Electrochromic element, eyewear lens, eyewear, and method for manufacturing electrochromic element

By adjusting the difference in transmittance of the electrochromic element and the grinding processing on the back of the lens substrate, the degree uneven problem caused by the surface ripple of the electrochromic element is solved, and a more uniform degree distribution and better use effect are achieved.

CN119096188APending Publication Date: 2024-12-06HOYA LENS THAILAND LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380036004.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-28
Filing Date
2023-04-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

When manufacturing electrochromic components, the presence of surface corrugation leads to uneven degrees, especially when applied to glasses lenses, there will be problems of uneven depth and shade, which will affect the use effect.

Method used

By adjusting the difference between the maximum and minimum values ​​of the transmission within a 40 mm square square in the center of the surface of the electrochromic element, it is within 0.30D, and grinding and processing is performed on the back of the lens substrate according to the shape of the electrochromic film. to form corresponding ups and downs, thereby reducing ripples.

Benefits of technology

It effectively reduces apparent ripple and improves the uniformity of degree distribution, so that electrochromic elements no longer have significant degree uneven problems when used in glasses lenses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119096188A_ABST
    Figure CN119096188A_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide an electrochromic element capable of reducing apparent corrugations, eyewear lenses, and a method for manufacturing an electrochromic element. This electrochromic element (10) is obtained by laminating a lens substrate (1) and an electrochromic film (2), and the absolute value of the difference between the maximum value and the minimum value of the degree of transmission over the entire range of 40 mm from the center of the surface of the electrochromic element is within 0.30 D.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an electrochromic element capable of reversibly controlling color development and color elimination by electric power, a lens for spectacles, spectacles, and a method for manufacturing the electrochromic element. Background Art

[0002] An electrochromic element utilizing an electrochromic phenomenon in which a redox reaction reversibly occurs by application of a voltage to reversibly change color can be used as, for example, a lens for spectacles.

[0003] In the process of manufacturing an electrochromic element, for example, an electrochromic film is preformed into a curved surface, and then the electrochromic film is placed in a mold and injection molded into a lens substrate. The manufactured electrochromic element has a curved surface shape in which the electrochromic film is laminated on the surface of the lens substrate.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2022-25243 Summary of the invention

[0007] Problems to be solved by the invention

[0008] On the other hand, the surface of the electrochromic element may produce ripples due to the heating process during the manufacturing of the electrochromic element, the process of attaching the electrochromic film to the lens substrate, etc. The ripples will cause unevenness in the degree of light, and appear as light and dark on the surface when the current flows through the electrochromic element to color it.

[0009] However, conventionally, the moire has not been controlled, so the diopter distribution tends to become non-uniform. For example, if the electrochromic element is made into a spectacle lens and applied to spectacles, there is a problem that the diopter distribution becomes larger.

[0010] The present invention has been made to solve the above problems, and an object of the present invention is to provide an electrochromic element, an eyeglass lens and eyeglasses, and a method for producing the electrochromic element, which can reduce apparent ripples.

[0011] Solutions to the problem

[0012] An electrochromic element according to one embodiment of the present invention is a lens substrate and an electrochromic film laminated together, wherein the absolute value of the difference between the maximum and minimum transmittances in the entire 40 mm square area at the center of the surface is within 0.30D.

[0013] In one embodiment of the present invention, the absolute value of the difference between the maximum and minimum transmittances of the electrochromic element in the entire area of ​​40 mm square at the center of the surface is within 0.15D.

[0014] An electrochromic element according to one embodiment of the present invention is formed by laminating a lens substrate and an electrochromic film, wherein the surface of the electrochromic film has corrugations, and the back surface of the lens substrate opposite to the surface on which the electrochromic element is disposed forms undulations in accordance with the shape of the surface.

[0015] In one aspect of the present invention, it is preferred that the back surface of the lens substrate opposite to the side on which the electrochromic film is disposed is polished to form undulations in accordance with the shape of the surface.

[0016] In one embodiment of the present invention, the electrochromic film is preferably disposed on a convex surface of the lens substrate, and a concave surface opposite to the convex surface is preferably polished.

[0017] An eyeglass lens according to one embodiment of the present invention uses the electrochromic element described above. An eyeglass lens according to one embodiment of the present invention uses a plurality of eyeglass lenses described above.

[0018] One embodiment of the present invention relates to a method for manufacturing an electrochromic element, wherein the electrochromic element is formed by laminating a lens substrate and an electrochromic film, the method comprising: measuring the surface diopter distribution of the electrochromic element, and based on the measurement result, grinding the back side of the lens substrate opposite to the side where the electrochromic film is disposed.

[0019] In one embodiment of the present invention, it is preferred that the surface intensity is measured as a reflectance, a polished shape of the back surface is measured based on a reflectance distribution, and the back surface is polished in accordance with the polished shape.

[0020] In one embodiment of the present invention, the polishing is preferably performed so that the absolute value of the difference between the maximum and minimum values ​​of the transmittance in the entire 40 mm square area at the center of the surface is within 0.30D.

[0021] In addition, in one embodiment of the present invention, the method for manufacturing the electrochromic element preferably comprises: a process of forming the above-mentioned electrochromic element; a process of arranging the above-mentioned electrochromic element in a mold and injection molding the above-mentioned lens substrate; a process of measuring the surface diopter distribution of the above-mentioned electrochromic element; and a process of grinding the above-mentioned back side based on the measurement result of the above-mentioned surface diopter distribution.

[0022] Effects of the Invention

[0023] According to the electrochromic element and the method for manufacturing the same of the present invention, by adjusting the absolute value of the difference between the maximum and minimum transmittance values ​​within a given range, it is possible to reduce the apparent moire and improve the uniformity of transmittance distribution. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a schematic cross-sectional view of the electrochromic element of this embodiment.

[0025] Figure 2A It is an explanatory diagram showing the manufacturing process of the electrochromic element of this embodiment.

[0026] Figure 2B It is an explanatory diagram showing the manufacturing process of the electrochromic element of this embodiment.

[0027] Figure 2C It is an explanatory diagram showing the manufacturing process of the electrochromic element of this embodiment.

[0028] Figure 2D It is an explanatory diagram showing the manufacturing process of the electrochromic element of this embodiment.

[0029] Figure 2E It is an explanatory diagram showing the manufacturing process of the electrochromic element of this embodiment.

[0030] Figure 3 This is a 3D image of glasses using electrochromic technology.

[0031] Figure 4A This is a diagram conceptually showing the waviness on the surface of a pair of eyeglass lenses, and shows a comparative example.

[0032] Figure 4B FIG. 1 is a diagram conceptually showing the corrugations on the surface of a pair of eyeglass lenses, which shows an embodiment.

[0033] Figure 5A is a conceptual diagram showing the surface degree distribution.

[0034] Figure 5B This is a conceptual diagram of eyeglass lenses, showing Figure 5A The surface intensity distribution (reflection intensity distribution) shown is the transmittance intensity distribution after back grinding. DETAILED DESCRIPTION

[0035] Hereinafter, a specific embodiment of the present invention (hereinafter referred to as “the present embodiment”) will be described in detail.

[0036] <Electrochromic element 10 of this embodiment>

[0037] Figure 11 is a schematic cross-sectional view of an electrochromic element 10 according to the present embodiment. The electrochromic element 10 includes a lens substrate 1 and an electrochromic film 2 laminated on the surface of the lens substrate 1 .

[0038] [Lens substrate 1]

[0039] The lens substrate 1 is required to be transparent and have high transmittance. The material of the lens substrate 1 is not limited, and may be, for example, a resin substrate capable of being molded, such as polycarbonate resin, acrylic resin, epoxy resin, phenolic resin, or a glass substrate. Among them, the lens substrate 1 is preferably formed of a polycarbonate resin from the viewpoint of moldability and manufacturing cost.

[0040] [Electrochromic film 2]

[0041] The electrochromic film 2 includes a pair of first substrates 3 and second substrates 4, a pair of first electrode layers 5 and second electrode layers 6 provided on the inner surfaces of the first substrates 3 and second substrates 4, and an electrochromic layer 7 provided between the first electrode layer 5 and the second electrode layer 6. The electrochromic layer 7 includes a reduction layer 7a provided on the first electrode layer 5 side, an oxidation layer 7b provided on the second electrode layer 6 side, and an electrolyte layer 7c provided between the reduction layer 7a and the oxidation layer 7b. In this way, the electrochromic film 2 is Figure 1 The layers are stacked in the order of second substrate 4 / second electrode layer 6 / oxidation layer 7b / electrolyte layer 7c / reduction layer 7a / first electrode layer 5 / first substrate 3 from the bottom. It should be noted that reference numeral 16 denotes a sealing layer, and reference numeral 17 denotes a metal terminal portion.

[0042] The substrates 3 and 4 constituting the electrochromic film 2 are in the form of films or sheets and can be formed of the same resin material as the lens substrate 1. The substrates 3 and 4 are also required to be transparent and have high transmittance, similarly to the lens substrate 1. The substrates 3 and 4 are preferably formed of polycarbonate resin, similarly to the lens substrate 1.

[0043] The properties required of the electrode layers 5 and 6 constituting the electrochromic film 2 include transparency, high transmittance, and excellent conductivity. In order to satisfy such properties, the electrode layers 5 and 6 are transparent electrode layers, and ITO (Indium Tin Oxide) is particularly preferably used.

[0044] The reduction layer 7 a , the oxidation layer 7 b , and the electrolyte layer 7 c constituting the electrochromic layer 7 can be made of existing materials.

[0045] The reduction layer 7a is a layer that develops color with the reduction reaction. The reduction layer 7a can use an existing reduced electrochromic compound. There is no limitation on whether it is an organic or inorganic substance, and examples thereof include azobenzenes, anthraquinones, diarylethenes, dihydroprenes, bipyridines, styryls, styrylspiropyrans, spiropyrans, and spiropyrans. Oxiranes, spirothiopyrans, thioindigos, tetrathiafulvalenes, terephthalic acids, triphenylmethanes, triphenylamines, naphthyrans, viologens, pyrazolines, phenazines, phenylenediamines, phenanthenes, Oxazines, phenothiazines, phthalocyanines, fluorenes, fulgides, benzopyrans, metallocenes, tungsten oxide, molybdenum oxide, iridium oxide, titanium oxide, etc.

[0046] The oxide layer 7b is a layer that develops color with an oxidation reaction. The oxide layer 7b can use an existing oxidative electrochromic compound. There is no limitation on whether it is an organic or inorganic substance, and for example, it can be selected from a composition containing a radical polymerizable compound having a triarylamine, a Prussian blue complex, nickel oxide, iridium oxide, etc.

[0047] The electrolyte layer 7c has electronic insulation and ion conductivity, and is preferably transparent. The electrolyte layer 7c can be a solid electrolyte, a gel, a liquid, etc. In order to maintain high ion conductivity, it is preferably a gel. Although not limited, existing electrolyte materials such as inorganic ion salts such as alkali metal salts and alkaline earth metal salts, quaternary ammonium salts, acids, etc. can be used.

[0048] In addition, although Figure 1 Although not shown in the figure, a functional layer such as a hard coating layer and an anti-reflection layer may be provided on the surface of the electrochromic film 2 .

[0049] <Method for producing electrochromic element according to the present embodiment>

[0050] FIG. 2 is an explanatory diagram showing a method for manufacturing the electrochromic element according to the present embodiment.

[0051] exist Figure 2A In the present invention, an electrochromic film 2 is prepared, which has a pair of substrates 3 and 4, electrode layers 5 and 6 disposed inside the substrates 3 and 4, and an electrochromic layer 7 sandwiched between the electrode layers 5 and 6. It should be noted that the stacked structure of the electrochromic film 2 is not limited, and may be any other structure. Figure 2A Other stacked structures.

[0052] Next, if Figure 2B As shown, the electrochromic film 2 is preformed into a curved surface. At this time, the electrochromic film 2 is heated. The heating temperature is not limited, and is, for example, about 100°C.

[0053] When the electrochromic element of the present embodiment is applied to eyeglass lenses, since the eyeglass lenses have three-dimensional curved surfaces, it is preferable to preform the electrochromic film 2 into a three-dimensional curved surface before molding the lens substrate 1 .

[0054] Then, in Figure 2C In the process, the preformed electrochromic film 2 is placed inside a mold 20 composed of a first mold 21 and a second mold 22, and the lens substrate 1 is injection molded using an injection molding machine 23. During the injection molding, heating is performed. The heating temperature is not limited, for example, it is about 120°C. It should be noted that Figure 2C In FIG. 1 , the internal space of the mold 20 is shown in a rectangular shape, but the inner surface in contact with the electrochromic film 2 and the inner surface on the injection port side are curved.

[0055] Next, if Figure 2D As shown, the electrochromic element 10 formed by laminating the lens substrate 1 and the electrochromic film 2 is taken out from the mold 20. Figure 2E As shown, the electrochromic element 10 is cut into the shape of a lens for glasses to obtain a lens 30 for glasses.

[0056] <About Conventional Problems of Electrochromic Elements and Overview of the Present Embodiment>

[0057] The electrochromic element is an element that utilizes the electrochromic phenomenon that a redox reaction reversibly occurs when a voltage is applied to both electrodes, thereby reversibly changing the color.

[0058] For example, Figure 3 As for the glasses 32 shown, the electrochromic element using electrochromic technology is made into a pair of glasses lenses 30 and mounted on a frame 31, so that it can function as sunglasses in bright places and as transparent lenses in dark places. It can be adjusted to the optimal brightness by switch operation or automatically.

[0059] like Figure 1 As shown, the electrochromic element 10 has a laminated structure in which an electrochromic film 2 having an electrode layer and an electrochromic layer is laminated on the surface of a lens substrate 1 .

[0060] However, when the electrochromic element is made into a spectacle lens 30 and applied to a pair of glasses 32, uneven power may occur. It is known that uneven power will be more obvious depending on the size of the ripples on the lens surface.

[0061] The waviness is generated by stress applied during the heating process in the manufacturing process of the electrochromic element 10, the process of bonding the electrochromic film 2 to the lens substrate 1, etc. The "waviness" refers to a wavy shape in which convex and concave portions are repeated, for example.

[0062] Figure 4A and Figure 4B 10 is a conceptual diagram showing the shapes of the surface 10a and the back surface 10b of the electrochromic element 10. Figure 4A A comparative example is shown. Figure 4B It should be noted that in Figure 4A and Figure 4B In FIG. 1 , the ripples are shown in an exaggerated manner.

[0063] like Figure 4A As shown in the comparative example of FIG. 1 , ripples A are generated on the surface 10a. The double-dashed line is an ideal value, so in reality, ripples A are generated by deviation from the ideal value. Figure 4A In the comparative example of FIG. 1 , a grinding process is performed to make the back surface 10b substantially flat. That is, the shape of the back surface 10b can be made close to Figure 4A The ideal value of the double-dotted line. However, in Figure 4A In that case, the surface 10a is corrugated and the back surface 10b is roughly flat, that is, the surface 10a deviates from the ideal value and the back surface 10b is close to the ideal value, which will cause uneven degree. "Uneven degree" refers to the deviation of the transmittance. It should be noted that in Figure 4A In the example above, the "Ideal Value" is set to flat. However, if the front and back surfaces are curved, the ideal value will be set to a shape that imitates the curved surface.

[0064] In view of the above-mentioned conventional problems, the present inventors conducted intensive research and found that the absolute value of the difference between the maximum and minimum transmittance values ​​was reduced to a given range, thereby reducing the apparent moire and suppressing degree unevenness.

[0065] Figure 4B This is an example of reducing the appearance of ripples. Figure 4B As shown in the embodiment of the present invention, the surface 10a of the electrochromic element 10 has a ripple A that deviates from the ideal value as in the comparative example, but the back surface 10b also has a ripple B that imitates the ripple A on the surface 10a. Figure 4B In the embodiment, both the surface 10a and the back surface 10b exceed the ideal value. As a result, the ripples can be reduced in appearance and the degree ratio can be improved. Figure 4A The comparison example is small,

[0066] It should be noted that, although not limited, the maximum height waviness (Wz) of the waviness A and B is approximately 10 μm to 50 μm.

[0067] It should be noted that, as another method of reducing the ripples, the surface 10a and the back surface 10b may be brought close to each other. Figure 4BThe ideal value shown in FIG. 1 is that a flat or curved surface with small corrugations is formed on both the surface 10a and the back surface 10b so that the absolute value of the difference between the maximum value and the minimum value of the transmittance falls within a given range. However, in order to control the corrugations A of the surface 10a to be small, the surface side cannot be ground. Therefore, it is necessary to limit the conditions of the manufacturing process and improve the yield, which easily leads to the complication of the manufacturing process. Therefore, it is preferred to Figure 4B As shown, by providing the back surface 10b with corrugations B in imitation of the corrugations A of the surface 10a, the corrugations are reduced in appearance. Therefore, the following describes a method for making both the surface 10a and the back surface 10b undulate in the same manner so that the absolute value of the difference between the maximum and minimum values ​​of the transmittance is reduced to within a given range.

[0068] <Detailed explanation of the difference between the maximum and minimum transmittance values>

[0069] In the present embodiment, the absolute value of the difference between the maximum and minimum transmittance values ​​in the entire 40 mm square area at the center of the surface of the electrochromic element is within 0.3 D (degree, Diopter).

[0070] The difference in transmittance is described below with reference to experiments.

[0071] [Example 1]

[0072] (1) Fabrication of electrochromic film

[0073] like Figure 2A As shown, an electrochromic film 2 is prepared which has a pair of substrates 3 and 4, electrode layers 5 and 6 arranged on the inner sides of each substrate 3 and 4, and an electrochromic layer 7 sandwiched between each electrode layer 5 and 6. The substrates 3 and 4 use polycarbonate sheets, the electrode layers 5 and 6 use conductive sheets formed by sputtering ITO, and the electrochromic layer 7 uses an organic electrochromic material.

[0074] (2) Preforming

[0075] In order to conform to the three-dimensional curved surface of the eyeglass lens with a transmittance of 0.00D, the electrochromic film 2 is preformed into a curved surface (refer to Figure 2B ). In pre-molding, the lens is molded using a mold in a shape that conforms to the shape of the lens curved surface while being heated.

[0076] (3) Fabrication of electrochromic elements

[0077] Next, as shown in 2C, the preformed electrochromic film 2 is placed in a mold 20 of an injection molding machine, and the polycarbonate constituting the lens substrate 1 is injected into the mold 20 to mold the lens substrate 1, thereby obtaining an electrochromic element 10 (see Figure 2D). It was confirmed that the electrochromic film 2 was closely attached to the lens substrate 1 and did not peel off. The electrochromic element 10 was observed from the concave surface side with the naked eye, and the presence of unnatural deformation was confirmed.

[0078] (4) Measurement of surface degree distribution and preparation of grinding data

[0079] The surface reflectance of the electrochromic element 10 was measured using a Dual Lensmapper (DLM) manufactured by Automation & Robotics. Figure 5A This is a conceptual diagram of the surface intensity distribution (reflectance distribution). Figure 5A The surface degree distribution is shown in a 40 mm square range at the center of the surface of the electrochromic element 10. Correction polishing data for the back surface are prepared using the measured surface degree distribution values.

[0080] (5) Back grinding

[0081] Correction grinding data was input into a numerical control (NC) processing machine, and free-form grinding of the back (concave) side was performed. As a free-form grinding method, existing technology can be used, for example, the grinding method disclosed in paragraph

[0044] of WO2009 / 048124 can be referred to. After free-form grinding, the back (concave) side of the electrochromic element was observed by naked eyes, and it was confirmed that there was no unnatural deformation.

[0082] (6) Measurement of transmittance

[0083] The transmittance of the electrochromic element after free-form grinding was measured using Dual Lensmapper (DLM). In the measurement, the transmittance within a 40 mm square range in the center of the surface of the electrochromic element was measured, and the maximum and minimum transmittances were obtained. It should be noted that, whether it is the case of myopia lenses (negative lenses) or hyperopia lenses (positive lenses), the larger the value, the higher the intensity number. Therefore, the maximum and minimum degrees are summarized based on the strength of the degree, not based on the size of the number. Furthermore, the absolute value of the difference between the maximum transmittance and the minimum transmittance was calculated. In the experiment, a total of 12 electrochromic elements were made by the same manufacturing method as above, and the maximum transmittance, the minimum transmittance and their difference (absolute value) of each electrochromic element were obtained. The results are shown in Table 1 below. It should be noted that the unit is D (degrees).

[0084] (7) Measurement method of maximum height ripple (Wz)

[0085] Dektak XT-A manufactured by Bruker was used to perform three-dimensional mapping within a 40 mm square range in the center of the surface. The scanning pitch at this time was set to 0.1 mm. It should be noted that for the uncorrected measurement data, since the curve shape of the eyeglass lens overlaps, correction was performed in a manner that the theoretical value based on the lens design reached a level, and then Wz was calculated. The results are shown in Table 2 below.

[0086] [Table 1]

[0087]

[0088] [Table 2]

[0089] Surface wz(μm) Wz on the back side (μm) Absolute value of wz difference (μm) n=1 11 13 2 n=2 13 12 1 n=3 10 14 4 n=4 12 15 3 n=5 14 13 1 n=6 14 12 2 n=7 13 14 1 n=8 15 13 2 n=9 11 14 3 n=10 14 15 1 n=1 1 15 14 1 n=12 13 14 1

[0090] [Example 2]

[0091] The target power of the manufactured eyeglass lenses was set from 0.00D to -2.00D. In addition, 12 electrochromic elements were manufactured by the same manufacturing method as in Example 1, and the maximum transmittance, the minimum transmittance and the difference (absolute value) of each electrochromic element were obtained. The results are shown in Table 3 below. It should be noted that the unit is D (degrees). In addition, the measurement results of the maximum height ripple (Wz) are shown in Table 4.

[0092] [Table 3]

[0093]

[0094] [Table 4]

[0095] <![CDATA[Surface Wz( μm )]]> Wz on the back side (μm) Absolute value of Wz difference (μm) n=1 17 16 1 n=2 16 16 0 n=3 15 17 2 n=4 14 15 1 n=5 15 18 3 n=6 16 19 3 n=7 17 18 1 n=8 17 19 2 n=9 15 17 2 n=10 16 16 0 n=11 18 17 1 n=12 18 17 1

[0096] [Example 3]

[0097] The target power of the manufactured eyeglass lenses was set from 0.00D to -4.00D. In addition, 12 electrochromic elements were manufactured by the same manufacturing method as in Example 1, and the maximum value of the transmittance, the minimum value of the transmittance and the difference (absolute value) of each electrochromic element were obtained. The results are shown in Table 5 below. It should be noted that the unit is D (degrees). In addition, the measurement results of the maximum height ripple (Wz) are shown in Table 6.

[0098] [Table 5]

[0099]

[0100] [Table 6]

[0101] <![CDATA[Surface Wz( μm )]]> <![CDATA[Wz on the back side ( μm )]]> Absolute value of Wz difference (μm) n=1 43 44 1 n=2 37 43 6 n=3 42 42 0 n=4 43 38 5 n=5 39 39 0 n=6 38 40 2 n=7 39 41 2 n=8 39 40 1 n=9 38 42 4 n=10 37 43 6 n=11 38 44 6 n=12 41 43 2

[0102] [Example 4]

[0103] The target power of the manufactured eyeglass lenses was set from 0.00D to +4.00D. In addition, 12 electrochromic elements were manufactured by the same manufacturing method as in Example 1, and the maximum transmittance, the minimum transmittance and the difference (absolute value) of each electrochromic element were obtained. The results are shown in Table 7 below. It should be noted that the unit is D (degrees). In addition, the measurement results of the maximum height ripple (Wz) are shown in Table 8.

[0104] [Table 7]

[0105]

[0106] [Table 8]

[0107] Surface Wz(μm) Wz on the back side (μm) Absolute value of Wz difference (μm) n=1 45 43 2 n=2 44 45 1 n=3 38 46 8 n=4 47 44 3 n=5 45 45 0 n=6 50 43 7 n=7 49 44 5 n=8 47 44 3 n=9 42 45 3 n=10 47 45 2 n=1 1 45 46 1 n=12 38 42 4

[0108] [Comparative Example 1]

[0109] The target power of the eyeglass lenses to be manufactured was set from 0.00D to -4.00D, and except for the process (4) of Example 1, non-corrected grinding processing data not based on the numerical value of the surface power distribution was used. In addition, 12 electrochromic elements were manufactured by the same manufacturing method as Example 1, and the maximum value of the transmittance, the minimum value of the transmittance and the difference (absolute value) of each electrochromic element were obtained. The results are shown in the following Table 9. It should be noted that the unit is D (degrees). In addition, the measurement results of the maximum height ripple (Wz) are shown in Table 10.

[0110] [Table 9]

[0111]

[0112] [Table 10]

[0113] Surface Wz(μm) Wz on the back side (μm) Absolute value of Wz difference (μm) n=1 43 2 41 n=2 45 1 44 n=3 44 3 41 n=4 43 2 41 n=5 42 1 41 n=6 41 2 39 n=7 43 2 41 n=8 44 5 39 n=9 45 3 42 n=10 43 2 41 n=1 1 44 2 42 n=12 43 2 41

[0114] [Comparative Example 2]

[0115] The target power of the manufactured eyeglass lenses was set from 0.00D to +4.00D, and the non-corrected grinding processing data not based on the numerical value of the surface power distribution was used except for the process (4) of Example 1. In addition, 12 electrochromic elements were manufactured by the same manufacturing method as Example 1, and the maximum value of the transmittance, the minimum value of the transmittance and the difference (absolute value) of each electrochromic element were obtained. The results are shown in the following Table 11. It should be noted that the unit is D (degrees). In addition, the measurement results of the maximum height ripple (Wz) are shown in Table 12.

[0116] [Table 11]

[0117]

[0118] [Table 12]

[0119] Surface Wz(μm) Wz on the back side (μm) Absolute value of Wz difference (μm) n=1 44 2 42 n=2 45 1 44 n=3 46 4 42 n=4 44 3 41 n=5 44 4 40 n=6 45 4 41 n=7 44 3 41 n=8 46 3 43 n=9 45 4 41 n=10 43 3 40 n=11 45 3 42 n=12 44 4 40

[0120] [Experimental results]

[0121] As shown in Tables 1, 3, 5 and 7, in Examples 1 to 4, the absolute value of the difference between the maximum and minimum transmittance values ​​in the entire 40 mm square range at the center of the surface of the electrochromic element is within 0.30D.

[0122] In addition, as shown in Tables 2, 4, 6, and 8, it can be seen that in Examples 1 to 4, the difference between the top and bottom of the maximum height waviness (Wz) can be suppressed to 20 μm or less, preferably to 10 μm or less.

[0123] On the other hand, as shown in Tables 9 and 11, the absolute value of the difference between the maximum and minimum transmittance values ​​in Comparative Examples 1 and 2 is greater than 0.30 D. In addition, as shown in Tables 10 and 12, the difference between the front and back of the maximum height waviness (Wz) in Comparative Examples 1 and 2 is about 40 μm or more.

[0124] In this embodiment, the surface density distribution of the electrochromic element is measured (refer to Figure 5A ), and based on the measurement results, the back side of the lens substrate opposite to the side where the electrochromic film is arranged is ground. As a result, in the example, the surface of the electrochromic film has ripples, but the back side also forms undulations in accordance with the shape of the surface, thereby reducing the ripples in appearance. As a result, the absolute value of the difference between the maximum value and the minimum value of the transmittance can be made smaller than that of the comparative example. Figure 5B is a conceptual diagram of the transmittance distribution. Figure 5B 3 shows the transmittance distribution in the spectacle lens 30. It can be seen that the dispersion of transmittance is suppressed as a whole.

[0125] According to the above experimental results, if the absolute value of the difference between the maximum and minimum values ​​of the transmittance is within 0.30D, it is equivalent to the embodiment. It can be seen that if it is within 0.30D, when the electrochromic element is observed from the back (concave) side with the naked eye, there is no unnatural deformation and it can be used as a spectacle lens. On the other hand, it can be seen that in the comparative example, unnatural deformation is observed and it cannot be used as a spectacle lens.

[0126] The reason for setting the absolute value of the difference between the maximum and minimum values ​​of the transmittance within 0.30D is based on the allowable difference in refractive power of single-vision spectacle lenses for refractive correction in JIS T7313. From the perspective of spectacle lens design, the center power must meet the allowable difference of the JIS standard, so it is set within 0.30D. Preferably, it is within 0.25D.

[0127] <Characteristic Configuration of the Present Embodiment>

[0128] The electrochromic element 10 of this embodiment is an electrochromic element 10 formed by laminating a lens substrate 1 and an electrochromic film 2, and the absolute value of the difference between the maximum and minimum transmittance values ​​in the entire 40 mm square range at the center of the surface is within 0.30 D. This can reduce the appearance of ripples and improve the uniformity of the diopter distribution.

[0129] In this embodiment, it is preferred that the absolute value of the difference between the maximum and minimum transmittance values ​​within the entire 40 mm square at the center of the surface is within 0.15 D. According to the above-mentioned experiments, a large number of samples falling within 0.15 D were observed in Examples 1 to 4. Thus, in this embodiment, it is also possible to control it within 0.15 D, which can further improve the uniformity of the degree distribution.

[0130] This embodiment relates to an electrochromic element 10, which is formed by laminating a lens substrate 1 and an electrochromic film 2, wherein the surface of the electrochromic film 2 has corrugations, and the back surface of the lens substrate 1 forms undulations in the shape of the surface. Figure 4B As shown in the schematic diagram, the surface 10a and the back surface 10b form undulations in approximately the same shape, so the absolute value of the difference between the maximum and minimum transmittances in the entire 40 mm square range in the center of the surface can be adjusted to within 0.30D, thereby reducing apparent ripples.

[0131] In this embodiment, the back surface of the lens substrate 1 is preferably ground to form undulations in accordance with the shape of the above-mentioned surface. As shown in "(4) Measurement of surface power distribution and preparation of grinding data" and "(5) Back surface grinding" of the above-mentioned experiment, the back surface is ground using the correction grinding data prepared using the numerical value of the surface power distribution. Figure 4B As shown in the schematic diagram of , the back surface can be ground in such a way that it forms undulations following the shape of the surface.

[0132] In this embodiment, the electrochromic film 2 is preferably disposed on the convex surface of the lens substrate 1, and the concave surface opposite to the convex surface is polished. Figure 4BAs shown in the schematic diagram of , the back surface is ground in such a way that it forms undulations following the shape of the surface.

[0133] The spectacle lens 30 of the present embodiment uses the electrochromic element 10 described above. In addition, the glasses 32 of the present embodiment use a plurality of the spectacle lenses 30. The electrochromic element 10 of the present embodiment can reduce the uneven power compared with the past, and therefore can be effectively applied to the spectacle lenses, and can reduce the power difference between the left and right lenses, so that the user can use the glasses without discomfort.

[0134] The present embodiment relates to a method for manufacturing an electrochromic element 10, wherein the electrochromic element 10 is formed by laminating a lens substrate 1 and an electrochromic film 2, the method comprising: measuring the surface diopter distribution of the electrochromic element 10, and grinding the back surface of the lens substrate 1 opposite to the side on which the electrochromic film 2 is disposed based on the measurement result. Thus, the apparent waviness can be reduced, and the absolute value of the difference between the maximum and minimum values ​​of the transmittance in the entire range of 40 mm square at the center of the surface can be easily adjusted to within 0.30D.

[0135] In this embodiment, it is preferred to measure the surface intensity distribution by reflectance, measure the grinding shape of the back surface based on the reflectance distribution, and grind the back surface according to the grinding shape. Figure 4B As shown in the schematic diagram of , the back surface can be ground in such a way that it forms undulations following the shape of the surface.

[0136] In this embodiment, the polishing process can be performed so that the absolute value of the difference between the maximum value and the minimum value of the transmittance in the entire range of 40 mm square at the center of the surface is within 0.30D.

[0137] In addition, in this embodiment, it is preferred to have: a step of forming the electrochromic element 10; a step of placing the electrochromic film 2 in the mold 20 to injection mold the lens substrate 1; a step of measuring the surface power distribution of the electrochromic element 10; and a step of grinding the back surface based on the measurement result of the surface power distribution. Figure 2C As shown, in this embodiment, the electrochromic film 2 is arranged in the mold 20 to injection mold the lens substrate 1, but after such a process, the surface of the electrochromic film 2 is prone to ripples. In the subsequent back grinding process, grinding is performed by the existing free form grinding method, but in this embodiment, the surface power distribution is measured, and then the back surface is ground based on the measurement result of the surface power distribution, thereby forming the same ripples as the surface on the back surface, thereby reducing the apparent ripples. As a result, an electrochromic element with high uniformity of power distribution can be easily manufactured with good precision.

[0138] <Application>

[0139] The electrochromic element of this embodiment is not limited in its application, but can be preferably applied to light-adjusting eyeglass lenses.

[0140] The electrochromic element of this embodiment can also be applied to other than eyeglass lenses, for example, electrochromic dimmers, anti-glare lenses, and the like.

[0141] Industrial Applicability

[0142] The electrochromic element of the present invention can reduce the apparent ripples and the unevenness of the diopter, so that the electrochromic element can be suitably applied to eyeglass lenses and the deformation of the visual field when wearing the eyeglasses can be eliminated.

[0143] This application is based on Japanese Patent Application No. 2022-074757 filed on April 28, 2022, and all the contents thereof are included in this application.

Claims

1. An electrochromic element, which is a lens substrate and an electrochromic film laminated together, The absolute value of the difference between the maximum and minimum transmittance values ​​of the electrochromic element in the entire 40 mm square range at the center of the surface is within 0.30D.

2. The electrochromic element according to claim 1, wherein the absolute value of the difference between the maximum and minimum transmittance values ​​in the entire 40 mm square range at the center of the surface is within 0.15D.

3. An electrochromic element, which is a lens substrate and an electrochromic film laminated together, The surface of the electrochromic film has corrugations, The back surface of the lens substrate, which is opposite to the surface on which the electrochromic element is disposed, is formed with undulations following the shape of the surface.

4. The electrochromic element according to any one of claims 1 to 3, wherein The back surface of the lens substrate opposite to the side where the electrochromic film is disposed is ground to form undulations in accordance with the shape of the surface.

5. The electrochromic element according to claim 4, wherein: The electrochromic film is disposed on the convex surface of the lens substrate, and the concave surface opposite to the convex surface is polished. 6 . A spectacle lens using the electrochromic element according to claim 1 .

7. A pair of spectacles using a plurality of the spectacles lenses according to claim 6.

8. A method for manufacturing an electrochromic element, wherein the electrochromic element is formed by laminating a lens substrate and an electrochromic film. The method includes: The surface power distribution of the electrochromic element is measured, and based on the measurement result, the back surface of the lens substrate opposite to the side where the electrochromic film is arranged is polished.

9. The method for manufacturing an electrochromic element according to claim 8, wherein: The surface intensity distribution is measured as reflectance, a polishing shape of the back surface is measured based on the reflectance distribution, and the back surface is polished according to the polishing shape.

10. The method for manufacturing an electrochromic element according to claim 8 or 9, wherein: The polishing was performed so that the absolute value of the difference between the maximum and minimum values ​​of the transmittance in the entire 40 mm square range at the center of the surface was within 0.30D.

11. The method for manufacturing an electrochromic element according to claim 8 or 9, comprising: A process for forming the electrochromic element; The electrochromic element is arranged in a mold, and the lens substrate is injection molded; A step of measuring the surface degree distribution of the electrochromic element; A step of grinding the back surface based on the measurement result of the surface density distribution.

Citation Information

Patent Citations

  • Electrochromic element, electrochromic light controlling element, and electrochromic device

    JP2022025243A

  • Progressive refractive power lens manufacturing method and progressive refractive power lens

    WO2009048124A1