makes it possible to reduce the surface resistance and increase the transparency to radio waves compared to stacks comprising metallic functional layers, in particular based on silver.
[0015] JP 2010180449 A [SUMITOMO METAL MINING CO [JP]] 08 / 19 / 2010 describes a tungsten oxide-based layer deposited by sputtering using a tungsten oxide target containing a chemical element selected from hydrogen, alkali metals, alkaline earth metals and rare earth metals. The layer has a "sunlight control" function due to its high absorption of near-infrared radiation.
[0016] EP 3686312 A1 [SUMITOMO METAL MINING CO [JP]] 07 / 29 / 2020 describes a layer based on tungsten oxide doped with cesium, and a method for depositing such a layer by sputtering. The layer has transparency to radio waves and a "sunlight control" function, in particular due to its high absorption of infrared radiation.
[0017] For some applications in the automotive industry, the glazing must comprise, in addition to the solar control function, a heating function in order to allow, for example, its defrosting and / or its defogging.
[0018] Whether these glazings are in the form of windshields, triangular windows, small windows, large windows and / or glazed roofs, the heating function is usually provided by the solar control stack itself. Due to the metal layers it contains, the stack is an electrical conductor. When powered by an alternator and / or the vehicle battery, it can release heat by the Joule effect.
[0019] For obvious safety reasons, the alternator and / or vehicle battery typically delivers low voltages at their terminals, typically 12 V to 48 V, often around 14 V. Likewise, in order to release enough heat for effective defogging and / or defrosting, the surface resistivity of the stack must be low enough to enhance the Joule effect at low voltages.
[0020] EP0726232 A2, EP1614325 A1 and US2015229030A1 describe examples of solar control heatable windshields, where the conductive stack provides both solar control and heating functions. SUMMARY OF THE INVENTION
[0022] Technical issues
[0023] There is a need for laminated glazing that combines "solar control" properties with head-up display applications and heating functionality. Such glazing must meet fivefold requirements: low solar factor, high light transmittance, color neutrality in reflection and / or transmission, high reflection of p-polarized electromagnetic radiation in the visible spectrum, and low surface resistance.
[0024] Solutions to technical problems
[0025] A first aspect of the invention relates to a laminated glazing as disclosed in claim 1, the dependent claims being advantageous embodiments. The laminated glazing comprises:
[0026] - a first glass sheet;
[0027] - a second glass sheet;
[0028] - a lamination interlayer in bonding contact with the first glass sheet and the second glass sheet;
[0029] a thin layer of functional coating arranged on the second glass sheet and comprising, starting from the second glass sheet, a first dielectric module, a metallic functional layer and a second dielectric module, the metallic functional layer being located between the first dielectric module and the second dielectric module;
[0030] The glazing is characterized in that:
[0031] The first dielectric module and / or the second dielectric module contains (or includes) a tungsten oxide layer, and is characterized in that:
[0032] - the tungsten oxide layer is made of pure substoichiometric tungsten oxide WOx, wherein x is preferably 2.55 to 2.98, or
[0033] - the tungsten oxide layer is a doped tungsten oxide and comprises at least one doping element selected from the chemical elements of Group 1 according to the IUPAC nomenclature.
[0034] Further advantageous embodiments are described in the detailed disclosure.
[0035] Preferably, the first glass sheet is an outer glass sheet and the second glass sheet is an inner glass sheet.
[0036] The functional metal layer may be the only functional metal layer of the functional coating.
[0037] According to a second aspect of the present invention, there is provided a head-up display projection device comprising the laminated glazing according to the first aspect of the present invention.
[0038] According to a third aspect of the present invention, there is provided a method for manufacturing a laminated glazing according to the first aspect of the present invention.
[0039] Advantages of the invention
[0040] Notable advantages of the glazing according to the invention are its low solar factor, high light transmittance, color neutrality in reflection and / or transmission, high reflection of electromagnetic radiation polarized according to p-polarization in the visible spectrum, and low surface resistance.
[0041] More specifically, the glazing according to the invention has a selectivity of more than 1.3, or even 1.35, for a light transmittance of more than 70%. It is also color neutral in transmission and reflection.
[0042] In head-up applications, glazings according to the invention have, in some embodiments, a level of reflection of electromagnetic radiation in p-type polarization at 65° of greater than 16%, or even 18%, or even 19%.
[0043] For certain embodiments, the glazing according to the invention also has a surface resistance of less than 3.5 Ω / □, in particular less than 2.5 or even 2.4. These resistance values are ideal for electrical heating applications.
[0044] BRIEF DESCRIPTION OF THE DRAWINGS
[0045] [ Figure 1 ] is a schematic diagram of a laminated glazing according to the present invention.
[0046] [ Figure 2 ] Figure 1 Detailed schematic diagram of the functional coating shown in .
[0047] [ Figure 3 ] is a schematic diagram of a projection device for a head-up display.
[0048] [ Figure 4 ] is a schematic diagram of the light transmittance and direct solar transmittance according to an embodiment of the present invention and two comparative examples.
[0049] [ Figure 5 ] is a schematic diagram of the transmittance and total solar factor according to an embodiment of the present invention and two comparative examples.
[0050] Implementation Detail
[0051] The following definitions and conventions apply.
[0052] The terms "over" and "below", respectively describing the position of a layer or a layer assembly and defined relative to the position of another layer or another assembly, mean that the layer or the layer assembly is closer to or farther away from the substrate, respectively.
[0053] The two terms "above" and "below" in no way mean that the layer or layer assembly they describe is in contact with another layer or another assembly defined relative to it. They do not exclude the presence of other intermediate layers between the two layers. The expression "in contact with" is explicitly used to indicate that no other layers are arranged between them.
[0054] In the absence of any more complete information or qualifiers, the term "thickness" used for a layer corresponds to the physical thickness, actual thickness or geometric thickness of said layer. It is expressed in nanometers.
[0055] The expression "layer" or "thin layer" refers to a material layer as usually defined in the technical field. Typically, this is a thin layer having a thickness of less than 1 μm, or even less than 500 nm, typically less than 100 nm.
[0056] The expression "dielectric module" means one or more layers in contact with one another, which form a layer assembly which is dielectric as a whole, that is to say which does not have the function of a functional metallic layer. If the dielectric module comprises a plurality of layers, these themselves may be dielectric. The physical thickness, actual thickness or geometric thickness of a dielectric module of layers corresponds to the sum of the physical thickness, actual thickness or geometric thickness of each of the layers constituting it.
[0057] In the present description, the expressions "layer of" or "layer based on" used to describe a material or a material contained in a layer are used equally. They mean that the mass fraction of the components contained therein is at least 50%, in particular at least 70%, preferably at least 90%. In particular, the presence of minority or doping elements is not excluded.
[0058] The term "transparent" as used to describe the substrate means that the substrate is preferably colorless, non-opaque and non-translucent to minimize light absorption and thereby maintain maximum light transmittance in the visible electromagnetic spectrum.
[0059] “Light transmittance” (TL) is understood to mean the light transmittance as defined and measured and / or calculated in standard ISO 13837:2021, denoted TL.
[0060] “Direct solar transmittance” (TE) is understood to mean the direct solar transmittance as defined and calculated according to standard ISO 13837:2021.
[0061] "Sun Factor" TTS (or T TS ) is understood to mean the solar factor as defined according to standard ISO 13837:2021.-Convention A. It is equal to the sum of the direct solar transmittance TE and the secondary heat flux qi.
[0062] "Selectivity" (s) is understood to mean the ratio of the light transmission LT to the solar factor TTS.
[0063] According to the IUPAC nomenclature, Group 1 chemical elements contain hydrogen and the alkaline elements, namely lithium, sodium, potassium, rubidium, cesium, and francium.
[0064] The expression “optical refractive index” is understood to be the optical refractive index n as defined in the technical field, in particular defined according to the Forouhi & Bloomer model described in Forouhi & Bloomer, Handbook of Optical Constants of Solids II, Palik, ED (ed.), Academic Press, 1991, Chapter 7.
[0065] According to a first aspect of the present invention, referring to Figure 1 and 2 , a laminated glazing 1000 is provided, comprising:
[0066] - a first glass sheet 1001;
[0067] - a second glass sheet 1002;
[0068] - a laminating interlayer 1003 in bonding contact with a first glass sheet 1001 (here the outer glass sheet) and a second glass sheet 1002 (here the inner glass sheet);
[0069] A thin layer of functional coating 1004 , which is arranged on the second glass sheet 1002 and, starting from the second glass sheet 1002 , comprises a first dielectric module 2001 , a metallic functional layer 2002 and a second dielectric module 2003 , the metallic functional layer 2002 being located between the first dielectric module 2001 and the second dielectric module 2003 .
[0070] The glazing is characterized in that:
[0071] The first dielectric module 2001 and / or the second dielectric module 2003 comprises a tungsten oxide layer 2004a, 2004b and is characterized in that:
[0072] - the tungsten oxide is made of pure substoichiometric tungsten oxide WOx, wherein x is preferably 2.55 to 2.98, or
[0073] The tungsten oxide comprises at least one doping element chosen from the chemical elements of group 1 according to the IUPAC nomenclature.
[0074] The glass sheets 1001, 1002 may be mineral or glass ceramic. The glass may preferably be a soda-lime-silicon type, a borosilicate type, an aluminosilicate type or an aluminoborosilicate type glass. According to a preferred embodiment of the present invention, the glass sheets 1001, 1002 are soda-lime-silicon mineral glass sheets.
[0075] According to some embodiments, the first glass sheet 1001 and / or the second glass sheet 1002 may be thin glass sheets, in particular having a thickness of 0.4 to 1.1 mm, especially 0.4 to 0.7 mm.
[0076] In a preferred embodiment, the glass sheets 1001, 1002 are transparent glass sheets.
[0077] According to certain embodiments, one of the two glass sheets 1001, 1002 may be an inorganic glass that is dyed in the mass. Dyeing or coloring in the mass of inorganic glass is known and is extensively described in the technical literature. The coloring can generally be obtained by adding a coloring oxide to the glass chemical composition. Examples of coloring oxides may be iron II oxide, copper oxide, chromium oxide, nickel oxide, gold oxide, manganese oxide, cobalt oxide, uranium oxide, neodymium oxide, and erbium oxide. Mixtures of oxides may also be used, such as copper tin oxide, or ionic complexes, such as iron-sulfur or cadmium-sulfur complexes.
[0078] The lamination interlayer 1003 may consist of one or more layers of thermoplastic material. Examples of thermoplastic materials are polyurethane, polycarbonate, polyvinyl butyral (PVB), polymethyl methacrylate (PMMA), ethylene vinyl acetate (EA) or ionomer resins.
[0079] The laminate interlayer 1003 may be in the form of a multilayer film. It may also have specific functions, such as acoustic or anti-UV properties.
[0080] Typically, the lamination interlayer 1003 comprises at least one PVB layer. Its thickness ranges from 50 μm to 4 mm. Typically, it is less than 1 mm.
[0081] The function of the functional metal layer 2002 is to reflect infrared radiation and / or a portion of solar radiation. It can be any suitable metal, for example based on gold or based on silver. The thickness of the functional metal layer 1003 can generally be 2nm to 25nm, preferably 10nm to 20nm.
[0082] According to a preferred embodiment, the functional metal layer 2002 is based on or made of silver.
[0083] According to certain preferred embodiments, the laminated glazing 1000, when used as a glazing for a motor vehicle, for example as a windshield, is such that the second glass sheet 1002 is located inside the vehicle. In other words, the functional coating 1004 is placed on face 3 of the glazing starting from the second glass sheet 1002 inside the vehicle, face 4 being the face facing inside, or on face 2 of the glazing starting from the first glass sheet 1001 facing outside the vehicle, face 1 being the face facing outside.
[0084] According to the first aspect of the present invention, the first dielectric module 2001 and / or the second dielectric module 2003 include tungsten oxide layers 2004a, 2004b. Thus, in a first embodiment, only the first dielectric module 2001 includes the tungsten oxide layer 2004a. In a second embodiment, only the second dielectric module 2002 includes the tungsten oxide layer 2004b. In a third embodiment, each of the dielectric modules 2001, 2002 includes the tungsten oxide layer 2004a, 2004b.
[0085] When the first dielectric module and the second dielectric module each include a tungsten oxide layer, the tungsten oxides of the two tungsten oxide layers may have different compositions.
[0086] According to other preferred embodiments, the optical refractive index of the tungsten oxide layers 2004a, 2004b decreases monotonically with wavelength from a maximum value greater than 2.4 at 350nm to a minimum value between 600nm and 1400nm, so that the difference between the maximum and the minimum is greater than 0.8, preferably greater than 1.0, or even greater than 1.4.
[0087] In other words, the value of the optical refractive index decreases monotonically by at least 0.8, preferably at least 1.0, or even at least 1.4 between a maximum value of greater than 2.4 at 350 nm and a minimum value of 600 nm to 1400 nm. For example, the optical refractive index value may decrease monotonically by at least 0.8, preferably at least 1.0, or even at least 1.4 between a maximum value of greater than 2.4 at 350 nm and a minimum value of less than 2.3 at 600 nm to 1400 nm, especially at 800 nm to 1100 nm.
[0088] While not particularly required to achieve the effects of the present invention, these optical refractive index values may still be beneficial in improving color neutrality in transmission and reflection.
[0089] According to some preferred additional embodiments, the optical extinction coefficient of the tungsten oxide layers 2004a, 2004b may be less than 0.2, or even 0.1 at 500 nm, and less than 2.0, or even 1.5 at 1200 nm, thereby further improving the selectivity.
[0090] The tungsten oxide in the tungsten oxide layers 2004a, 2004b can be pure substoichiometric tungsten oxide WOx, wherein x is preferably 2.55 to 2.98, or even 2.6 to 2.95. Values of x between 2.98 and 3.02 are believed to produce pure stoichiometric tungsten oxide WO3. These characteristics, combined with the presence of the metal functional layer, have a synergistic effect on the improvement of selectivity.
[0091] Surprisingly, tungsten oxide layers made of pure substoichiometric tungsten oxide WOx have unexpected optical properties, in particular in terms of the evolution of the optical extinction coefficient and the refractive index as a function of the wavelength of the electromagnetic radiation. These properties, combined with the presence of a metallic functional layer, have a synergistic effect on the improvement of selectivity.
[0092] Surprisingly, the tungsten oxide layers 2004a, 2004b comprising a doping element selected from the elements of group 1 according to the IUPAC nomenclature have unexpected optical properties, in particular with regard to the evolution of the optical extinction coefficient and the refractive index as a function of the wavelength of the electromagnetic radiation.
[0093] The optical extinction coefficient and the optical diffraction index can be varied according to:
[0094] - substoichiometric, or
[0095] - the nature and amount of the doping element chosen from the elements of group 1 according to the IUPAC nomenclature.
[0096] However, it is currently difficult to establish general laws for the behavior of the optical extinction coefficient and the refractive index depending on the nature and / or amount of the doping element in the substoichiometric fraction or in other fractions.
[0097] According to certain specific embodiments, the tungsten oxide layers 2004a, 2004b made of doped tungsten oxide contain a doping element X or multiple doping elements X1, X2... in a ratio such that the molar ratio X / W of the element to tungsten W or the sum of the molar ratios of each element to tungsten (X1+X2+...) / W is 0.01 to 0.4, preferably 0.01 to 0.2, or even 0.01 to 0.1.
[0098] It is observed that these molar ratio values can advantageously make it possible to obtain the values of the optical extinction coefficient and the refractive index described in the previous embodiments, while limiting the amount of doping elements. In addition, this can lead to saving in the mining of mineral resources of the doping elements, as well as reducing costs.
[0099] According to some embodiments, the tungsten oxide layers 2004a, 2004b made of doped tungsten oxide contain at least one doping element selected from hydrogen, lithium, sodium, potassium and cesium. Among the elements of Group 1, these specific elements can make it possible to obtain the values of the optical extinction coefficient and the refractive index that are optimal for the desired technical effect.
[0100] According to particularly preferred embodiments, the tungsten oxide layers 2004a, 2004b made of doped tungsten oxide contain cesium as a doping element, and the molar ratio of cesium to tungsten is 0.01 to 0.4, preferably 0.01 to 0.2. These embodiments allow for optimal performance to improve selectivity, maintain neutral color and cost savings.
[0101] According to some advantageous embodiments, the physical thickness of the tungsten oxide layers 2004a, 2004b may be 2nm to 50nm, in particular 5nm to 30nm, preferably 5nm to 20nm. These thickness intervals are sufficient to obtain the significant advantages of the first aspect of the present invention.
[0102] According to an embodiment, the first dielectric module 2001 and / or the second dielectric module 2002 may include one or more layers having a refractive index of less than 2.45 at 550 nm.
[0103] The layer or layers having a refractive index of less than 2.45 at 550 nm are preferably based on oxides or nitrides of silicon, zirconium, titanium or tin and zinc. For example, they may be based on silicon nitride, silicon oxide, zirconium nitride, or zinc tin oxide.
[0104] According to an embodiment, the thin layer of functional coating 1004 further comprises a barrier metal coating preferably based on a nickel and chromium alloy located above and in contact with the functional metal layer, and / or a barrier metal liner preferably based on a nickel and chromium alloy located below and in contact with the functional metal layer.
[0105] The presence of a barrier metal coating and / or barrier metal liner makes it possible to advantageously improve the durability of the stack, for example in terms of mechanical resistance to brushing or scratching. It also makes it possible to avoid degradation of the metallic functional layer 2002 during the deposition of subsequent layers and / or during thermal treatments, for example oxidation, in particular by limiting the diffusion of certain chemical elements from adjacent layers and / or the diffusion of oxygen.
[0106] In an advantageous embodiment, the first dielectric module 2001 and / or the second dielectric module 2002 can contain layers based on indium tin mixed oxide, indium zinc mixed oxide, fluorine-doped tin oxide, aluminum-doped zinc oxide, gallium-doped zinc oxide, antimony-doped tin oxide and / or niobium-doped titanium oxide.
[0107] Surprisingly, it has been found that the combination of one of these layers with a doped tungsten oxide layer as described in the present invention advantageously reduces the solar factor TTS due to a higher absorption of infrared radiation without compromising color neutrality and transmission.
[0108] Preferably, the thickness of the layer based on indium tin mixed oxide, indium zinc mixed oxide, fluorine-doped tin oxide, aluminum-doped zinc oxide, gallium-doped zinc oxide, antimony-doped tin oxide and / or niobium-doped titanium oxide is 50 to 100 nm.
[0109] This layer is distinguished from any wetting layer (also called crystalline layer) situated below and in contact with the metallic functional layer, which is usually based on aluminum-doped zinc oxide and usually has a thickness of less than 15 nm.
[0110] In a preferred embodiment, the first dielectric module 2001 and / or the second dielectric module 2002 may include an indium tin mixed oxide layer having a thickness of 50 nm to 100 nm.
[0111] According to a second aspect of the present invention, referring to Figure 3 , a projection device 3000 for a head-up display is provided, comprising:
[0112] - a laminated glass 1000 according to the first aspect of the invention;
[0113] A heads-up projector 3001 configured to emit electromagnetic radiation 3002 onto at least one area 3003 of the laminated glass 1000 , the electromagnetic radiation being polarized at least partially according to p-polarization.
[0114] In operation, the head-up projector 3001 projects an image onto the area 3003 of the laminated glazing, acting like a screen. The image is perceived by the user 3004 (in this case the driver) as a virtual image when the user 3004 (in this case the driver) looks at a stereoscopic viewing angle 3005 suitable for perceiving the image in the area 3003 of the laminated glazing 1000.
[0115] Laminated glazing manufacturing methods are well known in the glass industry. For example, a method for manufacturing laminated glazing may be a method of laminating a laminate interlayer between two glass sheets. The glass sheets may be preformed, for example in a curved shape using a bending process. They may also be coated with one or more thin film coatings using any suitable thin layer deposition process.
[0116] Methods for depositing thin layers on substrates, particularly glass sheets, are well known in the industry. For example, deposition of a stack of thin layers on a glass substrate is performed by successively depositing each thin layer of the stack by passing the glass substrate through a series of deposition chambers suitable for depositing a given thin layer.
[0117] The deposition chamber may use deposition methods such as magnetic field assisted sputtering, ion beam assisted deposition (IBAD), evaporation, chemical vapor deposition (CVD), plasma enhanced chemical vapor deposition (PECVD), low pressure chemical vapor deposition (LPCVD), and the like.
[0118] In particular, a magnetic field enhanced sputtering deposition method is used. The conditions for depositing the layers are widely described in the literature, for example in patent applications WO 2012 / 093238 A1 and WO 2017 / 00602 A1.
[0119] When a pure tungsten metal target or a pure tungsten oxide target is used, it can be used to deposit a layer of pure substoichiometric tungsten oxide WOx, wherein x is preferably between 2.55 and 2.98.
[0120] One advantage of using a ceramic target (ie containing oxygen) compared to a metal target, particularly for a rotary target, is that the ceramic target is lighter, making it easier to control the process using the ceramic target.
[0121] When a ceramic or metal target is used, it may contain one or more doping elements in particular in the proportions as described for the doped tungsten oxide layer in some embodiments of the first aspect of the invention.
[0122] According to a third aspect of the present invention, a method for manufacturing a laminated glazing 1000 according to the first aspect of the present invention is provided, wherein tungsten oxide layers 2004a, 2004b doped with tungsten oxide are deposited by magnetron sputtering using a tungsten oxide target, the oxide target being doped with a chemical element selected from chemical elements of Group 1 according to the IUPAC nomenclature.
[0123] The tungsten oxide target may contain one or more doping elements in particular in the ratios as described for the doped tungsten oxide layer in some embodiments of the first aspect of the present invention.
[0124] According to particularly preferred embodiments, the tungsten oxide layer contains cesium as doping element and the molar ratio of cesium to tungsten is 0.01 to 0.2, preferably 0.01 to 0.1. These embodiments make it possible to obtain the best performance to improve selectivity, maintain neutral color and cost savings.
[0125] It is of the utmost importance in the context of the present invention that the absorption of the tungsten oxide layer material in the visible light range (wavelength 380 to 780 nm) is as low as possible in order to maximize the gain in selectivity.
[0126] The tungsten oxide layer can be deposited by sputtering using the above target in a deposition atmosphere consisting of 60% to 100% argon and 0% to 40% molecular oxygen, preferably 70% to 85% argon and 15% to 30% molecular oxygen.
[0127] The tungsten oxide layer may be deposited at a pressure of 1 to 15 mTorr, preferably 3 to 10 mTorr.
[0128] Preferably, for this substrate, the deposition can be carried out under cold conditions, ie at a temperature of less than 100°C, in particular from 20°C to 60°C.
[0129] The deposition can also be carried out under thermal conditions, in particular at a temperature between 100°C and 400°C.
[0130] According to a particular embodiment, after depositing the stack 1004, the glass sheet 1002 may be subjected to an annealing heat treatment. The annealing temperature may be 450° C. to 800° C., in particular 550° C. to 750° C., or even 600° C. to 700° C. The annealing time may be 5 minutes to 30 minutes, in particular 5 minutes to 20 minutes, or even 5 minutes to 10 minutes.
[0131] The laminated glazing 1000 according to the first aspect is particularly suitable for use in head-up display applications in land, sea or air vehicles, preferably motor vehicles, railway vehicles, aircraft or ships, in particular passenger cars or trucks.
[0132] All embodiments described, whether they relate to the first or second aspect of the invention, can be combined with one another without modification or special adjustments. If technical incompatibilities arise during the implementation of one of these combinations, it is within the scope of the skilled person to be able to resolve these incompatibilities with the help of their knowledge without undue effort, in particular by implementing research solutions. Example
[0133] The features and advantages of the present invention are demonstrated by the examples and comparative examples described below.
[0134] Three examples E1-E3 according to the invention and two comparative examples CE1 and CE2 not according to the invention are described in Table 1, which show the composition and thickness of the various thin layers of glass sheets 1001, 1002, lamination interlayer 1003 and functional coating 1004. The thickness of the thin layer of functional coating 1004 is expressed in nanometers. The numbers in the first two columns correspond to the reference numbers in the drawings.
[0135] In the embodiments E1 to E3, the tungsten oxide layer 1005 denoted as CWO is a cesium-doped tungsten oxide layer having a refractive index of about 2.4 at 550 nm.
[0136] The molar ratio of cesium to tungsten in this layer is about 0.05-0.06.
[0137]
[0138]
[0139] In embodiment E1, the tungsten oxide layer is in the first module 2001 starting from the glass sheet 1002. In embodiment E2, the tungsten oxide layer is in the second module 2003 starting from the glass sheet 1002. Embodiment E3 differs from embodiments E1 and E2 in that it includes a layer of doped tungsten oxide (CWO) in each of the two dielectric modules 2002, 2003 and a layer of indium tin oxide (ITO) in the first dielectric module 2001 starting from the glass sheet 1002.
[0140] Analogously to Example E3, Example E4 according to the present invention is shown in Table 2.
[0141]
[0142]
[0143] Example E4 differs from example E3 by starting from a glass sheet 1002 comprising a layer of pure substoichiometric tungsten oxide WOx in each of the two dielectric modules 2002 , 2003 and a layer of silicon nitride (SiN) in the first dielectric module 2001 .
[0144] Comparative Example CE1 corresponds to Examples E1 and E2. The difference is that it does not have a tungsten oxide layer. Comparative Example CE2 corresponds to Examples E3 and E4. The difference is that it does not have a tungsten oxide layer.
[0145] The thin layers of the functional coating 1004 of Examples E1 to E4 and Comparative Examples CE1 to CE2 were deposited by magnetic field-assisted cathode sputtering (magnetron method), the properties of which are widely described in the literature, for example in patent applications WO 2012 / 093238 and WO 2017 / 00602.
[0146] The properties of the targets used and the deposition conditions for Examples E1 to E4 and Comparative Examples CE1 and CE2 are described in Table 3.
[0147] The functional coating is deposited directly on the glass sheet 1002. The glass sheet 1002 is a 2.1 mm thick soda-lime-silica mineral glass. Just after deposition, the functional coating is subjected to a heat treatment at 650° C. for 10 minutes.
[0148]
[0149] at.=atom
[0150] The WOx layer is deposited on a tungsten metal target in an atmosphere containing 60% molecular oxygen at a pressure of 12 mTorr. The WOx layer is thus a layer of pure substoichiometric tungsten oxide WOx, where x is about 2.9. It has a refractive index of about 2.2 at 550 nm.
[0151] Once the deposition and heat treatment are complete, each glass sheet 1002 with the functional coating 1004 is laminated with a laminating interlayer 1003 of 0.76 mm thick PVB and a second glass sheet 1001 of 1.6 mm thick soda-lime-silica mineral glass to form a laminate such as Figure 1 Laminated glazing shown in .
[0152] For each example and comparative example, the light transmittance TL, the "direct solar transmittance" TE and the "solar factor" TTS (or T TS ).
[0153] The "selectivity" (s), defined as the ratio TL / TTS of the light transmittance LT to the solar factor TTS, and the "solar selectivity" (SE), defined as the ratio TL / TE of the light transmittance TL to the direct solar transmittance TE, are calculated for each example and comparative example from previously measured and / or calculated parameters.
[0154] For each of the examples and comparative examples, the colorimetric parameters a* and b* were measured and / or calculated in the L*a*b* CIE 1976 color space according to standard ISO 11664-4:2019 with a D65 illuminant and a field of view of 2° or 10° for a reference observer relative to the first glass sheet 1001 (a*R1_65, b*R1_65) and relative to the second glass sheet 1001 (a*R2_65, b*R2_65) in transmission (a*T, b*T) and in reflection.
[0155] In the color space, the characteristic a* is the color position on the green-red axis (-500 to 500), and the characteristic b* is the color position on the blue-yellow axis (-200 to 200).
[0156] For each of the examples and comparative examples, the chromaticity parameters a* and b* were measured and / or calculated in the L*a*b* CIE 1976 color space according to standard ISO 11664-4:2019 with a D65 illuminant under p-polarized light and a field of view of 2° or 10° for a reference observer in transmission and in reflection relative to the second glass sheet 1001 (a*R2_65p, b*R2_65_p).
[0157] The chromaticity index, denoted as Chroma_R2_p, is calculated from the chromaticity parameters a*R2_65_p, b*R2_65_p obtained in reflection relative to the second glass plate 1002. This index represents the purity of the color and is an important parameter for head-up windshield applications.
[0158] The resistance of the surface, denoted as R 2, evaluated with a 4-point measurement method as described in the article Measurement of Sheet Resistivities with the Four-Point Probe, FMSmits, Bell Syst. Tech. J., 711 (1958) or in the standard ASTM F390-11. The measurement is carried out using an RT70V 4-point ohmmeter from Napson.
[0159] All measured and / or calculated results are summarized in Table 4.
[0160] Table 4 CE1 CE2 E1 E2 E3 E4 TST 57.1 52.1 53.4 54.4 52.3 52.7 TE 51.9 46.3 47.7 47.9 45.5 47.4 TL 72.5 72.5 72.5 72.5 72.5 72.5 s 1.27 1.39 1.36 1.33 1.39 1.38 a*T -2.8 -3.0 -4.6 -2.5 -4.5 -2.5 b*T 4.0 3.9 2.7 3.8 4.0 4.1 R1_65 29.8 29.0 29.9 28.5 27.6 29.1 a*R1_65 0.1 0.8 1.1 -0.5 1.0 -0.3 b*R1_65 0.7 2.5 1.4 -1.8 0.7 -0.3 R2 22.4 18.6 17.5 21.3 18.3 22.7 R2_p 18.7 17.1 15.8 18.9 16.9 17.1 a*R2_p 2.3 2.4 2.4 2.4 0.8 2.5 b*R2_65_p 1.0 -0.5 -0.5 -0.7 2.1 0.2 Chroma_R2_p 2.5 2.5 2.5 2.5 2.2 2.5 R2_65 31.3 28.2 27.6 30.9 28.3 31.0 a*R2_65 -0.1 0.7 -0.3 -0.2 -0.7 -1.0 b*R2_65 1.7 -0.9 -1.0 -0.2 1.2 1.3 <![CDATA[R 2 (Oh)]]> 2.56 2.35 2.50 2.45 2.44 2.95
[0161] For comparison purposes, Table 4 shows Examples and Comparative Examples having the same transmittance values.
[0162] exist Figure 4 The values of light transmittance TL and direct solar transmittance TE for the examples (solar circles) and comparative examples (solar circles) are shown in FIG. Also shown is the "solar selectivity" threshold SE, defined as the ratio TL / TE of light transmittance TL to direct solar transmittance TE, as a guide for the eye.
[0163] Compared to comparative example CE1, examples E1 and E2 have lower direct solar transmittance and thus higher solar selectivity values.Examples E3 and E4 both have direct solar transmittance and solar selectivity values comparable to comparative example CE2.
[0164] exist Figure 5 The values of light transmittance TL and total solar transmittance TTS for the examples (solid circles) and comparative examples (open circles) are shown in FIG. Also shown is the "selectivity" threshold s, defined as the ratio of light transmittance TL to total solar transmittance TTS TL / TTS, as a guide for the eye.
[0165] Compared to comparative example CE1, examples E1 and E2 have about 3 to 5% lower total solar transmittance TTS and thus higher solar selectivity values.Examples E3 and E4 have comparable total solar transmittance and solar selectivity values to comparative example CE2.
[0166] All examples E1 to E4 have a reflection of more than 15.5% under p-polarized light and a neutral color with a chromaticity index of at most 2.5. These values are suitable for head-up display applications.
[0167] All of Examples E1 to E4 also have a surface resistance of less than 2.5Ω, which is compatible with heating applications.
[0168] These examples clearly show the advantages of laminated glazings, namely their higher selectivity and color compatibility for windshield head-up display and heating applications.
Claims
1. A laminated glazing (1000), comprising: - a first glass sheet (1001); - a second glass sheet (1002); - a laminating interlayer (1003) in bonding contact with said first glass sheet (1001) and said second glass sheet (1002); a thin layer of functional coating (1004) arranged on the second glass sheet (1002) and comprising, starting from the second glass sheet (1002), a first dielectric module (2001), a metallic functional layer (2002) and a second dielectric module (2003), the metallic functional layer (2002) being located between the first dielectric module (2001) and the second dielectric module (2003); Features: The first dielectric module (2001) and / or the second dielectric module (2003) contain (or include) a tungsten oxide layer (2004a, 2004b), and are characterized in that: - the tungsten oxide layer (2004a, 2004b) is made of pure substoichiometric tungsten oxide WOx, wherein x is preferably 2.55 to 2.98, or - The tungsten oxide layer (2004a, 2004b) is doped tungsten oxide and contains at least one doping element selected from the chemical elements of Group 1 according to the IUPAC nomenclature.
2. The laminated glazing according to claim 1, wherein the optical refractive index of the tungsten oxide layer (2004a, 2004b) decreases monotonically with wavelength from a maximum value greater than 2.4 at 350 nm to a minimum value between 600 nm and 1400 nm, so that the difference between the maximum value and the minimum value is greater than 0.8, preferably greater than 1.0, or even greater than 1.
4.
3. The laminated glazing according to claim 1, wherein the optical extinction coefficient of the tungsten oxide layer (2004a, 2004b) is less than 0.2, or even 0.1 at 500 nm, and less than 2.0, or even less than 1.5 at 1200 nm.
4. The laminated glazing according to any one of claims 1 to 3, wherein the tungsten oxide layer (2004a, 2004b) made of doped tungsten oxide contains a doping element or multiple doping elements in a ratio such that the molar ratio of the element to tungsten or the sum of the molar ratios of each element to tungsten is 0.01 to 0.4, preferably 0.01 to 0.2, or even 0.01 to 0.
1.
5. The laminated glazing according to any one of claims 1 to 4, wherein the tungsten oxide layer (2004a, 2004b) made of doped tungsten oxide contains at least one doping element selected from the group consisting of hydrogen, lithium, sodium, potassium and cesium.
6. The laminated glazing according to claim 5, wherein the tungsten oxide layer (2004a, 2004b) made of doped tungsten oxide contains cesium as a doping element, and the molar ratio of cesium to tungsten is 0.01 to 0.4, preferably 0.01 to 0.
2.
7. The laminated glazing according to any one of claims 1 to 6, wherein the physical thickness of the tungsten oxide layer (2004a, 2004b) is 2 nm to 50 nm, in particular 5 nm to 30 nm, preferably 5 nm to 20 nm.
8. The laminated glazing according to any one of claims 1 to 7, wherein the first dielectric module (2001) and / or the second dielectric module (2002) comprises (or includes) one or more layers having a refractive index of less than 2.45 at 550 nm.
9. The laminated glazing according to any one of claims 1 to 8, wherein the thin layer of functional coating (1004) further comprises a barrier metal coating, preferably based on a nickel and chromium alloy, located above and in contact with the metallic functional layer, and / or a metal barrier lining, preferably based on a nickel and chromium alloy, located below and in contact with the metallic functional layer.
10. The laminated glazing according to any one of claims 1 to 9, wherein the first dielectric module (2001) and / or the second dielectric module (2002) comprises (or includes) a layer based on indium tin mixed oxide, indium zinc mixed oxide, fluorine-doped tin oxide, aluminum-doped zinc oxide, gallium-doped zinc oxide, antimony-doped tin oxide and / or niobium-doped titanium oxide. 11 . The glazing according to claim 10 , wherein the layer has a thickness of 50 nm to 100 nm.
12. The laminated glazing according to any one of claims 1 to 11, wherein the metallic functional layer (2002) is a silver-based layer.
13. A projection device (3000) for a head-up display, comprising: - The laminated glazing (1000) according to any one of claims 1 to 12, A heads-up projector (3001) configured to emit electromagnetic radiation (3002) onto at least one area (3003) of the laminated glazing (1001), the electromagnetic radiation being polarized at least partially according to p-polarization.
14. Use of the laminated glazing (1000) according to any one of claims 1 to 12 for a head-up display in a land, sea or air vehicle, preferably a motor vehicle, a railway vehicle, an aircraft or a ship, in particular a passenger car or a truck.
15. A method for producing a laminated glazing (1000) according to any one of claims 1 to 12, wherein a tungsten oxide layer (2004a, 2004b) made of doped tungsten oxide is deposited by magnetron sputtering using a tungsten oxide target, the oxide target being doped with a chemical element selected from the chemical elements of Group 1 according to the IUPAC nomenclature.
Citation Information
Patent Citations
Head-up display and method for generating a virtual image using a head-up display and use of p-polarized light in a head-up display
DE102014220189A1
A ghost-free automotive head-up display employing a wedged windshield
EP0420228A2
Vehicle glazing with an electroconductive layer
EP0726232A2
Conductive frequency selective surface utilizing arc and line elements
EP1614325A1
Target material of composite tungsten oxide, and method for manufacturing the same
JP2010180449A