Adhesive film for metal terminal and method for manufacturing same, metal terminal equipped with adhesive film for metal terminal, exterior material for electric storage device, kit having exterior material for electric storage device and adhesive film for metal terminal, and electric storage

By using an adhesive film of an acid-modified polyolefin resin layer between the metal terminal and the outer packaging material for electric storage devices, the problems of diversification of shapes and lightweighting and insufficient adhesion in the prior art are solved, and the problem of inadequate adhesion in the prior art is achieved. Improves high bonding and sealing properties.

CN119096397APending Publication Date: 2024-12-06DAI NIPPON PRINTING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380036392.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-28
Filing Date
2023-04-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing outer packaging materials for electric storage devices are difficult to cope with the requirements of diversification of shapes and lightweighting, and the interface adhesion between the metal terminals and the hot-welding resin layer is insufficient, which affects the sealing properties.

Method used

A metal terminal adhesive film is used, and the resin layer A contains acid-modified polyolefins, and the crystallinity of heating is 11 or more after being heated by an X-ray diffraction device under conditions of 200°C, 0.25 MPa, and 16 seconds is improved. Adhesiveness between metal terminals and outer packaging materials.

Benefits of technology

It significantly improves the adhesion and sealing of metal terminals to the outer packaging material, adapts to the needs of diversified shapes and lightweighting, and enhances the sealing strength after electrolyte impregnation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119096397A_ABST
    Figure CN119096397A_ABST
Patent Text Reader

Abstract

The present invention relates to an adhesive film for metal terminals, which is interposed between a metal terminal that is electrically connected to an electrode of an electricity storage device element and an exterior material for an electricity storage device that encapsulates the electricity storage device element, and wherein: a resin layer A that forms at least one surface of the adhesive film for metal terminals contains an acid-modified polyolefin; the adhesive film for a metal terminal has a crystallinity of 11 or more as measured in the resin layer A after heating the adhesive film for a metal terminal at 200 DEG C and 0.25 MPa for 16 seconds using an X-ray diffraction device under the following conditions. (Measurement conditions) X-ray irradiation angle is set to 0.09 DEG with respect to the surface (0 DEG) of the resin layer (A). The measurement range is a range from the surface of the resin layer (A) to a depth of 5 [mu] m. The camera length of the X-ray detector is set to be 500 mm, the X-ray wavelength is set to be # imgabs0 #, and the exposure time is set to be 30 seconds.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an adhesive film for metal terminals and a method for producing the same, a metal terminal with the adhesive film for metal terminals, an outer packaging material for a power storage device, a kit having the outer packaging material for a power storage device and the adhesive film for metal terminals, and a power storage device and a method for producing the same. Background Art

[0002] Various types of power storage devices have been developed. However, in all power storage devices, outer packaging materials for power storage devices are indispensable components for encapsulating power storage device components such as electrodes and electrolytes. In the past, outer packaging materials for power storage devices were mostly made of metal. However, in recent years, with the high performance of electric vehicles, hybrid electric vehicles, computers, cameras, mobile phones, etc., power storage devices require various shapes, and also require thinning and light weight. However, the outer packaging materials for power storage devices made of metal that are currently mostly used have the disadvantages of being difficult to cope with the diversity of shapes and having a limit to light weight.

[0003] Therefore, in recent years, as an outer packaging material for a storage device that can be easily processed into various shapes and can be thinned and lightened, a laminated sheet having a base layer / adhesive layer / barrier layer / thermo-fusible resin layer laminated in this order has been proposed. When such a laminated film-shaped outer packaging material for a storage device is used, the outer packaging material for the storage device is heat-sealed to heat-fuse the peripheral edge of the outer packaging material for the storage device while the innermost heat-fusible resin layers of the outer packaging material for the storage device are facing each other, thereby encapsulating the storage device element using the outer packaging material for the storage device.

[0004] The metal terminal extends from the heat-sealed portion of the outer packaging material for the storage device, and the storage device element encapsulated by the storage device outer packaging material is electrically connected to the outside through the metal terminal electrically connected to the electrode of the storage device element. That is, in the heat-sealed portion of the outer packaging material for the storage device, the portion where the metal terminal exists is heat-sealed in a state where the metal terminal is sandwiched by the heat-fusible resin layer. Since the metal terminal and the heat-fusible resin layer are composed of different types of materials, the adhesion at the interface between the metal terminal and the heat-fusible resin layer is easily reduced.

[0005] Therefore, an adhesive film may be disposed between the metal terminal and the heat-adhesive resin layer for the purpose of improving the adhesion between them. As such an adhesive film, for example, an adhesive film described in Patent Document 1 can be cited.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2015-79638 Summary of the invention

[0009] Technical problem to be solved by the invention

[0010] The main purpose of the present invention is to provide an adhesive film for metal terminals that has good adhesion to the metal terminals and is interposed between a metal terminal electrically connected to an electrode of an electric storage device element and an outer packaging material for an electric storage device that encapsulates the electric storage device element. The present invention also aims to provide a method for manufacturing the adhesive film for metal terminals, a metal terminal with the adhesive film for metal terminals, an outer packaging material for an electric storage device, a kit having an outer packaging material for an electric storage device and the adhesive film for metal terminals, an electric storage device, and a method for manufacturing the electric storage device.

[0011] Technical solutions for solving technical problems

[0012] The inventors of the present invention have conducted in-depth research to solve the above technical problems. As a result, it was found that an adhesive film for metal terminals is interposed between a metal terminal electrically connected to an electrode of an electric storage device element and an outer packaging material for an electric storage device that encapsulates the electric storage device element, and the resin layer A forming at least one surface thereof contains an acid-modified polyolefin, and the crystallinity of the surface of the resin layer A measured by an X-ray diffraction device under specified conditions after the adhesive film for metal terminals is heated at 200°C, 0.25MPa, and 16 seconds is 11 or more, and the surface of the resin layer A side of the adhesive film for metal terminals has good adhesion to the metal terminal. The present invention was completed by further repeated research based on the above cognition.

[0013] That is, the present invention provides the inventions of the following aspects.

[0014] An adhesive film for metal terminals, which is interposed between a metal terminal electrically connected to an electrode of an electric storage device element and an outer packaging material for an electric storage device encapsulating the electric storage device element, wherein a resin layer A forming at least one surface of the adhesive film for metal terminals contains an acid-modified polyolefin,

[0015] The crystallinity of the surface of the resin layer A measured by using an X-ray diffraction apparatus after heating the adhesive film for a metal terminal at 200° C., 0.25 MPa, and 16 seconds under the following conditions was 11 or more.

[0016] (Measurement conditions)

[0017] The X-ray irradiation angle was set to 0.09° with respect to the surface (0°) of the resin layer A.

[0018] The measurement range was set to be a range from the surface of the resin layer A to a depth of 5 μm.

[0019] The camera length of the X-ray detector is set to 500 mm and the X-ray wavelength is set to The exposure time was set to 30 seconds.

[0020] Effects of the Invention

[0021] According to the present invention, an adhesive film for metal terminals can be provided, which is interposed between a metal terminal electrically connected to an electrode of an electric storage device element and an outer packaging material for an electric storage device that encapsulates the electric storage device element, and has good adhesion to the metal terminal. Furthermore, the present invention also aims to provide a method for manufacturing the adhesive film for metal terminals, a metal terminal with the adhesive film for metal terminals, an outer packaging material for an electric storage device, a kit having an outer packaging material for an electric storage device and an adhesive film for metal terminals, and an electric storage device and a method for manufacturing the same. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a schematic top view of the power storage device of the present invention.

[0023] Figure 2 yes Figure 1 Schematic diagram of the cross section along line A-A'.

[0024] Figure 3 yes Figure 1 Schematic diagram of the cross section along line BB'.

[0025] Figure 4 It is a schematic cross-sectional view of the adhesive film for metal terminals of the present invention.

[0026] Figure 5 It is a schematic cross-sectional view of the adhesive film for metal terminals of the present invention.

[0027] Figure 6 It is a schematic cross-sectional view of the adhesive film for metal terminals of the present invention.

[0028] Figure 7 It is a schematic cross-sectional view of the adhesive film for metal terminals of the present invention.

[0029] Figure 8 It is a schematic cross-sectional view of the outer packaging material for an electric storage device of the present invention. DETAILED DESCRIPTION

[0030] The adhesive film for metal terminals of the present invention is an adhesive film for metal terminals between a metal terminal electrically connected to an electrode of a storage device element and an outer packaging material for a storage device that encapsulates the storage device element, and is characterized in that a resin layer A forming at least one side surface of the adhesive film for metal terminals contains an acid-modified polyolefin, and that the crystallinity of the resin layer A measured under the following conditions using an X-ray diffraction device after heating the adhesive film for metal terminals at 200°C, 0.25 MPa, and 16 seconds is greater than 11.

[0031] (Measurement conditions)

[0032] The X-ray irradiation angle was set to 0.09° with respect to the surface (0°) of the resin layer A.

[0033] The measurement range was set to be a range from the surface of the resin layer A to a depth of 5 μm.

[0034] The camera length of the X-ray detector is set to 500 mm and the X-ray wavelength is set to The exposure time was set to 30 seconds.

[0035] Since the adhesive film for metal terminals of the present invention has such characteristics, it has excellent adhesion to metal terminals.

[0036] In addition, the energy storage device of the present invention includes: an energy storage device element having at least a positive electrode, a negative electrode and an electrolyte; an outer packaging material for the energy storage device that encapsulates the energy storage device element; and metal terminals that are electrically connected to the positive electrode and the negative electrode, respectively, and extend to the outside of the outer packaging material for the energy storage device, characterized in that an adhesive film for the metal terminals of the present invention is present between the metal terminals and the outer packaging material for the energy storage device.

[0037] Hereinafter, the adhesive film for metal terminals and the method for producing the same, the power storage device and the method for producing the same of the present invention will be described in detail.

[0038] Among them, in this specification, regarding the numerical range, the numerical range shown by "~" means "above" or "below". For example, the expression 2 to 15 mm means above 2 mm and below 15 mm. In the numerical range recorded in sections in the present invention, the upper limit value or lower limit value recorded in a certain numerical range can be replaced by the upper limit value or lower limit value of the numerical range recorded in other sections. In addition, the combination of the upper limit value and the upper limit value, the upper limit value and the lower limit value, or the lower limit value and the lower limit value recorded separately can also form a numerical range respectively. In addition, in the numerical range recorded in the present invention, the upper limit value or the lower limit value recorded in a certain numerical range can also be replaced by the value shown in the embodiment.

[0039] 1. Adhesive film for metal terminals

[0040] The adhesive film for metal terminals of the present invention is interposed between the metal terminal electrically connected to the electrode of the storage device element and the outer packaging material for the storage device that seals the storage device element. Figures 1 to 3 As shown in the figure, the adhesive film 1 for metal terminals of the present invention is interposed between the metal terminal 2 electrically connected to the electrode of the storage device element 4 and the outer packaging material 3 for the storage device that encapsulates the storage device element 4. In addition, the metal terminal 2 extends to the outside of the outer packaging material 3 for the storage device, and is sandwiched by the outer packaging material 3 for the storage device via the adhesive film 1 for metal terminals at the peripheral edge portion 3a of the outer packaging material 3 for the storage device that is heat-sealed.

[0041] Among them, in the present invention, the preliminary bonding process of the adhesive film for metal terminals and the metal terminals is carried out under the conditions of, for example, a temperature of about 140 to 160°C, a pressure of about 0.01 to 1.0 MPa, a time of about 3 to 15 seconds, and a number of times of about 3 to 6 times, and the formal bonding process is carried out under the conditions of, for example, a temperature of about 160 to 240°C, a pressure of about 0.01 to 1.0 MPa, a time of about 3 to 15 seconds, and a number of times of about 1 to 3 times. In addition, the heating temperature when the metal terminal with the adhesive film for metal terminals is arranged on the outer packaging material for the storage device for heat sealing is usually in the range of about 180 to 210°C, and the pressure is usually carried out under the conditions of about 1.0 to 5.0 MPa, a time of about 1 to 5 seconds, and a number of times of about 1 time.

[0042] The adhesive film 1 for metal terminals of the present invention is provided to improve the closeness between the metal terminal 2 and the outer packaging material 3 for the storage device. By improving the closeness between the metal terminal 2 and the outer packaging material 3 for the storage device, the sealing of the storage device element 4 is improved. As described above, when the storage device element 4 is heat-sealed, the storage device element is packaged in a manner that the metal terminal 2 electrically connected to the electrode of the storage device element 4 extends to the outside of the outer packaging material 3 for the storage device. At this time, the metal terminal 2 formed of metal and the heat-fusible resin layer 35 (a layer formed of a heat-fusible resin such as polyolefin) located in the innermost layer of the outer packaging material 3 for the storage device are formed of different types of materials. Therefore, when such an adhesive film is not used, the sealing of the storage device element is easily reduced at the interface between the metal terminal 2 and the heat-fusible resin layer 35.

[0043] [Resin layer A]

[0044] The adhesive film 1 for metal terminals of the present invention has at least a resin layer A. The resin layer A forms at least one surface of the adhesive film 1 for metal terminals and is the outermost layer. That is, the adhesive film 1 for metal terminals of the present invention includes at least one resin layer A, and at least one surface of the adhesive film 1 for metal terminals is formed by the resin layer A. To achieve the effect of the present invention, the adhesive film 1 for metal terminals of the present invention can be as follows Figure 4 Single layer shown, can also be Figures 5 to 7 Multiple layers shown.

[0045] In the case where the adhesive film 1 for metal terminals of the present invention is a single layer, the adhesive film 1 for metal terminals is formed by a resin layer A, and the surface on the metal terminal side and the surface of the outer packaging material for the storage device are formed by the resin layer A. In this case, the resin forming the surface on the outer packaging material side of the adhesive film 1 for metal terminals and the resin forming the surface on the metal terminal side are common resins (i.e., resins constituting the resin layer A). Among them, the resin forming the surface on the outer packaging material side of the adhesive film 1 for metal terminals and the resin forming the surface on the metal terminal side are common means that among the components of these resins, for example, 80% or more of the same, 90% or more of the same, 95% or more of the same, 100% or more of the same, etc.

[0046] When the adhesive film 1 for metal terminals of the present invention is multi-layered, at least one layer may be formed of the resin layer A. For example, Figure 5 As shown, when the adhesive film 1 for metal terminals of the present invention is a double-layer structure, the adhesive film 1 for metal terminals is a laminate of a first resin layer 12a and a second resin layer 12b. As described later, in the present invention, the first resin layer 12a of these layers is formed by a resin layer A. When the adhesive film 1 for metal terminals of the present invention is multilayered, the resin forming the side surface of the outer packaging material for the storage device and the resin forming the side surface of the metal terminal may also be a common resin.

[0047] For example, Figure 6 As shown, when the adhesive film 1 for metal terminals of the present invention has a three-layer structure, the adhesive film 1 for metal terminals is a laminated body in which the first resin layer 12a, the intermediate layer 11 and the second resin layer 12b are laminated in sequence. In the present invention, the first resin layer 12a constitutes the surface on the metal terminal side, and the second resin layer 12b constitutes the surface on the outer packaging material side of the storage device.

[0048] The resin layer A on the metal terminal side surface of the adhesive film 1 for metal terminals of the present invention has the performance of thermally fusing with metal (metal constituting the metal terminal). Therefore, when the adhesive film 1 for metal terminals of the present invention is used, the resin layer A is preferably arranged on the metal terminal side for use. Therefore, in the present invention, at least the first resin layer 12a of the first resin layer 12a and the second resin layer 12b is formed by the resin layer A.

[0049] The surface of the adhesive film for metal terminal 1 of the present invention on the outer packaging material side of the power storage device (for example, the second resin layer 12b) is heat-sealed with the heat-sealed resin layer described below. The resin layer A is also heat-sealed with the heat-sealed resin layer described below.

[0050] The resin layer A is a layer containing an acid-modified polyolefin. From the perspective of better exhibiting the effects of the present invention, the resin layer A is preferably formed of an acid-modified polyolefin. That is, the resin layer A is more preferably formed of an acid-modified polyolefin film.

[0051] The acid-modified polyolefin is not particularly limited as long as it is an acid-modified polyolefin, and preferably, a polyolefin graft-modified with an unsaturated carboxylic acid or an anhydride thereof is used.

[0052] Specific examples of the acid-modified polyolefin include polyethylenes such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, and linear low-density polyethylene; crystalline or amorphous polypropylenes such as homopolypropylene, block copolymers of polypropylene (e.g., block copolymers of propylene and ethylene), and random copolymers of polypropylene (e.g., random copolymers of propylene and ethylene); terpolymers of ethylene-butene-propylene, etc. Among these polyolefins, polyethylene and polypropylene are preferred, and polypropylene is particularly preferred.

[0053] In addition, the acid-modified polyolefin may also be a cyclic polyolefin. For example, the carboxylic acid-modified cyclic polyolefin is a polymer obtained by replacing part of the monomers constituting the cyclic polyolefin with an α,β-unsaturated carboxylic acid or its anhydride, or by block polymerization or graft polymerization of an α,β-unsaturated carboxylic acid or its anhydride and a cyclic polyolefin.

[0054] The acid-modified cyclic polyolefin is a copolymer of an olefin and a cyclic monomer. Examples of olefins that are structural monomers of the cyclic polyolefin include ethylene, propylene, 4-methyl-1-pentene, butadiene, and isoprene. In addition, examples of cyclic monomers that are structural monomers of the cyclic polyolefin include cyclic olefins such as norbornene; specifically, cyclic dienes such as cyclopentadiene, dicyclopentadiene, cyclohexadiene, and norbornene. Among these polyolefins, cyclic olefins are preferably cited, and norbornene is further preferably cited. Styrene can also be cited as a structural monomer.

[0055] Examples of carboxylic acids or their anhydrides used for acid modification include maleic acid, acrylic acid, itaconic acid, crotonic acid, maleic anhydride, itaconic anhydride, etc. The resin layer A preferably has a peak derived from maleic anhydride when analyzed by infrared spectroscopy. For example, when maleic anhydride-modified polyolefin is measured by infrared spectroscopy, a peak at a wave number of 1760 cm -1 Nearby and wave number 1780cm -1 In the case where resin layer A is a layer composed of maleic anhydride-modified polyolefin, when infrared spectroscopy is used to measure, a peak from maleic anhydride is detected near the resin layer A. However, if the acid modification degree is low, the peak sometimes becomes smaller and cannot be detected. In this case, nuclear magnetic resonance spectroscopy can be used for analysis.

[0056] The crystallinity of the resin layer A after heating the adhesive film for metal terminals at 200°C, 0.25 MPa, and 16 seconds, measured under the following conditions using an X-ray diffraction device, is 11 or more. From the perspective of better expressing the effect of the present invention, the crystallinity is preferably about 12 or more, and preferably about 30 or less, more preferably about 20 or less, and further preferably about 15 or less. Preferred ranges include about 11 to 30, about 11 to 20, about 11 to 15, about 12 to 30, about 12 to 20, and about 12 to 15.

[0057] <Measurement of Crystallinity of Resin Layer A After Heating>

[0058] The specific heating of the adhesive film for metal terminals at 200°C, 0.25MPa, and 16 seconds is as follows. The adhesive film for metal terminals is cut into a length of 50mm and a width of 20mm. With a polytetrafluoroethylene film (PTFE film, thickness 100μm) placed on the laminate (the surface of the adhesive film for metal terminals is covered with the PTFE film), it is placed on a press machine heated to 200°C (resin layer A is on the heating plate side), and a silicone sponge sheet is placed, and the adhesive film is heated by standing at a pressure of 0.25MPa for 16 seconds. The heated laminate is naturally cooled to 25°C.

[0059] Next, the crystallinity of the heated resin layer A is measured under the following conditions using an X-ray diffraction apparatus (for example, Aichi Synchrotron Radiation Center., trade name BL8S3 Beamline).

[0060] (Measurement conditions)

[0061] The X-ray irradiation angle was set to 0.09° with respect to the surface (0°) of the resin layer A.

[0062] The measurement range was set to be a range from the surface of the resin layer A to a depth of 5 μm.

[0063] As an X-ray detector, for example, R-AXIS is used, the camera length is set to 500 mm, and the X-ray wavelength is set to The exposure time was set to 30 seconds.

[0064] (Analysis of Resin Layer A)

[0065] Using the X-ray scattering data analysis software FI2D, the data with azimuth angles of 80deg to 100deg are intercepted from the spectrum data of the two-dimensional detector and integrated in the azimuth direction to obtain a one-dimensional spectrum showing the intensity value relative to the diffraction angle 2θ. The straight line between the two points 2θ=4.0deg and 2θ=16.0deg is then subtracted from the one-dimensional spectrum as the background. Thereafter, the spectral intensity value A of the amorphous component is defined as A: the value with the minimum intensity value in the region of 2θ=8.8deg to 9.8deg, and the crystalline peak intensity values ​​P1, P2, P3, and P4 of the four crystal planes are defined as follows.

[0066] P1: Peak intensity value of the peak located in the region of 2θ=7.0deg to 9.2deg

[0067] P2: Peak intensity value of the peak located within 2θ=9.2deg to 10.6deg

[0068] P3: Peak intensity value of the peak located within 2θ=10.6deg to 12.0deg

[0069] P4: Peak top intensity value of the peak located within 2θ=12.0deg to 14.0deg

[0070] The crystallinity C is defined as C = (P1 + P2 + P3 + P4) / A,

[0071] The degree of orientation D is defined as D=P2 / P4.

[0072] As a method for adjusting the crystallinity of the resin layer A containing the acid-modified polyolefin after the above heating, for example, there can be cited the molding method when forming the resin layer A (for example, the type of molding method such as extrusion method and inflation method or the cooling temperature, cooling time, line speed, gap), adjustment of the resin ratio, selection of the resin type, cooling temperature at 200°C, 16 seconds, and 0.25 MPa, cooling time, etc. For example, when slow cooling or high-density resin is selected, there is a tendency for the crystallinity to increase, while when rapid cooling or low-density resin is selected, there is a tendency for the crystallinity to decrease, so it is possible to adjust so that the crystallinity of the resin layer A after heating is within the above range.

[0073] In the adhesive film 1 for metal terminals of the present invention, by setting the above-mentioned crystallinity of the resin layer A containing acid-modified polyolefin constituting at least one side surface of the adhesive film 1 for metal terminals to a high value of 11 or more, excellent adhesion to the metal terminal can be exhibited. The reason is considered to be as follows. That is, the heating conditions (200°C, 0.25MPa, 16 seconds) before measuring the crystallinity of the resin layer A are the conditions for thermal fusion of the resin layer A and the metal terminal. By setting the crystallinity of the heated resin layer A to a high value, the surface portion of the heated resin layer A that is in close contact with the metal terminal has appropriate crystallinity and has appropriate conformability to the shape of the metal terminal (in other words, it is neither too hard nor too soft), and as a result, excellent adhesion to the metal terminal can be exhibited. Moreover, by setting the crystallinity of the heated resin layer A within the above-mentioned specific range, the sealing strength after electrolyte immersion can also be appropriately improved (hereinafter referred to as "sealing strength to metal terminal (after electrolyte immersion)"). The reason is considered to be as follows. That is, by setting the crystallinity of the heated resin layer A within the above-mentioned specific range, the surface portion of the heated resin layer A that is in close contact with the metal terminal has appropriate crystallinity, and thus has appropriate conformity to the shape of the metal terminal (in other words, it is neither too hard nor too soft). It is not easy for a gap to be generated between the heated resin layer A and the metal terminal, and it is not easy for the electrolyte to penetrate into the interface between the resin layer A and the metal terminal. As a result, the sealing strength after electrolyte immersion can be appropriately improved.

[0074] In addition, from the perspective of better expressing the effect of the present invention, the island ratio of the sea-island structure in the heated resin layer A is preferably less than about 2.0, more preferably less than about 1.5, and further preferably less than about 1.0. The most preferred lower limit is 0. As preferred ranges, 0 to 2.0, 0 to 1.5, 0 to 1.0, 0 to 0.8, 0 to 0.5, and 0 to 0.3 can be listed. In addition, by making the island ratio of the heated resin layer A less than about 2.0, preferably less than about 1.5, more preferably less than about 1.0, further preferably less than about 0.8, further preferably less than 0.5, and further preferably less than 0.3, the sealing strength of the adhesive film 1 for metal terminals of the present invention after sealing with the metal terminal and immersing in the electrolyte (hereinafter referred to as "sealing strength to the metal terminal (after electrolyte immersion)") can be appropriately improved. The island ratio is a value measured according to the following measurement method.

[0075] <Measurement of the partiality of the island ratio of the resin layer A after heating>

[0076] [Pretreatment conditions]

[0077] Cut the sample into strips and embed it with thermosetting resin (50℃, 24 hours)

[0078] Ru dyeing after trimming

[0079] ·Use ultra-thin microtome to make cross sections (using diamond knife: finishing thickness 80nm)

[0080] Os coating (1~3nm)

[0081] [SEM observation conditions]

[0082] · Measurement device: Commercially available SEM (e.g. S-4800TYPE II manufactured by Hitachi High-Technologies Corporation)

[0083] Accelerating voltage: 5.0 kV

[0084] Emission current: 20μA

[0085] WD: 5mm

[0086] Detector: Upper+HA

[0087] ·Measurement magnification: 10k times

[0088] Resolution: 256dpi

[0089] [Image processing conditions]

[0090] The electron microscope image was subjected to the following image processing to obtain a binary image.

[0091] Image processing can be done using the Python image processing library OpenCV. The image processing conditions are as follows.

[0092] 1. Gaussian filter (kernel size 5px×5px)

[0093] 2. Magnify the measured image to 8 times in the vertical and horizontal directions (complementation method = CUBIC)

[0094] 3. Use fastNIMeansDenoising function to remove noise (set background color = black, parameters of fastNIMeansDenoising function are h = 10, hForColorComponents = 10, templateWindowSize = 7, searchWindowSize = 21)

[0095] 4. Binarization is performed with the bright part being white and the dark part being black (threshold = Otsu's threshold)

[0096] 5. Morphological transformation - Open processing (kernel size = 45px × 15px)

[0097] 6. Noise removal (remove the black area below 625px^2)

[0098] 7. Noise removal (remove the white area below 75px^2)

[0099] 8. Noise removal (remove black areas below 10000px^2)

[0100] 9. Morphological transformation - Open processing (kernel size = 65px × 25px)

[0101] 10. Morphological transformation - CLOSE processing (kernel size = 25px × 1px)

[0102] An area of ​​504 px×504 px (corresponding to a 1 μm×1 μm viewing angle) was cut out from the obtained binary image, and the ratio of the white portion in this area was defined as W (%).

[0103] The ratio W of the white portion is calculated by intercepting any 40 points, and the standard deviation of W at the 40 points is divided by the average value of W at the 40 points. The obtained value is defined as the degree of bias L of the sea-island structure.

[0104] As a method for adjusting the degree of bias in the island ratio of the above-mentioned heated resin layer A containing acid-modified polyolefin, for example, there can be cited the molding method (for example, the type of molding method such as extrusion method and inflation method or the cooling temperature, cooling time, line speed), the adjustment of the resin ratio, etc. when forming the resin layer A. For example, in the case of rapid cooling, accelerated line speed, and increased components forming the islands of the resin, the island ratio is prone to bias, while in the case of slow cooling, slow line speed, and reduced components forming the islands of the resin, the island ratio is not prone to bias, and thus the island ratio of the heated resin layer A can be adjusted to reduce the bias.

[0105] In the adhesive film 1 for metal terminals of the present invention, the crystallinity of the heated resin layer A is 11 or more, and the island ratio of the sea-island structure of the heated resin layer A containing acid-modified polyolefin constituting at least one side surface of the adhesive film 1 for metal terminals is about 0.5 or less, and the sealing strength after immersion in the electrolyte (hereinafter referred to as "sealing strength to metal terminal (after electrolyte immersion)") can be more appropriately improved. The reason is considered to be as follows. That is, with respect to the island portion of the resin layer A, the sea portion and the island portion are usually formed by different resins. For example, when the resin layer A is formed by acid-modified polypropylene (the cross section has a sea-island structure of resin), the sea portion is usually formed by an acid-modified polypropylene component, and the island portion is formed by a polyethylene component. The density of the polyethylene part of the island portion is lower than that of the acid-modified polypropylene part of the sea portion, and the volume expansion coefficient, viscosity, and swelling property of the electrolyte are also different from those of the sea portion. Therefore, when the deviation of the island portion on the cross section of the heated resin layer A is large, the performance after the electrolyte penetrates into the heated resin layer A will also be biased, resulting in an easy reduction in the mechanical strength of the heated resin layer A. In the present invention, by setting the deviation of the island portion ratio of the sea-island structure of the heated resin layer A to less than about 0.5, the deviation of the island portion on the cross section of the heated resin layer A is reduced, and it can be considered that the sealing strength after the electrolyte is impregnated is improved.

[0106] In addition, from the perspective of better demonstrating the effect of the present invention, the orientation degree in the heated resin layer A is preferably about 1.0 or more, more preferably about 1.1 or more, further preferably about 1.2 or more, and further preferably about 1.3 or more, and the preferred upper limit is 2.0. As preferred ranges, about 1.0 to 2.0, about 1.1 to 2.0, about 1.2 to 2.0, and about 1.3 to 2.0 can be listed. In addition, by having the orientation degree of the heated resin layer A be about 1.2 or more, the sealing strength after the adhesive film 1 for metal terminal of the present invention is sealed with the metal terminal and then immersed in the electrolyte (hereinafter referred to as "sealing strength to metal terminal (after electrolyte immersion)" can be appropriately improved. The orientation degree is a value measured according to the following measurement method.

[0107] <Measurement of Orientation Degree of Resin Layer A after Heating>

[0108] The crystallinity is measured under the following conditions using an X-ray diffraction apparatus (eg, Aichi Synchrotron Radiation Center., trade name BL8S3 Beamline).

[0109] (Measurement conditions: resin layer A)

[0110] The X-ray irradiation angle was set to 0.09° with respect to the surface (0°) of the resin layer A.

[0111] The measurement range was set to be a range from the surface of the resin layer A to a depth of 5 μm.

[0112] As an X-ray detector, for example, R-AXIS is used, the camera length is set to 500 mm, and the X-ray wavelength is set to The exposure time was set to 30 seconds.

[0113] (Analysis of Resin Layer A)

[0114] Using the X-ray scattering data analysis software FI2D, the data with azimuth angles of 80deg to 100deg are intercepted from the spectrum data of the two-dimensional detector and integrated in the azimuth direction to obtain a one-dimensional spectrum showing the intensity value relative to the diffraction angle 2θ. The straight line between the two points 2θ=4.0deg and 2θ=16.0deg is then subtracted from the one-dimensional spectrum as the background. Thereafter, the spectral intensity value A of the amorphous component is defined as A: the value with the minimum intensity value in the region of 2θ=8.8deg to 9.8deg, and the crystalline peak intensity values ​​P1, P2, P3, and P4 of the four crystal planes are defined as follows.

[0115] P1: Peak intensity value of the peak located in the region of 2θ=7.0deg to 9.2deg

[0116] P2: Peak intensity value of the peak located within 2θ=9.2deg to 10.6deg

[0117] P3: Peak intensity value of the peak located within 2θ=10.6deg to 12.0deg

[0118] P4: Peak top intensity value of the peak located within 2θ=12.0deg to 14.0deg

[0119] The crystallinity C is defined as C = (P1 + P2 + P3 + P4) / A,

[0120] The degree of orientation D is defined as D=P2 / P4.

[0121] The resin layer A may be formed of a single resin component or a blended polymer of two or more resin components. From the perspective of film-forming properties, the resin layer A is preferably formed of a blended polymer of two or more resin components. In the case of forming a blended polymer, the resin layer A preferably has acid-modified polypropylene as the main component (a component of 50% by weight or more) and other resins (preferably polyethylene from the perspective of improving flexibility) of 50% by weight or less. On the other hand, from the perspective of electrolyte resistance of the resin layer A, the resin layer A preferably contains acid-modified polypropylene as the resin alone.

[0122] The resin layer A may contain known additives as necessary.

[0123] For example, the resin layer A may contain a filler as needed. The resin layer A contains a filler, and the filler functions as a spacer, so that the short circuit between the metal terminal 2 and the barrier layer 33 of the outer packaging material 3 for the storage device can be effectively suppressed. As the particle size of the filler, a range of about 0.1 to 35 μm, preferably about 5.0 to 30 μm, and more preferably about 10 to 25 μm can be listed. In addition, as the content of the filler, about 5 to 30 parts by mass, and more preferably about 10 to 20 parts by mass, can be listed relative to 100 parts by mass of the resin component forming the resin layer A.

[0124] As filler, both inorganic and organic systems can be used. As inorganic filler, for example, carbon (charcoal, graphite), silicon dioxide, aluminum oxide, barium titanate, iron oxide, silicon carbide, zirconium oxide, zirconium silicate, magnesium oxide, titanium oxide, calcium aluminate, calcium hydroxide, aluminum hydroxide, magnesium hydroxide, calcium carbonate, etc. can be listed. In addition, as organic filler, for example, fluorine-containing resin, phenolic resin, urea resin, epoxy resin, acrylic resin, benzoguanamine-formaldehyde condensate, melamine-formaldehyde condensate, polymethyl methacrylate crosslinked product, polyethylene crosslinked product, etc. can be listed. From the aspect of shape stability, rigidity, and content tolerance, aluminum oxide, silicon dioxide, fluorine-containing resin, acrylic resin, benzoguanamine-formaldehyde condensate are preferred, wherein, spherical aluminum oxide and silicon dioxide are particularly preferred. The filler may be mixed into the resin component forming the resin layer A by: preliminarily melt-blending the two using a Banbury mixer or the like to form a masterbatch, and then setting the masterbatch to a specified mixing ratio; or directly mixing the filler with the resin component.

[0125] In addition, the resin layer A may contain a pigment as needed. As the pigment, various inorganic pigments can be used. As a specific example of the pigment, the carbon (charcoal, graphite) exemplified in the above-mentioned filler is preferably exemplified. Carbon (charcoal, graphite) is a material usually used inside the storage device, and there is no concern about the dissolution of the electrolyte. In addition, the coloring effect is good, and a sufficient coloring effect can be obtained with an amount added that does not damage the adhesion, and it will not melt due to heat, and the apparent melt viscosity of the resin after addition can be increased. In addition, it prevents the pressurized portion from becoming thinner during thermal bonding (heat sealing), and can impart excellent sealing properties between the outer packaging material for the storage device and the metal terminal.

[0126] When a pigment is added to the resin layer A, the amount of addition thereof, for example, when carbon black having a particle size of about 0.03 μm is used, can be about 0.05 to 0.3 parts by mass, preferably about 0.1 to 0.2 parts by mass, relative to 100 parts by mass of the resin component forming the resin layer A. By adding a pigment to the resin layer A, the presence or absence of the adhesive film 1 for metal terminals can be detected by a sensor, or by visual inspection. In addition, when a filler and a pigment are added to the resin layer A, the filler and the pigment can be added to the same resin layer A, but from the perspective of not damaging the thermal fusion property of the adhesive film 1 for metal terminals, it is preferred that the filler and the pigment are added separately to different layers (for example, the first resin layer 12a, the second resin layer 12b, the intermediate layer 11, etc. described later).

[0127] From the perspective of better expressing the effects of the present invention, the melting peak temperature of the resin layer A is preferably 125° C. or higher, more preferably about 130° C. or higher, and further preferably about 135° C. or higher. From the same perspective, the melting peak temperature is, for example, 180° C. or lower, preferably 175° C. or lower, more preferably 170° C. or lower, further preferably about 165° C. or lower, and further preferably about 160° C. or lower. Preferred ranges of the melting peak temperature include about 125 to 180° C., about 125 to 175° C., about 125 to 170° C., about 125 to 165° C., about 125 to 160° C., about 130 to 180° C., about 130 to 175° C., about 130 to 170° C., about 130 to 165° C., about 130 to 160° C., about 135 to 180° C., about 135 to 175° C., about 135 to 170° C., about 135 to 165° C., and about 135 to 160° C. In the present invention, the method for measuring the melting peak temperature is as follows.

[0128] <Determination of Melting Peak Temperature>

[0129] The melting peak temperature of each measurement sample is measured in accordance with the provisions of JIS K7121: 2012 (Determination method of transition temperature of plastics (Supplement 1 to JIS K7121: 1987)). The measurement is performed using a differential scanning calorimeter (DSC, such as the differential scanning calorimeter Q200 manufactured by TA Instruments). After the measurement sample is kept at -50°C for 15 minutes, the temperature is increased from -50°C to 210°C at a heating rate of 10°C / min, and the first melting peak temperature P (°C) is measured, and then it is kept at 210°C for 10 minutes. Then, the temperature is decreased from 210°C to -50°C at a cooling rate of 10°C / min and maintained for 15 minutes. The temperature is then increased from -50°C to 210°C at a heating rate of 10°C / min, and the second melting peak temperature Q (°C) is measured. The flow rate of nitrogen is 50 ml / min. According to the above steps, the melting peak temperature P (°C) measured for the first time and the melting peak temperature Q (°C) measured for the second time are calculated, and the melting peak temperature P (°C) value measured for the first time according to the above steps is used.

[0130] When the adhesive film 1 for metal terminal of the present invention is composed of a single layer of the resin layer A, the total thickness of the adhesive film 1 for metal terminal described later corresponds to the thickness of the resin layer A.

[0131] In addition, when the adhesive film 1 for metal terminals of the present invention is composed of multiple layers, from the perspective of better achieving the effect of the present invention, the thickness of the resin layer A is preferably about 10 μm or more, more preferably about 15 μm or more, and more preferably about 20 μm or more, and preferably about 120 μm or less, more preferably about 100 μm or less, and more preferably about 80 μm or less. As the preferred range of the thickness of the resin layer A, there can be listed about 10 to 120 μm, about 10 to 100 μm, about 10 to 80 μm, about 15 to 120 μm, about 15 to 100 μm, about 15 to 80 μm, about 20 to 120 μm, about 20 to 100 μm, and about 20 to 80 μm. From the perspective of improving the insulation of the adhesive film for metal terminals, the thickness of the resin layer A is preferably about 55 μm or more, more preferably about 60 μm or more, and preferably about 100 μm or less, more preferably about 90 μm or less, and as a preferred range, about 55 to 100 μm, about 55 to 90 μm, about 60 to 100 μm, and about 60 to 90 μm can be listed. Among them, when the adhesive film 1 for metal terminals of the present invention includes multiple layers of resin layers A, the thickness of each resin layer A is preferably the above thickness.

[0132] As described above, the adhesive film 1 for metal terminal of the present invention is, for example, Figure 6As shown in FIG. 1 , a structure in which at least the first resin layer 12a, the intermediate layer 11, and the second resin layer 12b are stacked in sequence can be formed. In this structure, since the first resin layer 12a is arranged on the side of the metal terminal 2, at least the first resin layer 12a becomes the resin layer A. In addition, the second resin layer 12b is arranged on the side of the outer packaging material 3 for the storage device. In this structure, the first resin layer 12a and the second resin layer 12b are respectively located on both side surfaces.

[0133] The second resin layer 12b is a layer formed of resin. The second resin layer 12b may be formed of a resin layer A, or may be formed of a resin layer B different from the resin layer A (i.e., the resin layer B is a resin layer that does not contain an acid-modified polyolefin, or contains an acid-modified polyolefin but has a crystallinity of less than 11 as measured under the above conditions using an X-ray diffraction device).

[0134] In addition, the intermediate layer 11 may be formed of the resin layer A or may be formed of a resin layer B different from the resin layer A.

[0135] [Resin layer B]

[0136] Examples of the resin constituting the resin layer B include polyolefin resins, polyamide resins, polyester resins, epoxy resins, acrylic resins, fluorine-containing resins, silicone resins, phenolic resins, polyetherimides, polyimides, polycarbonates, and mixtures or copolymers thereof, among which polyolefin resins are particularly preferred. Examples of the polyolefin resins include polyolefins, acid-modified polyolefins, and the like.

[0137] As described later, the second resin layer 12b preferably contains a polyolefin resin (i.e., has a polyolefin skeleton), more preferably contains a polyolefin, and further preferably is a layer formed of a polyolefin. The second resin layer 12b also preferably contains a polyolefin or an acid-modified polyolefin in the polyolefin resin, more preferably contains a polyolefin, and further preferably is a layer formed of a polyolefin.

[0138] The intermediate layer 11 preferably contains a polyolefin-based resin (that is, has a polyolefin skeleton), more preferably contains polyolefin, and further preferably is a layer formed of polyolefin.

[0139] In the second resin layer 12b and the resin layer B used in the intermediate layer 11, the polyolefin-based resin is preferably a polypropylene-based resin. The polyolefin is preferably polypropylene, and the acid-modified polyolefin is preferably acid-modified polypropylene.

[0140] The resin layer B can be formed by a single resin component or a blended polymer of two or more resin components. From the perspective of film-forming properties, the resin layer B is preferably formed by a blended polymer of two or more resin components. In the case of forming a blended polymer, the resin layer B containing acid-modified polypropylene preferably has acid-modified polypropylene as the main component (a component of 50% by weight or more) and other resins of 50% by mass or less (preferably polyethylene from the perspective of improving flexibility). In addition, the resin layer B containing polypropylene preferably has polypropylene as the main component (a component of 50% by weight or more) and other resins of 50% by mass or less (preferably polyethylene from the perspective of improving flexibility). On the other hand, from the perspective of the electrolyte resistance of the resin layer B, the resin layer B containing acid-modified polypropylene preferably contains acid-modified polypropylene as the resin alone, and the resin layer B containing polypropylene preferably contains acid-modified polypropylene or polypropylene as the resin alone.

[0141] As the resin constituting the resin layer B, the polyester resin is a resin containing a polyester structure such as polyethylene terephthalate and polybutylene terephthalate. In addition to the polyethylene terephthalate structure or the polybutylene terephthalate structure, a polyether structure may be included, and the polyether structure may have a polycondensation structure of terephthalic acid having a polybutylene terephthalate structure with at least one of polytetramethylene ether glycol and neopentyl glycol. In addition to the polyethylene terephthalate structure or the polybutylene terephthalate structure, another polyester structure may be included, and the polyester structure may have a polycondensation structure of 1,4-butanediol having a polybutylene terephthalate structure with at least one selected from isophthalic acid, dodecanedioic acid and sebacic acid.

[0142] The melting peak temperature of the resin layer B is preferably 125° C. or higher, more preferably about 130° C. or higher, and further preferably about 135° C. or higher. The melting peak temperature is, for example, 180° C. or lower, preferably 175° C. or lower, more preferably 170° C. or lower, further preferably about 165° C. or lower, and further preferably about 160° C. or lower. Preferred ranges of the melting peak temperature include about 125 to 180° C., about 125 to 175° C., about 125 to 170° C., about 125 to 165° C., about 125 to 160° C., about 130 to 180° C., about 130 to 175° C., about 130 to 170° C., about 130 to 165° C., about 130 to 160° C., about 135 to 180° C., about 135 to 175° C., about 135 to 170° C., about 135 to 165° C., and about 135 to 160° C.

[0143] In addition, when the adhesive film 1 for metal terminals of the present invention has a resin layer B as the second resin layer 12b, from the perspective of better achieving the effect of the present invention, the thickness of the resin layer B is preferably about 10 μm or more, more preferably about 15 μm or more, and more preferably about 20 μm or more, and preferably about 120 μm or less, more preferably about 100 μm or less, and more preferably about 80 μm or less. As the preferred range of the thickness of the resin layer B, there can be listed about 10 to 120 μm, about 10 to 100 μm, about 10 to 80 μm, about 15 to 120 μm, about 15 to 100 μm, about 15 to 80 μm, about 20 to 120 μm, about 20 to 100 μm, and about 20 to 80 μm.

[0144] In addition, when the adhesive film 1 for metal terminals of the present invention has a resin layer B as the intermediate layer 11, from the perspective of better achieving the effect of the present invention, the thickness of the resin layer B is preferably about 10 μm or more, more preferably about 20 μm or more, and more preferably about 30 μm or more, and preferably about 120 μm or less, more preferably about 110 μm or less, and more preferably about 100 μm or less. As the preferred range of the thickness of the resin layer B, there can be listed about 10 to 120 μm, about 10 to 110 μm, about 10 to 100 μm, about 20 to 120 μm, about 20 to 110 μm, about 20 to 100 μm, about 30 to 120 μm, about 30 to 110 μm, and about 30 to 100 μm.

[0145] In addition, the resin layer B may contain known additives (such as the filler and pigment described above) similarly to the resin layer A. The types and amounts of the filler and pigment added are the same as those of the resin layer A.

[0146] From the perspective of better achieving the effect of the present invention, the total thickness of the adhesive film 1 for metal terminals is, for example, about 50 μm or more, preferably about 80 μm or more, more preferably about 90 μm or more, further preferably about 100 μm or more, and further preferably about 180 μm or more. In addition, the total thickness of the adhesive film 1 for metal terminals of the present invention is preferably about 500 μm or less, about 300 μm or less, more preferably about 250 μm or less, and further preferably about 200 μm or less. Preferred ranges of the total thickness of the adhesive film 1 for metal terminals of the present invention include about 50 to 500 μm, about 50 to 300 μm, about 50 to 250 μm, about 50 to 200 μm, about 80 to 500 μm, about 80 to 300 μm, about 80 to 250 μm, about 80 to 200 μm, about 90 to 500 μm, about 90 to 300 μm, about 90 to 250 μm, about 90 to 200 μm, about 100 to 500 μm, about 100 to 300 μm, about 100 to 250 μm, about 100 to 200 μm, about 180 to 500 μm, about 180 to 300 μm, about 180 to 250 μm, and about 180 to 200 μm. As a more specific example, when the adhesive film 1 for metal terminals of the present invention is used for smaller power storage devices for portable phones, smart phones, and tablet computers, the total thickness is preferably about 60 to 100 μm; when used for larger power storage devices for power storage systems and vehicle-mounted uses, the total thickness is preferably about 100 to 200 μm.

[0147] The sealing strength (initial) of the adhesive film 1 for metal terminals of the present invention to the metal terminals measured by the following method is preferably about 20N / 15mm or more, more preferably about 25N / 15mm or more, and further preferably about 30N / 15mm or more. The upper limit of the sealing strength (initial) is usually about 80N / 15mm or less. As preferred ranges, about 20 to 80N / 15mm, about 25 to 80N / 15mm, and about 30 to 80N / 15mm can be listed.

[0148] <Measurement of Sealing Strength (Initial) of Metal Terminals>

[0149] Prepare aluminum (JIS H4160: 1994A8079H-O) with a length of 50 mm, a width of 22.5 mm, and a thickness of 0.4 mm as a metal terminal. In addition, cut the adhesive film for the metal terminal into a length of 45 mm and a width of 10 mm. Then, place the adhesive film for the metal terminal on the metal terminal to obtain a laminate of the metal terminal / adhesive film. At this time, the metal terminal is laminated in such a way that the longitudinal and lateral directions of the metal terminal are respectively consistent with the length direction and width direction of the adhesive film for the metal terminal, and the metal terminal is consistent with the center of the adhesive film for the metal terminal. In addition, the resin layer A of the adhesive film for the metal terminal is arranged on the side of the metal terminal. Next, a polytetrafluoroethylene film (PTFE film, thickness 100 μm) is placed on the adhesive film for the metal terminal of the laminate (the surface of the adhesive film for the metal terminal is covered with the PTFE film), and then placed on a press machine heated to 200°C (the metal terminal is on the heating plate side), and a silicone sponge sheet is placed, and the laminate is allowed to stand for 16 seconds at a pressure of 0.25 MPa to thermally fuse the adhesive film to the metal terminal. The laminate after thermal fusion is naturally cooled to 25°C. Next, under an environment of 25°C, the adhesive film for the metal terminal is peeled off from the metal terminal using a Tensilon universal material testing machine (e.g., RTG-1210 manufactured by A&D). The maximum strength during peeling is taken as the adhesion strength to the metal terminal (N / 15mm). The peeling speed is set to 50 mm / min, the peeling angle is set to 180°, the chuck spacing is set to 30 mm, and the average value of three measurements is taken. The treatment of standing for 16 seconds in a heating and pressurizing environment at a temperature of 200° C. and a surface pressure of 0.25 MPa is a treatment that assumes the heat and pressure applied in the above-mentioned preliminary bonding step and the main bonding step.

[0150] In addition, the sealing strength of the adhesive film 1 for metal terminals of the present invention to the metal terminals measured by the following method (after electrolyte immersion) is preferably about 15N / 15mm or more, more preferably about 20N / 15mm or more, and further preferably about 25N / 15mm or more. The upper limit of the sealing strength (after electrolyte immersion) is usually about 50N / 15mm or less. As preferred ranges, about 15 to 50N / 15mm, about 20 to 50N / 15mm, and about 25 to 50N / 15mm can be listed.

[0151] <Measurement of sealing strength of metal terminals (after electrolyte immersion)>

[0152] Prepare aluminum (JIS H4160: 1994A8079H-O) with a length of 50 mm, a width of 22.5 mm, and a thickness of 0.4 mm as a metal terminal. In addition, cut the adhesive film for the metal terminal into a length of 45 mm and a width of 10 mm. Then, place the adhesive film for the metal terminal on the metal terminal to obtain a laminate of the metal terminal / adhesive film. At this time, the metal terminal is laminated in such a way that the longitudinal and lateral directions of the metal terminal are respectively consistent with the length direction and width direction of the adhesive film for the metal terminal, and the metal terminal is consistent with the center of the adhesive film for the metal terminal. In addition, the resin layer A of the adhesive film for the metal terminal is arranged on the side of the metal terminal. Next, a polytetrafluoroethylene film (PTFE film, thickness 100 μm) is placed on the adhesive film for the metal terminal of the laminate (the surface of the adhesive film for the metal terminal is covered with an ETFE film), and the laminate is placed on a press machine heated to 200°C (the metal terminal is on the heating plate side), and a silicone sponge sheet is placed, and the laminate is allowed to stand for 16 seconds at a pressure of 0.25 MPa to thermally fuse the adhesive film to the metal terminal. The laminate after thermal fusion is naturally cooled to 25°C. Then the obtained laminate is placed in a 100mL plastic bottle, in which a mixed electrolyte (EC (ethylene carbonate) / DMC (dimethyl carbonate) / DEC (diethyl carbonate) = 1:1:1) 100g + pure water 1000ppm is tightly sealed. The sealed container is placed in an oven at 85°C, taken out after 24 hours, the electrolyte is washed off with water, and the obtained laminate is allowed to stand for 30 minutes to dry naturally. Next, at 25°C, use a Tensilon universal material testing machine (such as RTG-1210 manufactured by A&D) to peel off the adhesive film from the metal terminal. The maximum strength during peeling is taken as the adhesion strength to the metal terminal (N / 15mm). The peeling speed is set to 50mm / min, the peeling angle is set to 180°, the chuck spacing is set to 30mm, and the average value of three measurements is taken. Among them, the treatment of standing for 16 seconds in a heated and pressurized environment at a temperature of 200°C and a surface pressure of 0.25MPa is a treatment that assumes the heat and pressure applied by the above-mentioned pre-bonding process and the formal bonding process.

[0153] The adhesive film for metal terminals of the present invention preferably has fine concavo-convex on at least one side of the outermost surface. This can further improve the adhesion with the heat-fusible resin layer 35 of the outer packaging material for the storage device or the metal terminal. Among them, as a method for forming fine concavo-convex on the surface of the outermost layer of the adhesive film for metal terminals, a method of adding additives such as microparticles to the outermost layer, a method of abutting a cooling roller with concavo-convex on the surface to shape, etc. can be listed. As fine concavo-convex, the ten-point average roughness of the surface of the outermost layer is preferably about 0.1μm or more, more preferably about 0.2μm or more, and preferably about 35μm or less, more preferably about 10μm or less, and as a preferred range, about 0.1 to 35μm, about 0.1 to 10μm, about 0.2 to 35μm, about 0.2 to 35μm, about 0.2 to 10μm, about 0.2 to 10μm, about 0.1 to 35μm, about 0.2 to 35μm, about 0.2 to 35μm, about 0.2 to 10μm. The ten-point average roughness is a value measured by using a small surface roughness measuring machine SURFTEST SJ-210 manufactured by Mitutoyo in accordance with the method specified in JIS B0601:1994.

[0154] The adhesive film 1 for metal terminals of the present invention is preferably formed of a polyolefin resin. For example, the resin component contained in the adhesive film 1 for metal terminals of the present invention is preferably only an acid-modified polyolefin or only an acid-modified polyolefin and a polyolefin. Preferred acid-modified polyolefins and polyolefins are as described in the resin layer A and the resin layer B.

[0155] The adhesive film 1 for metal terminals of the present invention is preferably composed of a laminate having a first resin layer 12a, an intermediate layer 11, and a second resin layer 12b in sequence. Hereinafter, taking the case where the adhesive film 1 for metal terminals of the present invention is composed of a laminate having at least a first resin layer 12a, an intermediate layer 11, and a second resin layer 12b in sequence, and the first resin layer 12a is a resin layer A as an example, a preferred embodiment of the adhesive film 1 for metal terminals of the present invention is described in detail.

[0156] When the adhesive film 1 for metal terminals of the present invention is arranged between the metal terminal 2 of the storage device 10 and the outer packaging material 3 for the storage device, the surface of the metal terminal 2 composed of metal and the heat-melting resin layer 35 (a layer formed of a heat-melting resin such as polyolefin) of the outer packaging material 3 for the storage device are bonded by the adhesive film 1 for metal terminals. The first resin layer 12a of the adhesive film 1 for metal terminals is arranged on one side of the metal terminal 2, and the second resin layer 12b is arranged on one side of the outer packaging material 3 for the storage device. The first resin layer 12a is in close contact with the metal terminal 2, and the second resin layer 12b is in close contact with the heat-melting resin layer 35 of the outer packaging material 3 for the storage device. The first resin layer 12a can be a single layer or a multilayer. Moreover, the second resin layer 12b can be a single layer or a multilayer.

[0157] [First Resin Layer 12a and Second Resin Layer 12b]

[0158] The adhesive film 1 for metal terminal according to the preferred embodiment of the present invention is as follows Figure 6 As shown, the first resin layer 12a is provided on one side of one surface of the intermediate layer 11, and the second resin layer 12b is provided on one side of the other surface. The first resin layer 12a is arranged on one side of the metal terminal 2. In addition, the second resin layer 12b is arranged on one side of the outer packaging material 3 for the storage device. In the adhesive film 1 for metal terminals of the present invention, the first resin layer 12a and the second resin layer 12b are respectively located on both side surfaces.

[0159] In the present invention, the first resin layer 12a is formed of the resin layer A. The second resin layer 12b may be formed of the resin layer A or the resin layer B.

[0160] The first resin layer 12a and the second resin layer 12b can be formed of, for example, a resin film. When the first resin layer 12a and the second resin layer 12b are formed of resin films, when the first resin layer 12a and the second resin layer 12b are laminated with the intermediate layer 11 to manufacture the adhesive film 1 for metal terminals of the present invention, the preformed resin film can be used as the first resin layer 12a and the second resin layer 12b. In addition, the resins forming the first resin layer 12a and the second resin layer 12b can be formed into films on the surface of the intermediate layer 11 by extrusion molding or coating, respectively, to prepare the first resin layer 12a and the second resin layer 12b formed of resin films.

[0161] The first resin layer 12a (resin layer A) disposed on one side of the metal terminal 2 preferably contains an acid-modified polyolefin as a main component, and further preferably contains an acid-modified polypropylene as a main component. The main component refers to a resin component whose content in the resin component contained in the first resin layer 12a is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, more preferably 80% by mass or more, more preferably 90% by mass or more, more preferably 95% by mass or more, more preferably 98% by mass or more, and further preferably 99% by mass or more. For example, the first resin layer 12a contains an acid-modified polypropylene as a main component, which means that the content of the acid-modified polypropylene in the resin component contained in the first resin layer 12a is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, more preferably 80% by mass or more, more preferably 90% by mass or more, more preferably 95% by mass or more, more preferably 98% by mass or more, and further preferably 99% by mass or more.

[0162] As described above, the second resin layer 12b preferably contains a polyolefin resin (i.e., has a polyolefin skeleton), preferably contains a polyolefin, and more preferably is a layer formed of a polyolefin. The second resin layer 12b also preferably contains a polyolefin or an acid-modified polyolefin in the polyolefin resin, more preferably contains a polyolefin, and more preferably is a layer formed of a polyolefin. The polyolefin resin is preferably a polypropylene resin. The polyolefin is preferably polypropylene, and the acid-modified polyolefin is preferably polypropylene.

[0163] The second resin layer 12b disposed on one side of the outer packaging material 3 for the storage device preferably contains polyolefin as a main component, and further preferably contains polypropylene as a main component. Here, the main component refers to a resin component whose content in the resin component contained in the second resin layer 12b is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, more preferably 80% by mass or more, more preferably 90% by mass or more, more preferably 95% by mass or more, more preferably 98% by mass or more, and further preferably 99% by mass or more. For example, the second resin layer 12b contains polypropylene as a main component, which means that the content of polypropylene in the resin component contained in the second resin layer 12b is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, more preferably 80% by mass or more, more preferably 90% by mass or more, more preferably 95% by mass or more, more preferably 98% by mass or more, and further preferably 99% by mass or more.

[0164] The melting peak temperature of the second resin layer 12b is preferably 110°C or higher, more preferably about 120°C or higher, and further preferably about 130°C or higher. From the same viewpoint, the melting peak temperature is, for example, 200°C or lower, preferably 190°C or lower, more preferably 180°C or lower, further preferably about 170°C or lower, and further preferably about 160°C or lower. Preferred ranges of the melting peak temperature include about 110 to 200°C, about 110 to 190°C, about 110 to 180°C, about 110 to 170°C, about 110 to 160°C, about 120 to 200°C, about 120 to 190°C, about 120 to 180°C, about 120 to 170°C, about 120 to 160°C, about 130 to 200°C, about 130 to 190°C, about 130 to 180°C, about 130 to 170°C, and about 130 to 160°C.

[0165] From the perspective of better achieving the effect of the present invention, the thickness of the first resin layer 12a is preferably about 10 μm or more, more preferably about 15 μm or more, and further preferably about 20 μm or more, and preferably about 120 μm or less, more preferably about 100 μm or less, and further preferably 80 μm. Preferred ranges of the thickness of the first resin layer 12a include about 10 to 120 μm, about 10 to 100 μm, about 10 to 80 μm, about 15 to 120 μm, about 15 to 100 μm, about 15 to 80 μm, about 20 to 120 μm, about 20 to 100 μm, and about 20 to 80 μm.

[0166] In addition, from the perspective of better achieving the effect of the present invention, the thickness of the second resin layer 12b is preferably about 10 μm or more, more preferably about 15 μm or more, and further preferably about 20 μm or more, and preferably about 120 μm or less, more preferably about 100 μm or less, and further preferably 80 μm. As the preferred range of the thickness of the second resin layer 12b, there can be listed about 10 to 120 μm, about 10 to 100 μm, about 10 to 80 μm, about 15 to 120 μm, about 15 to 100 μm, about 15 to 80 μm, about 20 to 120 μm, about 20 to 100 μm, and about 20 to 80 μm.

[0167] [Middle layer 11]

[0168] In the adhesive film 1 for metal terminals, the intermediate layer 11 is a layer that functions as a support body of the adhesive film 1 for metal terminals.

[0169] The intermediate layer 11 may be formed of the resin layer A or the resin layer B described above.

[0170] The intermediate layer 11 may be formed of, for example, a resin film. When the intermediate layer 11 is formed of a resin film, when the intermediate layer 11 and the first resin layer 12a are laminated to produce the adhesive film 1 for metal terminals of the present invention, a preformed resin film may be used as the intermediate layer 11. In addition, the resin forming the intermediate layer 11 may be formed into a film on the surface of the first resin layer 12a, etc., by extrusion molding or coating, etc., to produce the intermediate layer 11 formed of a resin film.

[0171] There is no particular limitation on the material forming the intermediate layer 11. Examples of the material forming the intermediate layer 11 include polyolefin resins, polyamide resins, polyester resins, epoxy resins, acrylic resins, fluorine-containing resins, silicone resins, phenolic resins, polyetherimides, polyimides, polycarbonates, and mixtures or copolymers thereof. Among them, polyolefin resins are particularly preferred. That is, the material forming the intermediate layer 11 is preferably a resin containing a polyolefin skeleton, such as polyolefin and acid-modified polyolefin. The fact that the resin constituting the intermediate layer 11 contains a polyolefin skeleton can be analyzed by, for example, infrared spectroscopy, gas chromatography-mass spectrometry, and the like.

[0172] As described above, the middle layer 11 preferably contains a polyolefin resin, more preferably contains a polyolefin, and further preferably is a layer formed of a polyolefin. The layer formed of a polyolefin can be a stretched polyolefin film or an unstretched polyolefin film, and is preferably an unstretched polyolefin film. As polyolefins, specific examples include polyethylenes such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, and linear low-density polyethylene; crystalline or amorphous polypropylenes such as homopolypropylene, block copolymers of polypropylene (such as block copolymers of propylene and ethylene), and random copolymers of polypropylene (such as random copolymers of propylene and ethylene); ethylene-butene-propylene terpolymers, etc. Among these polyolefins, polyethylene and polypropylene are preferably listed, and polypropylene is more preferably listed. In addition, due to good electrolyte resistance, the middle layer 11 preferably contains homopolypropylene, and is more preferably formed of homopolypropylene, and is further preferably an unstretched homopolypropylene film.

[0173] Specific examples of polyamides include aliphatic polyamides such as nylon 6, nylon 66, nylon 610, nylon 12, nylon 46, and copolymers of nylon 6 and nylon 66; hexamethylenediamine-isophthalic acid-terephthalic acid copolymers such as nylon 6I, nylon 6T, nylon 6IT, and nylon 6I6T (I represents isophthalic acid and T represents terephthalic acid) containing structural units derived from terephthalic acid and / or isophthalic acid, and aromatic polyamides such as poly(meta-xylylene adipamide) (MXD6); alicyclic polyamides such as polyaminomethylcyclohexyl adipamide (PACM6); polyamides obtained by copolymerizing lactam components or isocyanate components such as 4,4'-diphenylmethane-diisocyanate, polyesteramide copolymers or polyetheresteramide copolymers which are copolymers of copolyamides and polyesters or polyalkylene ether glycols; copolymers thereof, etc. These polyamides may be used alone or in combination of two or more.

[0174] Specific examples of the polyester include polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polyethylene isophthalate, copolyesters containing ethylene terephthalate as a main repeating unit, and copolyesters containing butylene terephthalate as a main repeating unit. In addition, as copolyesters with ethylene terephthalate as the main body of repeating units, specific examples include copolyesters with ethylene terephthalate as the main body of repeating units and obtained by polymerization with ethylene isophthalate (hereinafter abbreviated as poly(terephthalic acid / isophthalic acid) glycol), poly(terephthalic acid / isophthalic acid) glycol, poly(terephthalic acid / adipate) glycol, poly(terephthalic acid / sodium sulfoisophthalate) glycol, poly(terephthalic acid / sodium isophthalate) glycol, poly(terephthalic acid / phenyl-dicarboxylic acid) glycol, poly(terephthalic acid / decanedicarboxylic acid) glycol, and the like. In addition, specific examples of the copolyester having butylene terephthalate as a main repeating unit include a copolyester having butylene terephthalate as a main repeating unit and polymerized with butylene isophthalate (hereinafter referred to as poly(butylene terephthalate / isophthalate)), poly(butylene terephthalate / adipate), poly(butylene terephthalate / sebacate), poly(butylene terephthalate / decanedicarboxylate), polybutylene naphthalate, etc. These polyesters may be used alone or in combination of two or more.

[0175] In addition, the intermediate layer 11 may be formed of a nonwoven fabric formed of the above-mentioned resin. When the intermediate layer 11 is a nonwoven fabric, the intermediate layer 11 is preferably formed of the above-mentioned polyolefin resin, polyamide resin, or the like.

[0176] The melting peak temperature of the intermediate layer 11 is preferably 120° C. or higher, more preferably about 130° C. or higher, and further preferably about 140° C. or higher. From the same viewpoint, the melting peak temperature is, for example, 210° C. or lower, preferably 200° C. or lower, more preferably 190° C. or lower, further preferably about 180° C. or lower, and further preferably about 170° C. or lower. Preferred ranges of the melting peak temperature include about 120 to 210°C, about 120 to 200°C, about 120 to 190°C, about 120 to 180°C, about 120 to 170°C, about 130 to 210°C, about 130 to 200°C, about 130 to 190°C, about 130 to 180°C, about 130 to 170°C, about 140 to 210°C, about 140 to 200°C, about 140 to 190°C, about 140 to 180°C, and about 140 to 170°C.

[0177] The crystallinity of the intermediate layer 11 measured under the following conditions using an X-ray diffraction device is preferably about 7.0 or more, more preferably about 8.0 or more, and further preferably about 9.0 or more, and is preferably about 25.0 or less, more preferably about 22.0 or less, and further preferably about 19.0 or less. Preferred ranges include about 8.0 to 25.0, about 8.0 to 22.0, about 8.0 to 19.0, about 9.0 to 25.0, about 9.0 to 22.0, and about 9.0 to 19.0. Conditions other than the following measurement conditions (device, analysis, etc.) are carried out in the same manner as the above-mentioned crystallinity measurement of the resin layer A.

[0178] (Measurement conditions)

[0179] The X-ray irradiation angles were set to 0.19° and 0.22° with respect to the surface (0°) of the intermediate layer.

[0180] As an X-ray detector, R-AXIS was used, the camera length was set to 500 mm, and the X-ray wavelength was set to The exposure time was set to 30 seconds.

[0181] The intermediate layer 11 may be a single layer or a multi-layer layer.

[0182] In addition, a colorant may be added to the intermediate layer 11 to make the intermediate layer 11 a layer containing a colorant. In addition, a resin with low transparency may be selected to adjust the light transmittance. When the intermediate layer 11 is a film, a colored film or a film with low transparency may be used. In addition, when the intermediate layer 11 is a nonwoven fabric, a nonwoven fabric using fibers or adhesives containing a colorant or a nonwoven fabric with low transparency may be used.

[0183] When the intermediate layer 11 is composed of a resin film, the surface of the intermediate layer 11 may be subjected to a known adhesion-facilitating means such as a corona discharge treatment, an ozone treatment, or a plasma treatment, as necessary.

[0184] In addition, from the perspective of better achieving the effect of the present invention, the thickness of the intermediate layer 11 is preferably about 20 μm or more, more preferably about 30 μm or more, and further preferably about 40 μm or more, and is preferably about 120 μm or less, more preferably about 110 μm or less, further preferably about 100 μm or less, and further preferably 80 μm or less. As the preferred range of the thickness of the intermediate layer 11, there can be listed about 20 to 120 μm, about 20 to 110 μm, about 20 to 100 μm, about 20 to 80 μm, about 30 to 120 μm, about 30 to 110 μm, about 30 to 100 μm, about 30 to 80 μm, about 40 to 120 μm, about 40 to 110 μm, about 40 to 100 μm, and about 40 to 80 μm.

[0185] From the same perspective, the ratio of the thickness of the intermediate layer 11 to the total thickness of the first resin layer 12a and the second resin layer 12b is preferably about 0.3 or more, more preferably about 0.4 or more, and preferably about 1.0 or less, more preferably about 0.8 or less, and the preferred ranges include about 0.3 to 1.0, about 0.3 to 0.8, about 0.4 to 1.0, and about 0.4 to 0.8. In addition, from the perspective of improving the insulation of the adhesive film 1 for metal terminals, the ratio is preferably about 0.55 or more, more preferably about 0.60 or more, and preferably about 1.0 or less, more preferably about 0.9 or less, and the preferred ranges include about 0.55 to 1.0, about 0.55 to 0.9, about 0.60 to 1.0, and about 0.60 to 0.9.

[0186] When the total thickness of the adhesive film for metal terminal 1 is taken as 100%, the ratio of the total thickness of the first resin layer 12a and the second resin layer 12b is preferably about 30 to 80%, more preferably about 50 to 70%.

[0187] The adhesive film 1 for metal terminals of the present invention can be manufactured, for example, by laminating the first resin layer 12a and the second resin layer 12b on both side surfaces of the intermediate layer 11. The intermediate layer 11, the first resin layer 12a and the second resin layer 12b can be laminated by a known method such as extrusion lamination, T-die method, inflation method, thermal lamination method, etc.

[0188] There is no particular limitation on the method of interposing the adhesive film 1 for metal terminals between the metal terminals 2 and the outer packaging material 3 for power storage devices. For example, Figure 1 to Figure 3 As shown, at the portion where the metal terminal 2 is clamped by the outer packaging material 3 for the storage device, the adhesive film 1 for the metal terminal is wound on the metal terminal 2. In addition, although the illustration is omitted, the adhesive film 1 for the metal terminal may be arranged on both sides of the metal terminal 2 in the portion where the metal terminal 2 is clamped by the outer packaging material 3 for the storage device so as to span two metal terminals 2.

[0189] The adhesion promoter layer 13 is a layer provided as needed in order to firmly adhere the intermediate layer 11 to the first resin layer 12a and to firmly adhere the intermediate layer 11 to the second resin layer 12b (see Figure 7 The adhesion promoter layer 13 may be provided only on one side between the intermediate layer 11 and the first resin layer 12a and the second resin layer 12b, or may be provided on both sides.

[0190] The adhesion promoter layer 13 can be formed using known adhesion promoters such as isocyanate, polyethyleneimine, polyester, polyurethane, and polybutadiene. From the perspective of obtaining a strong adhesion strength, it is preferably formed by an isocyanate adhesion promoter. As an isocyanate adhesion promoter, an adhesion promoter composed of an isocyanate component selected from triisocyanate monomers and polymerized MDI has excellent lamination strength and less reduction in lamination strength at high temperatures. In particular, it is particularly preferred that the adhesive agent be formed from triphenylmethane-4,4',4"-triisocyanate as a triisocyanate monomer or polymethylene polyphenyl polyisocyanate (NCO content of about 30% and viscosity of 200 to 700 mPa·s) as polymeric MDI. In addition, it is also preferred that the adhesive agent be formed from tri(p-isocyanatephenyl)thiophosphate as a triisocyanate monomer or a two-component curing type adhesive agent having a polyethyleneimine system as a main agent and polycarbodiimide as a crosslinking agent.

[0191] The adhesion promoter layer 13 can be formed by coating and drying using a known coating method such as a bar coating method, a roll coating method, or a gravure coating method. The coating amount of the adhesion promoter is 20 to 100 mg / m2 in the case of an adhesion promoter composed of triisocyanate. 2 About 40 to 60 mg / m 2 In the case of an adhesion promoter composed of polymeric MDI, it is 40 to 150 mg / m 2 About 60 to 100 mg / m 2 In the case of a two-liquid curing type adhesion promoter with polyethylene imine as the main agent and polycarbodiimide as the crosslinking agent, 5 to 50 mg / m 2 About 10 to 30 mg / m 2 Among them, the triisocyanate monomer is a monomer having three isocyanate groups in one molecule, and the polymeric MDI is a mixture of MDI and an MDI oligomer obtained by polymerizing MDI, and is represented by the following formula.

[0192]

[0193] From the perspective of achieving the effect of the present invention in a better manner, it is preferred that the first resin layer 12 a is in surface contact with the intermediate layer 11 , and the second resin layer 12 b is in surface contact with the intermediate layer 11 .

[0194] Specific examples of preferred laminated structures of the adhesive film 1 for metal terminals of the present invention include: a three-layer structure in which a first resin layer formed of acid-modified polypropylene / a substrate formed of polypropylene / a second resin layer formed of acid-modified polypropylene are laminated in sequence; a three-layer structure in which a first resin layer formed of acid-modified polypropylene / a substrate formed of polypropylene / a second resin layer formed of polypropylene are laminated in sequence, etc. Among them, the latter three-layer structure is particularly preferred from the perspective of adhesion between the heat-fusible resin layer 35 of the outer packaging material 3 for storage device and the second resin layer 12b.

[0195] The heat shrinkage rate of the adhesive film 1 for metal terminals of the present invention measured under the following conditions is preferably 60% or less, more preferably 38% or less, further preferably 30% or less, and further preferably 20% or less. The preferred range is about 0 to 60%, about 0 to 38%, about 0 to 30%, and about 0 to 20%.

[0196] (Method for measuring heat shrinkage (%))

[0197] Cut the adhesive film for metal terminals into a size of 110 mm (MD) in length and 10 mm (TD) in width as a test piece. Next, use a metal ruler to measure the length M (mm) of the test piece. Next, use tape to fix the end of the test piece in the length direction (about 10 mm) on the metal wire mesh so that the test piece is suspended on the metal wire mesh. In this state, place it in an oven heated to 190°C for 120 seconds, then take out the test piece together with the metal wire mesh and cool it naturally at room temperature (25°C). Next, use a metal ruler to measure the length N (mm) of the test piece after it has cooled naturally to room temperature. The thermal shrinkage rate of the adhesive film for metal terminals is calculated by the following formula.

[0198] Thermal shrinkage (%) = (1 - (length N / length M)) × 100

[0199] [Metal terminal 2]

[0200] The adhesive film 1 for metal terminals of the present invention is used between a metal terminal 2 and an outer packaging material 3 for an electrical storage device. The metal terminal 2 (tab) is a conductive component electrically connected to an electrode (positive electrode or negative electrode) of an electrical storage device element 4 and is made of a metal material. There are no particular restrictions on the metal material constituting the metal terminal 2, and examples thereof include aluminum, nickel, copper, and the like. For example, the metal terminal 2 connected to the positive electrode of a lithium-ion electrical storage device is usually made of aluminum or the like. In addition, the metal terminal 2 connected to the negative electrode of a lithium-ion electrical storage device is usually made of copper, nickel, or the like.

[0201] From the perspective of improving electrolyte resistance, it is preferred to perform chemical surface treatment on the surface of the metal terminal 2. For example, when the metal terminal 2 is formed of aluminum, as a specific example of chemical surface treatment, a known method of forming a corrosion-resistant film of phosphate, chromate, fluoride, triazine thiol compound, etc. can be cited. Among the methods for forming the corrosion-resistant film, it is preferred to use a phosphate chromate treatment of a material composed of three components: a phenolic resin, a chromium (III) fluoride compound, and phosphoric acid.

[0202] The size of the metal terminal 2 can be appropriately set according to the size of the power storage device used. As the thickness of the metal terminal 2, preferably about 50 to 1000 μm, more preferably about 70 to 800 μm. In addition, as the length of the metal terminal 2, preferably about 1 to 200 mm, more preferably about 3 to 150 mm. In addition, as the width of the metal terminal 2, preferably about 1 to 200 mm, more preferably about 3 to 150 mm.

[0203] [Outer packaging materials for power storage devices 3]

[0204] As the outer packaging material 3 for the power storage device, there can be mentioned a material having a laminated structure composed of a laminated body having at least a base layer 31, a barrier layer 33 and a heat-fusible resin layer 35 in this order. Figure 8 In the figure, as an example of the cross-sectional structure of the outer packaging material 3 for a storage device, a substrate layer 31, an adhesive layer 32 provided as required, a barrier layer 33, an adhesive layer 34 provided as required, and a heat-fusible resin layer 35 are sequentially stacked. In the outer packaging material 3 for a storage device, the substrate layer 31 is the outer layer side, and the heat-fusible resin layer 35 is the innermost layer. When assembling the storage device, the heat-fusible resin layers 35 located at the periphery of the storage device element 4 are brought into surface contact with each other and heat-fused to seal the storage device element 4, thereby encapsulating the storage device element 4. In addition, in Figures 1 to 3 In the figure, the storage device 10 is shown in which the storage device outer packaging material 3 is formed by bulging molding, but the storage device outer packaging material 3 may also be an unformed pocket type. Among them, the pocket type includes three-way sealing, four-way sealing, pillow type, etc., and any type is acceptable.

[0205] There is no particular restriction on the thickness of the laminate constituting the outer packaging material 3 for the storage device. As for the upper limit, from the perspective of cost reduction and energy density improvement, it is preferably about 190 μm or less, preferably about 180 μm or less, about 160 μm or less, about 155 μm or less, about 140 μm or less, about 130 μm or less, about 120 μm or less; as for the lower limit, from the perspective of maintaining the function of the outer packaging material 3 for the storage device such as protecting the storage device element 4, it is preferably about 35 μm or more, about 45 μm or more, about 60 μm or more, about 80 μm or more; as for the preferred range, for example, about 35 to 190 μm, about 35 to 180 μm, about 35 to 160 μm, about 35 to 155 μm, about 35 to About 140μm, about 35-130μm, about 35-120μm, about 45-190μm, about 45-180μm, about 45-160μm, about 45-155μm, about 45-140μm, about 45-130μm, about 45-120μm, about 60-190μm, about 60-180μm, about 60-160μm, about 60-155μm, about 60-140μm, about 60-130μm, about 60-120μm, about 80-190μm, about 80-180μm, about 80-160μm, about 80-155μm, about 80-140μm, about 80-130μm, about 80-120μm.

[0206] (Base material layer 31)

[0207] In the electricity storage device packaging material 3 , the base material layer 31 is a layer that functions as a base material of the electricity storage device packaging material and is a layer forming the outermost layer side.

[0208] There are no particular restrictions on the material forming the substrate layer 31 as long as it has insulating properties. Examples of the material forming the substrate layer 31 include polyester, polyamide, epoxy resin, acrylic resin, fluorine-containing resin, polyurethane, silicone resin, phenolic resin, polyetherimide, polyimide, and mixtures or copolymers thereof. Polyesters such as polyethylene terephthalate and polybutylene terephthalate have the advantages of excellent resistance to electrolyte and difficulty in whitening due to the adhesion of electrolyte, and are suitable for use as the material for forming the substrate layer 31. In addition, polyamide film has excellent stretchability and can prevent the substrate layer 31 from whitening due to resin rupture during molding, and is suitable for use as the material for forming the substrate layer 31.

[0209] The substrate layer 31 may be formed of a uniaxially stretched or biaxially stretched resin film or an unstretched resin film. Among them, a uniaxially stretched or biaxially stretched resin film, especially a biaxially stretched resin film, has improved heat resistance due to oriented crystallization, and is therefore suitable for use as the substrate layer 31.

[0210] Among these, as the resin film forming the base material layer 31, preferably nylon and polyester are used, and more preferably biaxially stretched nylon and biaxially stretched polyester are used.

[0211] In order to improve the pinhole resistance and the insulation when the packaging body of the storage device is made, the base layer 31 can also be a laminate of resin films of different materials. Specifically, a multilayer structure formed by laminating a polyester film and a nylon film, and a multilayer structure formed by laminating a biaxially stretched polyester and a biaxially stretched nylon, etc. can be cited. In the case of making the base layer 31 a multilayer structure, each resin film can be bonded by an adhesive or directly laminated without using an adhesive. In the case of bonding without using an adhesive, for example, a method of bonding in a hot melt state such as a coextrusion method, a sandwich lamination method, and a hot lamination method can be cited.

[0212] In addition, in order to improve the formability, the base layer 31 may also be subjected to low friction. When the base layer 31 is subjected to low friction, the friction coefficient of the surface thereof is not particularly limited, and for example, it may be 1.0 or less. In order to cause the base layer 31 to be subjected to low friction, for example, matte treatment, formation of a thin film layer of a lubricant, or a combination thereof may be used.

[0213] The thickness of the base material layer 31 is, for example, about 10 to 50 μm, preferably about 15 to 30 μm.

[0214] (Adhesive layer 32)

[0215] In the power storage device packaging material 3 , the adhesive layer 32 is a layer disposed on the base layer 31 as necessary in order to impart adhesion to the base layer 31 . That is, the adhesive layer 32 is provided between the base layer 31 and the barrier layer 33 .

[0216] The adhesive layer 32 is formed of an adhesive capable of bonding the substrate layer 31 to the barrier layer 33. The adhesive used to form the adhesive layer 32 may be a two-component curing adhesive or a one-component curing adhesive. In addition, there is no particular limitation on the bonding mechanism of the adhesive used to form the adhesive layer 32, and the adhesive may be a chemical reaction type, a solvent volatilization type, a hot melt type, a hot pressing type, or the like.

[0217] As the resin component of the adhesive that can be used to form the adhesive layer 32, from the perspectives of excellent ductility, durability under high humidity conditions and yellowing inhibition, thermal degradation inhibition during heat sealing, and inhibition of the reduction in the lamination strength between the base layer 31 and the barrier layer 33, thereby effectively inhibiting the occurrence of delamination, the following are preferably listed: polyurethane-based two-component curing adhesives; polyamides, polyesters, or blended resins of these with modified polyolefins.

[0218] In addition, the adhesive layer 32 may be multilayered with different adhesive components. In the case where the adhesive layer 32 is multilayered with different adhesive components, from the perspective of improving the lamination strength between the substrate layer 31 and the barrier layer 33, it is preferred that a resin having excellent adhesion to the substrate layer 31 be selected as the adhesive component disposed on the substrate layer 31 side, and an adhesive component having excellent adhesion to the barrier layer 33 be selected as the adhesive component disposed on the barrier layer 33 side. In the case where the adhesive layer 32 is multilayered with different adhesive components, specifically, as the adhesive component disposed on the barrier layer 33 side, preferably, acid-modified polyolefins, metal-modified polyolefins, mixed resins of polyesters and acid-modified polyolefins, resins containing copolyesters, and the like are listed.

[0219] The thickness of the adhesive layer 32 is, for example, about 2 to 50 μm, preferably about 3 to 25 μm.

[0220] (Barrier layer 33)

[0221] In the outer packaging material 3 for the storage device, the barrier layer 33 is a layer that improves the strength of the outer packaging material for the storage device and has the function of preventing water vapor, oxygen, light, etc. from invading the interior of the storage device. The barrier layer 33 is preferably a metal layer, that is, a layer formed of metal. As metals constituting the barrier layer 33, aluminum, stainless steel, titanium, etc. can be specifically listed, and aluminum is preferably listed. The barrier layer 33 can be formed, for example, of a metal foil, or a metal vapor-deposited film, an inorganic oxide vapor-deposited film, a carbon-containing inorganic oxide vapor-deposited film, a film provided with these vapor-deposited films, etc., preferably formed of a metal foil, and more preferably formed of an aluminum foil. When manufacturing an outer packaging material for a storage device, from the perspective of preventing wrinkles or pinholes from forming in the barrier layer 33, it is more preferable that the barrier layer is formed of a soft aluminum foil such as annealed aluminum (JIS H4160: 1994A8021H-O, JIS H4160: 1994A8079H-O, JIS H4000: 2014A8021P-O, JIS H4000: 2014A8079P-O).

[0222] The thickness of the barrier layer 33 is preferably about 10 to 200 μm, more preferably about 20 to 100 μm, about 20 to 45 μm, about 45 to 65 μm, or about 65 to 85 μm, from the perspective of making the outer packaging material for the storage device thinner and less likely to generate pinholes during molding.

[0223] In addition, the barrier layer 33 is preferably subjected to chemical surface treatment on at least one surface, more preferably on both surfaces, for the purpose of stabilizing adhesion, preventing dissolution or corrosion, etc. Here, the chemical surface treatment refers to a treatment for forming a corrosion-resistant film on the surface of the barrier layer.

[0224] (Adhesive layer 34)

[0225] In the power storage device packaging material 3 , the adhesive layer 34 is a layer provided between the barrier layer 33 and the thermally-adhesive resin layer 35 as necessary in order to firmly adhere the thermally-adhesive resin layer 35 .

[0226] The adhesive layer 34 is formed of an adhesive capable of bonding the barrier layer 33 and the heat-fusible resin layer 35. There are no particular restrictions on the composition of the adhesive used to form the adhesive layer, and for example, a resin composition containing an acid-modified polyolefin can be cited. Examples of the acid-modified polyolefin include those exemplified in the first resin layer 12a and the second resin layer 12b.

[0227] The thickness of the adhesive layer 34 is, for example, about 1 to 40 μm, preferably about 2 to 30 μm.

[0228] (Thermal Fusible Resin Layer 35)

[0229] In the electricity storage device packaging material 3 , the heat-fusible resin layer 35 corresponds to the innermost layer, and is a layer in which the heat-fusible resin layers are heat-fused to each other when the electricity storage device is assembled to seal the electricity storage device element.

[0230] The resin component used for the heat-fusible resin layer 35 is not particularly limited as long as it can be heat-fusible, and examples thereof include polyolefins and cyclic polyolefins.

[0231] As the above-mentioned polyolefin, specifically, polyethylene such as low-density polyethylene, medium-density polyethylene, high-density polyethylene, and linear low-density polyethylene can be cited; crystalline or amorphous polypropylene such as homopolypropylene, block copolymers of polypropylene (e.g., block copolymers of propylene and ethylene), and random copolymers of polypropylene (e.g., random copolymers of propylene and ethylene); terpolymers of ethylene-butene-propylene, etc. Among these polyolefins, polyethylene and polypropylene are preferably cited.

[0232] The cyclic polyolefin is a copolymer of an olefin and a cyclic monomer. Examples of olefins that are structural monomers of the cyclic polyolefin include ethylene, propylene, 4-methyl-1-pentene, butadiene, isoprene, and the like. In addition, examples of cyclic monomers that are structural monomers of the cyclic polyolefin include cyclic olefins such as norbornene; specifically, cyclic dienes such as cyclopentadiene, dicyclopentadiene, cyclohexadiene, and norbornene can be cited. Among these polyolefins, cyclic olefins are preferably cited, and norbornene is further preferably cited. Styrene can also be cited as a structural monomer.

[0233] Among these resin components, preferred are crystalline or amorphous polyolefins, cyclic polyolefins, and polymer blends thereof; more preferred are polyethylene, polypropylene, copolymers of ethylene and norbornene, and polymer blends of two or more thereof.

[0234] The heat-fusible resin layer 35 may be formed of a single resin component or a blended polymer of two or more resin components. Furthermore, the heat-fusible resin layer 35 may be formed of only one layer or of two or more layers of the same or different resin components. When the second resin layer 12b and the heat-fusible resin layer 35 use the same resin, the adhesion between these layers is improved, which is particularly preferred.

[0235] In addition, the thickness of the heat-fusible resin layer 35 is not particularly limited, and can be about 2 to 2000 μm, preferably about 5 to 1000 μm, and more preferably about 10 to 500 μm. In addition, the thickness of the heat-fusible resin layer 35 can be, for example, about 100 μm or less, preferably about 85 μm or less, and more preferably about 15 to 85 μm. Among them, for example, when the thickness of the adhesive layer 5 described later is 10 μm or more, the thickness of the heat-fusible resin layer 35 is preferably about 85 μm or less, and more preferably about 15 to 45 μm; for example, when the thickness of the adhesive layer 5 described later is less than 10 μm or when the adhesive layer 5 is not provided, the thickness of the heat-fusible resin layer 35 is preferably about 20 μm or more, and more preferably about 35 to 85 μm.

[0236] The outer packaging material for the storage device of the present invention may also be in the form of a kit including the outer packaging material for the storage device for the storage device and the adhesive film for the metal terminal of the present invention. In this case, the storage device as an applicable object also includes a storage device element having at least a positive electrode, a negative electrode and an electrolyte, an outer packaging material for the storage device that encapsulates the storage device element, and a metal terminal electrically connected to the positive electrode and the negative electrode, respectively, and extending to the outside of the outer packaging material for the storage device. When the kit of the present invention is used, the adhesive film for the metal terminal of the present invention is interposed between the metal terminal and the outer packaging material for the storage device.

[0237] 2. Power storage devices

[0238] The electric storage device 10 of the present invention includes: an electric storage device element 4 having at least a positive electrode, a negative electrode and an electrolyte; an outer packaging material 3 for an electric storage device that encapsulates the electric storage device element 4; and metal terminals 2 that are electrically connected to the positive electrode and the negative electrode, respectively, and extend to the outside of the outer packaging material 3 for the electric storage device. The electric storage device 10 of the present invention is characterized in that an adhesive film for metal terminals is interposed between the metal terminal 2 and the outer packaging material 3 for the electric storage device, and the crystallinity of the resin layer A of the adhesive film for metal terminals measured under the above conditions using an X-ray diffraction device is 11 or more. That is, the electric storage device 10 of the present invention can be manufactured by a method including a step of interposing the adhesive film 1 for metal terminals of the present invention between the metal terminal 2 and the outer packaging material 3 for the electric storage device.

[0239] In the energy storage device 10 of the present invention, the adhesive film for metal terminals is heat-fused to the metal terminal and the outer packaging material for the energy storage device in a state between the metal terminal 2 and the outer packaging material 3 for the energy storage device. The heating temperature, pressure, and time during the heat fusion may be the same as or different from the heating conditions (200°C, 0.25MPa, 16 seconds) for determining the crystallinity of the resin layer A of the adhesive film 1 for metal terminals of the present invention. Even if the heating conditions are different, it can be said that the heat applied to the resin layer A when heat-fusion bonding the resin layer A to the metal terminal is basically the same. In addition, when heat-fusion bonding the heat-fusible resin layers of the outer packaging material for the energy storage device are heat-fused to each other, the heat applied to the adhesive film for metal terminals is very small compared to the heat applied when the resin layer A is heat-fused to the metal terminal. Therefore, as long as the crystallinity of the resin layer A of the adhesive film for metal terminals included in the power storage device 10 measured using an X-ray diffraction device under the above conditions is 11 or more, it can be said that it has excellent adhesion to the metal terminal like the adhesive film 1 for metal terminals of the present invention.

[0240] Specifically, a storage device 10 using the storage device outer packaging material 3 is provided by wrapping a storage device element 4 having at least a positive electrode, a negative electrode, and an electrolyte in a state where metal terminals 2 connected to the positive electrode and the negative electrode are extended outward, the adhesive film 1 for metal terminals of the present invention is interposed between the metal terminals 2 and the heat-fusible resin layer 35, and a flange portion (a region where the heat-fusible resin layers 35 are in contact with each other, the peripheral portion 3a of the storage device outer packaging material 3) of the storage device outer packaging material 3 is formed at the periphery of the storage device element 4, and the heat-fusible resin layers 35 of the flange portion are heat-sealed to each other to seal. In addition, when the storage device outer packaging material 3 is used to accommodate the storage device element 4, the storage device outer packaging material 3 is used in a manner such that the heat-fusible resin layer 35 of the storage device outer packaging material 3 is on the inner side (the side in contact with the storage device element 4).

[0241] The outer packaging material for the storage device of the present invention is suitable for storage devices such as batteries (including capacitors (condensor), capacitors (capacitor) etc.). In addition, the outer packaging material for the storage device of the present invention can be used for any of primary batteries and secondary batteries, preferably secondary batteries. There is no particular restriction on the type of secondary battery to which the outer packaging material for the storage device of the present invention is applicable, for example, lithium ion batteries, lithium ion polymer batteries, all-solid batteries, semi-solid batteries, quasi-solid batteries, polymer batteries, all-resin batteries, lead batteries, nickel-hydrogen batteries, nickel-cadmium batteries, nickel-iron batteries, nickel-zinc batteries, silver oxide-zinc batteries, metal-air batteries, multivalent cation batteries, capacitors (condensor), capacitors (capacitor) etc. Among these secondary batteries, lithium ion batteries and lithium ion polymer batteries can be cited as preferred applicable objects of the outer packaging material for the storage device of the present invention.

[0242] Example

[0243] Hereinafter, the present invention will be described in detail with reference to Examples and Comparative Examples, but the present invention is not limited to the Examples.

[0244] <Manufacturing of Adhesive Film for Metal Terminal>

[0245] Example 1

[0246] Using an extruder and a T-die casting device, a polypropylene (PP layer, melting peak temperature 140°C) as the second resin layer on the outer packaging material side was extruded at a thickness of 50 μm on one side of a polypropylene (PP layer, homopolypropylene, melting peak temperature 163°C, thickness 50 μm) as an intermediate layer, and a carbon black-containing maleic anhydride-modified polypropylene (PPa layer, melting peak temperature 140°C) as the first resin layer (resin layer A) on the metal terminal side was extruded on the other side, to obtain an adhesive film (total thickness 150 μm) in which the first resin layer (resin layer A, PPa layer, melting peak temperature 140°C, thickness 50 μm) / substrate (PP layer, melting peak temperature 163°C, thickness 50 μm) / second resin layer (PP layer, melting peak temperature 140°C, thickness 50 μm) were sequentially laminated. The first resin layer as the resin layer A was manufactured under the film forming temperature reference condition, the film forming speed reference condition, and the cooling reference condition, and the crystallinity after heating described later was adjusted.

[0247] Example 2

[0248] Using an extruder and a T-die casting device, maleic anhydride-modified polypropylene (PPa layer, melting peak temperature 140°C) as the second resin layer on the outer packaging material side was extruded at a thickness of 25 μm on one surface of polypropylene (PP layer, random polypropylene, melting peak temperature 143°C, thickness 100 μm) as an intermediate layer, and maleic anhydride-modified polypropylene (PPa layer, melting peak temperature 140°C) as the first resin layer (resin layer A) on the metal terminal side was extruded on the other surface, to obtain an adhesive film (total thickness 150 μm) laminated in sequence with the first resin layer (resin layer A, PPa layer, melting peak temperature 140°C, thickness 25 μm) / substrate (PP layer, melting peak temperature 143°C, thickness 100 μm) / second resin layer (PPa layer, melting peak temperature 140°C, thickness 25 μm). The first resin layer as the resin layer A was produced under the conditions of a film forming temperature far lower than the reference, a film forming speed far lower than the reference, and rapid cooling relative to the cooling reference, and the crystallinity after heating described later was adjusted.

[0249] Example 3

[0250] Using an extruder and a T-die casting device, polypropylene (PP layer, melting peak temperature 140°C) as the second resin layer on the outer packaging material side was extruded at a thickness of 40 μm on one surface of carbon black-containing polypropylene (PP layer, homopolypropylene, melting peak temperature 160°C, thickness 60 μm) as an intermediate layer, and maleic anhydride-modified polypropylene (PPa layer, melting peak temperature 140°C) as the first resin layer (resin layer A) on the metal terminal side was extruded at a thickness of 50 μm on the other surface to obtain an adhesive film (total thickness 150 μm) in which the first resin layer (resin layer A, PPa layer, melting peak temperature 140°C, thickness 50 μm) / substrate (PP layer, melting peak temperature 160°C, thickness 60 μm) / second resin layer (PP layer, melting peak temperature 140°C, thickness 40 μm) were laminated in this order. The first resin layer as the resin layer A was produced under the conditions of a film forming temperature lower than a reference, a film forming speed higher than a reference, and slow cooling relative to a cooling reference, and the crystallinity after heating described later was adjusted.

[0251] Example 4

[0252] Using a blow extruder, maleic anhydride-modified polypropylene (PPa layer, melting peak temperature 140°C) as the second resin layer on the outer packaging material side was extruded at a thickness of 35 μm on one side of the polypropylene (PP layer, homopolypropylene, melting peak temperature 160°C, thickness 80 μm) as the intermediate layer, and maleic anhydride-modified polypropylene (PPa layer, melting peak temperature 140°C) as the first resin layer (resin layer A) on the metal terminal side was extruded on the other side, to obtain an adhesive film (total thickness 150 μm) in which the first resin layer (resin layer A, PPa layer, melting peak temperature 140°C, thickness 35 μm) / base material (PP layer, melting peak temperature 160°C, thickness 80 μm) / second resin layer (PPa layer, melting peak temperature 140°C, thickness 35 μm) was sequentially laminated. The first resin layer as the resin layer A was manufactured under the conditions of a film forming temperature lower than the reference, a film forming speed much lower than the reference, and a cooling condition that was quite slow relative to the cooling reference, and the crystallinity after heating described later was adjusted.

[0253] Example 5

[0254] Using an extruder and a T-die casting device, a polypropylene (PP layer, melting peak temperature 140°C) as the second resin layer on the outer packaging material side was extruded at a thickness of 60 μm on one side of a polypropylene (PP layer, homopolypropylene, melting peak temperature 163°C, thickness 80 μm) as an intermediate layer, and a carbon black-containing maleic anhydride-modified polypropylene (PPa layer, melting peak temperature 140°C) as the first resin layer (resin layer A) on the metal terminal side was extruded on the other side, to obtain an adhesive film (total thickness 200 μm) in which the first resin layer (resin layer A, PPa layer, melting peak temperature 140°C, thickness 60 μm) / base material (PP layer, melting peak temperature 163°C, thickness 80 μm) / second resin layer (PP layer, melting peak temperature 140°C, thickness 60 μm) was sequentially laminated. The first resin layer as the resin layer A was manufactured under the film forming temperature reference condition, the film forming speed reference condition, and the cooling reference condition, and the crystallinity was adjusted.

[0255] Example 6

[0256] Using an extruder and a T-die casting device, a polypropylene (PP layer, melting peak temperature 140°C) as the second resin layer on the outer packaging material side was extruded at a thickness of 60 μm on one side of a polypropylene (PP layer, homopolypropylene, melting peak temperature 163°C, thickness 80 μm) as an intermediate layer, and a carbon black-containing maleic anhydride-modified polypropylene (PPa layer, melting peak temperature 140°C) as the first resin layer (resin layer A) on the metal terminal side was extruded on the other side, to obtain an adhesive film (total thickness 200 μm) in which the first resin layer (resin layer A, PPa layer, melting peak temperature 140°C, thickness 60 μm) / base material (PP layer, melting peak temperature 163°C, thickness 80 μm) / second resin layer (PP layer, melting peak temperature 140°C, thickness 60 μm) was sequentially laminated. The first resin layer as the resin layer A was manufactured under the film forming temperature reference condition, the film forming speed reference condition, and the cooling reference condition, and the crystallinity was adjusted.

[0257] Example 7

[0258] Using an extruder and a T-die casting device, a polypropylene (PP layer, melting peak temperature 140°C) as a second resin layer on the outer packaging material side was extruded at a thickness of 60 μm on one side of a polypropylene (PP layer, homopolypropylene, melting peak temperature 163°C, thickness 80 μm) as an intermediate layer, and a carbon black-containing maleic anhydride-modified polypropylene (PPa layer, melting peak temperature 140°C) was extruded at a thickness of 20 μm on the other side, and a first resin layer on the metal terminal side was extruded at a thickness of 40 μm on the same side. The maleic anhydride modified polypropylene (PPa layer, melting peak temperature 140°C) of the lipid layer (resin layer A) was obtained to obtain an adhesive film (total thickness 200μm) in which the first resin layer (resin layer A, PPa layer, melting peak temperature 140°C, thickness 40μm) / third resin layer (PPa layer, melting peak temperature 140°C, thickness 20μm) / base material (PP layer, melting peak temperature 163°C, thickness 80μm) / second resin layer (PP layer, melting peak temperature 140°C, thickness 60μm) were laminated in sequence. The first resin layer as the resin layer A was manufactured under the film forming temperature reference condition, the film forming speed reference condition, and the cooling reference condition, and the crystallinity was adjusted.

[0259] Comparative Example 1

[0260] An acid-modified polypropylene film (melting peak temperature 140° C., thickness 100 μm) was used alone to prepare an adhesive film for a metal terminal using an extruder and a T-die casting device.

[0261] <Measurement of Crystallinity of Resin Layer A and Intermediate Layer after Heating>

[0262] The specific heating of the adhesive films of Examples 1 to 7 and Comparative Example 1 at 200° C., 0.25 MPa, and 16 seconds is as follows.

[0263] Each adhesive film for metal terminals obtained in the examples and comparative examples was cut into a length of 50 mm and a width of 20 mm. In a state where polytetrafluoroethylene (PTFE film, thickness 100 μm) is placed on the laminate (the surface of the adhesive film for metal terminals is covered with the PTFE film), it is placed on a press machine heated to 200°C (resin layer A is on the heating plate side), and a silicone sponge sheet is placed, and the adhesive film is heated by standing at a pressure of 0.25 MPa for 16 seconds. The heated laminate is naturally cooled to 25°C. Next, an X-ray diffraction device (Aichi Synchrotron Radiation Center., trade name BL8S3Beamline) is used to measure the crystallinity of the first resin layer (resin layer A) and the intermediate layer after heating under the following conditions. In addition, the crystallinity of the acid-modified polypropylene film after heating is measured for the adhesive film of Comparative Example 1 in the same manner as in Examples 1 to 7. The results are shown in Table 1.

[0264] (Measurement conditions: resin layer A)

[0265] The X-ray irradiation angle was set to 0.09° with respect to the surface of the resin layer A (0°).

[0266] The measurement range was set to be the range from the surface of the resin layer A to a depth of 5 μm.

[0267] The camera length of the X-ray detector is set to 500 mm and the X-ray wavelength is set to The exposure time was set to 30 seconds.

[0268] (Measurement conditions: middle layer)

[0269] The X-ray irradiation angles were set to 0.19° and 0.22° with respect to the surface of the resin layer A (0°).

[0270] As an X-ray detector, R-AXIS was used, the camera length was set to 500 mm, and the X-ray wavelength was set to The exposure time was set to 30 seconds.

[0271] (Analysis of the middle layer)

[0272] Using the X-ray scattering data analysis software FI2D, the data with azimuth angles of 80deg to 100deg are intercepted from the spectrum data of the two-dimensional detector and integrated in the azimuth direction to obtain a one-dimensional spectrum showing the intensity value relative to the diffraction angle 2θ. The straight line between the two points 2θ=4.0deg and 2θ=16.0deg is then subtracted from the one-dimensional spectrum as the background. Thereafter, the spectral intensity value A of the amorphous component is defined as A: the value with the minimum intensity value in the region of 2θ=8.8deg to 9.8deg, and the crystalline peak intensity values ​​P1, P2, P3, and P4 of the four crystal planes are defined as follows.

[0273] P1: Peak intensity value of the peak located in the region of 2θ=7.0deg to 9.2deg

[0274] P2: Peak intensity value of the peak located within 2θ=9.2deg to 10.6deg

[0275] P3: Peak intensity value of the peak located within 2θ=10.6deg to 12.0deg

[0276] P4: Peak top intensity value of the peak located within 2θ=12.0deg to 14.0deg

[0277] The difference between the P1+P2+P3+P4 values ​​when the X-ray irradiation angle is set to 0.22° and the P1+P2+P3+P4 values ​​when the X-ray irradiation angle is set to 0.19° is divided by the difference between the A value when the X-ray irradiation angle is set to 0.22° and the A value when the X-ray irradiation angle is set to 0.19°. The resulting value is the crystallinity Ci of the intermediate layer.

[0278] <Measurement of the partiality of the island ratio of the resin layer A after heating>

[0279] The island ratio partiality of the first resin layer (resin layer A) after heating was measured under the following conditions. The island ratio partiality of the acid-modified polypropylene film after heating was measured for the adhesive film of Comparative Example 1 in the same manner as in Examples 1 to 7. The results are shown in Table 1.

[0280] [Pretreatment conditions]

[0281] Cut the sample into strips and embed it with thermosetting resin (50℃, 24 hours)

[0282] Ru dyeing after trimming

[0283] ·Use ultra-thin microtome to make cross sections (using diamond knife: finishing thickness 80nm)

[0284] Os coating (1~3nm)

[0285] [SEM observation conditions]

[0286] · Measurement device: Commercially available SEM (e.g. S-4800TYPE II manufactured by Hitachi High-Technologies Corporation)

[0287] Accelerating voltage: 5.0 kV

[0288] Emission current: 20μA

[0289] WD: 5mm

[0290] Detector: Upper+HA

[0291] ·Measurement magnification: 10k times

[0292] Resolution: 256dpi

[0293] [Image processing conditions]

[0294] The electron microscope image was subjected to the following image processing to obtain a binary image.

[0295] Image processing can be done using the Python image processing library OpenCV. The image processing conditions are as follows.

[0296] 1. Gaussian filter (kernel size 5px×5px)

[0297] 2. Magnify the measured image to 8 times in the vertical and horizontal directions (complementation method = CUBIC)

[0298] 3. Use fastNIMeansDenoising function to remove noise (set background color = black, parameters of fastNIMeansDenoising function are h = 10, hForColorComponents = 10, templateWindowSize = 7, searchWindowSize = 21)

[0299] 4. Binarization is performed with the bright part being white and the dark part being black (threshold = Otsu's threshold)

[0300] 5. Morphological transformation - Open processing (kernel size = 45px × 15px)

[0301] 6. Noise removal (remove the black area below 625px^2)

[0302] 7. Noise removal (remove the white area below 75px^2)

[0303] 8. Noise removal (remove black areas below 10000px^2)

[0304] 9. Morphological transformation - Open processing (kernel size = 65px × 25px)

[0305] 10. Morphological transformation - CLOSE processing (kernel size = 25px × 1px)

[0306] An area of ​​504 px×504 px (corresponding to a 1 μm×1 μm viewing angle) was cut out from the obtained binary image, and the ratio of the white portion in this area was defined as W (%).

[0307] The ratio W of the white portion is calculated by intercepting any 40 points, and the standard deviation of W at the 40 points is divided by the average value of W at the 40 points. The obtained value is defined as the degree of bias L of the sea-island structure.

[0308] <Measurement of Orientation Degree of Resin Layer A after Heating>

[0309] The orientation degree of the first resin layer (resin layer A) of the adhesive films of Examples 1 to 7 was measured under the following conditions. The orientation degree of the acid-modified polypropylene film of the adhesive film of Comparative Example 1 was measured in the same manner as in Examples 1 to 7. The results are shown in Table 1.

[0310] (Measurement conditions)

[0311] The crystallinity was measured under the following conditions using an X-ray diffraction apparatus (Aichi Synchrotron Radiation Center., trade name BL8S3 Beamline).

[0312] (Measurement conditions)

[0313] The X-ray irradiation angle was set to 0.09° with respect to the surface (0°) of the resin layer A.

[0314] The measurement range was set to be a range from the surface of the resin layer A to a depth of 5 μm.

[0315] As an X-ray detector, for example, R-AXIS is used, the camera length is set to 500 mm, and the X-ray wavelength is set to The exposure time was set to 30 seconds.

[0316] (Analysis of the middle layer)

[0317] Using the X-ray scattering data analysis software FI2D, the data with azimuth angles of 80deg to 100deg are intercepted from the spectrum data of the two-dimensional detector and integrated in the azimuth direction to obtain a one-dimensional spectrum showing the intensity value relative to the diffraction angle 2θ. The straight line between the two points 2θ=4.0deg and 2θ=16.0deg is then subtracted from the one-dimensional spectrum as the background. Thereafter, the spectral intensity value A of the amorphous component is defined as A: the value with the minimum intensity value in the region of 2θ=8.8deg to 9.8deg, and the crystalline peak intensity values ​​P1, P2, P3, and P4 of the four crystal planes are defined as follows.

[0318] P1: Peak intensity value of the peak located in the region of 2θ=7.0deg to 9.2deg

[0319] P2: Peak intensity value of the peak located within 2θ=9.2deg to 10.6deg

[0320] P3: Peak intensity value of the peak located within 2θ=10.6deg to 12.0deg

[0321] P4: Peak top intensity value of the peak located within 2θ=12.0deg to 14.0deg

[0322] The crystallinity C is defined as C = (P1 + P2 + P3 + P4) / A,

[0323] The degree of orientation D is defined as D=P2 / P4.

[0324] <Measurement of Sealing Strength (Initial) of Metal Terminals>

[0325] The sealing strength (initial) of the adhesive film of Examples 1 to 7 and Comparative Example 1 to the metal terminal was measured by the following method. The results are shown in Table 1. Aluminum (JIS H4160: 1994 A8079H-O) with a length of 50 mm, a width of 22.5 mm, and a thickness of 0.4 mm was prepared as a metal terminal. In addition, each adhesive film for metal terminals obtained in the Examples and Comparative Examples was cut into a length of 45 mm and a width of 10 mm. The adhesive film for metal terminals was then placed on the metal terminal to obtain a laminate of metal terminal / adhesive film. At this time, the layers are stacked in such a manner that the longitudinal and lateral directions of the metal terminal are respectively consistent with the length direction and width direction of the adhesive film for the metal terminal, and the metal terminal is consistent with the center of the adhesive film for the metal terminal. In addition, the resin layer A of the adhesive film for the metal terminal is arranged on the side of the metal terminal. Next, a polytetrafluoroethylene film (PTFE film, thickness 100 μm) is placed on the adhesive film for the metal terminal of the laminate (the surface of the adhesive film for the metal terminal is covered with the PTFE film), and is placed on a press machine heated to 200°C (the metal terminal is on the heating plate side), and a silicone sponge sheet is placed, and a pressure of 0.25 MPa is allowed to stand for 16 seconds to thermally fuse the adhesive film to the metal terminal. The laminate after thermal fusion is naturally cooled to 25°C. Then, under an environment of 25°C, the adhesive film for the metal terminal is peeled off from the metal terminal using a Tensilon universal material testing machine (RTG-1210 manufactured by A&D Company). The maximum strength during peeling is taken as the adhesion strength (N / 15mm) to the metal terminal. Among them, the adhesion strength (N / 15mm) is a conversion value of the adhesion strength (N / 15mm) measured for the adhesive film for the metal terminal with a width of 10mm. The peeling speed was set to 50 mm / min, the peeling angle was set to 180°, the chuck distance was set to 30 mm, and the average value of three measurements was taken. The results are shown in Table 1. Among them, the treatment of standing for 16 seconds under a heating and pressurizing environment at a temperature of 200°C and a surface pressure of 0.25 MPa is a treatment that assumes the heat and pressure applied in the above-mentioned preliminary bonding process and the formal bonding process.

[0326] <Measurement of sealing strength of metal terminals (after electrolyte immersion)>

[0327] The sealing strength of the adhesive film of Examples 1 to 7 and Comparative Example 1 to the metal terminal (after immersion in the electrolyte) was measured according to the following method. The results are shown in Table 1. Aluminum (JIS H4160: 1994A8079H-O) with a length of 50 mm, a width of 22.5 mm, and a thickness of 0.4 mm was prepared as a metal terminal. In addition, each adhesive film for metal terminals obtained in the Examples and Comparative Examples was cut into a length of 45 mm and a width of 10 mm. The adhesive film for metal terminals was then placed on the metal terminal to obtain a laminate of metal terminal / adhesive film. At this time, the layers are stacked in such a manner that the longitudinal and lateral directions of the metal terminal are respectively consistent with the length direction and width direction of the adhesive film for the metal terminal, and the metal terminal is consistent with the center of the adhesive film for the metal terminal. In addition, the resin layer A of the adhesive film for the metal terminal is arranged on the side of the metal terminal. Next, a polytetrafluoroethylene film (PTFE film, thickness 100 μm) is placed on the adhesive film for the metal terminal of the laminate (the surface of the adhesive film for the metal terminal is covered with the PTFE film), and then placed on a press machine heated to 200°C (the metal terminal is on the heating plate side), and a silicone sponge sheet is placed, and the laminate is allowed to stand for 16 seconds at a pressure of 0.25 MPa to thermally fuse the adhesive film to the metal terminal. The laminate after thermal fusion is naturally cooled to 25°C. Then the obtained laminate is placed in a 100mL plastic bottle, in which a mixed electrolyte (EC (ethylene carbonate) / DMC (dimethyl carbonate) / DEC (diethyl carbonate) = 1:1:1) 100g + pure water 1000ppm is tightly sealed. The sealed container is placed in an oven at 85°C, taken out after 24 hours, the electrolyte is washed off with water, and the obtained laminate is allowed to stand for 30 minutes to dry naturally. Next, in an environment of 25°C, the adhesive film for the metal terminal is peeled off from the metal terminal using a Tensilon universal material testing machine (RTG-1210 manufactured by A&D). The maximum strength during peeling is taken as the adhesion strength to the metal terminal (N / 15mm). The peeling speed is set to 50mm / min, the peeling angle is set to 180°, the chuck spacing is set to 30mm, and the average value of three measurements is taken. The results are shown in Table 1. Among them, the treatment of standing for 16 seconds in a heated and pressurized environment at a temperature of 200°C and a surface pressure of 0.25MPa is a treatment that assumes the heat and pressure applied in the above-mentioned pre-bonding step and the formal bonding step. <Ten-point average roughness of the outermost surface of the adhesive film>

[0328] The ten-point average roughness of the surface of the resin layer A of each adhesive film for metal terminal obtained in Examples 1 to 7 and Comparative Example 1 was measured according to the method specified in JIS B0601:1994. The measurement was performed using a small surface roughness measuring machine SURFTEST SJ-210 manufactured by Mitutoyo under the measurement conditions of a measurement speed of 0.5 mm and area AUTO. As a result, the ten-point average roughness was 0.34 μm in Example 1, 0.90 μm in Example 2, 0.26 μm in Example 3, 0.24 μm in Example 4, 0.35 μm in Example 5, 0.35 μm in Example 6, 0.35 μm in Example 7, and 0.40 μm in Comparative Example 1.

[0329] <Determination of Thermal Shrinkage (%)>

[0330] Cut the adhesive film for metal terminals into a size of 110 mm (MD) in length and 10 mm (TD) in width as a test piece. Next, use a metal ruler to measure the length M (mm) of the test piece. Next, use tape to fix the end of the test piece in the length direction (about 10 mm) on the metal wire mesh so that the test piece is suspended on the metal wire mesh. In this state, place it in an oven heated to 190°C for 120 seconds, then take out the test piece together with the metal wire mesh and cool it naturally at room temperature (25°C). Next, use a metal ruler to measure the length N (mm) of the test piece after it has cooled naturally to room temperature. The thermal shrinkage rate of the adhesive film for metal terminals is calculated by the following formula.

[0331] Thermal shrinkage (%) = (1 - (length N / length M)) × 100

[0332] [Table 1]

[0333]

[0334] As described above, the present invention provides the following aspects of the invention.

[0335] Item 1: An adhesive film for metal terminals, which is interposed between a metal terminal electrically connected to an electrode of an electric storage device element and an outer packaging material for an electric storage device encapsulating the electric storage device element, wherein:

[0336] The resin layer A forming at least one surface of the adhesive film for metal terminals contains an acid-modified polyolefin.

[0337] The crystallinity of the resin layer A measured using an X-ray diffraction apparatus after heating the adhesive film for a metal terminal at 200° C., 0.25 MPa, and 16 seconds under the following conditions was 11 or more.

[0338] (Measurement conditions)

[0339] The X-ray irradiation angle was set to 0.09° with respect to the surface (0°) of the resin layer A.

[0340] The measurement range was set to be a range from the surface of the resin layer A to a depth of 5 μm.

[0341] The camera length of the X-ray detector is set to 500 mm and the X-ray wavelength is set to The exposure time was set to 30 seconds.

[0342] Item 2: The adhesive film for a metal terminal according to Item 1, wherein a peak derived from maleic anhydride is detected in the resin layer A when the resin layer A is analyzed by infrared spectroscopy.

[0343] Item 3: The adhesive film for a metal terminal according to Item 1 or 2, wherein the degree of partiality of the island ratio of the sea-island structure in the resin layer A is 1.0 or less.

[0344] Item 4: The adhesive film for a metal terminal according to any one of Items 1 to 3, wherein the resin layer A has an orientation degree after the heating of 1.0 or more.

[0345] Item 5: The adhesive film for a metal terminal according to any one of Items 1 to 4, wherein the adhesive film for a metal terminal is formed of a polyolefin-based resin.

[0346] Item 6: An adhesive film for metal terminals according to any one of Items 1 to 5, wherein the adhesive film for metal terminals is composed of a laminate having, in sequence, a first resin layer arranged on the metal terminal side, an intermediate layer and a second resin layer arranged on the outer packaging material side of the power storage device, and the first resin layer is the resin layer A.

[0347] Item 7: The adhesive film for a metal terminal according to Item 6, wherein the crystallinity of the intermediate layer measured using an X-ray diffraction apparatus under the following conditions is 7.0 or more.

[0348] The X-ray irradiation angles were set to 0.19° and 0.22° with respect to the surface (0°) of the intermediate layer.

[0349] The camera length of the X-ray detector is set to 500 mm and the X-ray wavelength is set to The exposure time was set to 30 seconds.

[0350] Item 8: A method for producing an adhesive film for a metal terminal, wherein the adhesive film for a metal terminal is interposed between a metal terminal electrically connected to an electrode of an electric storage device element and an outer packaging material for an electric storage device encapsulating the electric storage device element,

[0351] The resin layer A forming at least one surface of the adhesive film for metal terminals contains an acid-modified polyolefin.

[0352] The crystallinity of the resin layer A measured using an X-ray diffraction apparatus after heating the adhesive film for a metal terminal at 200° C., 0.25 MPa, and 16 seconds under the following conditions was 11 or more.

[0353] (Measurement conditions)

[0354] The X-ray irradiation angle was set to 0.09° with respect to the surface (0°) of the resin layer A.

[0355] The measurement range was set to be a range from the surface of the resin layer A to a depth of 5 μm.

[0356] The camera length of the X-ray detector is set to 500 mm and the X-ray wavelength is set to The exposure time was set to 30 seconds.

[0357] Item 9: A metal terminal with an adhesive film for a metal terminal, wherein the adhesive film for a metal terminal according to any one of Items 1 to 7 is attached to a metal terminal.

[0358] Item 10: An electric storage device comprising:

[0359] An electric storage device element having at least a positive electrode, a negative electrode and an electrolyte;

[0360] An outer packaging material for an electric storage device that encapsulates the above-mentioned electric storage device element; and

[0361] the metal terminals electrically connected to the positive electrode and the negative electrode respectively and extending to the outside of the outer packaging material for the energy storage device,

[0362] An adhesive film for metal terminal is provided between the metal terminal and the outer packaging material for the power storage device.

[0363] The crystallinity of the resin layer A of the adhesive film for a metal terminal measured using an X-ray diffraction apparatus under the following conditions is 11 or more.

[0364] (Measurement conditions)

[0365] The X-ray irradiation angle was set to 0.09° with respect to the surface (0°) of the resin layer A.

[0366] The measurement range was set to be a range from the surface of the resin layer A to a depth of 5 μm.

[0367] The detector uses R-AXIS, the camera length is set to 500mm, and the X-ray wavelength is set to The exposure time was set to 30 seconds.

[0368] Item 11: A method for manufacturing an electric storage device, wherein:

[0369] The above-mentioned power storage device includes:

[0370] An electric storage device element having at least a positive electrode, a negative electrode and an electrolyte;

[0371] an outer packaging material for the above-mentioned power storage device that encapsulates the above-mentioned power storage device element; and

[0372] the metal terminals electrically connected to the positive electrode and the negative electrode respectively and extending to the outside of the outer packaging material for the energy storage device,

[0373] The manufacturing method includes the step of interposing the adhesive film for metal terminal according to any one of items 1 to 7 between the metal terminal and the electricity storage device packaging material, and sealing the electricity storage device element with the electricity storage device packaging material.

[0374] Item 12: An outer packaging material for an electric storage device used for an electric storage device, wherein:

[0375] The above-mentioned power storage device includes:

[0376] An electric storage device element having at least a positive electrode, a negative electrode and an electrolyte;

[0377] an outer packaging material for the above-mentioned power storage device that encapsulates the above-mentioned power storage device element; and

[0378] the metal terminals electrically connected to the positive electrode and the negative electrode respectively and extending to the outside of the outer packaging material for the energy storage device,

[0379] An adhesive film for metal terminal is provided between the metal terminal and the outer packaging material for the power storage device.

[0380] The adhesive film for metal terminal is the adhesive film for metal terminal according to any one of items 1 to 7,

[0381] The packaging material for an electric storage device is composed of a laminate having at least a base layer, a barrier layer, and a thermally fusible resin layer.

[0382] Item 13: A kit comprising an outer packaging material for an electric storage device used for an electric storage device and the adhesive film for a metal terminal according to any one of Items 1 to 7,

[0383] The above-mentioned power storage device includes:

[0384] An electric storage device element having at least a positive electrode, a negative electrode and an electrolyte;

[0385] an outer packaging material for the above-mentioned power storage device that encapsulates the above-mentioned power storage device element; and

[0386] the metal terminals electrically connected to the positive electrode and the negative electrode respectively and extending to the outside of the outer packaging material for the energy storage device,

[0387] When used, the adhesive film for metal terminal is used in a manner interposed between the metal terminal and the outer packaging material for the electric storage device.

[0388] Description of Reference Numerals

[0389] 1: Adhesive film for metal terminal; 2: Metal terminal; 3: Outer packaging material for storage device; 3a: Peripheral portion of outer packaging material for storage device; 4: Storage device element; 10: Storage device; 11: Intermediate layer; 12a: First resin layer; 12b: Second resin layer; 31: Base material layer; 32: Adhesive layer; 33: Barrier layer; 34: Adhesive layer; 35: Thermally fusible resin layer.

Claims

1. An adhesive film for a metal terminal, characterized in that: The adhesive film for metal terminals is interposed between metal terminals electrically connected to electrodes of the power storage device element and a packaging material for the power storage device that seals the power storage device element. The resin layer A forming at least one surface of the adhesive film for metal terminals contains an acid-modified polyolefin. The crystallinity of the resin layer A measured by using an X-ray diffraction device after heating the adhesive film for a metal terminal at 200° C., 0.25 MPa, and 16 seconds is 11 or more. Determination conditions: The X-ray irradiation angle is set to 0.09° relative to the surface of the resin layer A at 0°, The measurement range is set to be from the surface of the resin layer A to a depth of 5 μm, The camera length of the X-ray detector is set to 500 mm and the X-ray wavelength is set to The exposure time was set to 30 seconds.

2. The adhesive film for metal terminals according to claim 1, characterized in that: When the resin layer A was analyzed by infrared spectroscopy, a peak derived from maleic anhydride was detected.

3. The adhesive film for metal terminals according to claim 1 or 2, characterized in that: The degree of partiality of the island ratio of the sea-island structure in the resin layer A is 2.0 or less.

4. The adhesive film for metal terminals according to claim 1 or 2, characterized in that: The orientation degree of the resin layer A after the heating is 1.0 or more.

5. The adhesive film for metal terminals according to claim 1 or 2, characterized in that: The adhesive film for metal terminals is formed of a polyolefin-based resin.

6. The adhesive film for metal terminals according to claim 1 or 2, characterized in that: The adhesive film for metal terminals is composed of a laminate having, in this order, a first resin layer disposed on the metal terminal side, an intermediate layer, and a second resin layer disposed on the outer packaging material side for the power storage device. The first resin layer is the resin layer A.

7. The adhesive film for metal terminals according to claim 6, characterized in that: The crystallinity of the intermediate layer measured using an X-ray diffraction device under the following conditions is 7.0 or more, The X-ray irradiation angles were set to 0.19° and 0.22° relative to the surface of the intermediate layer at 0°, The camera length of the X-ray detector is set to 500 mm and the X-ray wavelength is set to The exposure time was set to 30 seconds.

8. A method for producing an adhesive film for a metal terminal, characterized in that: The adhesive film for metal terminals is interposed between metal terminals electrically connected to electrodes of the power storage device element and a packaging material for the power storage device that seals the power storage device element. The resin layer A forming at least one surface of the adhesive film for metal terminals contains an acid-modified polyolefin. The crystallinity of the resin layer A measured by using an X-ray diffraction device after heating the adhesive film for a metal terminal at 200° C., 0.25 MPa, and 16 seconds is 11 or more. Determination conditions: The X-ray irradiation angle is set to 0.09° relative to the surface of the resin layer A at 0°, The measurement range is set to be from the surface of the resin layer A to a depth of 5 μm, The camera length of the X-ray detector is set to 500 mm and the X-ray wavelength is set to The exposure time was set to 30 seconds. 9 . A metal terminal with an adhesive film for a metal terminal, wherein the adhesive film for a metal terminal according to claim 1 or 2 is attached to a metal terminal.

10. An electric storage device, characterized in that: include: An electric storage device element having at least a positive electrode, a negative electrode and an electrolyte; An outer packaging material for an electric storage device that encapsulates the electric storage device element; and metal terminals electrically connected to the positive electrode and the negative electrode and extending to the outside of the outer packaging material for the power storage device, An adhesive film for metal terminals is provided between the metal terminals and the outer packaging material for the power storage device, The crystallinity of the resin layer A of the adhesive film for a metal terminal measured using an X-ray diffraction device under the following conditions is 11 or more, Determination conditions: The X-ray irradiation angle is set to 0.09° relative to the surface of the resin layer A at 0°, The measurement range is set to be from the surface of the resin layer A to a depth of 5 μm, The detector uses R-AXIS, the camera length is set to 500mm, and the X-ray wavelength is set to The exposure time was set to 30 seconds.

11. A method for manufacturing an electric storage device, characterized in that: The power storage device comprises: An electric storage device element having at least a positive electrode, a negative electrode and an electrolyte; an outer packaging material for the electricity storage device that encapsulates the electricity storage device element; and the metal terminals electrically connected to the positive electrode and the negative electrode respectively and extending to the outside of the outer packaging material for the electricity storage device, The manufacturing method includes the step of interposing the adhesive film for metal terminal according to claim 1 or 2 between the metal terminal and the outer packaging material for the electric storage device, and sealing the electric storage device element with the outer packaging material for the electric storage device.

12. An outer packaging material for an electric storage device for an electric storage device, characterized in that: The power storage device comprises: An electric storage device element having at least a positive electrode, a negative electrode and an electrolyte; an outer packaging material for the electricity storage device that encapsulates the electricity storage device element; and the metal terminals electrically connected to the positive electrode and the negative electrode respectively and extending to the outside of the outer packaging material for the electricity storage device, An adhesive film for metal terminals is provided between the metal terminals and the outer packaging material for the power storage device, The adhesive film for metal terminals is the adhesive film for metal terminals according to claim 1 or 2, The packaging material for an electric storage device is composed of a laminate having at least a base layer, a barrier layer, and a thermally fusible resin layer.

13. A kit, characterized in that: A packaging material for an electric storage device used for an electric storage device and the adhesive film for a metal terminal according to claim 1 or 2, The power storage device comprises: An electric storage device element having at least a positive electrode, a negative electrode and an electrolyte; an outer packaging material for the electricity storage device that encapsulates the electricity storage device element; and the metal terminals electrically connected to the positive electrode and the negative electrode respectively and extending to the outside of the outer packaging material for the electricity storage device, When used, the adhesive film for metal terminal is used so as to be interposed between the metal terminal and the outer packaging material for the power storage device.