Granular lithium adsorbent and preparation method thereof

Highly efficient granule form is prepared by the synergistic effect of components such as lithium adsorbent powder, anionic surfactant, triethanolamine, ethyl cellulose and resorcinol diphenyl bisphosphonate in lithium ion sieve adsorbents. Lithium adsorbent solves the problems of dense materials and uneven distribution of water flow during extrusion molding, improves adsorption rate and capacity, and extends service life.

CN119186521APending Publication Date: 2024-12-27BEIJING HUATEYUAN TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411463376.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-18
Publication Date
2024-12-27

AI Technical Summary

Technical Problem

During the extrusion molding process, existing lithium ion sieve adsorbents have problems such as large extrusion pressure, excessive material, insufficient pore structure, low adsorption capacity, slow adsorption rate and uneven water flow distribution, resulting in difficult production and short service life.

Method used

The synergistic effect of lithium adsorbent powder, anionic surfactant, triethanolamine, ethyl cellulose, resorcinol diphenyl bisphosphate and other components is prepared through extrusion granulation and cleaning hardening processes. Granular lithium adsorbent with adsorption rate and adsorption capacity, and improve water flow distribution uniformity by designing extrusion disks of various shapes.

Benefits of technology

The lithium adsorbent has achieved a fast adsorption rate, high adsorption capacity, operating stability and extended service life, while reducing the density and viscosity of the prepared materials, solving the problems of dense material and uneven distribution of water flow during extrusion molding, and improving The powder utilization rate and the service life of the adsorbent are achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119186521A_ABST
    Figure CN119186521A_ABST
Patent Text Reader

Abstract

The invention provides a granular lithium adsorbent and a preparation method thereof, and relates to the technical field of salt lake lithium extraction adsorbents. According to the granular lithium adsorbent, the anionic surfactant, the triethanolamine, the ethyl cellulose and the diphenyl resorcinol bisphosphate are added into the lithium adsorbent powder, a synergistic relationship is formed among the components, the prepared granular lithium adsorbent has the advantages of high adsorption rate and high adsorption capacity, and meanwhile, through the addition of the components, the adsorption capacity of the granular lithium adsorbent is greatly improved. The compactness and the viscosity of the prepared material are effectively reduced, and the problems that a small-size adsorbent is difficult to produce and extruded and returned due to overhigh extrusion pressure during extrusion molding of an existing lithium adsorbent are solved. In addition, through the design of the extrusion disc, the problems of low adsorption performance exertion degree and short service life caused by non-uniform water flow distribution in the use process of the adsorbent are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium adsorbents for extracting lithium from salt lakes, and in particular to a granular lithium adsorbent and a preparation method thereof. Background Art

[0002] Lithium and its salts are widely used in glass, ceramics, batteries and other industries. They are called "energy elements of the 21st century" and are currently important strategic resources at home and abroad. Most of the world's lithium exists in salt lake water and seawater, and adsorption is one of the most effective means of extracting lithium. The development of ion sieves provides key materials for subsequent lithium extraction processes. However, the existing synthetic ion sieves are micro-nano powders, which have problems such as powder loss, compaction, and high water resistance during use, and cannot be applied in engineering.

[0003] Molding the powder can effectively solve the above problems. At present, the main molding methods include film forming, extrusion molding, droplet molding, etc. Extrusion molding has been widely studied due to its advantages such as simple process and adsorption capacity.

[0004] For example, patent CN111215040B discloses a method for preparing a lithium extraction adsorbent, which kneads the powder with a polymer and a solvent evenly, then extrude and shape, and crushes it into particles with a particle size of 0.6 to 2.0 mm after drying, and crushes the particles with a particle size of less than 0.6 mm to powder secondary molding. Small-sized adsorbents have better adsorption performance, but small-sized adsorbents are difficult to produce due to excessive pressure during the extrusion process. This patent extrude large-sized particles and then crush them, which will reduce the yield rate and make the process complicated. Patent CN118142487A discloses a method for preparing a lithium ion sieve adsorbent based on thermal molding, which mixes an adsorbent precursor, an adhesive molding agent, a pore-forming agent and a molding aid, and heats the obtained mixture under high pressure, kneads it, heats it, extrudes it, cools it to shape it, cuts it, and acid-activates it, and then dries it to obtain a lithium ion sieve adsorbent. The method proposed in this patent requires pressurized heating during the kneading process, which consumes a lot of energy. At the same time, high pressure easily causes the collapse of the pore structure and the problem of over-density of the material.

[0005] It can be seen from this that the existing extrusion molding process has a large extrusion pressure (extrusion pressure is between 10 and 150MPa), so small-sized (size <2mm) adsorbents are difficult to mass-produce. At the same time, extrusion molding adsorbents generally have problems such as low adsorption capacity and slow adsorption rate caused by over-dense materials and insufficient pore structure. In addition, in order to meet the state requirements of the material during the extrusion process, it takes a long time or heat and pressurize to knead. The process is cumbersome and causes energy loss, which increases the difficulty of production. In addition, extrusion molding adsorbents are prone to dead zones during the filling of the adsorption tower, which loses the performance of the adsorbent. Due to the uneven action of water flow, the adsorbent pulverization rate is increased, reducing the service life of the adsorbent.

[0006] Therefore, it is necessary and urgent to research and develop a granular lithium adsorbent and a preparation method thereof to alleviate the problems of low adsorption capacity caused by the difficulty in producing existing small-sized adsorbents, long extrusion molding and kneading process with high energy consumption, excessive extrusion pressure, and poor pore structure, as well as low adsorption performance and short life caused by uneven water flow distribution during the use of existing adsorbents.

[0007] In view of this, the present invention is proposed. Summary of the invention

[0008] The object of the present invention is to provide a granular lithium adsorbent and a preparation method thereof. The granular lithium adsorbent has the advantages of fast adsorption rate, high adsorption capacity, and can effectively improve the operating stability of the adsorbent and extend the service life through the synergistic effect of raw materials. At the same time, the density and viscosity of the prepared materials are effectively reduced, and the problems of the existing granular lithium adsorbent being too dense due to the excessive extrusion pressure during extrusion molding, making it difficult to mass-produce small-sized adsorbents, and the low adsorption rate and low powder utilization rate of the prepared granular lithium adsorbent are solved.

[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0010] The present invention provides a method for preparing a granular lithium adsorbent, the preparation method comprising:

[0011] The lithium adsorbent powder, anionic surfactant, triethanolamine, ethyl cellulose and resorcinol diphenyl phosphate are mixed, and then an adhesive is added and kneaded to obtain an extrudate;

[0012] Then, extrusion granulation, washing and hardening are carried out in sequence to obtain a granular lithium adsorbent.

[0013] Furthermore, the mass ratio of the lithium adsorbent powder, the anionic surfactant, triethanolamine, ethyl cellulose, and resorcinol diphenyl phosphate is 1: 0.05-0.1: 0.01-0.05: 0.01-0.12: 0.02-0.08.

[0014] Furthermore, the lithium adsorbent powder is selected from any one of a titanium-based lithium adsorbent, an aluminum-based lithium adsorbent, and a manganese-based lithium adsorbent;

[0015] Preferably, the particle size of the lithium adsorbent powder is 20 to 50 μm.

[0016] Furthermore, the anionic surfactant includes at least one of sodium dodecylbenzene sulfonate, sodium hexadecyl sulfonate, and sodium dodecyl sulfate.

[0017] Furthermore, the mass ratio of the adhesive to the total mass of the powder raw material is 0.3 to 0.6:1;

[0018] The total mass of the powder raw materials is the sum of the masses of the lithium adsorbent powder, the anionic surfactant, the triethanolamine, the ethyl cellulose and the resorcinol diphenyl phosphate.

[0019] Furthermore, the kneading temperature of adding the adhesive is 20 to 30° C., and the kneading time is 20 to 40 minutes.

[0020] Furthermore, the shapes of the extrusion granulation include: four-leaf clover-shaped particles, three-leaf clover-shaped particles and cylindrical particles.

[0021] Preferably, the length of the extruded granulated particles is 0.5 to 3 mm, the cylinder diameter is 0.8 to 1.2 mm, and the diameter of the circumscribed circle of the three-leaf clover and four-leaf clover is 1.4 to 1.6 mm.

[0022] Furthermore, the cleaning and hardening method comprises:

[0023] The extruded particles are soaked in hot water at 40 to 70° C. for 30 to 90 minutes, and then dried to obtain a granular lithium adsorbent.

[0024] Furthermore, during the soaking process, the ratio of the extruded particles to water is 1:2-10;

[0025] And / or, the drying temperature is 60-120° C. and the drying time is 0.5-12 h.

[0026] The present invention provides a granular lithium adsorbent, wherein the average length of the granular lithium adsorbent is 0.5 to 3 mm, and the granular lithium adsorbent has a pore structure with an average pore size of 10 to 300 nm;

[0027] The water content of the granular lithium adsorbent is 1-5%, the wet water content is 70%-90%, and the saturated adsorption capacity is 29-33 mg / g.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] The granular lithium adsorbent of the present application forms a synergistic relationship between the components by adding anionic surfactants, triethanolamine, ethyl cellulose, and hydroquinone diphenyl phosphate to the lithium adsorbent powder. The prepared granular lithium adsorbent has the advantages of fast adsorption rate, high adsorption capacity, and can effectively improve the operating stability of the adsorbent and extend its service life. At the same time, the addition of the above components effectively reduces the density and viscosity of the prepared material, solves the problems of the existing granular lithium adsorbent being too dense due to the excessive extrusion pressure during extrusion molding, low adsorption rate, low powder utilization, etc., as well as the problem of small-sized adsorbents being difficult to produce and extrusion return.

[0030] In addition, the present application designs the extrusion disc to simultaneously obtain three forms of adsorbent materials: clover, four-leaf clover and cylindrical. Adsorbents of different forms form a bridging effect, increase the porosity, and increase the contact time between the adsorbent and the brine. At the same time, dispersed turbulence is generated to make the water flow distribution more even, reduce dead zones, thereby reducing the adsorbent pulverization rate and significantly improving the life of the adsorbent, thereby solving the problem of low adsorption performance and short life caused by uneven water flow distribution during the use of the adsorbent. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0032] Figure 1 A schematic diagram of an extrusion molding die plate of an extruder provided in Example 1 of the present invention;

[0033] Figure 2a This is an electron microscope image of the internal pore structure of the granular lithium adsorbent prepared in Example 1 of the present invention at a scale of 500 nm;

[0034] Figure 2b This is an electron microscope image of the internal pore structure of the granular lithium adsorbent prepared in Example 1 of the present invention at a scale of 1 μm;

[0035] Figure 3 This is a graph showing the variation of the adsorption capacity of Example 1 and Comparative Examples 1 and 2 with adsorption time provided in Test Example 1 of the present invention. DETAILED DESCRIPTION

[0036] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] According to one aspect of the present invention, a method for preparing a granular lithium adsorbent comprises:

[0038] The lithium adsorbent powder, anionic surfactant, triethanolamine, ethyl cellulose and resorcinol diphenyl phosphate are mixed, and then an adhesive is added and kneaded to obtain an extrudate;

[0039] Then, extrusion granulation, washing and hardening are carried out in sequence to obtain a granular lithium adsorbent.

[0040] The invention provides a method for preparing a granular lithium adsorbent, which comprises: firstly mixing lithium adsorbent powder, anionic surfactant, triethanolamine, ethyl cellulose and resorcinol diphenyl phosphate, then adding an adhesive and kneading to obtain an extrusion material; then sequentially performing extrusion granulation, washing and hardening to obtain a granular lithium adsorbent.

[0041] The addition of each component in this application is to:

[0042] 1. Anionic surfactant: The present invention introduces anionic surfactant to make the granular lithium adsorbent have rapid wettability. At the same time, a through-pore structure can be formed during the preparation process, which can increase the lithium ion adsorption rate and achieve a higher adsorption capacity in the same time.

[0043] 2. Triethanolamine: The present invention adds triethanolamine as a penetrant. Triethanolamine cooperates with anionic surfactants to form pores while controlling the pores to have a uniform microporous structure, thereby not only ensuring the mass transfer rate but also effectively preventing calcium and magnesium scale formed in the water from entering the pores and blocking ion channels, thereby causing rapid attenuation of adsorption capacity.

[0044] 3. Ethyl cellulose: During the preparation of the granular lithium adsorbent of the present invention, the addition of ethyl cellulose can effectively increase the extrusion smoothness, reduce the density of the material, and solve the problems of the material being too dense and the low adsorption rate.

[0045] 4. Resorcinol diphenyl phosphate (RDP): Ethyl cellulose and RDP have a dual dispersion effect, which effectively improves the dispersion state of the adsorbent powder during the kneading process, and can achieve a uniform dispersion effect in a shorter time. The kneading time can be shortened by more than 50%, which reduces energy consumption and solves the problem of material return caused by excessive viscosity of the material during the extrusion molding process, effectively ensuring efficient and stable production. In addition, since ethyl cellulose and RDP are both easily soluble in water, the soaking process can slowly precipitate the two materials to form a rich specific surface area, effectively improving the utilization rate of the powder.

[0046] In summary, the granular lithium adsorbent of the present application forms a synergistic relationship between the components by adding anionic surfactants, triethanolamine, ethyl cellulose, and hydroquinone diphenyl phosphate to the lithium adsorbent powder, and the prepared granular lithium adsorbent has the advantages of fast adsorption rate, high adsorption capacity, and can effectively improve the operating stability of the adsorbent and extend its service life. At the same time, the present application effectively reduces the density and viscosity of the prepared material by adding the above components, and solves the problems of the existing granular lithium adsorbent being too dense due to the excessive extrusion pressure during extrusion molding, low adsorption rate, low powder utilization, etc., as well as the difficulty in producing small-sized adsorbents and extrusion return.

[0047] Furthermore, the working principles of the components of the granular lithium adsorbent of the present application during the preparation process can be summarized as follows:

[0048] The present application uses lithium adsorbent powder as the main component and adds anionic surfactants. The anionic surfactants can effectively reduce the surface tension of water, accelerate the exchange rate between solvent and water during the phase transformation process, and form a uniform and transparent pore structure. In addition, by adding surfactants, the low surface tension of the adsorbent can be maintained. During the use of the adsorbent, the brine can be promoted to impregnate the internal and external pore structures of the adsorbent, shorten the time for lithium ions to reach the adsorption site, and improve the adsorption efficiency.

[0049] At the same time, triethanolamine is added as a penetrant during the kneading process. During the immersion process, the triethanolamine penetrant can quickly migrate into the water. During the migration process, a large number of microporous structures are formed, which increases the contact area between the adsorbent and water, which is beneficial to the rapid absorption of ions.

[0050] In addition, in order to solve the problem of excessive extrusion pressure during the extrusion process, lubricants and dispersants are added during the kneading process of powder and glue solution. Ethyl cellulose is selected as a lubricant. The addition of ethyl cellulose can effectively increase the smoothness of extrusion, reduce the density of materials, and effectively improve the utilization rate of powder. Using RDP (resorcinol diphenyl phosphate) as a material dispersant can increase the steric hindrance between catalyst particles, reduce the agglomeration of particles, and achieve an ideal kneading state in a shorter time, effectively reducing energy consumption. At the same time, the addition of dispersants can reduce the viscosity of powder-glue kneading and avoid returning materials during the extrusion process. The extruded material is immersed in 40-70℃ hot water, the ratio of mixed material to water is 1:2-1:10, and the soaking time is 30-90min. During the soaking process, ethyl cellulose and RDP are gradually precipitated, the original position is vacated, and a through cavity structure is formed, which is conducive to the rapid migration of ions and improves the adsorption rate.

[0051] In a preferred embodiment of the present invention, the mass ratio of the lithium adsorbent powder, the anionic surfactant, triethanolamine, ethyl cellulose and resorcinol diphenyl phosphate is 1: 0.05-0.1: 0.01-0.05: 0.01-0.12: 0.02-0.08.

[0052] In the present invention, the performance of the granular lithium adsorbent of the present invention is further optimized by further adjusting and optimizing the usage ratio of the raw materials of each component.

[0053] In a preferred embodiment of the present invention, the lithium adsorbent powder is selected from any one of a titanium-based lithium adsorbent, an aluminum-based lithium adsorbent, and a manganese-based lithium adsorbent;

[0054] In the above preferred embodiment, the particle size of the lithium adsorbent powder is 20 to 50 μm.

[0055] As a preferred embodiment, the particle size of the lithium adsorbent powder is 20-50 μm. When the particle size of the powder is greater than 50 μm, there is a risk of pore blockage during the extrusion process, and the utilization rate of the powder is reduced, and the adsorption rate and capacity are reduced accordingly. When the particle size of the powder is less than 20 μm, more adhesive is required to wrap the material, reducing the exposed area of ​​the powder, thereby reducing the adsorption performance.

[0056] In a preferred embodiment of the present invention, the anionic surfactant includes at least one of sodium dodecylbenzene sulfonate, sodium hexadecyl sulfonate and sodium dodecyl sulfate.

[0057] In a preferred embodiment of the present invention, the mass ratio of the adhesive to the total mass of the powder raw material is 0.3 to 0.6:1;

[0058] The total mass of the powder raw materials is the sum of the masses of the lithium adsorbent powder, the anionic surfactant, the triethanolamine, the ethyl cellulose and the resorcinol diphenyl phosphate.

[0059] As a preferred implementation, the mass ratio of the above-mentioned adhesive to the total mass of the powder raw material is 0.3-0.6:1. When the adhesive exceeds this ratio range, the adsorption capacity will be reduced.

[0060] In a preferred embodiment of the present invention, the kneading temperature for adding the adhesive is 20 to 30° C., and the kneading time is 20 to 40 minutes.

[0061] In a preferred embodiment of the present invention, the shapes of the extrusion granules include: four-leaf clover-shaped particles, three-leaf clover-shaped particles and cylindrical particles.

[0062] As a preferred embodiment, the present application can obtain three forms of adsorbent materials, namely, clover, four-leaf clover and cylindrical, by designing the extrusion disc. Adsorbents of different forms form a bridging effect, increase the porosity, and increase the contact time between the adsorbent and the brine. At the same time, dispersed turbulence is generated to make the water flow more evenly distributed and reduce dead zones, thereby reducing the pulverization rate of the adsorbent and significantly improving the life of the adsorbent.

[0063] Preferably, the present application designs the extrusion disc so that one-third of the extrusion holes are in a four-leaf clover shape with a size of 1.4*1.6mm, one-third are in a three-leaf clover shape with a size of 1.5mm, and one-third are in a cylindrical shape with a size of 1mm. The three shapes have the same area, so that the extrusion pressure is evenly distributed. The adsorbent exists in three shapes, which can form abundant flow channels in the filling column, increase the porosity, and increase the contact time between the adsorbent and the brine. At the same time, dispersed turbulence is generated to make the water flow distribution more even, reduce dead zones, and thus reduce the pulverization rate of the adsorbent.

[0064] Preferably, the length of the extruded granulated particles is 0.5 to 3 mm, the cylinder diameter is 0.8 to 1.2 mm, and the diameter of the circumscribed circle of the three-leaf clover and four-leaf clover is 1.4 to 1.6 mm.

[0065] In a preferred embodiment of the present invention, the cleaning and hardening method comprises:

[0066] The extruded particles are soaked in hot water at 40 to 70° C. for 30 to 90 minutes, and then dried to obtain a granular lithium adsorbent.

[0067] In the above preferred embodiment, during the soaking process, the ratio of the extruded particles to water is 1:2-10;

[0068] In the above preferred embodiment, the drying temperature is 60-120° C. and the drying time is 0.5-12 hours.

[0069] According to one aspect of the present invention, a granular lithium adsorbent has an average length of 0.5 to 3 mm, and has a pore structure with an average pore size of 10 to 300 nm;

[0070] The water content of the granular lithium adsorbent is 1-5%, the wet water content is 70%-90%, and the saturated adsorption capacity is 29-33 mg / g.

[0071] The granular lithium adsorbent provided by the present invention has an average length of 0.5 to 3 mm, and has a pore structure with an average pore size of 10 to 300 nm. After testing, the water content of the granular lithium adsorbent is 1 to 5%, the wet water content is 70% to 90%, and the saturated adsorption capacity is 29 to 33 mg / g.

[0072] The technical solution of the present invention will be further described below in conjunction with embodiments.

[0073] Example 1

[0074] A method for preparing a granular lithium adsorbent, the method comprising:

[0075] (1) Weigh the lithium ion adsorbent powder and add it to a kneader. At the same time, add anionic surfactant, penetrant triethanolamine, ethyl cellulose, and resorcinol diphenyl phosphate (RDP) in a certain proportion and mix them evenly. The mixing time range is 15 minutes.

[0076] Wherein: the manufacturers and models of the raw materials used in this embodiment are shown in Table 1, and the raw materials not specified in Table 1 are purchased from the market.

[0077] Table 1:

[0078]

[0079]

[0080] (2) After the above five raw materials are mixed evenly, 350g of adhesive is added and kneaded at a kneading temperature of 25°C for 30 minutes. The kneaded materials are added to an extruder for molding.

[0081] The extrusion molding extruder uses a four-leaf clover, a three-leaf clover and a cylindrical die plate, each accounting for one-third of the area, and three forms of adsorbent materials are mixed while extruding.

[0082] Figure 1 Schematic diagram of the extrusion molding die plate of the extruder provided in this embodiment.

[0083] The extrusion molding pressure is 2Mpa, and the extruded particles are in the shape of a four-leaf clover with a size of 1.4*1.6mm, a three-leaf clover with a size of 1.5mm, and a cylinder with a size of 1mm.

[0084] (3) Soak the extruded particles in 3L of 50°C hot water for 60 minutes, and then dry them in a 100°C oven for 8 hours, controlling the moisture content to be 1-5%, and obtain a granular lithium adsorbent after drying.

[0085] Figure 2a This is an electron microscope image of the internal pore structure of the granular lithium adsorbent prepared in this example at a scale of 500 nm;

[0086] Figure 2b This is an electron microscope image of the internal pore structure of the granular lithium adsorbent prepared in this example at a scale of 1 μm.

[0087] Depend on Figure 2a and Figure 2b It can be seen that a rich pore structure is formed inside the adsorbent, with uniform pore size, good connectivity, and a large specific surface area, which effectively improves the adsorption rate of lithium ions by the adsorbent and achieves a higher adsorption capacity.

[0088] Example 2

[0089] A method for preparing a granular lithium adsorbent, the method comprising:

[0090] (1) This step is the same as Example 1 except that the amounts of the components of the raw materials are different from those in Example 1;

[0091] The components and amounts of the raw materials used in this example are shown in Table 2.

[0092] Table 2:

[0093]

[0094] (2) This step is the same as Example 1 except that the amount of adhesive added is 600 g.

[0095] (3) Same as Example 1.

[0096] Example 3

[0097] A method for preparing a granular lithium adsorbent, the method comprising:

[0098] (1) Weigh the lithium ion adsorbent powder and add it to a kneader, and add anionic surfactant, penetrant triethanolamine, ethyl cellulose, and resorcinol diphenyl phosphate (RDP) in a certain proportion and mix them evenly. The mixing time range is 30 minutes;

[0099] Wherein: the manufacturers and models of the raw materials used in this embodiment are shown in Table 3, and the raw materials not specified in Table 3 are purchased from the market.

[0100] Table 3:

[0101]

[0102]

[0103] (2) After the above five raw materials are mixed evenly, 490g of adhesive is added and kneaded at a kneading temperature of 30°C for 30 minutes. The kneaded materials are added to an extruder for molding.

[0104] The extruder and extrusion parameters of the extrusion molding are the same as those in Example 1.

[0105] (3) Soak the extruded particles in 5.5L of 40°C hot water for 40 minutes, and then dry them in an oven at 80°C for 10 hours, controlling the moisture content to 1-5%, and obtain the formed granular lithium adsorbent after drying.

[0106] Embodiments 4 to 6

[0107] The preparation methods of the granular lithium adsorbents in Examples 4 to 6 are the same as in Example 1 except that the amounts of the components of the raw materials in step (1) are different from those in Example 1. The amounts of the components in Examples 4 to 6 are shown in Table 4.

[0108] Table 4:

[0109]

[0110] Example 7

[0111] This embodiment is the same as Embodiment 1 except that the amount of adhesive added in step (2) is 850 g.

[0112] Example 8

[0113] This embodiment is the same as Embodiment 1 except that the extruder for extrusion molding in step (2) only uses a cylindrical die plate and the extruded particles are all cylindrical.

[0114] Example 9

[0115] This embodiment is the same as Embodiment 1 except that the extruder for extrusion molding in step (2) only uses a four-leaf clover die plate and the extruded particles are all in the shape of a four-leaf clover.

[0116] Example 10

[0117] This embodiment is the same as Embodiment 1 except that the extruder for extrusion molding in step (2) only uses a cloverleaf die plate and the extruded particles are all clover-shaped.

[0118] Comparative Examples 1 to 6

[0119] The preparation methods of the granular lithium adsorbents in Comparative Examples 1 to 6 are the same as those in Example 1 except that the amounts of the components of the raw materials in step (1) are different from those in Example 1. The amounts of the components in Comparative Examples 1 to 6 are shown in Tables 5 and 6.

[0120] Table 5:

[0121]

[0122] Table 6:

[0123]

[0124]

[0125] Test Example 1

[0126] In order to show that the granular lithium adsorbent prepared by the present invention has the characteristics of fast adsorption rate and high adsorption capacity, the granular lithium adsorbents prepared by Examples 1 to 10 and Comparative Examples 1 to 6 are tested for performance, and the existing commercially available granular lithium adsorbent is used for comparison;

[0127] Control group 1: commercially available lithium adsorbent A;

[0128] Control group 2: commercially available lithium adsorbent B;

[0129] The specific test results are shown in Table 7 and Table 8:

[0130] Table 7:

[0131]

[0132]

[0133] Table 8:

[0134]

[0135] The adsorption rate of the lithium adsorbent prepared in Examples 1 to 3 of the present application is much higher than that of the lithium adsorbent products on the market (Control Groups 1 and 2). The saturated adsorption capacity of the high-porosity composite adsorbent is 32 mg / g, which is much higher than the saturated capacity of 20 mg / g of the adsorbent on the market. This shows that the lithium adsorbent of the present application has the characteristics of fast adsorption rate and high adsorption capacity, and has broad application prospects in the field of lithium extraction from salt lakes.

[0136] Figure 3 This is a graph showing the variation of the adsorption capacity of Example 1 and Comparative Examples 1 and 2 with the adsorption time provided in this test example.

[0137] Compared with Examples 1 to 3, in Example 4, since the amount of anionic surfactant added is too small, the wettability of the adsorbent becomes poor and the adsorption capacity shows a decreasing trend.

[0138] Compared with Examples 1 to 3, Example 5 has a poor adsorption capacity due to the fact that the amount of penetrant triethanolamine added is too small, resulting in a non-through pore structure of the adsorbent, a small number of micropores, and a poor adsorption capacity.

[0139] Compared with Examples 1 to 3, in Example 6, since the amount of ethyl cellulose added is too large, a wrapping effect is produced on the adsorbent powder, which hinders mass transfer, resulting in a decrease in adsorption rate and adsorption capacity.

[0140] In Example 7 relative to Examples 1 to 3, due to the excessive amount of adhesive added, the mass ratio of the adhesive to the total mass of the powder raw material is 850:1090, resulting in a decrease in the powder content as the adhesive content increases, resulting in a decrease in the adsorption capacity.

[0141] Since only a mold plate of a single shape is used in Examples 8 to 10, the filling column cannot produce a good bridging effect, causing the adsorbent to be piled too densely and creating dead zones, resulting in excessive adsorbent loss and reduced service life.

[0142] Compared with Examples 1 to 3, Comparative Example 1 does not contain the penetrant triethanolamine, so the adsorbent bulk density increases and the performance decreases.

[0143] Compared with Examples 1 to 3, Comparative Example 2 does not contain the dispersant ethyl cellulose, resulting in an increase in extrusion pressure, excessive density of the material, and reduced adsorption performance.

[0144] Comparative Example 3 is relative to Examples 1 to 3, because the dispersant resorcinol diphenyl bisphosphate is not included, the kneading time is prolonged, the energy consumption is increased, and the adsorption capacity is reduced.

[0145] Compared with Examples 1 to 3, since the overall components of Comparative Example 4 do not contain a dispersant, the extrusion difficulty is increased and the adsorbent performance is reduced.

[0146] Comparative Example 5 does not contain resorcinol diphenyl bisphosphate relative to Examples 1 to 3, but the amount of the dispersant is the same as that of Example 1. The adsorbent does not form a rich pore structure, and the adsorption capacity shows a decreasing trend.

[0147] Comparative Example 6 does not contain ethyl cellulose relative to Examples 1 to 3, but the amount of dispersant is the same as that of Example 1, resulting in increased extrusion resistance, reduced powder utilization, and reduced adsorption capacity.

[0148] In summary, this application aims to solve the problems of serious loss of adsorption performance, low powder utilization, rapid attenuation of long-term operating performance, and short life after the lithium adsorbent extracted from salt lakes is formed. A method for preparing a granular lithium adsorbent with fast lithium ion adsorption rate, high adsorption capacity, and effective improvement of adsorbent operation stability and extended life is proposed. This method solves the problems of too dense materials, low adsorption rate, low powder utilization, and difficulty in producing small-sized adsorbents and extrusion return caused by excessive extrusion pressure during extrusion molding. At the same time, by setting the shape of extrusion granulation, the problems of low adsorption performance and short life caused by uneven water flow distribution during the use of the adsorbent are solved.

[0149] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a granular lithium adsorbent, characterized in that: The preparation method comprises: The lithium adsorbent powder, anionic surfactant, triethanolamine, ethyl cellulose and resorcinol diphenyl phosphate are mixed, and then an adhesive is added and kneaded to obtain an extrudate; Then, extrusion granulation, washing and hardening are carried out in sequence to obtain a granular lithium adsorbent.

2. The method for preparing a granular lithium adsorbent according to claim 1, characterized in that: The mass ratio of the lithium adsorbent powder, the anionic surfactant, triethanolamine, ethyl cellulose and resorcinol diphenyl phosphate is 1: 0.05-0.1: 0.01-0.05: 0.01-0.12: 0.02-0.

08.

3. The method for preparing a granular lithium adsorbent according to claim 1, characterized in that: The lithium adsorbent powder is selected from any one of titanium-based lithium adsorbent, aluminum-based lithium adsorbent, and manganese-based lithium adsorbent; Preferably, the particle size of the lithium adsorbent powder is 20 to 50 μm.

4. The method for preparing a granular lithium adsorbent according to claim 1, characterized in that: The anionic surfactant includes at least one of sodium dodecylbenzene sulfonate, sodium hexadecyl sulfonate and sodium dodecyl sulfate.

5. The method for preparing a granular lithium adsorbent according to claim 1, characterized in that: The mass ratio of the adhesive to the total mass of the powder raw material is 0.3-0.6:1; The total mass of the powder raw materials is the sum of the masses of the lithium adsorbent powder, the anionic surfactant, the triethanolamine, the ethyl cellulose and the resorcinol diphenyl phosphate.

6. The method for preparing a granular lithium adsorbent according to claim 1, characterized in that: The kneading temperature for adding the adhesive is 20 to 30°C, and the kneading time is 20 to 40 minutes.

7. The method for preparing a granular lithium adsorbent according to claim 1, characterized in that: The shapes of the extrusion granulation include: four-leaf clover-shaped particles, three-leaf clover-shaped particles and cylindrical particles; Preferably, the length of the extruded granulated particles is 0.5 to 3 mm, the cylinder diameter is 0.8 to 1.2 mm, and the diameter of the circumscribed circle of the three-leaf clover and four-leaf clover is 1.4 to 1.6 mm.

8. The method for preparing a granular lithium adsorbent according to claim 1, characterized in that: The cleaning and hardening method comprises: The extruded particles are soaked in hot water at 40-70° C. for 30-90 minutes, and then dried to obtain a granular lithium adsorbent.

9. The method for preparing a granular lithium adsorbent according to claim 8, characterized in that: During the soaking process, the ratio of the extruded particles to water is 1:2-10; And / or, the drying temperature is 60-120° C. and the drying time is 0.5-12 h.

10. A granular lithium adsorbent, characterized in that: The average length of the granular lithium adsorbent is 0.5 to 3 mm, and the granular lithium adsorbent has a pore structure with an average pore size of 10 to 300 nm; The water content of the granular lithium adsorbent is 1-5%, the wet water content is 70%-90%, and the saturated adsorption capacity is 29-33 mg / g.