Double-doped material and application thereof
By preparing the double-doped HNKVOH of sodium chloride, potassium chloride and vanadium pentoxide, the pre-insertion of sodium and potassium ions is used to solve the problems of slow reaction kinetics and poor circulation performance of vanadium-based compounds in electrochemical reactions, and the capacity and circulation stability of the positive electrode of zinc ion battery are significantly improved.
Patent Information
- Application Number
- CN202510135513.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-02-07
- Publication Date
- 2025-03-07
AI Technical Summary
Vanadium-based compounds have problems with slow reaction kinetics and poor cycling performance during electrochemical reactions, mainly due to their instability during ion transport and chemical dissolution during cycling.
The HNKVOH double-doped material is prepared by mixing sodium chloride, potassium chloride and vanadium pentoxide in a specific mass ratio and heating reaction in an autoclave. The structural changes of the material are adjusted by using the pre-insertion of sodium and potassium ions to improve its electrochemical performance.
This double-doped material significantly improves the capacity and cycle stability of the positive electrode of the zinc ion battery, exhibits high specific capacity, good conductivity and long cycle life, and does not require calcination during the preparation process, which has the characteristics of energy saving and environmentally friendly.
Smart Images

Figure CN119581545A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery materials, and in particular to a dual-doped material and application thereof. Background Art
[0002] Lithium-ion batteries (LIBs) stand out among many secondary batteries due to their low self-discharge rate, high energy density and environmental friendliness. They are widely used in various fields and have become a vital energy storage device in contemporary society. However, the relatively high manufacturing and processing costs of LIBs have seriously hindered their widespread application. In addition, lithium dendrites formed during battery operation significantly reduce the battery life and safety, and the limited supply of lithium resources also restricts the long-term development of lithium-ion batteries.
[0003] In this context, almost neutral rechargeable aqueous zinc-ion batteries (AZIBs) have attracted widespread attention due to their significant advantages. Compared with lithium resources, zinc resources are abundant and low in cost. In addition, aqueous electrolytes are non-flammable, non-explosive, non-toxic and non-polluting, and divalent zinc ions can provide a larger theoretical capacity and capacity density. Therefore, AZIBs stand out among many ion batteries and show broad application prospects. Common positive electrode materials in AZIBs include manganese oxides, vanadium-based compounds, and Prussian blue analogs. Generally, manganese oxides exhibit poor cycle stability due to irreversible phase changes during the reaction process, and Prussian blue analogs usually have a low specific capacity (usually less than 100 mAh g -1 ) and poor cycle performance. In contrast, vanadium-based compounds have a rich layered structure and valence state (V 5+ , V 4+ , V 3+ ,V 2+ ), which can achieve more electron transfer in redox reactions, have higher capacity, and show broad application prospects.
[0004] However, vanadium-based compounds have the disadvantages of slow reaction kinetics and poor cycle performance during electrochemical reactions. The main reasons are the instability of vanadium-based compounds during ion transport and chemical dissolution during the cycle. In order to overcome these defects of vanadium-based compounds, a technical solution for metal ion embedding has been proposed. Embedding metal ions into vanadium-based compounds can effectively regulate their structural changes, thereby affecting their electrochemical properties. In addition, the embedding of water molecules can shield the electrostatic interaction between charge carriers and the matrix, and promote the embedding / deintercalation of ions in the interface and the main framework. For example, in the preparation method of VO2 / CNTs microspheres as negative electrode materials for lithium-ion batteries (CN 107579211), VO2 / CNTs microspheres, as negative electrode materials for lithium-ion batteries, have shown good performance, but due to the single source and high price of CNTs (carbon nanotubes), it is difficult to extend to other aqueous metal battery fields. In another study, Min Du et al. (Advanced Science, 2020,7(13)) designed and synthesized Na 0.97 Mn 0.02 V8O 20 0.32H2O material, Mn found 2+ / Mn 3+ The embedding of Na + The embedding of Zn 2+ The migration rate and conductivity of the nanostructured carbon nanotubes are determined by experimental tests and theoretical calculations. Hao Yu et al. (ChemNanoMat, 2020, 6 (5)) showed that K + Ion insertion into vanadium pentoxide (K 0.5 V2O5) forms a strong chemical bond, firmly combining the vanadium pentoxide layers together, effectively avoiding K 0.5 V2O5 dissolves in the electrolyte. Compared with vanadium pentoxide, K 0.5 The V2O5 electrolyte remained transparent and colorless after being immersed in the electrolyte for 8 days. These studies show that the embedding of single potassium and sodium metal ions can change the structure of vanadium-based compounds to varying degrees and have a significant impact on the electrochemical properties of the materials, while sodium-potassium co-doped materials and their synergistic optimization methods have not been reported. Summary of the invention
[0005] In view of this, the present invention provides a dual-doped material and its application, the main purpose of which is to provide a dual-doped material that can effectively increase the capacity of the positive electrode while enhancing the ion mobility and battery stability.
[0006] In order to achieve the above object, the present invention mainly provides the following technical solutions: On one hand, the present invention provides a dual-doped material, which is prepared from three materials: sodium chloride, potassium chloride and vanadium pentoxide, wherein the mass ratio of the sodium chloride, the potassium chloride and the vanadium pentoxide is in the range of (0.005-0.075):(0.1-0.15):1.
[0007] Preferably, the dual-doped material is prepared by the following steps: (1) Weigh sodium chloride, potassium chloride and vanadium pentoxide according to mass ratio to prepare vanadium pentoxide solution; (2) Mix sodium chloride and potassium chloride evenly; (3) adding a mixture of sodium chloride and potassium chloride to the vanadium pentoxide solution and stirring to form an orange-red mixture; (4) The orange-red mixture is placed in an autoclave and heated to react to obtain HNKVOH (i.e., the dual-doping chemical formula HNa x K y V6O 16 ·4H2O abbreviation) double doped material.
[0008] Preferably, the step (1) further comprises the following steps: (1.1) adding vanadium pentoxide to a solution of deionized water and 30 wt% hydrogen peroxide in a volume ratio of 40:1; (1.2) stirring the solution and heating it at 25-35° C. for 4 to 6 hours to obtain an orange-red vanadium pentoxide solution.
[0009] Preferably, the stirring time of the stirred solution is 1 h to 3 h.
[0010] Preferably, in step (3), the mixture of sodium chloride and potassium chloride is added to the vanadium pentoxide solution and stirred for 25 min to 35 min.
[0011] Preferably, the step (4) further comprises the following steps: repeatedly washing the HNKVOH dual-doped material with deionized water, and obtaining a powder material after drying.
[0012] Preferably, the drying temperature of the drying treatment is 60° C. to 80° C., and the drying time is 12 h to 16 h.
[0013] Preferably, the heating time of the autoclave in step (4) is 6 h to 10 h.
[0014] Preferably, the temperature range of heating the autoclave in step (4) is 110° C. to 130° C.
[0015] Another aspect of the present invention further provides an application of the dual-doped material, wherein the dual-doped material is applied to the positive electrode material of a zinc ion battery and is arranged on the positive electrode of the zinc ion battery.
[0016] Compared with the prior art, the present invention prepares HNKVOH dual-doped material by ion pre-insertion method, which has the following significant technical effects: 1. Potassium ions form KO bonds in layered metal oxides, which has a "pillar" effect, effectively enhancing the thermodynamic properties and structural stability of V2O5·nH2O (VOH), thereby significantly improving the cyclic stability of the material; 2. The pre-inserted sodium ions significantly increase the lattice spacing and ion migration channels of VOH, effectively improving the capacity of the positive electrode of the zinc ion battery; 3. HNKVOH dual-doped material as a positive electrode material for zinc-ion batteries exhibits high specific capacity, good conductivity and long cycle life through the coordination effect caused by dual doping of sodium ions and potassium ions; 4. This material does not require calcination during the preparation process, and is energy-saving and environmentally friendly.
[0017] Therefore, the present invention provides an efficient and sustainable method for preparing positive electrode materials, which significantly enhances the electrical performance of zinc ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 An X-ray diffraction spectrum of a HNKVOH dual-doped material provided in an embodiment of the present invention; Figure 2 A transmission electron microscope image and a high-magnification transmission electron microscope image of a HNKVOH dual-doped material provided in an embodiment of the present invention; Figure 3 A cyclic voltammetry curve of a HNKVOH dual-doped material provided in an embodiment of the present invention as a positive electrode material for a zinc ion battery; Figure 4 A cycle performance diagram of a zinc ion battery prepared in Example 1 provided by the present invention; Figure 5 A cycle performance diagram of a zinc ion battery prepared in Comparative Example 1 provided by the present invention; Figure 6 This is a cycle performance diagram of a zinc ion battery prepared in Comparative Example 2 provided by the present invention. DETAILED DESCRIPTION
[0019] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.
[0020] On the one hand, an embodiment of the present invention provides a dual-doped material, including: Potassium chloride, sodium chloride and vanadium pentoxide, wherein the mass ratio of the potassium chloride, the sodium chloride and the vanadium pentoxide is 0.005-0.075:0.1-0.15:1.
[0021] The chemical formula of the dual-doped material prepared by the present invention is HNa x K y V6O 16 4H2O, where x and y vary with the feeding difference of Na and K atoms, referred to as HNKVOH. In the HNKVOH dual-doped material of the present invention, the pillar effect of potassium ions in HNKVOH can effectively enhance the thermodynamic properties and structural stability of VOH, thereby effectively increasing the cycle stability; while sodium ions significantly increase the migration kinetics of VOH, thereby effectively increasing the capacity of the positive electrode.
[0022] On the other hand, an embodiment of the present invention further provides a method for preparing a dual-doped material, comprising the following steps: (1) Weigh sodium chloride, potassium chloride and vanadium pentoxide according to mass ratio to prepare vanadium pentoxide solution; (2) Mix sodium chloride and potassium chloride evenly; (3) adding a mixture of sodium chloride and potassium chloride to the vanadium pentoxide solution and stirring to form an orange-red mixture; (4) The orange-red mixture is placed in an autoclave and heated to react to obtain HNKVOH (i.e., the dual-doping chemical formula HNa x K y V6O 16 ·4H2O) double-doped material.
[0023] The ion pre-insertion method is used to mix vanadium pentoxide, potassium chloride and sodium chloride and heat them to react to form HNKVOH dual-doped material. The HNKVOH material with abundant active sites is used as the positive electrode material of zinc ion battery. The sodium ions in HNKVOH significantly increase the interplanar spacing and diffusion channels of VOH, thereby effectively increasing the capacity of the positive electrode; and the pillar effect of KO bonds can effectively enhance the structural stability of VOH, thereby effectively increasing the cycle stability.
[0024] Example 1 An embodiment of the present invention provides a method for preparing a dual-doped material, comprising the following steps: 100. Weigh sodium chloride, potassium chloride and vanadium pentoxide in a mass ratio of 0.005:0.1:1.
[0025] 101. Add 0.182 g of vanadium pentoxide to 40 mL of a solution containing deionized water and 30 wt% hydrogen peroxide in a volume ratio of 40:1.
[0026] 102. Stir for 1 hour and heat at 35°C for 4 hours to obtain an orange-red vanadium pentoxide solution.
[0027] 103. Mix sodium chloride and potassium chloride evenly.
[0028] 104. Add a mixture of sodium chloride and potassium chloride into the vanadium pentoxide solution and stir for 25 minutes to form an orange-red mixture.
[0029] 105. The orange-red mixture is placed in an autoclave for heating reaction. The heating time is 6 hours and the heating temperature is 120° C. to obtain HNKVOH dual-doped material.
[0030] 106. The dual-doped material is repeatedly rinsed with deionized water and then dried at a temperature of 60° C. for 12 h to obtain a powder material.
[0031] like Figure 1 As shown, the dual-doped material is represented by the code HNKVOH-S2, and the diffraction peaks at 7.9°, 24.6°, 25.6°, 47.3°, and 50.7° correspond to HNaV6O 16 ·Characteristic peak of 4H2O (PDF#49-0996). “PDF#49-0996” is the X-ray diffraction card number of the material, corresponding to HNaV6O 16 Characteristic peaks of 4H2O (Powder Diffraction File, PDF# 49-0996).
[0032] like Figure 2 As shown by Figure 2 It can be seen that the HNKVOH material is composed of uniform and loose nanoribbons. HNaV6O 16 The lattice fringes of the (110) crystal plane corresponding to 4H2O.
[0033] The present invention uses CR2032 coin cells to test the electrochemical performance of the dual-doped HNKVOH material. When preparing the electrode, 70% HNKVOH active material, 20% Super P and 10% polyvinylidene fluoride (PVDF) are mixed and dispersed using N-methylpyrrolidone (NMP) to form a uniform slurry. Then, the slurry is coated on a titanium foil and dried under a vacuum environment at 60 °C for 12 h. The mass loading is about 1.8 mg cm -2When assembling zinc ion batteries, glass fiber is used as a separator, 3MZn(CF3SO3)2 is used as an electrolyte, and zinc foil is used as a counter electrode. All components are assembled into CR2032 type ZIBs in air. Cyclic voltammetry (CV) performance tests are performed using an electrochemical workstation with a scanning voltage range of 0.3-1.5 V. In the CV curve, two pairs of redox peaks can be clearly observed, located at 1.03 V / 0.96 V and 0.61 V / 0.51 V, corresponding to V 5+ / V 4+ and V 4+ / V 3+ The transformation, such as Figure 3 As shown. At 1 A g -1 At this current density, the battery capacity reaches 350.7 mAh g after 2 cycles. -1 After 100 cycles, the specific capacity remains at 319.3 mAh g -1 , the capacity retention rate is about 91%. Figure 4 These data indicate that the battery has excellent cycling stability and electrochemical performance.
[0034] In this embodiment, vanadium pentoxide, potassium chloride and sodium chloride are mixed and heated to react to form HNKVOH dual-doped material by ion pre-insertion method, and HNKVOH material with abundant active sites is used as positive electrode material of zinc ion battery. The sodium ions in HNKVOH significantly increase the interplanar spacing and diffusion channels of VOH, thereby effectively increasing the capacity of the positive electrode; and the pillar effect of KO bond can effectively enhance the structural stability of VOH, thereby effectively increasing the cycle stability.
[0035] Example 2 The embodiment of the present invention provides a second method for preparing a dual-doped material, comprising the following steps: 200. Weigh sodium chloride, potassium chloride and vanadium pentoxide in the mass ratio of 0.075:0.1:1.
[0036] 201. Add 0.182 g of vanadium pentoxide to 40 mL of a solution containing deionized water and 30 wt% hydrogen peroxide in a volume ratio of 40:1.
[0037] 202. Stir for 2 h and heat at 30 °C for 5 h to obtain an orange-red vanadium pentoxide solution.
[0038] 203. Mix sodium chloride and potassium chloride evenly.
[0039] 204. Add a mixture of sodium chloride and potassium chloride into the vanadium pentoxide solution and stir for 30 minutes to form an orange-red mixture.
[0040] 205. The orange-red mixture is placed in an autoclave for heating reaction. The heating time is 7 hours and the heating temperature is 110° C. to obtain HNKVOH dual-doped material.
[0041] 206. The dual-doped material is repeatedly rinsed with deionized water, and then dried at a temperature of 70° C. for 14 hours to obtain a powder material.
[0042] A mixture of vanadium pentoxide, potassium chloride and sodium chloride is chemically reacted in a high temperature and high pressure environment to obtain HNKVOH dual-doped material, which is denoted by the code HNKVOH-S1.
[0043] The diffraction peaks of HNKVOH-S1 and HNKVOH-S2 are very similar, but the diffraction peaks of HNKVOH-S1 are weaker than those of HNKVOH-S2. Referring to the method of Example 1, HNKVOH-S1 was used as the positive electrode material to assemble a zinc ion battery. The battery was heated to 1 A g -1 After running for 10 cycles at the same current density, the specific capacity reached 287.8 mAh g -1 ; After running 100 cycles, the capacity retention rate relative to the 10th cycle is about 82.9%.
[0044] Example 3 The embodiment of the present invention provides a third method for preparing a dual-doped material, comprising the following steps: 300. Weigh sodium chloride, potassium chloride and vanadium pentoxide in a mass ratio of 0.01:0.1:1.
[0045] 301. Add 0.182 g of vanadium pentoxide to 40 mL of a solution containing deionized water and 30 wt% hydrogen peroxide in a volume ratio of 40:1.
[0046] 302. Stir for 3 h and heat at 25 °C for 6 h to obtain an orange-red vanadium pentoxide solution.
[0047] 303. Mix sodium chloride and potassium chloride evenly.
[0048] 304. Add a mixture of sodium chloride and potassium chloride into the vanadium pentoxide solution and stir for 35 minutes to form an orange-red mixture.
[0049] 305. The orange-red mixture is placed in an autoclave for heating reaction. The heating time is 6 hours and the heating temperature is 130° C. to obtain HNKVOH dual-doped material.
[0050] 306. The dual-doped material is repeatedly rinsed with deionized water, and then dried at a temperature of 70° C. for 14 hours to obtain a powder material.
[0051] A mixture of vanadium pentoxide, potassium chloride and sodium chloride is chemically reacted in a high temperature and high pressure environment to obtain HNKVOH dual-doped material, which is denoted by the code HNKVOH-S3.
[0052] Referring to the method of Example 1, HNKVOH-S3 was used as the positive electrode material to assemble a zinc ion battery. -1 After running for 10 cycles at the same current density, the specific capacity reached 255.8 mAh g -1 ; After running 100 cycles, the capacity retention rate relative to the first cycle is about 78.6%.
[0053] Example 4 The embodiment of the present invention provides a fourth method for preparing a dual-doped material, comprising the following steps: 400. Weigh sodium chloride, potassium chloride and vanadium pentoxide in the mass ratio of 0.06:0.1:1.
[0054] 401. Add 0.182 g of vanadium pentoxide to 40 mL of a solution containing deionized water and 30 wt% hydrogen peroxide in a volume ratio of 40:1.
[0055] 402. Stir for 3 h and heat at 25 °C for 6 h to obtain an orange-red vanadium pentoxide solution.
[0056] 403. Mix sodium chloride and potassium chloride evenly.
[0057] 404. Add a mixture of sodium chloride and potassium chloride into the vanadium pentoxide solution and stir for 35 minutes to form an orange-red mixture.
[0058] 405. The orange-red mixture is placed in an autoclave for heating reaction. The heating time is 10 hours and the heating temperature is 110° C. to obtain HNKVOH dual-doped material.
[0059] 406. The dual-doped material is repeatedly rinsed with deionized water, and then dried at a temperature of 80° C. for 16 hours to obtain a powder material.
[0060] A mixture of vanadium pentoxide, potassium chloride and sodium chloride is chemically reacted in a high temperature and high pressure environment to obtain HNKVOH dual-doped material, which is denoted by the code HNKVOH-S4.
[0061] Referring to the method of Example 1, HNKVOH-S4 was used as the positive electrode material to assemble a zinc ion battery. -1 After running for 10 cycles at the same current density, the specific capacity reached 216.3 mAh g -1; After running 100 cycles, the capacity retention rate relative to the first cycle is about 68%.
[0062] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that the mass ratio of sodium chloride, potassium chloride and vanadium pentoxide is 0.1:0.001:1, and the chemical formula of the obtained dual-doped material is HNaV6O 16 4H2O, represented by the code HNVOH.
[0063] Referring to the method of Example 1, HNVOH was used as the positive electrode material, and a detailed X-ray diffraction (XRD) test and zinc ion battery performance evaluation were performed on it. The diffraction peaks of HNVOH at 8.0°, 24.3°, 25.5°, 47.3°, and 50.7° correspond to HNaV6O 16 The characteristic peaks of ·4H2O (PDF#49-0996) correspond to (100), (300), (011), (-421), and (031) crystal planes respectively; compared with HNKVOH, the peaks of HNVOH shift to higher angles, indicating a reduction in the interplanar spacing. This result may be due to the insertion of Na-O bonds into the matrix crystal structure in the HNKVOH sample. In contrast, the KO bond has a higher binding energy than Na-O, resulting in a larger interplanar spacing for HNVOH. In addition, there are no other impurity peaks in the XRD spectrum, confirming that HNVOH is composed of a single phase. Figure 5 As shown, it is used as the positive electrode material to assemble zinc-ion batteries at 1 A g -1 After running for 10 cycles at the same current density, the specific capacity reached 287 mAh g -1 After running 100 cycles, the capacity retention rate relative to the first cycle was about 41.8%. In Example 1, after the battery ran 2 cycles under the same conditions, the specific capacity reached 350.7 mAh g -1 After 100 cycles, the specific capacity remains at 319.3 mAh g -1 , the capacity retention rate of the second cycle is about 91%. Its specific capacity and capacity retention rate are significantly lower than those of Example 1.
[0064] This significant difference shows that the electrochemical performance of HNKVOH material is better than that of HNVOH material. The larger interplanar spacing and lower binding energy of HNVOH lead to a significant decrease in its specific capacity and capacity retention rate. Therefore, by introducing sodium and potassium ions into vanadium-based compounds at the same time, the electrochemical performance of the positive electrode material can be effectively improved, the specific capacity can be increased, and the cycle life can be improved. This comparison result demonstrates the superiority of the HNKVOH dual-doped material of the present invention in the application of zinc ion batteries.
[0065] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that the mass ratio of sodium chloride, potassium chloride and vanadium pentoxide is 0.001:0.1:1, and the chemical formula of the obtained dual-doped material is HKV6O 16 4H2O, represented by the code HKVOH.
[0066] Referring to the method of Example 1, HKVOH was used as the positive electrode material to assemble a zinc ion battery, such as Figure 6 As shown, the battery is at 1A g -1 After running for 2 cycles at the current density, the specific capacity reached 230 mAh g -1 After running 100 cycles, its specific capacity decreased significantly, and the capacity retention rate relative to the first cycle was about 66.5%. Its specific capacity and capacity retention rate were much lower than those in Example 1.
[0067] From the above examples 1 to 4 and comparative examples 1 and 2, it can be seen that in example 1, sodium chloride and potassium chloride are mixed and reacted to form HNKVOH dual-doped material by ion pre-insertion method. The dual-doping synergistic effect significantly increases the interplanar spacing and diffusion channel of VOH, thereby significantly increasing the capacity of the positive electrode. -1 After 20 cycles at the same current density, the battery capacity reaches 358 mAh g -1 In addition, the pillar effect of KO bond effectively enhances the structural stability of VOH, significantly improves the cycle stability, and the capacity retention rate is about 91%. Therefore, compared with other examples and comparative examples, Example 1 shows higher specific capacity and superior cycle performance, verifying the significant advantages of this technical path in improving battery performance.
[0068] On the other hand, an embodiment of the present invention further provides an application of a dual-doped material, wherein the dual-doped material is applied to a positive electrode material of a zinc ion battery and is used to be arranged in a positive electrode of the zinc ion battery.
[0069] The HNKVOH dual-doped material prepared by the present invention can be used as a positive electrode material for a zinc ion battery and has good electrical conductivity, high specific capacity and long cycle life.
[0070] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A dual-doped material, characterized in that: The invention is prepared from three materials: sodium chloride, potassium chloride and vanadium pentoxide, wherein the mass ratio of the sodium chloride, the potassium chloride and the vanadium pentoxide is in the range of (0.005-0.075):(0.1-0.15):
1.
2. The dual-doped material according to claim 1, characterized in that: Prepared by the following steps: (1) Weigh sodium chloride, potassium chloride and vanadium pentoxide according to mass ratio to prepare vanadium pentoxide solution; (2) Mix sodium chloride and potassium chloride evenly; (3) adding a mixture of sodium chloride and potassium chloride to the vanadium pentoxide solution and stirring to form an orange-red mixture; (4) The orange-red mixture is placed in an autoclave and heated to react to obtain the HNKVOH dual-doped material.
3. The dual-doped material according to claim 2, characterized in that: The step (1) further comprises the following steps: (1.1) adding vanadium pentoxide to a solution of deionized water and 30 wt% hydrogen peroxide in a volume ratio of 40:1; (1.2) stirring the solution and heating it at 25-35° C. for 4 to 6 hours to obtain an orange-red vanadium pentoxide solution.
4. The dual-doped material according to claim 3, characterized in that: The stirring time of the stirred solution is 1 h to 3 h.
5. The dual-doped material according to claim 2, characterized in that: In the step (3), the mixture of sodium chloride and potassium chloride is added to the vanadium pentoxide solution and stirred for 25 to 35 minutes.
6. The dual-doped material according to claim 2, characterized in that: The step (4) further includes the following steps: repeatedly washing the HNKVOH dual-doped material with deionized water, and obtaining a powder material after drying.
7. The dual-doped material according to claim 6, characterized in that: The drying temperature of the drying treatment is 60° C. to 80° C., and the drying time is 12 h to 16 h.
8. The dual-doped material according to claim 2, characterized in that: The heating time of the autoclave in step (4) is 6 to 10 hours.
9. The dual-doped material according to claim 8, characterized in that: The temperature range of heating the autoclave in step (4) is 110° C. to 130° C.
10. An application of the dual-doped material according to any one of claims 1 to 9, characterized in that: The dual-doped material is applied to the positive electrode material of a zinc ion battery and is arranged on the positive electrode of the zinc ion battery.
Citation Information
Patent Citations
Preparation method and application of double-ion doped vanadium pentoxide positive electrode material
CN110364726A
Preparation method of positive electrode material, water-based zinc ion battery positive electrode and application
CN113979473A
Co-doped material, preparation method and application thereof
CN118073550A