Bismaleimide compound, resin composition using same, cured product thereof, and semiconductor element
By introducing cyclic imide bonds and aromatic ring skeletons into bismaleimide resins, the problem of insufficient dielectric characteristics and compatibility in high-frequency applications of existing resins is solved, and high glass transfer temperature and good quality are achieved Bismaleimide compound with photohardening properties is suitable for protective films and insulating films of semiconductor components.
Patent Information
- Application Number
- CN202280095398.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-25
- Filing Date
- 2022-08-31
- Publication Date
- 2024-12-06
AI Technical Summary
The existing long-chain alkyl bismaleimide resins have deteriorated dielectric properties when increasing the glass transfer temperature, and their compatibility and hardening properties with other resins are insufficient, making it difficult to meet the high-frequency application needs of semiconductor components.
Using a bismaleimide compound with a cyclic imide bond, the reaction of aromatic diamine, tetrabasic dianhydride and maleic anhydride is carried out further with a divalent organic diamine with a carbon number of 6 to 200. React to form a bismaleimide compound with an aromatic ring backbone to improve its compatibility with other resins and glass transfer temperature.
The good compatibility of bismaleimide compounds with other resins and high glass transfer temperature are achieved, providing better dielectric properties and photohardening properties, and are suitable for protective films and insulating films of semiconductor components.
Smart Images

Figure CN119095899A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a bismaleimide compound, a resin composition using the same, a cured product thereof, and a semiconductor element. The resin composition of the present invention can be used as a protective film for a semiconductor element, an interlayer insulating film, an insulating film for a rewiring layer, and the like. Background Art
[0002] In recent years, electronic devices have been miniaturized and have become more powerful. In the surface protection films, interlayer insulation films, and insulation films of the rewiring layers of semiconductor elements, wiring has also been required to be miniaturized and denser. In addition, the next generation needs materials suitable for high-frequency bands. As a noise countermeasure, it is necessary to reduce transmission losses, which requires the development of insulating materials with excellent dielectric properties.
[0003] In the past, polyimide resins, polybenzoxazole resins, etc., which are excellent in heat resistance and mechanical properties, have been widely used in surface protection films and interlayer insulating films of semiconductor elements (e.g., Patent Document 1). When polyimide resins or polybenzoxazole resins are used as surface protection films or interlayer insulating films, a method of forming through holes and the like by etching a positive photoresist containing the same resin as these resins is known. However, the problem with this method is that it requires cumbersome steps such as coating and stripping of the photoresist. Therefore, with the purpose of rationalizing the operating steps, some people have begun to study heat-resistant materials that have been given photosensitivity (Patent Document 2).
[0004] It is known that materials such as polyimide resin and polybenzoxazole resin cannot meet the dielectric properties in high-frequency band applications represented by the keyword 5G. In response to this, Patent Document 3 reports that an epoxy resin composition containing an epoxy resin, an active ester compound, and a triazine-containing cresol novolac resin is effective in reducing the dielectric loss tangent, but this material must also be further reduced in dielectric properties for high-frequency applications.
[0005] On the other hand, Patent Document 4 reports that a resin film composed of a resin composition containing a bismaleimide resin having a long-chain alkyl group as a non-epoxy material and a curing agent has excellent low dielectric properties.
[0006] Patent Documents 5 and 6 disclose polyimides using as raw materials dimer diamines and alicyclic diamines derived from dimer acids of aromatic tetracarboxylic acids and unsaturated fatty acids such as octadecenoic acid.
[0007] [Prior art literature]
[0008] [Patent Document]
[0009] [Patent Document 1] Japanese Patent Application Laid-Open No. 11-199557
[0010] [Patent Document 2] Japanese Patent Application Laid-Open No. 11-24271
[0011] [Patent Document 3] Japanese Patent Application Publication No. 2011-132507
[0012] [Patent Document 4] International Publication No. 2016 / 114287
[0013] [Patent Document 5] Japanese Patent Application Publication No. 2017-119361
[0014] [Patent Document 6] Japanese Patent Publication No. 2019-104843. Summary of the invention
[0015] [Problems to be solved by the invention]
[0016] The film described in the above-mentioned patent document 4 is a combination of a bismaleimide resin having a long-chain alkyl group and a hard low-molecular aromatic maleimide. Its compatibility is not preferred and is prone to uneven properties and hardening, making it extremely difficult to achieve the high glass transition temperature (Tg) of more than 200°C required in the semiconductor element application. In addition, in recent years, it is known that the aforementioned bismaleimide resin with a long-chain alkyl group has a trade-off relationship in resin design such as "if the glass transition temperature is increased, the dielectric properties deteriorate, and if the dielectric properties are improved, the glass transition temperature decreases". It is known that if the glass transition temperature is increased, even if it is the same bismaleimide resin with a long-chain alkyl group, resins will condense or separate from each other, and the compatibility of resins is not preferred. In addition, the polyimide described in patent documents 5 and patent documents 6 is difficult to be hardened and used alone, and its compatibility with other resins is not preferred. In addition, polyimide is closed-loop dehydrated during hardening, so for example, when stacking the rewiring layer, holes will be generated according to its use conditions and it cannot be flattened.
[0017] Therefore, an object of the present invention is to provide a bismaleimide compound having good compatibility with other resins and a high glass transition temperature.
[0018] [Methods to solve the problem]
[0019] The inventors of the present application have intensively conducted studies to solve the above problems and, as a result, have found that the following bismaleimide compound (I) can achieve the above objects, thereby completing the present invention.
[0020] That is, the present invention includes the following aspects.
[0021] <1>
[0022] A bismaleimide compound (I) having a cyclic imide bond and obtained by reacting an aromatic diamine (A) represented by the following formula (1), a tetrabasic acid dianhydride (C) and maleic anhydride;
[0023]
[0024] In formula (1), R1 each independently represents a hydrogen atom, a linear or branched alkyl group having 1 to 6 carbon atoms, a halogen atom, a hydroxyl group, or a linear or branched alkoxy group having 1 to 6 carbon atoms. l each independently represents an integer of 1 to 4.
[0025] <2>
[0026] like <1> The bismaleimide compound (I) is obtained by reacting the diamine (A), the tetrabasic acid dianhydride (C), and the maleic anhydride with a divalent organic diamine (B) having 6 to 200 carbon atoms other than the aromatic diamine (A).
[0027] <3>
[0028] like <1> or <2> The bismaleimide compound (I), wherein the bismaleimide compound (I) is represented by the following general formula (2):
[0029]
[0030] In formula (2),
[0031] C independently represents a tetravalent organic group containing a ring structure.
[0032] B is independently a divalent hydrocarbon group having 6 to 200 carbon atoms.
[0033] W is A or B.
[0034] m is 1 to 100, and n is 0 to 100. In addition, the order of each repeating unit indicated by m and n and enclosed in parentheses is not limited, and the bonding pattern may be alternating, block-like, or random.
[0035] A is independently a divalent linking group represented by the following formula (3):
[0036]
[0037] In formula (3), R1 each independently represents a hydrogen atom, a linear or branched alkyl group having 1 to 6 carbon atoms, a halogen atom, a hydroxyl group, or a linear or branched alkoxy group having 1 to 6 carbon atoms. l each independently represents an integer of 1 to 4.
[0038] <4>
[0039] like <1> to <3> The bismaleimide compound (I) described in any one of the above, wherein the tetrabasic acid dianhydride (C) comprises a compound selected from the group consisting of the following formulae (4) to (12):
[0040]
[0041] In formula (7), Y represents C(CF3)2, SO2, CO, an oxygen atom, a direct bond, or a divalent linking group represented by the following formula (13).
[0042]
[0043] <5>
[0044] like <1> to <4> The bismaleimide compound (I) described above is a maleimide of an amine compound represented by the following formula (14):
[0045]
[0046] In formula (14), C independently represents a tetravalent organic group containing a cyclic structure. B independently represents a divalent hydrocarbon group having 6 to 200 carbon atoms. W represents A or B. m represents 1 to 100, and n represents 0 to 100. In addition, the order of each repeating unit marked with m and n and enclosed in parentheses is not limited, and the bonding pattern may be alternating, block-like, or irregular. A independently represents a divalent linking group represented by the following formula (3):
[0047]
[0048] In formula (3), R1 each independently represents a hydrogen atom, a linear or branched alkyl group having 1 to 6 carbon atoms, a halogen atom, a hydroxyl group, or a linear or branched alkoxy group having 1 to 6 carbon atoms. l each independently represents an integer of 1 to 4.
[0049] <6>
[0050] like <1> to <5> The bismaleimide compound (I) described above, wherein the tetrabasic acid dianhydride (C) is a compound of the following formula (15).
[0051]
[0052] <7>
[0053] like <1> to <5> The bismaleimide compound (I) described above, wherein the tetrabasic acid dianhydride (C) is a compound of the following formula (8).
[0054]
[0055] <8>
[0056] like <1> to <5> The bismaleimide compound (I) described above, wherein the tetrabasic acid dianhydride (C) is a compound of the following formula (5).
[0057]
[0058] <9>
[0059] like <1> to <5> The bismaleimide compound (I) described above, wherein the tetrabasic acid dianhydride (C) is a compound of the following formula (9).
[0060]
[0061] <10>
[0062] like <1> to <5> The bismaleimide compound (I) described above, wherein the tetrabasic acid dianhydride (C) is a compound of the following formula (10).
[0063]
[0064] <11>
[0065] A composition comprising <1> to <10> The bismaleimide compound (I) described above and the compound reactive with a maleimide group.
[0066] <12>
[0067] The resin composition according to claim 11, further comprising <1> to <10> One or more selected from the group consisting of maleimide compounds other than any one of the maleimide compounds (I), cyanate compounds, phenol resins, epoxy resins, cyclohexane resins, benzoxazine compounds, carbodiimide compounds, and compounds having an ethylenically unsaturated group.
[0068] <13>
[0069] A composition comprising <1> to <10> The bismaleimide compound (I) described above and a photopolymerization initiator or a curing catalyst.
[0070] <14>
[0071] like <11> to <13> The resin composition described above further comprises a filler.
[0072] <15>
[0073] A cured product of a resin composition, comprising <1> to <10> The bismaleimide compound (I) described above.
[0074] <16>
[0075] A semiconductor device comprising <1> to <10> A surface protection film, an interlayer insulating film or an insulating film for a rewiring layer comprising the bismaleimide compound (I) described above.
[0076] <17>
[0077] A dry film photoresist, comprising: <1> to <10> A composition comprising the bismaleimide compound (I) described above and a photopolymerization initiator.
[0078] [Effects of the Invention]
[0079] The bismaleimide compound (I) of the present invention, especially the bismaleimide compound having an aromatic ring skeleton, has excellent compatibility with resins having different structures, and is therefore easy to use with other resins, and it is easy to complement each other's performance to lead to better performance. In addition, if it is a bismaleimide compound of the present invention, especially a bismaleimide compound having an aromatic ring skeleton, it is possible to provide a bismaleimide resin composition that can provide a cured product with a high glass transition point (Tg). DETAILED DESCRIPTION
[0080] The present invention is described in detail below.
[0081] <Bismaleimide compound (I)>
[0082] The bismaleimide compound (I) of the present invention is a compound having two maleimide groups, and has an aromatic diamine (A) represented by the following formula (1) and a cyclic imide bond. Such a bismaleimide compound (I) can be obtained by reacting an aromatic diamine (A) represented by the following formula (1), a tetrabasic acid dianhydride (C) and maleic anhydride.
[0083]
[0084] In formula (1), R1 each independently represents a hydrogen atom, a linear or branched alkyl group having 1 to 6 carbon atoms, a halogen atom, a hydroxyl group, or a linear or branched alkoxy group having 1 to 6 carbon atoms. l each independently represents an integer of 1 to 4.
[0085] In addition to the aromatic diamine (A), the tetrabasic acid dianhydride (C) and the maleic anhydride, a divalent aliphatic diamine (B) having 6 to 200 carbon atoms is reacted with the aromatic diamine (A) to form an imide bond, thereby introducing the bismaleimide compound.
[0086] The bismaleimide compound (I) is preferably a bismaleimide compound represented by the following general formula (2).
[0087]
[0088] The bismaleimide compound is preferably a maleimide of an amine compound represented by the following formula (14).
[0089]
[0090] In formula (2) and formula (14), C independently represents a tetravalent organic group containing a cyclic structure. B independently represents a divalent hydrocarbon group having a carbon number of 6 to 200. W is A or B. m is 1 to 100, and n is 0 to 100. In addition, the order of each repeating unit marked with m and n and enclosed in parentheses is not limited, and the bonding pattern can be alternating, block, or irregular. A independently represents a divalent linking group represented by the following formula (3).
[0091]
[0092] In formula (3), R1 each independently represents a hydrogen atom, a linear or branched alkyl group having 1 to 6 carbon atoms, a halogen atom, a hydroxyl group, or a linear or branched alkoxy group having 1 to 6 carbon atoms. l each independently represents an integer of 1 to 4.
[0093] The linear or branched alkyl group having 1 to 6 carbon atoms is not particularly limited, and examples thereof include methyl, ethyl, n-propyl, isopropyl, butyl, isobutyl, sec-butyl, and tert-butyl. Among these, alkyl groups having 1 to 4 carbon atoms are more preferred, and methyl, ethyl, n-propyl, and isopropyl are more preferred, in addition to excellent adhesion to chips and substrates, etc., because of good solubility in solvents, low melting point, low water absorption, and good compatibility with other resins.
[0094] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.
[0095] The linear or branched alkoxy group having 1 to 6 carbon atoms is not particularly limited, and examples thereof include methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, 2-methylpropoxy, 1-methylpropoxy, and tert-butoxy. Among these, in addition to excellent adhesion to chips and substrates, alkoxy groups having 1 to 4 carbon atoms are more preferred, and methoxy, ethoxy, n-propoxy, and isopropoxy are more preferred, in terms of good solubility in solvents, low melting points, low water absorption, and good compatibility with other resins.
[0096] As R1, in addition to excellent adhesion to chips and substrates, etc., hydrogen atoms, methyl groups, ethyl groups, hydroxyl groups, methoxy groups and ethoxy groups are more preferred, hydrogen atoms, methyl groups and hydroxyl groups are more preferred, and hydrogen atoms are still more preferred, in terms of good solubility in solvents, low melting point, low water absorption and good compatibility with other resins.
[0097] In the above formula (1) or formula (3), l each independently represents an integer of 1 to 4. As for l, in addition to excellent adhesion to chips and substrates, it is more preferred that R1 is a hydrogen atom, and 4 is more preferred, because it exhibits good solubility in solvents, low melting point, low water absorption, and good compatibility with other resins.
[0098] Specific examples of the aromatic diamine (A) represented by the above formula (1) include meta-xylylenediamine (the following formula (17)), para-xylylenediamine (the following formula (18)), and o-xylylenediamine (the following formula (19)). Meta-xylylenediamine (MXDA: manufactured by Mitsubishi Gas Chemical Co., Ltd.) is easily available as a commercial product. The aromatic diamine (A) represented by the above formula (1) is preferably meta-xylylenediamine (the following formula (17)).
[0099]
[0100] The maleimide compound of the present embodiment is not particularly limited as long as the effects of the present invention can be exerted. From the viewpoint of good solubility in solvents, low melting point, low water absorption and good compatibility with other resins, the weight average molecular weight is preferably 100 to 100,000, and more preferably 500 to 30,000. In addition, in the present embodiment, the "weight average molecular weight" refers to the weight average molecular weight converted to polystyrene standard obtained by gel permeation chromatography (GPC).
[0101] Generally, the light transmittance of maleimide compounds is not preferred. Therefore, if the resin composition described later contains maleimide compounds, light cannot fully reach the photocuring initiator dispersed in the resin composition, and the photocuring initiator is difficult to generate free radicals. Therefore, in general, the photoradical reaction of maleimide compounds is not easy to proceed. Even if the free radical polymerization and dimerization reaction of the maleimide monomer proceed, the reactivity of the photoradical reaction of the maleimide compound is still very low. However, in the maleimide compound of the present embodiment, the maleimide group is bonded to the aromatic ring through the methylene group, and the conjugation length is short. For this reason, the light transmittance is extremely excellent, and the light can fully reach the photocuring initiator, and the photoradical reaction of maleimide occurs efficiently. In addition, when a chloroform solution containing 1% by mass of the maleimide compound is prepared and the light transmittance of the chloroform solution is measured using light with a wavelength of 405nm (h line), the transmittance is more than 3%, showing extremely excellent light transmittance. Therefore, for example, when a printed wiring board having a high-density and high-definition wiring formation (pattern) is manufactured using a direct writing exposure method, the photoradical reaction of maleimide can be efficiently caused even when an active energy line including a wavelength of 405 nm (h line) is used.
[0102] When using active energy rays including a wavelength of 405 nm (h-line), polymerization cannot proceed unless the photocuring initiator absorbs the light with a wavelength of 405 nm (h-line) and generates free radicals. Therefore, when using active energy rays including a wavelength of 405 nm (h-line), it is more preferable to use a photocuring initiator having an absorbance of 0.1 or more at a wavelength of 405 nm (h-line) as the photocuring initiator described later, which exhibits extremely favorable absorption for the light with a wavelength of 405 nm (h-line).
[0103] As mentioned above, the maleimide compound of this embodiment has excellent light transmittance. Therefore, even when light with a wavelength of 405 nm is used, the light can fully reach the photocuring initiator, and a free radical reaction using free radicals generated from the photocuring initiator can be carried out. Therefore, photocuring can be carried out even in a resin composition containing a large amount of the maleimide compound.
[0104] Then, the cured product obtained from the resin composition of the present embodiment has excellent light curing property, heat resistance, and thermal stability, and thus can preferably form a protective film and an insulating layer.
[0105] In addition, in the aforementioned formula (2), B is independently a divalent hydrocarbon group having 6 to 200 carbon atoms, preferably 8 to 100, and more preferably 10 to 50 carbon atoms. Among them, it is more preferred that one or more hydrogen atoms in the aforementioned divalent hydrocarbon group are substituted by an alkyl or alkenyl group having 6 to 200 carbon atoms, preferably 8 to 100, and more preferably 10 to 50 carbon atoms. As a branched divalent hydrocarbon group, it can be any of a saturated aliphatic hydrocarbon group and an unsaturated hydrocarbon group, and it can also have an alicyclic structure or an aromatic ring structure in the middle of the molecular chain. The aforementioned branched divalent hydrocarbon group specifically includes: a hydrocarbon group derived from diamines at both ends, which is called "dimer diamine". In addition, the so-called dimer diamine is formed by replacing two carboxyl groups of a dimer acid belonging to a dimer of an unsaturated fatty acid such as octadecenoic acid with primary amino groups as shown in the following formulas (20) to (25) (see Japanese Patent Publication No. 9-12712, etc.). Specific examples of commercially available products of dimer diamine include: PRIAMINE (registered trademark) 1074 and PRIAMINE (registered trademark) 1075 (both manufactured by Croda Japan Co., Ltd.), and Versamine 551 (manufactured by Cognis Japan Co., Ltd.). These can be used alone or in combination of two or more. The following is a non-limiting general formula of dimer diamine. In each formula, m+n=6 to 17 is more preferred, p+q=8 to 19 is more preferred, and the dotted line portion represents a carbon-carbon single bond or a carbon-carbon double bond.
[0106]
[0107] In addition, the tetrabasic acid dianhydride (C) used in the synthesis of the bismaleimide resin of the present invention is not particularly limited as long as it has two anhydride groups in one molecule. Specific examples of the (C) component include: pyromellitic anhydride, ethylene glycol-bis(anhydrotrimellitate), glycerol-bis(anhydrotrimellitate) monoacetate, 1,2,3,4,-butanetetracarboxylic anhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic anhydride, 3,3',4,4'-benzophenonetetracarboxylic anhydride, 3,3',4,4'-biphenyltetracarboxylic anhydride, 3,3',4,4'-diphenylethertetracarboxylic anhydride, 5-(2,5-dioxo-tetrahydro-3-furanyl)-3-methylcyclohexene-1,2-dicarboxylic anhydride, 3a,4,5,9b-tetrahydro-5-(tetrahydro-2 ,5-dioxo-3-furyl)-naphtho[1,2-c]furan-1,3-dione, 1,2,4,5-cyclohexanetetracarboxylic dianhydride, bicyclo(2,2,2)-oct-7-ene-2,3,5,6-tetracarboxylic dianhydride and bicyclo[2.2.2]octane-2,3,5,6-tetracarboxylic dianhydride, 5,5'-((propane-2,2-diylbis(4,1-phenylene))bis(oxy))bis(isobenzofuran-1,3-dione), 4,4'-oxydiphthalic anhydride, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, 4,4'-bisphenol A dianhydride, etc. Among them, 4,4'-oxydiphthalic anhydride, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, and 4,4'-bisphenol A dianhydride are more preferred from the viewpoint of solvent solubility and adhesion to the substrate.
[0108] The tetrabasic acid dianhydride (C) used in the synthesis of the bismaleimide resin of the present invention preferably contains a compound selected from the group consisting of the following formulae (4) to (12) from the viewpoint of solvent solubility of the bismaleimide resin finally obtained.
[0109]
[0110]
[0111] In formula (7), Y represents C(CF3)2, SO2, CO, an oxygen atom, a direct bond, or a divalent linking group represented by the following formula (13).
[0112]
[0113] In the present invention, the tetrabasic acid dianhydride (C) is more preferably a tetrabasic acid dianhydride (C) represented by the following general formula (15).
[0114]
[0115] In the present invention, the tetrabasic acid dianhydride (C) is more preferably a tetrabasic acid dianhydride (C) represented by the following general formula (8).
[0116]
[0117] In the present invention, the tetrabasic acid dianhydride (C) is more preferably a tetrabasic acid dianhydride (C) represented by the following general formula (5).
[0118]
[0119] In the present invention, the tetrabasic acid dianhydride (C) is more preferably a tetrabasic acid dianhydride (C) represented by the following general formula (9).
[0120]
[0121] In the present invention, the tetrabasic acid dianhydride (C) is more preferably a tetrabasic acid dianhydride (C) represented by the following general formula (10).
[0122]
[0123] In addition, the bismaleimide compound (I) of the present invention may be a bismaleimide compound obtained by reacting the aromatic diamine (A), an organic diamine (B) other than the aromatic diamine (A), the tetracarboxylic dianhydride (C) and the maleic anhydride. By copolymerizing with the organic diamine (B) other than the aromatic diamine (A), the desired physical properties can be controlled to meet the need to further improve the heat resistance of the obtained cured product.
[0124] The organic diamine (B) other than the aromatic diamine (A) (hereinafter referred to as the organic diamine (B) as the case may be) refers to a diamine other than the diamine included in the aromatic diamine (A) in the present invention. Such organic diamine (B) is not particularly limited, and examples thereof include aliphatic diamines such as 1,6-hexamethylenediamine; alicyclic diamines such as 1,4-diaminocyclohexane, 1,3-bis(aminomethyl)cyclohexane, isophoronediamine, and norbornene diamine; 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(aminomethyl)benzene, 1,3-bis(4-aminophenoxy)benzene, Aromatic diamines such as 1,4-diaminobenzene, 1,3-bis(3-aminophenoxy)benzene, 1,4-diaminobenzene, 1,3-diaminobenzene, 2,4-diaminotoluene, and 4,4'-diaminodiphenylmethane; 4,4'-diaminodiphenyl sulfone; 3,3'-diaminodiphenyl sulfone; 4,4-diaminobenzophenone; 4,4-diaminodiphenyl sulfide; 2,2-bis[4-(4-aminophenoxy)phenyl]propane. Of these, aliphatic diamines having 6 to 12 carbon atoms such as 1,6-hexamethylenediamine; and diaminocyclohexanes such as 1,3-bis(aminomethyl)cyclohexane, isophoronediamine, and norbornenediamine are more preferred from the viewpoint of obtaining a cured product having high heat resistance. When the bismaleimide compound (I) of the present invention is obtained by using these organic diamines (B), one of these organic diamines (B) may be used alone or two or more of them may be used in combination.
[0125] The above-mentioned bismaleimide compound (I), especially the bismaleimide compound (I) having an aromatic ring skeleton, has excellent compatibility with resins having different structures and is easy to be used in combination with other resins, and it is easy to make the performances of each other complement each other and lead to better performance. In addition, if it is a bismaleimide compound of the present invention, especially a bismaleimide compound having an aromatic ring skeleton, it is possible to provide a bismaleimide resin composition that has little difference in curability and physical properties when formed into a film or substrate and can provide a cured product with a high glass transition point (Tg).
[0126] <Method for producing bismaleimide compound (I)>
[0127] The method for producing the bismaleimide compound (I) is not particularly limited, and the bismaleimide compound (I) can be efficiently produced by, for example, the method shown below.
[0128] As a basic process, step A is to synthesize amic acid from tetrabasic dianhydride and diamine and perform ring-closing dehydration, then synthesize maleamic acid by reacting maleic anhydride, and finally step B is to seal the molecular chain end with maleimide group by ring-closing dehydration, thereby obtaining a bismaleimide compound.
[0129] In the above-mentioned production method, each step can be roughly divided into two types: the synthesis reaction of amic acid or maleamic acid and the ring-closing dehydration reaction, which are described in detail below.
[0130] In step A, amic acid is first synthesized by reacting a specific tetrabasic acid dianhydride with a specific diamine. This reaction is generally carried out in an organic solvent (eg, a nonpolar solvent or a high-boiling-point aprotic polar solvent) at room temperature (25°C) to 100°C.
[0131] Then, the ring-closing dehydration reaction of the amic acid is carried out under the conditions of 90 to 120° C., while removing the water produced as a by-product of the condensation reaction from the system. In order to promote the ring-closing dehydration reaction, an organic solvent (e.g., a nonpolar solvent, a high-boiling-point aprotic polar solvent, etc.) and an acid catalyst may be added.
[0132] Examples of organic solvents include toluene, xylene, anisole, biphenyl, naphthalene, N,N-dimethylformamide (DMF), dimethyl sulfoxide (DMSO), etc. These can be used alone or in combination of two or more. In addition, examples of acid catalysts include sulfuric acid, methanesulfonic acid, trifluoromethanesulfonic acid, etc. These can be used alone or in combination of two or more.
[0133] The molar ratio of diamine to tetrabasic acid dianhydride is preferably diamine / tetrabasic acid dihydrate = 2.5 to 1.02 / 1.0, and more preferably diamine / tetrabasic acid dianhydride = 2.0 to 1.15 / 1.0. By mixing in this ratio, a copolymer containing amino groups at both ends can be synthesized.
[0134] In step B, the amic acid having amino groups at both ends obtained in step A is reacted with maleic anhydride at room temperature (25° C.) to 100° C. to synthesize maleamic acid, and finally, under the condition of 95 to 120° C., while removing the water produced as a by-product in the system, a closed-loop dehydration is performed to seal the molecular chain ends with maleimide groups to obtain the target bismaleimide compound. If the reaction of sealing the molecular chain ends with maleimide groups is performed at 120° C. or below, side reactions and high molecular weight products are less likely to occur, and thus it is more preferred.
[0135] The bismaleimide compound obtained by this production method has a block copolymer structure, and thus can improve the compatibility of the synthesized resin and make it uniform.
[0136] The compound of the present invention may be purified by a common method, and reprecipitation or the like may be used.
[0137] The composition containing the bismaleimide compound (I) preferably contains a compound reactive with a maleimide group.
[0138] The compound that can react with the maleimide group may include one or more selected from the group consisting of maleimide compounds other than the maleimide compound of the present embodiment (hereinafter also referred to as "other maleimide compounds"), cyanate compounds, phenol resins, epoxy resins, cyclohexane resins, benzoxazine compounds, carbodiimide compounds and compounds having ethylenically unsaturated groups.
[0139] The bismaleimide compound (I) component is preferably 1 to 99% by mass, and more preferably 5 to 95% by mass, in the solid content of the resin of the present invention. Each component of the compound reactive with a maleimide group is described below.
[0140] (Maleimide compounds other than bismaleimide compound (I))
[0141] As other maleimide compounds, there are no particular limitations as long as they are compounds other than the maleimide compound (I) of the present embodiment and have one or more maleimide groups in the molecule. Specific examples thereof include: N-phenylmaleimide, N-cyclohexylmaleimide, N-hydroxyphenylmaleimide, N-anilinophenylmaleimide, N-carboxyphenylmaleimide, N-(4-carboxy-3-hydroxyphenyl)maleimide, 6-maleimidocaproic acid, 4-maleimidobutyric acid, bis(4-maleimidophenyl)methane, 2,2-bis{4-(4-maleimidophenoxy)-phenyl}propane, 4,4-diphenylmethanebismaleimide, bis(3,5-dimethyl-4-maleimidophenyl)methane, bis(3-ethyl-5-methyl-4-maleimidophenyl)methane, bis(3,5- diethyl-4-maleimidophenyl)methane, phenylmethane maleimide, o-phenylene bismaleimide, m-phenylene bismaleimide, p-phenylene bismaleimide, o-phenylene bismethylmaleimide, m-phenylene bismethylmaleimide, p-phenylene bismethylmaleimide, 2,2-bis(4-(4-maleimidophenoxy)-phenyl)propane, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, 1,2-bismaleimidoethane, 1,4-bismaleimidobutane, 1,5-bismaleimidopentane 1,5-bismaleimide-2-methylpentane, 1,6-bismaleimide hexane, 1,6-bismaleimide-(2,2,4-trimethyl)hexane, 1,8-bismaleimide-3,6-dioxaoctane, 1,11-bismaleimide-3,6,9-trioxaundecane, 1,3-bis(maleimidomethyl)cyclohexane, 1,4-bis(maleimidomethyl)cyclohexane, 4,4-diphenyl ether bismaleimide, 4,4-diphenyl sulfone bismaleimide, 1,3-bis(3-maleimidophenoxy)benzene, 1,3-bis(4-maleimidophenoxy)benzene, 4,4-diphenylmethane dimethyl cis- Maleimide, 2,2-bis[4-(4-methylmaleimidephenoxy)phenyl]propane, bis(3,5-dimethyl-4-methylmaleimidephenyl)methane, bis(3-ethyl-5-methyl-4-methylmaleimidephenyl)methane, bis(3,5-diethyl-4-methylmaleimidephenyl)methane, polyphenylmethane maleimide, maleimide compounds represented by polyphenylmethane maleimide formula (6), maleimide compounds represented by formula (7), fluorescein-5-maleimide, prepolymers of these maleimide compounds, or prepolymers of maleimide compounds and amine compounds, etc. These maleimide compounds may be used alone or in combination of two or more.
[0142] As other maleimide compounds represented by formula (26), commercial products may be used, for example, BMI-2300 (trade name) manufactured by Yamato Chemical Industry Co., Ltd. As other maleimide compounds represented by formula (27), commercial products may be used, for example, MIR-3000 (trade name) manufactured by Nippon Kayaku Co., Ltd. As other maleimide compounds represented by formula (28), commercial products may be used, for example, MIR-5000 (trade name) manufactured by Nippon Kayaku Co., Ltd.
[0143]
[0144]
[0145] In the composition of the present embodiment, the total content of other maleimide compounds is not particularly limited, but is more preferably 0.01 to 50 parts by mass based on 100 parts by mass of the resin solid content in the composition of the present embodiment.
[0146] (Cyanate ester compound)
[0147] Cyanate compounds are cyanate compounds obtained by reacting a phenol resin with a cyanogen halide. Specific examples thereof include, but are not limited to, dicyanobenzene, tricyanobenzene, dicyanonaphthalene, dicyanobiphenyl, 2,2'-bis(4-cyanophenyl)propane, bis(4-cyanophenyl)methane, bis(3,5-dimethyl-4-cyanophenyl)methane, 2,2'-bis(3,5-dimethyl-4-cyanophenyl)propane, 2,2'-bis(4-cyanophenyl)ethane, 2,2'-bis(4-cyanophenyl)hexafluoropropane, bis(4-cyanophenyl)sulfone, bis(4-cyanophenyl)sulfide, phenol novolac cyanate, and a hydroxyl group of a phenol / dicyclopentadiene co-condensate converted into a cyanate group.
[0148] In addition, a cyanate compound whose synthesis method is described in Japanese Patent Application Laid-Open No. 2005-264154 is particularly preferred as the cyanate compound because of its low hygroscopicity, flame retardancy, and excellent dielectric properties.
[0149] The cyanate compound may contain a catalyst such as zinc naphthenate, cobalt naphthenate, copper naphthenate, lead naphthenate, zinc octanoate, tin octanoate, lead acetylacetonate, dibutyltin maleate, etc., in order to trimerize the cyanate group to form a sym-triazine ring as required. The catalyst is usually used in an amount of 0.0001 to 0.10 parts by mass, preferably 0.00015 to 0.0015 parts by mass, relative to 100 parts by mass of the total mass of the composition.
[0150] In the composition of the present embodiment, the total content of the cyanate ester compound is not particularly limited, but is more preferably 0.01 to 50 parts by mass based on 100 parts by mass of the resin solid content in the composition of the present embodiment.
[0151] (Phenolic resin)
[0152] As phenol resin, as long as it is a phenol resin with more than two hydroxyl groups in one molecule, generally known ones can be used. For example, bisphenol A type phenol resin, bisphenol E type phenol resin, bisphenol F type phenol resin, bisphenol S type phenol resin, phenol novolac resin, bisphenol A novolac type phenol resin, glycidyl ester type phenol resin, aralkyl novolac type phenol resin, biphenyl aralkyl type phenol resin, cresol novolac type phenol resin, multifunctional phenol resin, naphthol resin, naphthol novolac resin, multifunctional naphthol resin, anthracene type phenol resin, naphthalene skeleton modified novolac type phenol resin, phenol aralkyl type phenol resin, naphthol aralkyl type phenol resin, dicyclopentadiene type phenol resin, biphenyl type phenol resin, alicyclic phenol resin, polyol type phenol resin, phosphorus-containing phenol resin, phenol resin containing polymerizable unsaturated hydrocarbon group and hydroxyl-containing polysilicone resin, etc. can be listed, but not particularly limited. These phenol resins can be used alone or two or more can be appropriately mixed for use.
[0153] In the composition of the present embodiment, the total content of the phenol resin is not particularly limited, but is more preferably 0.01 to 50 parts by mass based on 100 parts by mass of the resin solid content in the composition of the present embodiment.
[0154] The epoxy resin is not particularly limited, and generally known epoxy resins can be used. Examples thereof include bisphenol A epoxy resin, bisphenol E epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, bisphenol A novolac epoxy resin, biphenyl epoxy resin, phenol novolac epoxy resin, cresol novolac epoxy resin, xylene novolac epoxy resin, multifunctional phenol epoxy resin, naphthalene epoxy resin, naphthalene skeleton modified novolac epoxy resin, naphthalene ether epoxy resin, phenol aralkyl epoxy resin, anthracene epoxy resin, trifunctional phenol epoxy resin, quadrifunctional phenol epoxy resin, tri-glycidyl isocyanurate Acid esters, glycidyl ester type epoxy resins, alicyclic epoxy resins, dicyclopentadiene novolac type epoxy resins, biphenyl novolac type epoxy resins, phenol aralkyl novolac type epoxy resins, naphthol aralkyl novolac type epoxy resins, aralkyl novolac type epoxy resins, naphthol aralkyl type epoxy resins, dicyclopentadiene type epoxy resins, polyol type epoxy resins, phosphorus-containing epoxy resins, glycidylamine, compounds obtained by epoxidizing double bonds of butadiene, etc., compounds obtained by reacting hydroxyl-containing polysiloxane resins with epichlorohydrin, and halides thereof. These epoxy resins may be used alone or in combination of two or more thereof.
[0155] In the composition of the present embodiment, the total content of the epoxy resin is not particularly limited, but is more preferably 0.01 to 50 parts by mass based on 100 parts by mass of the resin solid content in the composition of the present embodiment.
[0156] (Oxycyclobutane resin)
[0157] Oxycyclobutane resin can use generally known. For example, alkyloxycyclobutanes such as oxycyclobutane, 2-methyloxycyclobutane, 2,2-dimethyloxycyclobutane, 3-methyloxycyclobutane, 3,3-dimethyloxycyclobutane, 3-methyl-3-methoxymethyloxycyclobutane, 3,3-bis(trifluoromethyl)perfluorooxycyclobutane, 2-chloromethyloxycyclobutane, 3,3-bis(chloromethyl)oxycyclobutane, biphenyl-type oxycyclobutane, OXT-101 (manufactured by Toagosei Co., Ltd., trade name) and OXT-121 (manufactured by Toagosei Co., Ltd., trade name), etc., are not particularly limited. These oxycyclobutane resins can be used alone, or two or more kinds can be appropriately mixed for use.
[0158] In the composition of the present embodiment, the total content of the oxetane resin is not particularly limited, but is more preferably 0.01 to 40 parts by mass based on 100 parts by mass of the resin solid content in the composition of the present embodiment.
[0159] (Benzoxazine compounds)
[0160] As the benzoxazine compound, any generally known compound having two or more dihydrobenzoxazine rings in one molecule can be used. Examples thereof include bisphenol A benzoxazine BA-BXZ (manufactured by Konishi Chemical Co., Ltd., trade name), bisphenol F benzoxazine BF-BXZ (manufactured by Konishi Chemical Co., Ltd., trade name), bisphenol S benzoxazine BS-BXZ (manufactured by Konishi Chemical Co., Ltd., trade name), phenolphthalein benzoxazine, etc., but are not particularly limited. These benzoxazine compounds may be used alone or in combination of two or more.
[0161] In the composition of the present embodiment, the total content of the benzoxazine compounds is not particularly limited, but is more preferably 0.01 to 40 parts by mass based on 100 parts by mass of the resin solid content in the composition of the present embodiment.
[0162] (Carbodiimide compound)
[0163] As a carbodiimide compound, there is no particular limitation as long as there are at least one or more carbodiimide groups in the molecule, and generally known ones can be used. For example, dicyclohexylcarbodiimide, diisopropylcarbodiimide, dimethylcarbodiimide, diisobutylcarbodiimide, dioctylcarbodiimide, tert-butylisopropylcarbodiimide, diphenylcarbodiimide, di-tert-butylcarbodiimide, di-β-naphthylcarbodiimide, N,N'-di-2,6-diisopropylphenylcarbodiimide, 2,6,2',6'-tetraisopropyldiphenylcarbodiimide, cyclic carbodiimide, CARBODILITE (registered trademark: Nisshinbo Chemical Co., Ltd.), and Stabaxol (registered trademark: LANXESS Deutschland GmbH) and other polycarbodiimides can be used alone. One of these carbodiimide compounds can be used alone, or two or more can be appropriately mixed and used.
[0164] In the composition of the present embodiment, the total content of the carbodiimide compound is not particularly limited, but is more preferably 0.01 to 40 parts by mass based on 100 parts by mass of the resin solid content in the composition of the present embodiment.
[0165] (Compound having ethylenically unsaturated group)
[0166] The compound having an ethylenically unsaturated group is not particularly limited as long as it has an ethylenically unsaturated group in one molecule.
[0167] Specific examples of the compound having an ethylenically unsaturated group include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, lauryl (meth)acrylate, polyethylene glycol (meth)acrylate, polyethylene glycol (meth)acrylate monomethyl ether, phenyl ethyl (meth)acrylate, isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, tetrahydrofuran methyl (meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, nonanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene di(meth)acrylate, polyethylene glycol di(meth)acrylate, tris(meth)acryloyloxyethyl isocyanate, polypropylene glycol dimethacrylate, (Meth)acrylate, adipic acid epoxy di(meth)acrylate, bisphenol ethylene oxide di(meth)acrylate, hydrogenated bisphenol ethylene oxide (meth)acrylate, bisphenol di(meth)acrylate, ε-caprolactone modified hydroxypivalate neopentyl glycol di(meth)acrylate, ε-caprolactone modified dipentaerythritol hexa(meth)acrylate, ε-caprolactone modified dipentaerythritol poly(meth)acrylate, dipentaerythritol poly(meth)acrylate, trimethylolpropane tri(meth)acrylate, triethylolpropane tri(meth)acrylate and ethylene oxide adducts thereof; pentaerythritol tri(meth)acrylate and ethylene oxide adducts thereof; pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate and ethylene oxide adducts thereof, etc.
[0168] In addition, specific examples of compounds having ethylenically unsaturated groups can also be listed as: urethane (meth)acrylates having both a (meth)acryloyl group and a urethane bond in the same molecule; polyester (meth)acrylates having both a (meth)acryloyl group and an ester bond in the same molecule; epoxy (meth)acrylates derived from epoxy resins having a (meth)acryloyl group; reactive oligomers using these bonds in combination, etc.
[0169] Examples of urethane (meth)acrylates include reaction products of a hydroxyl group-containing (meth)acrylate and a polyisocyanate and other alcohols used as needed. Examples include urethane (meth)acrylates obtained by reacting hydroxyalkyl (meth)acrylates such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxybutyl (meth)acrylate; glycerol (meth)acrylates such as glycerol mono(meth)acrylate and glycerol di(meth)acrylate; and sugar alcohol (meth)acrylates such as pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate with toluene diisocyanate, hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, isophorone diisocyanate, norbornene diisocyanate, xylene diisocyanate, hydrogenated xylene diisocyanate, dicyclohexyl methylene diisocyanate, and polyisocyanates such as triisocyanates and biuret reaction products thereof.
[0170] Examples of the polyester (meth)acrylates include: monofunctional (poly)ester (meth)acrylates such as caprolactone-modified 2-hydroxyethyl (meth)acrylate, ethylene oxide and / or propylene oxide-modified phthalic acid (meth)acrylate, ethylene oxide-modified succinic acid (meth)acrylate, and caprolactone-modified tetrahydrofuran methyl (meth)acrylate; di(poly)ester (meth)acrylates such as hydroxypivalate neopentyl glycol di(meth)acrylate, caprolactone-modified hydroxypivalate neopentyl glycol di(meth)acrylate, and epichlorohydrin-modified phthalic acid di(meth)acrylate; and mono-, di-, or tri(meth)acrylates of triols obtained by adding 1 mol or more of cyclic lactone compounds such as ε-caprolactone, γ-butyrolactone, and δ-valerolactone to 1 mol of trimethylolpropane or glycerol.
[0171] In addition, examples include: mono-, di-, tri- or tetra-(meth)acrylates of triols obtained by adding 1 mol or more of cyclic lactone compounds such as ε-caprolactone, γ-butyrolactone, δ-valerolactone, etc. to 1 mol of pentaerythritol, dimethylolpropane, trimethylolpropane or tetramethylolpropane; mono- or poly-(meth)acrylates of triols obtained by adding 1 mol or more of cyclic lactone compounds such as ε-caprolactone, γ-butyrolactone, δ-valerolactone, etc. to 1 mol of dipentaerythritol; and mono- or poly-(meth)acrylates of triols, tetraols, pentaols or hexaols, which are polyols.
[0172] In addition, examples include: (meth)acrylates of polyester polyols which are reaction products of diol components such as (poly)ethylene glycol, (poly)propylene glycol, (poly)tetramethylene glycol, (poly)butylene glycol, 3-methyl-1,5-pentanediol, and hexanediol with polyacids such as maleic acid, fumaric acid, succinic acid, adipic acid, phthalic acid, isophthalic acid, hexahydrophthalic acid, tetrahydrophthalic acid, dimer acid, sebacic acid, azelaic acid, and sodium 5-sulfoisophthalate, and their anhydrides; (meth)acrylates of cyclic lactone-modified polyester diols composed of diol components, polyacids and their anhydrides and ε-caprolactone, γ-butyrolactone, δ-valerolactone, and the like; and the like.
[0173] Epoxy (meth) acrylates are compounds having an epoxy group and a carboxylic acid ester compound of (meth) acrylic acid. Examples thereof include phenol novolac epoxy (meth) acrylate, cresol novolac epoxy (meth) acrylate, trishydroxyphenylmethane epoxy (meth) acrylate, dicyclopentadienol epoxy (meth) acrylate, bisphenol A epoxy (meth) acrylate, bisphenol F epoxy (meth) acrylate, biphenol epoxy (meth) acrylate, bisphenol A novolac epoxy (meth) acrylate, naphthalene skeleton-containing epoxy (meth) acrylate, glyoxal epoxy (meth) acrylate, heterocyclic epoxy (meth) acrylate, and anhydride-modified epoxy acrylates thereof.
[0174] Specific examples of the compound having an ethylenically unsaturated group include vinyl ethers such as ethyl vinyl ether, propyl vinyl ether, hydroxyethyl vinyl ether, and ethylene glycol divinyl ether; styrenes such as styrene, methyl styrene, ethyl styrene, and divinylbenzene; or compounds having a vinyl group such as triallyl isocyanate, trimethylallyl isocyanate, and bisallylnadic imide.
[0175] As the compound having an ethylenically unsaturated group, commercially available products can be used, and examples thereof include KAYARAD (registered trademark) ZXR-801H (trade name, manufactured by Nippon Kayaku Co., Ltd.), propylene glycol monomethyl ether acetate of a dicyclopentadiene type epoxy acrylate compound (KAYARAD (registered trademark) ZXR-1806H (trade name), KAYARAD (registered trademark) ZXR-1810H (trade name), and KAYARAD (registered trademark) ZXR-1889H (trade name), manufactured by Nippon Kayaku Co., Ltd.). These compounds having an ethylenically unsaturated group may be used alone or in combination of two or more.
[0176] In the composition of the present embodiment, the total content of the compound having an ethylenically unsaturated group is not particularly limited, but is more preferably 0.01 to 60 parts by mass based on 100 parts by mass of the resin solid content in the composition of the present embodiment.
[0177] The aforementioned composition contains ingredients other than the compound represented by the aforementioned general formula (2). Other ingredients contained in the aforementioned resin composition include, for example, an organic solvent, a photopolymerization initiator, a hardener having a reactive group that can react with a maleimide group, a hardening catalyst, or a close-fitting enhancer such as a coupling agent, a filler, etc. Various ingredients other than the aforementioned may also be used in conjunction with the purpose and usage of the resin composition, without particular limitation. From the perspective of easy operation, a resin composition containing an organic solvent is more preferred.
[0178] Furthermore, since the compound of the present invention can undergo a self-polymerization reaction, it can be used without using a photopolymerization initiator, a curing agent, a curing catalyst, and the like.
[0179] (Photopolymerization Initiator)
[0180] The bismaleimide compound represented by the general formula (2) can be self-polymerized alone, but the compound represented by the general formula (2) can also be used together with a photopolymerization initiator or a curing catalyst to form a composition, and then self-polymerized. By using a photopolymerization initiator together, it can be self-polymerized by irradiation with light, and by using a curing catalyst together, the heating temperature during self-polymerization can be lower than when no catalyst is used.
[0181] There is no particular limitation on the photopolymerization initiator that can be used together when self-polymerization is performed, and any photopolymerization initiator that is used in the past can be appropriately used. Specific examples of photopolymerization initiators include acetophenone, 2,2-dimethoxyacetophenone, p-dimethylaminoacetophenone, Michelle's ketone, diphenylethylenedione, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin n-propyl ether, benzoin isopropyl ether, benzoin n-butyl ether, benzyl dimethyl ketal, thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,2-dimethoxy-1,2-diphenylethane-1-one, 1-hydroxy-cyclohexyl-phenyl-ketone, 2-hydroxy-2-methyl-1-phenyl-propane-1-one, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propane-1-one, 2-hydroxy-1- {4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propane-1-one, 2-methyl-1-(4-methylthiophenyl)-2-N-morpholinopropane-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 1-[4-(phenylthio)phenyl]-1,2-octanedione=2-(O-benzoyloxime), 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone 1-(O-acetyloxime), 2,4-dimethylthioxanthone, etc. These photopolymerization initiators may be used alone or in combination of two or more.
[0182] Among these, from the viewpoint that fine patterns can be formed using a reduced projection exposure machine (stepper; light source wavelength: 365nm, 436nm) that is standardly used in the manufacturing steps of semiconductor protective films, etc., it is more preferred to use one that efficiently generates free radicals at an exposure wavelength of 310nm to 436nm (more preferably 365nm). Preferred examples of the photopolymerization initiator include 1-[4-(phenylthio)phenyl]-1,2-octanedione=2-(O-benzoyloxime) (manufactured by BASF Japan, “IRGACURE OXE-01”), 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone 1-(O-acetyloxime) (manufactured by BASF Japan, “IRGACURE OXE-02”), 2,4-dimethylthioxanthone (manufactured by Nippon Kayaku Co., Ltd., “DETX-S”), and 2-methyl-1-[4-(methylthio)phenyl]-2-N-morpholinopropane-1-one (manufactured by IGM Resins BV, “Omirad 907”).
[0183] The amount of the photopolymerization initiator used is preferably 0.1 to 20 parts by mass, and more preferably 1 to 5 parts by mass, based on 100 parts by mass of the compound represented by formula (1).
[0184] A photopolymerization initiator and a sensitizer may be used together. The sensitizer that can be used together is not particularly limited as long as it is conventionally known, and examples thereof include 4,4′-bis(diethylamino)benzophenone and the like.
[0185] The amount of the sensitizer used is preferably 2 parts by mass or less, more preferably 0.05 to 0.5 parts by mass, based on 100 parts by mass of the compound represented by formula (2). The combined use of a sensitizer can increase the sensitivity to light during self-polymerization.
[0186] (Hardening Catalyst)
[0187] The curing catalyst that can be used in combination when self-polymerizing is not particularly limited as long as it can promote the self-polymerization of the maleimide groups at both ends of the compound represented by formula (1) of the present invention by heating, and can be appropriately used in the past. Specific examples of the curing catalyst include imidazoles such as 2-methylimidazole, 2-ethylimidazole, 2-phenylimidazole, 2-ethyl-4-methylimidazole, 2-undecylimidazole and 1-cyanoethyl-2-ethyl-4-methylimidazole, triethylamine, triethylenediamine, 2-(dimethylaminomethyl)phenol, 1,8-diaza-bicyclo(5,4,0)undecene-7, 3-(dimethylaminomethyl)phenol and benzyldimethylamine, triphenylphosphine, tributylamine, Phosphines such as octyl phosphine and trioctyl phosphine, organic metal salts such as tin octanoate, zinc octanoate, dibutyltin maleate, zinc naphthenate, cobalt naphthenate and tin octadecenoate, metal chlorides such as zinc chloride, aluminum chloride and tin chloride, organic peroxides such as di-tert-butyl peroxide and diisopropylphenyl peroxide, azo compounds such as azobisisobutyronitrile and azobisdimethylvaleronitrile, mineral acids such as hydrochloric acid, sulfuric acid and phosphoric acid, Lewis acids such as boron trifluoride, salts such as sodium carbonate and lithium chloride, etc.
[0188] The amount of the curing catalyst used is preferably 10 parts by mass or less, and more preferably 1 part by mass to 5 parts by mass, based on 100 parts by mass of the compound represented by formula (1).
[0189] The curing agent of the present invention is not particularly limited, and a conventionally used compound can be appropriately used. The curing agent is not particularly limited as long as it is a compound having a functional group (or structure) such as an amine group, a cyanate group, a phenolic hydroxyl group, an alcoholic hydroxyl group, etc. that can undergo a cross-linking reaction with the maleimide compound. In addition, it is not harmful to use a maleimide compound other than the maleimide compound of the present invention in combination.
[0190] (Organic Solvent)
[0191] The organic solvent is not particularly limited, and examples thereof include γ-butyrolactone, ethyl lactate, propylene glycol monomethyl ether acetate, benzyl acetate, n-butyl acetate, ethoxyethyl propionate, 3-methylmethoxy propionate, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, hexamethylphosphoramide, tetramethylene sulfone, cyclohexanone, cyclopentanone, diethyl ketone, diisobutyl ketone, and methyl amyl ketone. These organic solvents may be used alone or in combination of two or more. From the viewpoint of improving the operability of the composition, it is more preferred to use an organic solvent in combination.
[0192] The content of the organic solvent in the composition of the present invention is not particularly limited. Generally, the content of the solvent in the composition is 95% by mass or less, and more preferably 20% by mass to 90% by mass.
[0193] (Coupling agent)
[0194] The silane coupling agent is not particularly limited, and examples thereof include 3-chloropropyltrimethoxysilane, vinyltrichlorosilane, vinyltriethoxysilane, vinyltrimethoxysilane, vinyl / tris(2-methoxyethoxy)silane, 3-methacryloxypropyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, and 3-ureidopropyltriethoxysilane, etc. These may be used alone or in combination of two or more.
[0195] Silane coupling agent and compound of the present invention etc. (compound, self-polymerization compound, benzoxazole) are non-reactive, therefore, except the component acting on the substrate interface, can exist as residual component after hardening.Therefore, if close fit enhancer is used in a large amount, there is the doubt that causes the adverse effects such as physical property reduction.According to substrate type, as long as a small amount can play the effect, from this point of view, it is advisable to use in the scope of not causing adverse effects.Relative to composition, its use ratio is usually below 15 mass %, more preferably more than 0 mass % and below 5 mass %, but the upper limit of use ratio can change according to substrate type.
[0196] (Thermoplastic resin)
[0197] Examples of thermoplastic resins include polyethersulfone, polystyrene, and polycarbonate. Examples of colorants include phthalocyanine blue, phthalocyanine green, iodine green, crystal violet, titanium oxide, carbon black, and naphthalene black. Examples of thickeners include orben, benton, and montmorillonite. Examples of thermal polymerization inhibitors include hydroquinone and 2,6-di-tert-butyl-p-methylphenol. Examples of defoamers include silicone-based, fluorine-based, and polymer-based defoamers.
[0198] The amount of these additives used in the composition of the present invention is preferably, for example, 30% by mass or less, respectively, but can be appropriately increased or decreased depending on the intended use.
[0199] (Filling material)
[0200] The resin composition of the present embodiment may further contain a filler in order to improve various properties such as coating properties and heat resistance. As the filler, it is more preferable that the filler has insulating properties and does not inhibit the permeability to the wavelength of 405 nm (h line). The filler is not particularly limited, and examples thereof include: silica (e.g., natural silica, fused silica, amorphous silica, hollow silica, etc.), aluminum compounds (e.g., diaspore, aluminum hydroxide, aluminum oxide, aluminum nitride, etc.), boron compounds (e.g., boron nitride, etc.), magnesium compounds (e.g., magnesium oxide, magnesium hydroxide, etc.), calcium compounds (e.g., calcium carbonate, etc.), molybdenum compounds (e.g., molybdenum oxide, zinc molybdate, etc.), barium compounds (e.g., barium sulfate, barium silicate, etc.), talc (e.g., natural talc, calcined talc, etc.), mica (MICA), glass (e.g., short fiber glass, spherical glass, fine powder glass (e.g., E glass, T glass, D glass, etc.), silicone powder, fluororesin-based fillers, urethane resin-based fillers, (meth) acrylic resin-based fillers, polyethylene-based fillers, styrene / butadiene rubber, silicone rubber, etc. These fillers may be used alone or in combination of two or more.
[0201] Among these, more preferred are at least one selected from the group consisting of silica, diaspore, barium sulfate, silicone powder, fluororesin fillers, urethane resin fillers, (meth)acrylic resin fillers, polyethylene fillers, styrene / butadiene rubber and silicone rubber.
[0202] These fillers may be surface-treated with a silane coupling agent or the like described below.
[0203] From the viewpoint of improving the heat resistance of the cured product obtained by curing the resin composition of the present embodiment and obtaining good coating properties, silicon dioxide is more preferred, and fused silica is more preferred. Specific examples of silicon dioxide include: SFP-130MC manufactured by Denka Co., Ltd., SC2050-MB, SC1050-MLE, YA010C-MFN, and YA050C-MJA manufactured by Admatechs Co., Ltd.
[0204] The particle size of the filler is not particularly limited, but is generally 0.005 to 100 μm, and more preferably 0.01 to 50 μm.
[0205] In the resin composition of the present embodiment, the content of the filler is not particularly limited. From the viewpoint of making the heat resistance of the cured product good, relative to 100 parts by mass of the resin solids in the resin composition, it is preferably less than 1000 parts by mass, more preferably less than 500 parts by mass, and most preferably less than 300 parts by mass. In addition, in the case of containing a filler, the lower limit is not particularly limited. From the viewpoint of being able to obtain the effect of improving various characteristics such as film coating and heat resistance, relative to 100 parts by mass of the resin solids in the resin composition, it is usually 1 part by mass.
[0206] Other components that may be contained in the resin composition of the present invention include various additives such as a colorant, a thickener, a thermal polymerization inhibitor, a defoaming agent, and a leveling agent.
[0207] The hardened material containing the above-mentioned bismaleimide compound (I) is hardened to form the resin composition of the present embodiment. The hardened material is not particularly limited, and can be obtained, for example, by the following method: after the resin composition is melted or dissolved in a solvent, it is injected into a mold, and hardened under general conditions using heat or light. In the case of thermal hardening, the hardening temperature is not particularly limited, and from the viewpoint of efficiently hardening and preventing the hardened material from deteriorating, it is more preferably in the range of 120°C to 300°C. In the case of light hardening, the wavelength region of the light is not particularly limited, and it is more preferably hardened in the range of 100nm to 500nm where hardening is efficiently performed with a photopolymerization initiator, etc.
[0208] The heat-resistant resin coating formed by the resin composition of the present invention can be used for electronic parts such as semiconductor devices and multilayer wiring boards, and organic EL display devices. Specifically, it is suitable for use in semiconductor passivation films, surface protection films of semiconductor elements, interlayer insulation films, insulation films of rewiring layers, interlayer insulation films of multilayer wiring for high-density mounting, interlayer insulation films of electronic parts such as sensors or surface acoustic wave (SAW) filters, and insulation films or planarization layers of organic electroluminescent elements, but is not limited to these, and various structures can be formed.
[0209] The compounds and compositions of the present invention can also be used in the form of dry film photoresists. That is, after the compounds and compositions of the present invention are coated on the base film using a roller coater, a die coater, a blade coater, a coating rod, a gravure coater, etc., they are dried in a drying oven set at 45°C to 140°C to remove a predetermined amount of solvent, and a protective film is laminated as required, thereby forming a dry film photoresist. At this time, the thickness of the photoresist on the base film is adjusted to 2μm to 200μm. As base films and protective films, for example, films of polyester, polypropylene, polyethylene, TAC, polyimide, etc. can be used. These films can also be treated with a silicone release agent or a non-silicone release agent as required. If supplied as a dry film photoresist, the steps of coating on a support and drying can be omitted, and the photosensitive resin composition of the present invention can be used more simply.
[0210] [Example]
[0211] The present invention is described in more detail below with reference to the following examples and comparative examples, but the present invention is not limited to the following examples. In addition, the "parts" and "%" in the examples are based on mass. In addition, the evaluation of compatibility, dielectric properties, and heat resistance (glass transition temperature (Tg)) in each example and comparative example was performed in the following manner.
[0212] The conditions for measuring the molecular weight are as follows.
[0213] Model: GPC TOSOH HLC-8220GPC
[0214] Column: Super HZM-N
[0215] Solvent: THF (tetrahydrofuran); 0.35 ml / min, 40°C
[0216] Detector: RI (differential refractometer)
[0217] Molecular weight standard: polystyrene
[0218] Synthesis Example 1 (I-1)
[0219] 162 g of toluene and 162 g of N-methylpyrrolidone were placed in a 1 L round bottom flask equipped with a thermometer, reflux cooler, Dean-Stark apparatus, powder inlet, nitrogen inlet and stirring device. Then, 32.4 g (0.24 mol) of m-xylene diamine (Mitsubishi Gas Chemical Co., Ltd.) was added, and then 22.9 g (0.24 mol) of methanesulfonic acid was slowly added to form a salt. After stirring for about 10 minutes to mix, 4,4'-(hexafluoroisopropylidene) diphthalic anhydride (52.8 g, 0.12 mol) was slowly added to the stirred mixture. The mixture was heated for 6 hours and refluxed to form an amine-terminated diimide. At this time, the theoretical amount of water generated by the condensation was obtained. The reaction mixture was cooled to below room temperature, and 28.0 g (0.29 mol) of maleic anhydride was added to the flask. The mixture was refluxed for another 8 hours to obtain the expected amount of generated water. After cooling to room temperature, the organic layer was washed with water (100 ml x 5 times) to remove salts and unreacted raw materials to obtain a varnish of a bismaleimide compound. Then, the varnish was dropped into 1,000 g of methanol, and a reprecipitation step was performed, the solvent was removed and dried, and 78 g (yield 78%, Mw = 3,600) (I-1) of the target light brown solid bismaleimide compound was obtained.
[0220] Synthesis Example 2 (I-2)
[0221] 165 g of toluene and 165 g of N-methylpyrrolidone were placed in a 1L round-bottom flask equipped with a thermometer, reflux cooler, Dean-Stark apparatus, powder inlet, nitrogen inlet and stirring device. Next, 26.6 g (0.20 mol) of m-xylene diamine (Mitsubishi Gas Chemical Co., Ltd.) and 11.7 g (0.02 mol) of dimer diamine (PRIAMINE (registered trademark) 1075, Croda Japan Co., Ltd.) were added, and then 20.9 g (0.22 mol) of methanesulfonic acid was slowly added to form a salt. After stirring for about 10 minutes to mix, 4,4'-(hexafluoroisopropylidene) diphthalic anhydride (48.2 g, 0.11 mol) was slowly added to the stirred mixture. The mixture was heated and refluxed for 6 hours to form an amine-terminated diimide. At this point, the theoretical amount of water generated by the condensation can be obtained. The reaction mixture is cooled to below room temperature, and 25.5g (0.26mol) of maleic anhydride is added to the flask. The mixture is refluxed for another 8 hours to obtain the expected amount of water. After cooling to room temperature, the organic layer is washed with water (100ml×5 times) to remove salts and unreacted raw materials to obtain a varnish of the bismaleimide compound. Then, the varnish is dropped into 1,000g of methanol, and a reprecipitation step is performed to remove the solvent and dry it, thereby obtaining 72g (yield 72%, Mw=4,000) (I-2) of the target light brown solid bismaleimide compound.
[0222] Synthesis Example 3 (I-3)
[0223] 165 g of toluene and 165 g of N-methylpyrrolidone were placed in a 1L round-bottom flask equipped with a thermometer, reflux cooler, Dean-Stark apparatus, powder inlet, nitrogen inlet and stirring device. Then, 29.7 g (0.22 mol) of m-xylenediamine (Mitsubishi Gas Chemical Co., Ltd.) was added, and then 21.0 g (0.22 mol) of methanesulfonic acid was slowly added to form a salt. After stirring for about 10 minutes to mix, 4,4'-bisphenol A dianhydride (56.8 g, 0.11 mol) was slowly added to the stirred mixture. The mixture was heated for 6 hours and refluxed to form an amine-terminated diimide. At this point, the theoretical amount of water generated by the condensation was obtained. The reaction mixture was cooled to below room temperature, and 25.7 g (0.26 mol) of maleic anhydride was added to the flask. The mixture was refluxed for another 8 hours to obtain the expected amount of water generated. After cooling to room temperature, the organic layer was washed with water (100 ml x 5 times) to remove salts and unreacted raw materials to obtain a varnish of a bismaleimide compound. Then, the varnish was dropped into 1,000 g of methanol, and a reprecipitation step was performed, and the solvent was removed and dried to obtain 78 g (yield 80%, Mw = 4,500) of the target light brown solid bismaleimide compound (I-3).
[0224] Synthesis Example 4 (I-4)
[0225] 150 g of toluene and 150 g of N-methylpyrrolidone were placed in a 1L round-bottom flask equipped with a thermometer, reflux cooler, Dean-Stark apparatus, powder inlet, nitrogen inlet and stirring device. Then, 43.9 g (0.32 mol) of m-xylene diamine (Mitsubishi Gas Chemical Co., Ltd.) was added, and then 31.0 g (0.32 mol) of methanesulfonic acid was slowly added to form a salt. After stirring for about 10 minutes to mix, 1,2,4,5-cyclohexanetetracarboxylic dianhydride (36.1 g, 0.16 mol) was slowly added to the stirred mixture. The mixture was heated for 6 hours and refluxed to form an amine-terminated diimide. At this time, the theoretical amount of water generated by the condensation was obtained. The reaction mixture was cooled to below room temperature, and 37.9 g (0.38 mol) of maleic anhydride was added to the flask. The mixture was refluxed for another 8 hours to obtain the expected amount of generated water. After cooling to room temperature, the organic layer was washed with water (100 ml x 5 times) to remove salts and unreacted raw materials to obtain a varnish of a bismaleimide compound. Then, the varnish was dropped into 1,000 g of methanol, and a reprecipitation step was performed, the solvent was removed and dried, and 78 g (yield 78%, Mw = 3,000) of the target white solid bismaleimide compound (I-4) was obtained.
[0226] Synthesis Example 5 (I-5)
[0227] 150 g of toluene and 150 g of N-methylpyrrolidone were placed in a 1 L round bottom flask equipped with a thermometer, reflux cooler, Dean-Stark apparatus, powder inlet, nitrogen inlet and stirring device. Then, 41.2 g (0.30 mol) of m-xylene diamine (Mitsubishi Gas Chemical Co., Ltd.) was added, and then 29.1 g (0.30 mol) of methanesulfonic acid was slowly added to form a salt. After stirring for about 10 minutes to mix, 5-(2,5-dioxotetrahydrofuranyl)-3-methyl-3-cyclohexene-1,2-dicarboxylic dianhydride (40.0 g, 0.15 mol) was slowly added to the stirred mixture. The mixture was heated for 6 hours and refluxed to form an amine-terminated diimide. At this time, the theoretical amount of water generated by the condensation was obtained. The reaction mixture was cooled to below room temperature, and 35.6 g (0.36 mol) of maleic anhydride was added to the flask. The mixture was refluxed for another 8 hours to obtain the expected amount of generated water. After cooling to room temperature, the organic layer was washed with water (100 ml x 5 times) to remove salts and unreacted raw materials to obtain a varnish of the bismaleimide compound. Then, the varnish was dropped into 1,000 g of methanol, and a reprecipitation step was performed to remove the solvent and dry it, thereby obtaining 75 g (yield 75%, Mw = 3,500) (I-5) of the target white solid bismaleimide compound.
[0228] Synthesis Example 6 (I-6)
[0229] 154 g of toluene and 154 g of N-methylpyrrolidone were placed in a 1 L round bottom flask equipped with a thermometer, reflux cooler, Dean-Stark apparatus, powder inlet, nitrogen inlet and stirring device. Then, 39.1 g (0.28 mol) of m-xylenediamine (Mitsubishi Gas Chemical Co., Ltd.) was added, and then 27.6 g (0.28 mol) of methanesulfonic acid was slowly added to form a salt. After stirring for about 10 minutes to mix, 4-(2,5-dioxotetrahydrofuran-3-yl)-1,2,3,4-tetrahydronaphthalene-1,2-dicarboxylic anhydride (43.1 g, 0.14 mol) was slowly added to the stirred mixture. The mixture was heated for 6 hours and refluxed to form an amine-terminated diimide. At this time, the theoretical amount of water generated by the condensation was obtained. The reaction mixture was cooled to below room temperature, and 33.8 g (0.34 mol) of maleic anhydride was added to the flask. The mixture was refluxed for another 8 hours to obtain the expected amount of generated water. After cooling to room temperature, the organic layer was washed with water (100 ml x 5 times) to remove salts and unreacted raw materials to obtain a varnish of the bismaleimide compound. Then, the varnish was dropped into 1,000 g of methanol, and a reprecipitation step was performed to remove the solvent and dry it, thereby obtaining 75 g (yield 75%, Mw = 3,200) (I-6) of the target white solid bismaleimide compound.
[0230] Comparative Synthesis Example 1 (BMI-1)
[0231] In a 500 ml round bottom flask equipped with a stirring rod coated with fluororesin, 110 g of toluene and 36 g of N-methylpyrrolidone (Methyl pyrrolidone) were placed. Then, 90.9 g (0.17 mol) of dimer diamine (PRIAMINE (registered trademark) 1075, manufactured by Croda Japan Co., Ltd.) was added, and then 16.4 g (0.17 mol) of methanesulfonic anhydride was slowly added to form a salt. Stir for about 10 minutes to mix, and then benzene tetracarboxylic anhydride (18.6 g, 0.08 mol) was slowly added to the stirred mixture. A Dean-Stark separator and a condenser were installed in the flask. The mixture was heated for 6 hours and refluxed to form an amine-terminated diimide. At this point, the theoretical amount of water generated by the condensation can be obtained. The reaction mixture was cooled to below room temperature, and 20.0 g (0.20 mol) of maleic anhydride was added to the flask. The mixture was refluxed for another 8 hours to obtain the expected amount of generated water. After cooling to room temperature, 200 ml of toluene was added to the flask. Next, the diluted organic layer was washed with water (100 ml x 3 times) to remove salts and unreacted raw materials. Then, the solvent was removed under vacuum to obtain 102 g of a brown waxy bismaleimide compound (yield 85%, Mw = 3,800).
[0232] The bismaleimide compound of Comparative Synthesis Example 1 represented by the following formula can be easily obtained from DESIGNER MOLECURES Inc. as "BMI-3000".
[0233]
[0234] Comparative Synthesis Example 2 (BMI-2)
[0235] In a 500 ml round bottom flask equipped with a stirring rod coated with fluororesin, 110 g of toluene and 36 g of N-methylpyrrolidone were placed. Then, 85.3 g (0.16 mol) of dimer diamine (PRIAMINE (registered trademark) 1075, manufactured by Croda Japan Co., Ltd.) was added, and then 15.4 g (0.16 mol) of methanesulfonic anhydride was slowly added to form a salt. Stir for about 10 minutes to mix, and then 4,4'-oxydiphthalic anhydride (24.8 g, 0.08 mol) was slowly added to the stirred mixture. A Dean-Stark separator and a condenser were installed in the flask. The mixture was heated for 6 hours and refluxed to form an amine-terminated diimide. At this point, the theoretical amount of water generated by the condensation can be obtained. The reaction mixture was cooled to below room temperature, and 18.8 g (0.19 mol) of maleic anhydride was added to the flask. The mixture was refluxed for another 8 hours to obtain the expected amount of generated water. After cooling to room temperature, 200 ml of toluene was added to the flask. Next, the diluted organic layer was washed with water (100 ml x 3 times) to remove salts and unreacted raw materials. Then, the solvent was removed in vacuo to obtain 106 g of a brown waxy bismaleimide compound (yield 88%, Mw = 3,700).
[0236] The bismaleimide compound of Comparative Synthesis Example 2 represented by the following formula can be easily obtained from DESIGNER MOLECURES Inc. as "BMI-1500".
[0237]
[0238] Comparative Synthesis Example 3 (BMI-3)
[0239] The bismaleimide compound (BMI-3) was synthesized by a known method using the method described in Example 1 of JP-A-2021-123672.
[0240] In a 2L glass 4-necked flask equipped with a stirrer, a Dean-Stark tube, a cooling condenser, and a thermometer, 37.25 g (0.219 mol) of isophorone diamine, 76.94 g (0.35 mol) of pyromellitic anhydride, and 350 g of toluene were added, and stirred at 80° C. for 3 hours to synthesize an amide acid. Then, the temperature was raised to 110° C. in this state, and stirred for 4 hours while distilling off the by-product water to synthesize a block copolymer.
[0241] Then, 116.88 g (0.219 mol) of dimer diamine (PRIAMINE (registered trademark) 1075, manufactured by Croda Japan Co., Ltd.) was added to the flask containing the block copolymer solution cooled to room temperature, and stirred at 80° C. for 3 hours to synthesize an amic acid. Then, the temperature was raised to 110° C. in this state, and stirred for 4 hours while distilling off the by-produced water, to synthesize a diamine at both ends.
[0242] After cooling the flask containing the obtained two-terminal diamine solution to room temperature, 18.88 g (0.193 mol) of maleic anhydride was added, and the mixture was heated to 80°C again and stirred for 3 hours to synthesize amide acid. Then, the mixture was heated to 110°C in this state, stirred for 15 hours while distilling off the by-product water, and washed with 300 g of water 5 times to obtain a varnish of the bismaleimide compound. Then, 3,000 g of isopropyl alcohol (IPA) was dropped into the varnish, and a reprecipitation step was performed to remove the solvent and dry it to obtain the target dark brown solid. (Yield 85%, Mw = 8,000)
[0243] The bismaleimide compound of Comparative Synthesis Example 3 is represented by the following formula.
[0244]
[0245] m≒3, n≒1 (respectively the average value)
[0246] The materials used in this example are shown.
[0247] [(I) component: bismaleimide compound]
[0248] I: Bismaleimide compounds shown in Synthesis Examples (I-1) to (I-6) and Bismaleimide compounds (BMI-1) to (BMI-3) shown in Comparative Synthesis Examples 1 to 3
[0249] [Component (II); photopolymerization initiator]
[0250] II-1: Ethyl ketone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]-, 1-(O-acetyl oxime) (manufactured by BASF JAPAN, "IRGACURE OXE-02")
[0251] II-2: 2,4-dimethylthioxanthone (manufactured by Nippon Kayaku Co., Ltd., “DETX-S”)
[0252] (Examples 1 to 6 and Comparative Examples 1 to 3)
[0253] The components (I) to (II) in the amounts (parts by mass) shown in Table 1 and 50 parts by mass of cyclopentanone as a solvent were mixed to prepare photosensitive resin compositions of Examples 1 to 6 and Comparative Examples 1 to 3.
[0254] [Table 1]
[0255]
[0256] <Evaluation of Photosensitive Resin Composition>
[0257] The following evaluations were performed on the photosensitive resin compositions of Examples 1 to 5 and Comparative Examples 1 to 3. The results are summarized in Table 2.
[0258] [Table 2]
[0259]
[0260] (Compatibility)
[0261] <Compatibility with MIR-3000>
[0262] In a 100 mL transparent glass bottle, 20 g of each of the above-modulated bismaleimide resin compositions, 20 g of the bismaleimide resin represented by formula (21) (MIR-3000, manufactured by Nippon Kayaku Co., Ltd.), and 20 g of cyclopentanone were mixed and heated at 80° C. for 30 minutes. Then, the mixture was cooled to room temperature and the appearance was confirmed. The evaluation results are recorded in Table 2.
[0263] The bismaleimide resin compositions of Examples 1 to 6 were compatible with MIR-3000 and were transparent and uniform even after cooling.
[0264] In contrast, the bismaleimide resin compositions of Comparative Examples 1 to 3 were separated from MIR-3000.
[0265] <Compatibility with MIR-5000>
[0266] In a 100 mL transparent glass bottle, 20 g of each of the above-modulated bismaleimide resin compositions, 20 g of the bismaleimide resin represented by formula (22) (MIR-5000, manufactured by Nippon Kayaku Co., Ltd.), and 20 g of cyclopentanone were mixed and heated at 80° C. for 30 minutes. Then, the mixture was cooled to room temperature and the appearance was confirmed. The evaluation results are recorded in Table 2.
[0267] The bismaleimide resin compositions of Examples 1 to 6 were compatible with MIR-5000 and were transparent and uniform even after cooling.
[0268] In contrast, the bismaleimide resin compositions of Comparative Examples 1 to 3 were separated from MIR-5000.
[0269] (Sensitivity, developer residue evaluation)
[0270] The photosensitive resin compositions obtained in Examples 1 to 6 and Comparative Examples 1 to 3 were spin-coated on a silane-based substrate and heated at 100°C for 2 minutes to form a coating film with a thickness of 10 to 15 μm. Then, a "Ultra-High Pressure Mercury Lamp 500W MultiLight" manufactured by USHIO was used, and a step exposure table No. 2step tablet manufactured by Kodak was used to perform reduced projection exposure with i-line (365 nm). The exposure amount was 2000 mJ / cm 2 After exposure, the film was heated at 150° C. for 15 minutes and developed using cyclopentanone.
[0271] The sensitivity is determined by the following method: among the exposed parts of the coating film exposed by light penetrating a step exposure meter (No. 2step tablet) manufactured by Kodak, the part exposed by light penetrating the density part of the step exposure meter with the highest transmittance is determined to be the part that remains during development. The unit is segment. The larger the number of segments (values) of the step exposure meter, the lower the transmittance. The higher the sensitivity is, the more the exposed part exposed by light penetrating the density part of the larger number of segments (values) remains during development.
[0272] In addition, when the pattern after development is observed under a microscope, if residue is observed in the whole or part of the pattern opening, it is rated as B (bad) in the item of development residue. If there is no residue, it is rated as A (good). Then, the photoresist pattern is heated at a temperature of 250° C. for 60 minutes in nitrogen to be thermally cured.
[0273] The evaluation results of sensitivity and developability are shown in Table 2.
[0274] (Evaluation of dielectric properties (relative dielectric constant: Dk, dielectric loss tangent: Df))
[0275] In order to evaluate the dielectric properties, the varnish was applied on the copper foil by a table-top coater to a thickness of 50 μm after drying and dried to obtain a semi-cured resin film. Then, the semi-cured resin film was irradiated with 2000 mJ / cm 2 The resin film was then heat treated at 250°C for 60 minutes in nitrogen to thermally harden it. The copper foil as a support was then removed by physical stripping or etching to obtain a resin film for evaluation. A resin film was formed / laminated on the prepared resin film in the same manner to a thickness of 300 μm.
[0276] Then, the resin film was cut into test pieces with a length of 60 mm, a width of 2 mm, and a thickness of 0.3 mm, and its dielectric properties (relative dielectric constant Dk and dielectric loss tangent Df) were measured by the cavity resonator perturbation method. The measuring instrument used was Vectortype Network Analyzer ADMSO10c1 manufactured by AET, and the cavity resonator used was CP531 (10 GHz band resonator) manufactured by Kanto Electronics Application Development Co., Ltd. The conditions were a frequency of 10 GHz and a measurement temperature of 25°C. The results are shown in Table 2.
[0277] (Glass transition temperature (Tg) evaluation)
[0278] In order to evaluate the glass transition temperature, the varnish was applied on the copper foil by a table-top coater so that the thickness after drying was 20 μm and dried to obtain a semi-cured resin film. Then, the obtained semi-cured resin film was irradiated with 2000 mJ / cm 2 Then, the resin film was heat treated at 250°C for 60 minutes in nitrogen to thermally cure the resin film. In addition, the copper foil as a support was removed by physical peeling or etching to obtain a cured product of the resin film for evaluation.
[0279] The dynamic viscoelasticity of the cured product of the bismaleimide prepared above was measured using a dynamic viscoelasticity measuring device (DMA) (RSA-G2 manufactured by TA Instruments) (frequency 1 Hz, tensile mode, heating rate 3°C / min), and the glass transition temperature Tg (°C) was determined from the maximum value of the loss tangent (tan δ). The results are shown in Table 2.
[0280] (5% weight loss temperature (Td5) evaluation)
[0281] In order to evaluate the weight loss temperature, the varnish was applied on the copper foil by a table-top coater so that the thickness after drying was 20 μm and dried to obtain a resin film (semi-cured). Then, the obtained resin film (semi-cured) was irradiated with 2000 mJ / cm 2 Then, the resin film was heat treated (thermal hardening) at 250°C for 60 minutes in nitrogen. The copper foil as a support was removed by physical peeling or etching to obtain a resin film (hardened product) for evaluation.
[0282] The weight change of the cured bismaleimide prepared above was measured in nitrogen at a temperature increase of 10°C / min using a differential thermogravimeter (TG / DTA6200 manufactured by Seiko Instruments) to determine the temperature Td5 (°C) at which the weight decreased by 5% compared to the initial weight measurement. The results are shown in Table 2.
[0283] The results shown in Table 1 clearly show that the bismaleimide compound obtained by using the photosensitive resin composition of the present invention has good compatibility with other resins, and the photocuring of the maleimide group is still sufficient even at a low exposure, so it has an excellent maleimide compound with low dielectric properties and high heat resistance.
[0284] In addition, the present application claims priority based on Japanese patent application (Japanese Patent Application No. 2022-071709) filed on April 25, 2022.
[0285] [Industrial Applicability]
[0286] As described above, the present invention can provide a relatively low exposure dose (2000mJ / cm 2 A bismaleimide compound that can form a fine pattern, has good compatibility with other resins and can increase Tg.
[0287] Therefore, the bismaleimide compound and the photosensitive resin composition of the present invention are very useful as a surface protective film of a semiconductor element, an interlayer insulating film, an insulating film of a rewiring layer, and the like.
Claims
1. A bismaleimide compound (I) having a cyclic imide bond and obtained by reacting an aromatic diamine (A) represented by the following formula (1), a tetrabasic acid dianhydride (C), and maleic anhydride: In formula (1), R1 each independently represents a hydrogen atom, a linear or branched alkyl group having 1 to 6 carbon atoms, a halogen atom, a hydroxyl group, or a linear or branched alkoxy group having 1 to 6 carbon atoms, l each independently represents an integer of 1 to 4.
2. A bismaleimide compound (I) having a cyclic imide bond and obtained by reacting an aromatic diamine (A) represented by the following formula (1), a tetrabasic acid dianhydride (C) and maleic anhydride, wherein the bismaleimide compound (I) is further reacted with a divalent organic diamine (B) having 6 to 200 carbon atoms other than the aromatic diamine (A) in addition to the diamine (A), the tetrabasic acid dianhydride (C) and the maleic anhydride: In formula (1), R1 each independently represents a hydrogen atom, a linear or branched alkyl group having 1 to 6 carbon atoms, a halogen atom, a hydroxyl group, or a linear or branched alkoxy group having 1 to 6 carbon atoms; l each independently represents an integer of 1 to 4.
3. A bismaleimide compound (I) represented by the following general formula (2): In formula (2), C independently represents a tetravalent organic group containing a ring structure, B is independently a divalent hydrocarbon group having 6 to 200 carbon atoms, W is A or B, m is 1 to 100, n is 0 to 100, the order of the repeating units marked with m and n and enclosed in parentheses is not limited, and the bonding pattern can be alternating, block, or irregular. A is independently a divalent linking group represented by the following formula (3): In formula (3), R1 each independently represents a hydrogen atom, a linear or branched alkyl group having 1 to 6 carbon atoms, a halogen atom, a hydroxyl group, or a linear or branched alkoxy group having 1 to 6 carbon atoms; l each independently represents an integer of 1 to 4.
4. The bismaleimide compound (I) according to claim 1, wherein the tetrabasic acid dianhydride (C) comprises a compound selected from the group consisting of the following formulae (4) to (12): In formula (7), Y represents C(CF3)2, SO2, CO, an oxygen atom, a direct bond, or a divalent linking group represented by the following formula (13):
5. The bismaleimide compound (I) according to claim 3, which is a maleimide of an amine compound represented by the following formula (14): In formula (14), C independently represents a tetravalent organic group containing a ring structure, B is independently a divalent hydrocarbon group having 6 to 200 carbon atoms, W is A or B, m is 1 to 100, n is 0 to 100, the order of the repeating units marked with m and n and enclosed in parentheses is not limited, and the bonding pattern can be alternating, block, or irregular. A is independently a divalent linking group represented by the following formula (3): In formula (3), R1 each independently represents a hydrogen atom, a linear or branched alkyl group having 1 to 6 carbon atoms, a halogen atom, a hydroxyl group, or a linear or branched alkoxy group having 1 to 6 carbon atoms, l each independently represents an integer of 1 to 4.
6. The bismaleimide compound (I) according to claim 1, wherein the tetrabasic acid dianhydride (C) is a compound of the following formula (15):
7. The bismaleimide compound (I) according to claim 1, wherein the tetrabasic acid dianhydride (C) is a compound of the following formula (8):
8. The bismaleimide compound (I) according to claim 1, wherein the tetrabasic acid dianhydride (C) is a compound of the following formula (5):
9. The bismaleimide compound (I) according to claim 1, wherein the tetrabasic acid dianhydride (C) is a compound of the following formula (9):
10. The bismaleimide compound (I) according to claim 1, wherein the tetrabasic acid dianhydride (C) is a compound of the following formula (10): 11 . A resin composition comprising the bismaleimide compound (I) according to claim 1 , and a compound reactive with a maleimide group.
12. The resin composition according to claim 11, wherein the compound capable of reacting with a maleimide group is at least one selected from the group consisting of maleimide compounds other than the bismaleimide compound (I), cyanate compounds, phenol resins, epoxy resins, cyclohexane resins, benzoxazine compounds, carbodiimide compounds and compounds having an ethylenically unsaturated group. 13 . A resin composition comprising the bismaleimide compound (I) according to claim 1 and a photopolymerization initiator or a curing catalyst. The resin composition according to claim 11 , further comprising a filler. 15 . A cured product of a resin composition, comprising the bismaleimide compound (I) according to claim 1 . 16 . A semiconductor element comprising a surface protection film, an interlayer insulating film or an insulating film of a rewiring layer comprising the bismaleimide compound (I) according to claim 1 . 17 . A dry film photoresist, comprising: a composition comprising the bismaleimide compound (I) according to any one of claims 1 to 10 and a photopolymerization initiator.