Semiconductor module and method for manufacturing semiconductor module

By forming a roughening recess and a peel suppression portion on the upper surface of the metal wiring board joint portion of the semiconductor module, the problem of degradation of adhesion between the sealing resin and the metal wiring board is solved, and higher adhesion and bonding strength are achieved.

CN119096365APending Publication Date: 2024-12-06FUJI ELECTRIC CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380036744.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-11-04
Filing Date
2023-10-10
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In semiconductor modules, temperature changes in power semiconductor elements cause internal stress to change, which may reduce the bonding adhesion between the sealing resin and the metal wiring board.

Method used

A plurality of roughening recesses are formed on the upper surface of the joint portion of the metal wiring board, and a peeling suppression portion is provided in at least a part of the recesses to narrow the opening width to improve the adhesion of the sealing resin.

Benefits of technology

Through the design of surface roughening and peel suppression portions, the adhesion between the metal wiring board and the sealing resin is enhanced, the peeling of the sealing resin is suppressed, and the bonding strength is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119096365A_ABST
    Figure CN119096365A_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to improve adhesion between a bonding portion of a metal wiring board and a sealing resin in a semiconductor module. A semiconductor module (1) is provided with: a laminated substrate (2) in which a plurality of circuit boards (22) are arranged on the upper surface of an insulating plate (20); a semiconductor element (3) disposed on the upper surface of the at least one circuit board; and a metal wiring board (4) disposed on the upper surface of the semiconductor element. The metal wiring board has a bonding portion (40) that is bonded to the upper surface of the semiconductor element via a bonding material (S3). The joining portion includes a plate-like portion having an upper surface and a lower surface, the plate-like portion having a plurality of roughened recessed portions (49) that roughen the upper surface, and at least a portion of the roughened recessed portions (49a) among the plurality of roughened recessed portions having a peeling suppression portion (70) that protrudes inward to narrow an opening width.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a semiconductor module and a method for manufacturing the semiconductor module. Background Art

[0002] The semiconductor module has a substrate on which semiconductor elements such as IGBT (Insulated Gate Bipolar Transistor), power MOSFET (Metal Oxide Semiconductor Field Effect Transistor), and FWD (Free Wheeling Diode) are provided, and is used in inverter devices and the like.

[0003] In such semiconductor modules, for example, in Patent Documents 1 to 3, a semiconductor element is arranged on an insulating substrate (also referred to as a laminated substrate), and a metal wiring plate (also referred to as a lead frame) for wiring is arranged on the upper surface electrode of the semiconductor element. The metal wiring plate is formed into a predetermined shape by, for example, stamping a metal plate. One end of the metal wiring plate is electrically bonded to the upper surface electrode via a bonding material such as solder.

[0004] In a semiconductor module, a sealing resin is filled inside a housing member, and an internal structure including a metal wiring board is covered with the sealing resin. In order to improve the adhesion strength of the sealing resin to the metal wiring board, in Patent Document 4, an ant nest-shaped groove whose opening is narrower than the width of the bottom is formed in the metal wiring board, and in Patent Document 5, a plurality of grid-shaped grooves are formed in the metal wiring board.

[0005] Patent Documents 6 to 9 describe forming a plurality of shallow pits on the surface of a metal wiring board and providing protrusions (returning portions, folded portions, hook-shaped portions) on the inner walls of the shallow pits to improve the sealing strength of the sealing resin. As a method of forming such shallow pits, a hole is formed by a first punching process, and a second punching process is performed on the periphery of the hole to deform the hole locally, so that a protrusion protrudes from the inner wall.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2018-088448

[0009] Patent Document 2: Japanese Patent Application Publication No. 2016-139635

[0010] Patent Document 3: Japanese Patent Application Publication No. 2015-176871

[0011] Patent Document 4: Japanese Patent Application Laid-Open No. 6-163773

[0012] Patent Document 5: Japanese Patent Application Publication No. 2021-077718

[0013] Patent Document 6: Japanese Patent Application Laid-Open No. 7-273270

[0014] Patent Document 7: Japanese Patent Application Publication No. 2005-191178

[0015] Patent Document 8: Japanese Patent Application Publication No. 2017-005124

[0016] Patent Document 9: Japanese Patent Application Publication No. 2007-258587 Summary of the invention

[0017] Problem that the invention aims to solve

[0018] In addition, in such semiconductor modules, the power semiconductor element generates heat due to switching operation. In the structure in which the metal wiring plate is soldered to the surface of the power semiconductor element as described above, deformation may occur at the joint portion due to the change of internal stress caused by temperature change. As a result, it is conceivable that the adhesion of the sealing resin to the joint portion of the metal wiring plate is reduced.

[0019] The present invention has been made in view of the above-mentioned situation, and one object of the present invention is to provide a semiconductor module capable of improving the adhesion between a joint portion of a metal wiring plate and a sealing resin.

[0020] Solutions for solving problems

[0021] A semiconductor module according to one technical solution of the present invention comprises: a stacked substrate having a plurality of circuit boards arranged on the upper surface of an insulating plate; a semiconductor element arranged on the upper surface of at least one of the circuit boards; and a metal wiring plate arranged on the upper surface of the semiconductor element, the metal wiring plate having a joining portion which is joined to the upper surface of the semiconductor element via a joining material, the joining portion comprising a plate-like portion having an upper surface and a lower surface, the plate-like portion having a plurality of roughened recesses which roughen the upper surface, and at least a portion of the plurality of roughened recesses having a peeling-inhibiting portion which protrudes inwardly to narrow the opening width.

[0022] Effects of the Invention

[0023] According to the present invention, it is possible to improve the adhesion between the joint portion of the metal wiring plate and the sealing resin in the semiconductor module. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a schematic diagram of the semiconductor device according to this embodiment as viewed from above.

[0025] Figure 2 Yes Figure 1 The semiconductor device shown is a cross-sectional view taken along line AA.

[0026] Figure 3 This is an enlarged view of the metal wiring plate of this embodiment.

[0027] Figure 4 Observe from the direction of arrow B Figure 3 A top view of the metal wiring plate is shown.

[0028] Figure 5 yes Figure 3 An enlarged view of portion C of the metal wiring board is shown.

[0029] Figure 6 It is a plan view showing a specific example of a semiconductor module to which the metal wiring plate according to the present embodiment is applied.

[0030] Figure 7 This is an equivalent circuit diagram of the semiconductor device according to this embodiment.

[0031] Figure 8 Yes means Figure 4 FIG. 1 is a top view of the structure of the roughened recessed portion in the region D of the first embodiment.

[0032] Fig. 9 It is along Figure 8 A cross-sectional view taken along the E-E line.

[0033] Fig.10 Yes means Figure 4 A top view of the structure of the roughened recessed portion of the second embodiment in the region D.

[0034] Fig.11 Yes means Figure 4 A top view of the structure of the roughened recessed portion of the third embodiment in the region D.

[0035] Fig.12 Yes means Figure 5 A top view of the structure of the roughened recessed portion of the fourth embodiment in the region D.

[0036] Fig.13 Yes means Figure 4 A top view of the structure of the roughened recessed portion of the fifth embodiment in the region D.

[0037] Fig.14It is a diagram showing an example of a manufacturing method for forming a roughened recessed portion having a peeling inhibiting portion. DETAILED DESCRIPTION

[0038] The following describes a semiconductor module and a semiconductor device to which the present invention can be applied. Figures 1 to 7 The overall structure of a semiconductor module and a semiconductor device and the outline of a metal wiring plate included in the semiconductor module and the semiconductor device are described. Figure 1 This is a schematic diagram of the semiconductor device according to this embodiment as viewed from above. Figure 2 Yes Figure 1 The semiconductor device shown is a cross-sectional view taken along line AA. Figure 3 This is an enlarged view of the metal wiring plate of this embodiment. Figure 4 Observe from the direction of arrow B Figure 3 A top view of the metal wiring plate is shown. Figure 5 yes Figure 3 An enlarged view of portion C of the metal wiring board is shown. Figure 6 It is a plan view showing a specific example of a semiconductor module to which the metal wiring plate according to the present embodiment is applied. Figure 7 : is an equivalent circuit diagram of the semiconductor device of the present embodiment. Here, as the semiconductor element 3, a structure in which an IGBT and an anti-parallel circuit of a FWD are connected in series is used.

[0039] In addition, in the following drawings, the length direction of the semiconductor module (cooler) is defined as the X direction, the width direction of the semiconductor module (cooler) is defined as the Y direction, and the height direction (thickness direction of the substrate) is defined as the Z direction. In addition, the length direction of the semiconductor module represents the direction in which multiple circuit boards are arranged. The X, Y, and Z axes shown in the figure are orthogonal to each other and constitute a right-hand system. In addition, depending on the situation, the X direction is sometimes referred to as the left-right direction, the Y direction is referred to as the front-back direction, and the Z direction is referred to as the up-down direction. These directions (front-back, left-right, up-down, and down-down directions) are terms used for the convenience of explanation, and sometimes the corresponding relationship with the XYZ directions will change depending on the installation posture of the semiconductor module. For example, the heat dissipation surface side (cooler side) of the semiconductor module is referred to as the lower surface side, and the opposite side is referred to as the upper surface side. In addition, in this specification, a top view refers to the situation of observing the upper or lower surface of the semiconductor module from the Z direction. In addition, the aspect ratios and the size relationships of the components in the figures are only represented by schematic diagrams, and therefore may not be consistent. For the convenience of explanation, it is also envisioned that there are situations in which the size relationships of the components are exaggerated.

[0040] The semiconductor device 100 of this embodiment is applied to a power conversion device such as an inverter for an industrial or vehicle-mounted motor. Figure 1 and Figure 2As shown in FIG. 1 , the semiconductor device 100 is configured by placing the semiconductor module 1 on the upper surface of the cooler 10. The cooler 10 may have any structure with respect to the semiconductor module 1. FIG.

[0041] The cooler 10 is used to release the heat of the semiconductor module 1 to the outside, and has a rectangular parallelepiped shape as a whole. Although not specifically shown in the figure, the cooler 10 is provided with a plurality of heat sinks on the lower surface side of the base plate, and these heat sinks are housed in a water cooling jacket. In addition, the cooler 10 is not limited to this and can be appropriately changed.

[0042] Semiconductor module 1 is configured by arranging multilayer substrate 2 , semiconductor element 3 , metal wiring plate 4 and the like in casing 11 .

[0043] The laminated substrate 2 is composed of, for example, a DCB (Direct Copper Bonding) substrate, an AMB (Active Metal Brazing) substrate, or a metal base substrate. The laminated substrate 2 is formed by laminating an insulating plate 20, a heat sink 21, and a plurality of circuit boards 22, and is formed in a rectangular shape in plan view as a whole.

[0044] Specifically, the insulating plate 20 is formed of a plate-like body having an upper surface and a lower surface, and has a rectangular shape in a plan view that is long in the X direction. The insulating plate 20 may be made of, for example, aluminum oxide (Al 2 O 3 ), aluminum nitride (AlN), silicon nitride (Si 3 N 4 ), aluminum oxide (Al 2 O 3 ) and zirconium oxide (ZrO 2 ) and other ceramic materials.

[0045] In addition, the insulating plate 20 can be formed of, for example, a thermosetting resin such as epoxy resin or polyimide resin, or a composite material in which glass or ceramic material is used as a filler in the thermosetting resin. The insulating plate 20 is preferably flexible and can be formed of, for example, a material containing a thermosetting resin. In addition, the insulating plate 20 can also be called an insulating layer or an insulating film.

[0046] The heat sink 21 has a predetermined thickness in the Z direction and has a rectangular shape in a top view that is longer in the Y direction. The heat sink 21 is formed of a metal plate with good thermal conductivity, such as copper or aluminum. The heat sink 21 is arranged on the lower surface of the insulating plate 20. The lower surface of the heat sink 21 is a mounting surface relative to the cooler 10, which is the mounting object of the semiconductor module 1, and also functions as a heat dissipation surface (heat dissipation area) for releasing the heat of the semiconductor module 1. The heat sink 21 is joined to the upper surface of the cooler 10 via a joining material S1 such as solder. The heat sink 21 can also be arranged on the upper surface of the cooler 10 via a thermally conductive material such as thermal grease or a thermally conductive compound.

[0047] The plurality of circuit boards 22 each have a predetermined thickness and are arranged on the upper surface of the insulating plate 20. Each circuit board 22 is formed into an electrically independent island. For example, the circuit boards 22 have a rectangular shape in plan view and are arranged on the insulating plate 20 in a row along the X direction. Figure 1 As shown, the number is limited to two, but can be changed appropriately. Figure 6 As shown, more than three circuit boards 22 may be arranged on the insulating plate 20. In addition, the shape and arrangement position of the circuit board 22 are not limited thereto and can be appropriately changed. These circuit boards 22 are formed of metal plates with good thermal conductivity such as copper and aluminum. The circuit board 22 may also be called a circuit layer or a circuit pattern.

[0048] A semiconductor element 3 is arranged on the upper surface of a predetermined circuit board 22 (circuit board 22 on the negative side in the X direction) via a bonding material S2 such as solder. The semiconductor element 3 is formed into a rectangular shape in a plan view by a semiconductor substrate such as silicon (Si) or silicon carbide (SiC). The semiconductor element 3 may be a power semiconductor element. The semiconductor element 3 uses switching elements such as IGBT (Insulated Gate Bipolar Transistor), power MOSFET (Metal Oxide Semiconductor Field Effect Transistor), and diodes such as FWD (Free Wheeling Diode).

[0049] In the present embodiment, the semiconductor element 3 is formed of an RC (Reverse Conducting)-IGBT element in which the functions of an IGBT (Insulated Gate Bipolar Transistor) element and a FWD (Free Wheeling Diode) element are integrated.

[0050] In addition, the semiconductor element 3 is not limited thereto, and may also be composed of the above-mentioned switch elements, diodes, etc. For example, the IGBT element and the FWD element may also be separately constructed. In addition, as the semiconductor element 3, a RB (Reverse Blocking: reverse blocking)-IGBT or the like having sufficient withstand voltage against the reverse bias may also be used. In addition, the shape, number of configurations, configuration location, etc. of the semiconductor element 3 may be appropriately changed.

[0051] In addition, the semiconductor element 3 has electrodes (not shown) formed on the upper surface and the lower surface, respectively. For example, the electrode on the upper surface side (upper surface electrode) is composed of an emitter electrode (source electrode) or a gate electrode, and the electrode on the lower surface side (lower surface electrode) is composed of a collector electrode (drain electrode).

[0052] Furthermore, the semiconductor element 3 of the present embodiment is a so-called vertical switching element in which the above-mentioned functional element is formed on a semiconductor substrate, but the present invention is not limited thereto and may be a horizontal switching element.

[0053] A metal wiring plate 4 is disposed on the upper surface of the semiconductor element 3. The metal wiring plate 4 is composed of a plate-like body having an upper surface and a lower surface, and is formed of a metal material such as a copper material, a copper alloy material, an aluminum alloy material, an iron alloy material, etc. The metal wiring plate 4 is formed into a predetermined shape by, for example, stamping. In addition, the shape of the metal wiring plate 4 shown below is only an example, and can be appropriately changed. In addition, the metal wiring plate can also be called a lead frame.

[0054] The metal wiring plate 4 of this embodiment is a long strip extending in the X direction so as to span across a plurality of circuit boards 22 when viewed from above, and has a crank shape formed by bending multiple times when viewed from the side. Figure 2 and Figure 3 As shown, the metal wiring plate 4 is constructed to include: a first joining portion 40, which is joined to the upper surface (upper surface electrode) of the semiconductor element 3 via a joining material S3; a second joining portion 41, which is joined to the upper surface of the circuit board 22 on the positive side of the X direction via a joining material S4; and a connecting portion 42, which connects the first joining portion 40 and the second joining portion 41.

[0055] The width of the metal wiring plate 4 in the Y direction is the same from the first joint portion 40 to the second joint portion 41. In addition, the first joint portion 40, the second joint portion 41 and the connecting portion 42 are arranged in a row along the X direction when viewed from above. In addition, the width of the metal wiring plate 4 in the Y direction does not necessarily have to be the same from the first joint portion 40 to the second joint portion 41. Figure 6 As shown, they may also have different widths. In addition, the first joining portion 40, the second joining portion 41 and the connecting portion 42 are not necessarily arranged in a row. Figure 6 As shown, they may be arranged in an obliquely offset manner.

[0056] The first bonding portion 40 is formed in a rectangular shape smaller than the outer shape of the semiconductor element 3 in a plan view, and includes a plate-like portion having an upper surface and a lower surface. A first bent portion 43 is formed at the end of the first bonding portion 40 on the positive side in the X direction (on the connecting portion 42 side), and the first bent portion 43 is bent at a substantially right angle and stands upward. One end (left end) of the connecting portion 42 is connected to the upper end of the first bent portion 43.

[0057] A plurality of through holes 46 are formed in the first joining portion 40. A total of four through holes 46 are provided, two in each X direction and two in each Y direction. The four through holes 46 are arranged slightly inside the four corners of the first joining portion 40. Each through hole 46 penetrates the first joining portion 40 in the Z direction.

[0058] The second joint portion 41 is formed in a rectangular shape smaller than the outer shape of the circuit board 22 in a plan view, and includes a plate-like portion having an upper surface and a lower surface. A second bent portion 44 is formed at the end of the second joint portion 41 on the negative side in the X direction (the connecting portion 42 side), and the second bent portion 44 is bent at a substantially right angle and stands upward. The other end (right end) of the connecting portion 42 is connected to the upper end of the second bent portion 44.

[0059] A plurality of through holes 48 are formed in the second bonding portion 41. Two through holes 48 are provided at different positions in the Y direction. Each through hole 48 penetrates the second bonding portion 41 in the Z direction.

[0060] The connecting portion 42 extends in the horizontal direction, and as described above, one end is connected to the first curved portion 43 , and the other end is connected to the second curved portion 44 .

[0061] The length of the first bent portion 43 in the Z direction is shorter than the length of the second bent portion 44 in the Z direction by an amount corresponding to the thickness of the semiconductor element 3. That is, the first bonding portion 40 and the second bonding portion 41 are provided at positions of different heights. More specifically, the first bonding portion 40 is provided at a position higher than the second bonding portion 41.

[0062] In addition, the shape, number, and arrangement position of the metal wiring plate 4 are merely examples and are not limited thereto, and can be appropriately changed. Figure 6 As shown, a plurality of (e.g., four) metal wiring plates 4 may be provided for one semiconductor module, and the details are described later. In addition, in the present embodiment, the semiconductor element 3, the metal wiring plate 4, and the main terminals described later form a semiconductor module. Figure 7 The inverter circuit is shown.

[0063] The stacked substrate 2, the semiconductor element 3 and the metal wiring plate 4 are surrounded by a shell 11. The shell 11 has a cylindrical shape or a frame shape that is a square ring when viewed from above, and is formed of, for example, a synthetic resin. The shell 11 can also be formed of a thermosetting resin material such as epoxy resin, silicone rubber, etc. The lower end of the shell 11 is bonded to the upper surface of the cooler 10 via an adhesive (not shown), and the upper end extends to a position that is sufficiently higher than the upper surface of the metal wiring plate 4. Thus, the shell 11 surrounds the stacked substrate 2, the semiconductor element 3 and the metal wiring plate 4, and defines a space for storing the stacked substrate 2, the semiconductor element 3 and the metal wiring plate 4.

[0064] The internal space defined by case 11 is filled with sealing resin 5. Sealing resin 5 may be filled to the upper surface and reach the upper end of case 11. Thus, laminated substrate 2, semiconductor element 3 and metal wiring plate 4 are sealed. Metal wiring plate 4 is entirely covered with sealing resin 5.

[0065] The sealing resin 5 may be made of, for example, a thermosetting resin. The sealing resin 5 preferably contains at least one of epoxy, silicone, polyurethane, polyimide, polyamide, and polyamide-imide. From the viewpoint of insulation, heat resistance, and heat dissipation, the sealing resin 5 is preferably, for example, an epoxy resin mixed with a filler.

[0066] In addition, if Figure 6 As shown in the specific example, a plurality of main terminals 60 for main current and a plurality of control terminals 61 for control may be provided in the housing 11. The main terminals 60 are formed of a plate-like elongated body and embedded in the side wall of the housing 11. Figure 6 In the embodiment, two main terminals 60 constituting an N terminal and a P terminal are arranged in the X direction on the side wall of the housing 11 located on the negative side in the Y direction. In addition, a main terminal 60 constituting an M terminal is arranged on the side wall of the housing 11 located on the positive side in the Y direction.

[0067] As described above, in this embodiment, semiconductor element 3, metal wiring plate 4, main terminal 60, etc. form a Figure 7 The inverter circuit shown in FIG. These main terminals 60 (N terminal, P terminal, M terminal) each correspond to Figure 7 IN(N) (also called low potential side input terminal or negative terminal), IN(P) (also called high potential side input terminal or positive terminal), OUT(M) (also called output terminal or intermediate terminal).

[0068] In addition, the control terminal 61 is formed of a plate-like long strip and embedded in the side wall of the housing 11 located on the positive side in the Y direction. The control terminal 61 is electrically connected to a predetermined control electrode of the semiconductor element 3 via a wiring member such as a bonding wire. These main terminals 60 and control terminals 61 are formed of metal materials such as copper materials, copper alloy materials, aluminum alloy materials, and iron alloy materials, and have a predetermined electrical conductivity and a predetermined mechanical strength. The shape, number, and arrangement position of the main terminals 60 and control terminals 61 are not limited to these, and can be appropriately changed.

[0069] In addition, in the semiconductor module, it is sought to prevent peeling from progressing along the interface between the metal wiring board and the sealing resin. As a method of reducing peeling, for example, it is considered to increase the surface area of ​​the metal wiring board to improve the closeness between the metal wiring board and the sealing resin (anchor effect). As a method of increasing the surface area of ​​the metal wiring board, it can be cited that a concave-convex shape is formed on the surface of the metal wiring board. However, if the lower surface of the metal wiring board (the surface opposite to the semiconductor element) has a concave-convex shape, it will be easy for the bonding material to produce gaps and shrinkage. As a result, the installation quality of the metal wiring board may be affected.

[0070] In addition, as methods for roughening the surface of the metal wiring plate, laser processing, wet methods based on chemical solutions, etc. can be cited. However, these methods will not only become the main cause of cost increase, but also the lower surface side of the metal wiring plate will be roughened, which will easily cause gaps and shrinkage in the bonding material. In other words, it is difficult to roughen the surface of the metal wiring plate without affecting the quality of the bonding material directly below the metal wiring plate.

[0071] In the present embodiment, a plurality of through holes 46 are provided in the first bonding portion 40, and a plurality of roughened recessed portions 49 are provided on the upper surface (outer surface) of the first bonding portion 40. By forming a plurality of through holes 46, the thickness of the bonding material S3 can be ensured in the bonding process of the metal wiring plate 4, and the first bonding portion 40 is prevented from being tilted relative to the upper surface of the semiconductor element 3, so that the posture of the metal wiring plate 4 (first bonding portion 40) is stabilized.

[0072] Through hole 48 formed in second bonding portion 41 has the same effect as through hole 46 of first bonding portion 40. Therefore, in the bonding process of metal wiring plate 4, the thickness of bonding material S4 can be ensured, and second bonding portion 41 can be prevented from tilting relative to the upper surface of circuit board 22, so that the posture of metal wiring plate 4 (second bonding portion 41) is stabilized.

[0073] The through hole 46 and the through hole 48 are cylindrical. In addition, the shape of the through hole formed in the first bonding part 40 and the second bonding part 41 is not limited to the cylindrical shape.

[0074] In addition, a plurality of roughened recesses 49 are formed on the upper surface of the first joint portion 40, thereby roughening the surface. As a result, the surface area of ​​the upper surface of the first joint portion 40 increases, and the adhesion (anchoring effect) between the upper surface of the first joint portion 40 and the sealing resin 5 can be improved. In particular, it is preferred that the sealing resin 5 enters the roughened recesses 49. Thus, a further anchoring effect can be expected. Therefore, above the semiconductor element 3, the peeling progress of the sealing resin 5 at the upper surface of the metal wiring plate 4 caused by thermal stress can be suppressed.

[0075] The through hole 46 and the roughened recessed portion 49 in the first joining portion 40 and the through hole 48 in the second joining portion 41 are formed by, for example, press working.

[0076] In addition, the plurality of roughened recessed portions 49 may be formed on the upper surface of the second joining portion 41, or may be formed only on the upper surface of the first joining portion 40. That is, the roughened recessed portions 49 may not be formed on the connecting portion 42, the first curved portion 43, and the second curved portion 44 that constitute the portion other than the first joining portion 40.

[0077] Since the semiconductor element 3 as a heat source is arranged directly below the first joint portion 40, it can be easily affected by the anchoring effect of the surface roughening. In addition, by roughening only the surface of the portion where the anchoring effect should be improved, there is no need to spend extra processing costs. That is, it can be said that the second joint portion 41, the connecting portion 42, the first bent portion 43 and the second bent portion 44 have less effect on the peeling of the sealing resin 5 than the first joint portion 40. In this case, the surfaces of the second joint portion 41, the connecting portion 42, the first bent portion 43 and the second bent portion 44 are flat, and their surface roughness can be equal to the surface roughness of the lower surface of the first joint portion 40.

[0078] In addition, the lower surface of the first bonding part 40 is preferably a flat surface except for the through hole 46. That is, preferably, the roughened recessed portion 49 is not formed on the lower surface of the first bonding part 40. For example, the surface roughness of the lower surface of the first bonding part 40 is preferably smaller than the surface roughness of the upper surface of the first bonding part 40. By making the lower surface of the first bonding part 40 flat, it is not easy to generate gaps and shrinkage in the bonding material S3.

[0079] In addition, if Figure 5 As shown, a coating film F may be interposed at the interface between the upper surface of the first bonding portion 40 and the sealing resin 5 .

[0080] Next, refer to Figures 8 to 13 An embodiment showing the structure of a plurality of roughened recessed portions 49 provided on the upper surface of the first bonding portion 40 will be described. Figure 8 , Fig.10 , Fig.11, Fig.12 as well as Fig.13 The equivalent of Figure 4 The area of ​​the region portion of D surrounded by the dotted line. Figure 8 and Fig. 9 This is the first embodiment. Fig.10 This is the second embodiment. Fig.11 This is the third embodiment. Fig.12 This is the fourth embodiment. Fig.13 This is the fifth embodiment. In each embodiment, the upper surface of the first bonding portion 40 has a roughened region whose surface is roughened by a plurality of roughened recessed portions 49 and a non-roughened region having no roughened recessed portions 49 , and the non-roughened region includes four through holes 46 .

[0081] In each embodiment, at least a portion of the roughened recesses 49 among the plurality of roughened recesses 49 is provided with a peeling-inhibiting portion 70. The peeling-inhibiting portion 70 is a portion that protrudes toward the inside of the roughened recesses 49 to narrow the opening width of the roughened recesses, and this structure is used to produce an effect of inhibiting the peeling of the sealing resin 5. In the following description, among the plurality of roughened recesses 49, the roughened recesses 49 having the peeling-inhibiting portion 70 are referred to as first roughened recesses 49a, and the roughened recesses 49 not having the peeling-inhibiting portion 70 are referred to as second roughened recesses 49b for distinction. In addition, Figure 4 The arrangement of the first roughened recessed portion 49a and the second roughened recessed portion 49b shown in FIG. Figures 8 to 13 The embodiments shown are different, but can also be applied Figure 4 That kind of configuration.

[0082] Figure 8 and Fig. 9 The first embodiment shown is an example in which a plurality of first roughened recessed portions 49a having peeling inhibiting portions 70 are provided on the entire roughened area of ​​the upper surface of the first bonding portion 40. In other words, in the first embodiment, the upper surface of the first bonding portion 40 is not provided with second roughened recessed portions 49b. The first roughened recessed portion 49a has a bottom surface 71 that is rectangular in plan view and four inclined surfaces 72 that extend upward from the four sides of the bottom surface 71, and has a flange portion 73 that protrudes inwardly from the inclined surface 72 at the upper end of the inclined surface 72. The first roughened recessed portion 49a has the smallest opening width at the flange portion 73, and the opening width increases as it moves from the flange portion 73 toward the bottom surface 71.

[0083] The flange portion 73 and the inclined surface 72 constitute the peeling inhibiting portion 70. Fig. 9As shown, the peeling inhibition portion 70 is a protrusion that protrudes toward the inner side (the center side of the opening) of the first roughened recess 49a from the outer edge (four sides) of the bottom surface 71. An opening recess 74 in the shape of a quadrangular prism is formed on the upper part of the peeling inhibition portion 70, and the opening recess 74 is open on the upper surface of the first bonding portion 40. The central part of the bottom surface of the opening recess 74 is connected to the bottom side of the first roughened recess 49a having the inclined surface 72 and the bottom surface 71, and the flange portion 73 constitutes the periphery of the connecting portion. In other words, the first roughened recess 49a has a shape in which the opening width is narrowed at the position of the flange portion 73. In addition, it becomes an overhanging structure in which the intervals between the four inclined surfaces 72 gradually narrow as they go from the bottom surface 71 toward the flange portion 73.

[0084] The first roughened recessed portion 49a of the above structure makes it difficult for the sealing resin 5 that has entered the interior below the opening recessed portion 74 to escape toward the opening recessed portion 74 due to the flange portion 73 configured to partially block the upper portion of the sealing resin 5 and the four inclined surfaces 72 formed below the flange portion 73. Therefore, the effect of improving the closeness between the first roughened recessed portion 49a and the sealing resin 5 can be obtained. In particular, the roughened recessed portions 49 in the roughened area are all formed as the first roughened recessed portions 49a. Figure 8 The structure can maximize the adhesion between the first roughened recessed portion 49 a and the sealing resin 5 .

[0085] exist Fig.14 2 shows an example of a method for manufacturing first roughened recessed portion 49 a having peeling suppressing portion 70 . First roughened recessed portion 49 a is manufactured by punching a metal plate that is a raw material of metal wiring plate 4 .

[0086] exist Fig.14 In the process of step A, the first die 80 as the upper die is pressed against the flat upper surface of the first joint portion 40 to perform a stamping process. The first die 80 has a plurality of stamping protrusions 81 in the shape of a quadrangular prism, and by pressing the stamping protrusions 81, a quadrangular prism-shaped initial concave portion 82 is formed in the first joint portion 40 (see Fig.14 B).

[0087] Next, in Fig.14 In the step B, the second die 83 as the upper die is pressed against the first joining portion 40 in a state where a plurality of initial recesses 82 are formed to perform a stamping process. The second die 83 has a plurality of quadrangular prism-shaped stamping protrusions 84. Each stamping protrusion 84 is larger than the opening shape of the four corners of each initial recess 82. Moreover, the bottom surface of each stamping protrusion 84 abuts against the periphery of the opening of each initial recess 82 from above.

[0088] like Fig.14As shown in process C, the force of stamping the second mold 83 is utilized to form an opening recess 74 at the location where each stamping protrusion 84 enters the first joining portion 40, and the wall portion around the opening of each initial recess 82 is pressed in and protrudes toward the center side from the inner surface of the initial recess 82.

[0089] When the second die 83 is pressed to a predetermined depth, the inclined surface 72 and the flange portion 73 are formed by the wall portion protruding toward the center side of the initial recessed portion 82 (see Fig. 9 ). In this way, by two-stage pressing using the first die 80 and the second die 83 , the first roughened recessed portion 49 a having the peeling inhibiting portion 70 can be formed.

[0090] In the case where the first roughened recessed portion 49a is formed by the above-mentioned two-stage stamping, when the metal wiring plate 4 is large and the portions to be stamped in the two-stage stamping (the number of the first roughened recessed portions 49a) are large, the load applied to the stamping device becomes large, and it is difficult to manufacture using a small and low-output stamping device. In addition, when the intervals between the plurality of first roughened recessed portions 49a are narrow, it is difficult to form the first roughened recessed portion 49a of a good shape with high precision due to the influence of the relative positional offset of the first die 80 and the second die 83 relative to the first joint 40. In addition, when the intervals between the plurality of first roughened recessed portions 49a are narrow and the number of the plurality of first roughened recessed portions 49a is large, it is easy to cause deformation and strain of the metal wiring plate 4 at portions other than the first roughened recessed portions 49a due to the influence of the load applied during manufacturing.

[0091] On the other hand, when the intervals between the plurality of first roughened recessed portions 49 a are increased, the smooth portion of the upper surface of the first bonding portion 40 becomes wider, and the sealing resin 5 is easily peeled off at the smooth portion.

[0092] Considering the above conditions, such as Figures 10 to 13 As shown, it is also possible to select a structure that uses both the first roughened recessed portion 49 a having the peeling inhibiting portion 70 and the second roughened recessed portion 49 b not having the peeling inhibiting portion 70 .

[0093] Fig.10 The second embodiment shown is a structural example in which only the outermost row of roughened recessed portions on the upper surface of the first bonding portion 40 is set as the first roughened recessed portion 49a having the peeling inhibiting portion 70, and the roughened recessed portions on the inner side thereof are set as the second roughened recessed portion 49b not having the peeling inhibiting portion 70. The second roughened recessed portion 49b is a quadrangular prism-shaped recessed portion having a bottom surface 75 that is rectangular in plan view and four substantially parallel side surfaces 76 that extend upward from the four sides of the bottom surface 75, and the upper end portion of each side surface 76 is open on the upper surface of the first bonding portion 40 (see Figure 5 ).

[0094] according to Fig.10 In the structure, by disposing the first roughened recessed portion 49a having a high degree of adhesion with the sealing resin 5 on the outer peripheral side of the first bonding portion 40 where peeling is most likely to occur, the peeling suppression effect of the sealing resin 5 can be effectively improved even if the first roughened recessed portion 49a is formed in a small number of locations. In addition, the surface of the area other than the outer peripheral side of the upper surface of the first bonding portion 40 is roughened by using the second roughened recessed portion 49b having a simple structure that is easy to manufacture and does not easily cause deformation and strain to the metal wiring plate 4, and the peeling suppression effect of the sealing resin 5 can be obtained by using a plurality of second roughened recessed portions 49b.

[0095] Fig.11 The third embodiment shown is a structure in which two rows of roughened recesses located on the upper surface of the first joining portion 40 at a position further outward than the through hole 46 serving as the non-roughened area are set as first roughened recesses 49a having peeling inhibition portions 70, and the roughened recesses further inward than the two rows of roughened recesses are set as second roughened recesses 49b not having peeling inhibition portions 70.

[0096] like Fig.11 By making the entire area closer to the end surface (outside) of the metal wiring plate 4 than the through hole 46 as the non-roughened area into the first roughened recessed portion 49a with a high degree of adhesion to the sealing resin 5, it is easy to prevent the sealing resin 5 from peeling off and advancing to the non-roughened area. In addition, the area closer to the inside of the through hole 46 is roughened by the second roughened recessed portion 49b of a simple structure that is easy to manufacture and does not easily cause deformation and strain to the metal wiring plate 4, and the effect of suppressing the peeling of the sealing resin 5 can be obtained by using a plurality of second roughened recessed portions 49b.

[0097] On the upper surface of the first bonding portion 40, the first roughened recessed portions 49a having the peeling inhibiting portion 70 may be intermittently arranged in a manner such that the second roughened recessed portions 49b having no peeling inhibiting portion 70 are interposed between the first roughened recessed portions 49a. Figure 4 As shown in the arrangement of the roughened recesses 49 in the X direction, if an intermittent arrangement is adopted in which two first roughened recesses 49a are arranged, a second roughened recess 49b is arranged, and then two first roughened recesses 49a are arranged, deformation and strain of the metal wiring plate 4 are less likely to occur.

[0098] Fig.12The fourth embodiment shown is an example in which the first roughened recess 49a and the second roughened recess 49b are alternately arranged as an intermittent arrangement of the first roughened recess 49a and the second roughened recess 49b. The first roughened recess 49a is arranged at a corner of the first joint 40, the second roughened recess 49b is arranged at a position adjacent to the first roughened recess 49a in the X direction and the Y direction, and then the first roughened recess 49a is arranged again at a position adjacent to the first roughened recess 49a in the X direction and the Y direction. Thus, the first roughened recess 49a and the second roughened recess 49b are alternately arranged, so that the first roughened recess 49a formed by the two-stage stamping process becomes an intermittent arrangement every other one. As a result, it is easy to manufacture the first roughened recess 49a throughout the entire first joint 40, and it is not easy to cause deformation and strain of the metal wiring plate 4.

[0099] Fig.13 The fifth embodiment shown is an embodiment in which the first roughened recessed portion 49a having the peeling inhibiting portion 70 and the second roughened recessed portion 49b not having the peeling inhibiting portion 70 are alternately arranged on the upper surface of the first bonding portion 40 in the area outside the through hole 46 as the non-roughened area (the first roughened recessed portion 49a is arranged intermittently). That is, in the area inside the through hole 46 (non-roughened area) and Fig.10 Similarly, in the region outside the through hole 46 (non-roughened region), Fig.12 The structure is the same.

[0100] exist Figure 4 , Figure 8 , Fig.10 , Fig.11 , Fig.12 as well as Fig.13 In the embodiment, the first roughened recessed portions 49a and the second roughened recessed portions 49b are arranged regularly in a rectangular grid, but the first roughened recessed portions 49a and the second roughened recessed portions 49b may be arranged in a staggered manner.

[0101] The above-mentioned peeling inhibiting portion 70 has the flange portion 73 of a continuous shape along the entire circumference of the inner surface of the first roughened recessed portion 49a in plan view, but a plurality of peeling inhibiting portions may be provided in a dispersed arrangement in plan view in one first roughened recessed portion.

[0102] In addition, the first roughened recessed portion 49a described above is formed by two-stage stamping using the first die 80 and the second die 83, but a roughened recessed portion having a peeling-inhibiting portion may be formed by three or more stages of stamping. In this case, the peeling-inhibiting portion formed inside the roughened recessed portion may be different from the peeling-inhibiting portion 70 of the first roughened recessed portion 49a and may have a structure including a multi-layer flange portion.

[0103] In addition, the first roughened concave portion 49a described above has a quadrangular prism-shaped opening concave portion 74 on the upper side of the flange portion 73, and has a space surrounded by four inclined surfaces 72 and a bottom surface 71 on the lower side of the flange portion 73, but the shape of the roughened concave portion having the peeling inhibition portion is not limited thereto. For example, the basic shape of the roughened concave portion may be a cylindrical shape or a hemispherical shape, and the peeling inhibition portion may be formed as a protruding portion on its inner surface.

[0104] In addition, in the above-mentioned embodiment, the first joint portion 40 of the metal wiring plate 4 has a through hole 46 in the non-roughened area on the upper surface, but the structure of the non-roughened area is not limited to the through hole. For example, in the case where a wire is connected to the upper surface of the metal wiring plate 4, the portion where the wire is connected may also be the non-roughened area. In addition, a protrusion protruding upward from the metal wiring plate 4, a bottomed hole (a concave portion having a shape, depth, etc. different from the roughened concave portion) provided on the upper surface of the metal wiring plate 4, etc. may also be applied as the non-roughened area.

[0105] Furthermore, the present invention can also be applied to a joint portion of a metal wiring plate having no non-roughened region such as through-hole 46 on the upper surface (a plurality of roughened recessed portions are arranged on the entire surface).

[0106] As described above, according to this embodiment, the adhesion between the metal wiring plate and the sealing resin can be improved. In addition, the bonding strength between the semiconductor element and the metal wiring plate can be improved while ensuring the thickness of the bonding material.

[0107] Although the present embodiment and the modified examples have been described, the above-described embodiment and the modified examples may be combined in whole or in part as other embodiments.

[0108] In addition, in the above-mentioned embodiment, the number and arrangement positions of the semiconductor elements are not limited to the above-mentioned configurations, and can be changed as appropriate.

[0109] In addition, in the above-mentioned embodiment, the number and layout of the circuit boards are not limited to the above-mentioned configuration, but can be changed as appropriate.

[0110] In the above-described embodiments, the laminate substrate and the semiconductor element are configured to be rectangular or square in plan view, but the present invention is not limited to this configuration and these structures may be configured to be polygonal in addition to the above-described configurations.

[0111] In addition, the present embodiment is not limited to the above-mentioned embodiment and variation, and various changes, substitutions, and variations can be made within the scope of the main purpose of the technical idea. In addition, if the technical idea can be realized in other ways due to technological progress or other derived technologies, the method can also be used for implementation. Therefore, the claims cover all embodiments that can be included in the scope of the technical idea.

[0112] The characteristic points of the above-mentioned embodiment are summarized below.

[0113] The semiconductor module of the above-mentioned embodiment comprises: a stacked substrate having a plurality of circuit boards arranged on the upper surface of an insulating plate; a semiconductor element arranged on the upper surface of at least one of the circuit boards; and a metal wiring plate arranged on the upper surface of the semiconductor element, the metal wiring plate having a joining portion which is joined to the upper surface of the semiconductor element via a joining material, the joining portion comprising a plate-like portion having an upper surface and a lower surface, the plate-like portion having a plurality of roughened recesses which roughen the upper surface, and at least a portion of the plurality of roughened recesses having a peeling-inhibiting portion which protrudes inwardly to narrow the opening width.

[0114] In addition, a non-roughened area is provided on the upper surface of the plate-like portion, and the non-roughened area does not have the roughened recessed portion. The plurality of roughened recessed portions include a first roughened recessed portion having the peeling inhibition portion and a second roughened recessed portion not having the peeling inhibition portion. The first roughened recessed portion is arranged at a position closer to the outside of the bonding portion than the non-roughened area, and the second roughened recessed portion is arranged at a position closer to the inside of the bonding portion than the non-roughened area.

[0115] Furthermore, the non-roughened region has a through hole that penetrates the plate-like portion.

[0116] Furthermore, the plurality of roughened recessed portions include first roughened recessed portions having the peeling inhibiting portion and second roughened recessed portions not having the peeling inhibiting portion, and the first roughened recessed portions are intermittently arranged with the second roughened recessed portions interposed therebetween.

[0117] In addition, the method for manufacturing the semiconductor module uses a plurality of press processes to form the roughened recessed portion having the peeling inhibiting portion.

[0118] Industrial Applicability

[0119] As described above, the present invention has an effect of improving the adhesion between the joint portion of the metal wiring plate and the sealing resin, and is particularly useful for semiconductor modules for industrial use or electrical equipment.

[0120] This application is based on Japanese Patent Application No. 2022-177078 filed on November 4, 2022, the contents of which are incorporated herein in their entirety.

[0121] Description of Reference Numerals

[0122] 1. semiconductor module; 2. laminated substrate; 3. semiconductor element; 4. metal wiring board; 5. sealing resin; 10. cooler; 11. housing; 20. insulating plate; 21. heat sink; 22. circuit board; 40. first joint (joint); 41. second joint; 42. connecting part; 43. first bent part; 44. second bent part; 46. through hole (non-roughened area); 48. through hole; 49. roughened concave part; 49a. first roughened concave part (with peeling , a roughened recess having a peeling inhibition portion); 49b, a second roughened recess (a roughened recess having no peeling inhibition portion); 60, a main terminal; 61, a control terminal; 70, a peeling inhibition portion; 71, a bottom surface; 72, an inclined surface; 73, a flange portion; 74, an opening recess; 75, a bottom surface; 76, a side surface; 80, a first mold; 83, a second mold; 100, a semiconductor device; F, a coating film; S1, a bonding material; S2, a bonding material; S3, a bonding material; S4, a bonding material.

Claims

1. A semiconductor module, wherein: The semiconductor module has: A laminate substrate having a plurality of circuit boards arranged on an upper surface of an insulating plate; a semiconductor element disposed on an upper surface of at least one of the circuit boards; and a metal wiring plate disposed on the upper surface of the semiconductor element, The metal wiring plate has a bonding portion bonded to the upper surface of the semiconductor element via a bonding material. The engaging portion includes a plate-shaped portion having an upper surface and a lower surface, The plate-like portion has a plurality of roughened recessed portions, and the plurality of roughened recessed portions roughen the upper surface, At least a part of the plurality of roughened recessed portions has a peeling-inhibiting portion that protrudes inward to narrow an opening width.

2. The semiconductor module according to claim 1, wherein: The upper surface of the plate-shaped portion has a non-roughened area, the non-roughened area does not have the roughened recessed portion, The plurality of roughened recessed portions include a first roughened recessed portion having the peeling inhibiting portion and a second roughened recessed portion not having the peeling inhibiting portion, The first roughened recessed portion is disposed at an outer side of the bonding portion than the non-roughened region, and the second roughened recessed portion is disposed at an inner side of the bonding portion than the non-roughened region.

3. The semiconductor module according to claim 2, wherein: The non-roughened region has a through hole that penetrates the plate-shaped portion.

4. The semiconductor module according to claim 1, wherein: The plurality of roughened recessed portions include a first roughened recessed portion having the peeling inhibiting portion and a second roughened recessed portion not having the peeling inhibiting portion, The first roughened recessed portions are intermittently arranged such that the second roughened recessed portions are interposed between the first roughened recessed portions.

5. A method for manufacturing a semiconductor module, which is the method for manufacturing a semiconductor module according to claim 1, wherein: The roughened recessed portion having the peeling inhibiting portion is formed by a plurality of press processes.