A large-size self-supporting diamond, its preparation method and application

By growing diamond films and depositing SiO2 dielectric layers on Ir/Sapphire heterostructure substrates, and defining circular hole array nucleation templates, the problems of difficult nucleation, high dislocation density, and thermal stress fracture of heteroepitaxial diamonds were solved by using lateral epitaxy and thermal stress self-exfoliation methods. Large-size self-supporting diamonds with low defect density were prepared, which are suitable for semiconductor materials.

CN123108736APending Publication Date: 2026-11-17HU-NAN NEW FRONTIER SCI & TECH LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611264376.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing heteroepitaxial diamond technology suffers from problems such as difficulty in nucleation, high dislocation density, metal contamination, and thermal stress fracture, leading to large-area fabrication failures and making it difficult to meet the needs of semiconductor industrial applications.

Method used

A method was adopted to grow diamond films on Ir/Sapphire heteroplanar substrates and deposit SiO2 dielectric layers. A circular hole array nucleation template was defined, and large-size self-supporting diamonds were prepared by lateral epitaxial growth and thermal stress self-exfoliation, avoiding the problems caused by metal masks and thermal mismatch.

Benefits of technology

This technology enables the fabrication of large-size self-supporting diamonds with low defect density, reducing dislocation density, avoiding metal contamination, simplifying substrate reuse, reducing costs, and meeting the requirements of high-performance electronic devices.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a large-size self-supporting diamond, its preparation method, and its applications. A diamond film is grown on the surface of an Ir / Sapphire heteroplanar substrate, followed by the deposition of a SiO2 dielectric layer on the diamond film surface. Then, a boundary layer is defined along the Ir... <110> A circular hole array region with periodically arranged crystal orientation is used to etch the SiO2 dielectric layer within the defined circular hole array region to obtain a circular hole array nucleation template. Then, diamond is grown laterally on the circular hole array nucleation template to obtain a large-size self-supporting diamond. The method provided by this invention is a heteroepitaxial method that can prepare inch-scale large-size single-crystal diamond wafers, breaking through the bottleneck of traditional high-temperature high-pressure methods or homoepitaxial methods that are limited by the seed crystal size. The preparation method described in this invention can significantly reduce the through dislocation density of the diamond epitaxial layer, so as to prepare high-quality crystals that meet the requirements of high-performance electronic devices.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of semiconductor materials and device processing, specifically relating to a large-size self-supporting diamond, its preparation method, and its application. Background Technology

[0002] Single-crystal diamond, due to its extremely wide bandgap, high room-temperature thermal conductivity, and excellent radiation resistance, is considered the ultimate semiconductor material for manufacturing next-generation deep ultraviolet detectors, high-power radio frequency devices, and nuclear radiation detectors in extreme environments. Due to the lack of large-area homogeneous seed crystals, the industry currently commonly uses chemical vapor deposition heteroepitaxial growth on Ir / Sapphire composite substrates to prepare wafer-level single-crystal diamond.

[0003] However, direct heteroepitaxial fabrication of diamond films faces three major bottlenecks: First, the film contains an extremely high density of through dislocations, which, as deep recombination centers, severely degrade carrier lifetime. Second, traditional dislocation reduction methods often employ metal (such as Al or Fe) masks for selective growth, but this introduces transition metal impurities into the strong microwave plasma environment, and the surface of the Ir substrate after mask patterning exhibits severe electric field distortion, making bias-enhanced nucleation exceptionally difficult and resulting in extremely low process tolerance. Third, there is a significant thermal mismatch between diamond and the Sapphire substrate, which can easily lead to uncontrolled film rupture during cooling, resulting in large-area fabrication failures. Summary of the Invention

[0004] Addressing the technical challenges of nucleation difficulties, high dislocation density, metal contamination, and thermal stress fracture in existing heteroepitaxial diamond technology, the first objective of this invention is to provide a method for preparing large-size self-supporting diamond. The method provided by this invention is a heteroepitaxial method capable of preparing inch-scale large-size single-crystal diamond wafers, overcoming the bottleneck of traditional high-temperature high-pressure (HPHT) or homoepitaxial methods limited by seed crystal size. Specifically, the goal is to achieve the direct synthesis of single-crystal diamond wafers ranging from 2 inches to 4 inches and even larger, meeting the basic requirements for substrate size in semiconductor industrial applications. Simultaneously, the preparation method of this invention can significantly reduce the penetration dislocation density in the diamond epitaxial layer, thereby producing high-quality crystals that meet the requirements of high-performance electronic devices. Specifically, the dislocation density of heteroepitaxial diamond is reduced from the typical 10-1... 8 -10 9 cm -2 The magnitude was reduced to 10. 6 -10 7 cm -2 Its scale allows its crystal quality to be comparable to high-quality HPHT or homoepitaxial diamond.

[0005] The second objective of this invention is to provide large-size self-supporting diamond wafers prepared by the above-described method, capable of controllable and low-damage self-exfoliation, thus solving the problem that diamond, due to its extremely high hardness, is difficult to completely separate from heterogeneous substrates using traditional mechanical or chemical methods. This objective aims to utilize the difference in thermal expansion coefficients between materials, generating directional thermal stress during cooling through process design, thereby promoting the automatic and complete exfoliation of the diamond epitaxial layer from the substrate. Its technical advantages include: avoiding the problems of low efficiency, fragility, and high material loss associated with mechanical processing such as laser cutting; directly obtaining ultra-thin, such as 100-micron-level thickness, complete self-supporting diamond wafers to meet the specific application requirements of X-ray lenses, detectors, etc.; and the potential for this process to allow expensive heterogeneous substrates to be reused without polishing, simplifying the process and reducing costs.

[0006] A third objective of this invention is to provide applications for large-size self-supporting diamonds prepared by the above-described method. The large-size self-supporting diamonds provided by this invention are generally applicable to semiconductor materials.

[0007] To achieve the aforementioned objective of fabricating large-size, low-defect-density, and self-supporting single-crystal diamond wafers, the technical solution adopted in this invention is as follows:

[0008] This invention discloses a method for preparing large-size self-supporting diamond, comprising growing a diamond film on the surface of an Ir / Sapphire heteroplanar substrate, followed by depositing a SiO2 dielectric layer on the surface of the diamond film; and then defining a layer along the Ir on the SiO2 dielectric layer. <110> A circular hole array region with periodically arranged crystal orientation is used to etch the SiO2 dielectric layer in the defined circular hole array region to obtain a circular hole array nucleation template. Then, diamond is grown laterally on the circular hole array nucleation template to obtain a large-size self-supporting diamond.

[0009] The preparation method of this invention utilizes the pre-growth of an initial diamond film on a flat heterogeneous substrate to avoid nucleation minefields, and uses SiO2 deposition as a hard mask to guide lateral epitaxy, thereby realizing the preparation of large-area high-quality single-crystal diamond and stress self-exfoliation. The use of an insulating mask avoids metal impurity contamination, and the lateral growth promotes dislocation bending and annihilation. Furthermore, the method cleverly utilizes interfacial thermal mismatch to achieve automatic exfoliation of high-quality thick films, demonstrating good engineering feasibility.

[0010] In a preferred embodiment, the thickness of the bottom metal Ir film in the Ir / Sapphire heteroplanar substrate is 100 nm to 300 nm.

[0011] In this invention, the process of obtaining the Ir / Sapphire heteroplanar substrate can be carried out using existing conventional techniques. First, a single-crystal sapphire substrate with the (11-20) crystal orientation is selected, which is the standard orientation for epitaxial (100) oriented Ir thin films. Then, an Ir thin film is formed by deposition. Before depositing the Ir thin film, the sapphire substrate must be annealed in air at 1000-1400℃ for 10-15 hours to obtain an atomically flat surface. Then, the Ir thin film is deposited using a magnetron sputtering system. The deposition process is as follows: base vacuum: ≤2×10 -6 In an argon atmosphere, the cavity pressure is approximately 0.1-1 Pa, and the temperature of the sapphire substrate is controlled at 600-900℃.

[0012] The preferred method for growing a diamond film on an Ir / Sapphire heteroplanar substrate is as follows: The Ir / Sapphire heteroplanar substrate is placed in an MPCVD chamber, and a mixed atmosphere of methane and hydrogen is introduced. The volume concentration of methane in the mixed atmosphere is controlled to be 0.5% to 5%. First, bias-enhanced nucleation is performed for 5 to 60 minutes under a negative bias voltage of -200V to -300V. Then, the bias voltage is turned off, and the volume concentration of methane in the mixed atmosphere is adjusted to 0.5% to 8%. Finally, the diamond film is grown under the conditions of microwave power of 1.5 to 6kW, gas pressure of 5 to 15kPa, and growth time of 3 to 10 hours.

[0013] In a preferred embodiment, the thickness of the diamond film is 40~80μm.

[0014] In a preferred embodiment, a SiO2 dielectric layer is deposited on the surface of a diamond film using a pure SiO2 target by magnetron sputtering.

[0015] In a preferred embodiment, the thickness of the SiO2 dielectric layer is 200nm to 800nm, preferably 300nm to 500nm.

[0016] In a preferred embodiment, after magnetron sputtering, the SiO2 dielectric layer is annealed at 300℃~400℃ for 30 min~2 h. Annealing increases the density of the SiO2 dielectric layer and enhances its stability in the subsequent high-temperature hydrogen plasma environment.

[0017] In a preferred embodiment, the etching process uses a mixture of fluorine-containing gas and Ar gas, wherein the fluorine-containing gas is selected from CF4 and / or CHF3. During etching, only the SiO2 dielectric layer is etched to avoid damage to the diamond film.

[0018] In a preferred embodiment, in the circular hole array core template, the line connecting the centers of any adjacent holes is parallel to the underlying metal Ir film. <110> Crystal orientation. By controlling the line connecting the centers of any two adjacent holes to be parallel to the underlying Ir metal film. <110> Crystal orientation ensures that the {111} side crystal planes can achieve seamless stitching when the diamond grains are laterally closed.

[0019] In a preferred embodiment, the diameter of a single circular hole in the circular hole array nucleation template is 5μm to 15μm, and the center-to-center distance between adjacent circular holes is 15μm to 30μm.

[0020] In a preferred embodiment, the lateral epitaxial growth of diamond is performed using MPCVD technology, with the microwave power controlled at 3–5 kW, the cavity gas pressure at 10–20 kPa, and a mixture of hydrogen and methane introduced, controlling the volume concentration of methane in the mixture to be 2–8%. After lateral epitaxial growth under the above-mentioned unbiased conditions for a period of time, large-size self-supporting diamonds are obtained.

[0021] Further optimization involves stopping the CH4 supply after the lateral epitaxial growth of diamond and cooling it at a rate of ≥40°C in a pure H2 plasma atmosphere. When the temperature drops to 200–600°C, large-sized self-supporting diamonds with cleavage separation are obtained. After cooling by turning off the microwave, due to the huge difference in thermal expansion coefficients between SiO2, Sapphire, and diamond, extremely high local tensile stress is generated at the diamond bridging points within the pores, prompting the high-quality top diamond film to automatically cleave and separate from the inferior bottom layer.

[0022] A second objective of this invention is to provide large-size self-supporting diamonds prepared by the above-described preparation method.

[0023] The third objective of this invention is to provide an application for the large-size self-supporting diamond prepared by the above-described preparation method, wherein the large-size self-supporting diamond is used as a semiconductor material in at least one of deep ultraviolet / solar-blind ultraviolet detectors, nuclear radiation detectors, and electronic devices, preferably nuclear radiation detectors.

[0024] The positive effects of this invention are as follows:

[0025] Perfectly avoiding the pitfalls of BEN: The process abandons the extremely challenging technique of bias nucleation on porous Ir metal surfaces, instead performing nucleation on a flat substrate and directly growing the film within pores containing diamond seed crystals. This results in exceptional process stability and high tolerance for equipment requirements.

[0026] Zero metal contamination ensures electronic-grade purity: No metals such as Al or Fe are used as etching or growth masks throughout the process. The SiO2 hard mask not only effectively blocks the formation of impurities, but also has no deep-level metal contamination, meeting the material requirements of high signal-to-noise ratio radiation detectors.

[0027] Efficient dislocation filtering and thermal stress self-exfoliation: The ELO lateral growth mechanism reduces the dislocation density of diamond by 2-3 orders of magnitude; at the same time, it cleverly turns the disadvantage of thermal mismatch of sapphire into an advantage, and utilizes the stress concentration effect of the patterned dielectric layer to achieve non-destructive automatic exfoliation, saving the high cost of laser cutting and greatly promoting the industrialization process of large-area single crystal diamond. Detailed Implementation

[0028] The present invention is further described in conjunction with the embodiments, but is not intended to limit the invention in any way. Any modifications or alterations made to the present invention that are easily achievable by those skilled in the art without departing from the technical solutions of the present invention shall fall within the scope of the claims of the present invention.

[0029] The specifications of the key equipment and materials involved in the embodiments are as follows.

[0030] MPCVD System Core Specifications

[0031] The bias-enhanced nucleation, longitudinal growth, and lateral epitaxial growth steps in this embodiment were all performed in a microwave plasma chemical vapor deposition (MPCVD) system.

[0032] Core parameters:

[0033] Microwave source: frequency 2.45GHz, maximum output power ≥5kW.

[0034] Vacuum system: Base vacuum level can reach 10 -4 Pa or 10 -6 Torr.

[0035] Process pressure range: 6~500 Torr

[0036] Temperature control: Equipped with an infrared thermometer, with a temperature measurement range of 475~1475℃.

[0037] Gas path system: equipped with at least five gas paths: H2, CH4, N2, O2 and Ar, and equipped with a mass flow controller (MFC) to achieve precise flow control at the sccm level.

[0038] Key accessory: Bias power supply with an output range of -500V to +500V for implementing BEN processes.

[0039] Cavity and sample stage: The cavity is a stainless steel cylindrical structure with a water-cooling jacket, and the sample stage is made of molybdenum (Mo).

[0040] Composite substrate (Ir / Sapphire)

[0041] Sapphire substrate: A single-crystal sapphire substrate with the a-plane, i.e. (11-20) crystal orientation, is used. The orientation of the Ir film is (100). In the pretreatment: before depositing the Ir film, the sapphire substrate must be annealed in air at 1000-1400℃ for 10-15h to obtain an atomically flat surface, and then the Ir film is deposited.

[0042] Deposition equipment: Ir thin films are deposited using a magnetron sputtering system.

[0043] Deposition process: Base vacuum: ≤2×10 -6 Pa, working atmosphere and pressure: Ar atmosphere, cavity pressure approximately 0.1-1 Pa. Substrate temperature: 600-900℃; film thickness: 100-300 nm.

[0044] Specifications for fabrication of patterned SiO2 masks:

[0045] The fabrication of patterned masks used for ELO involves thin film deposition and pattern etching.

[0046] SiO2 dielectric layer deposition:

[0047] Deposition equipment: Magnetron sputtering equipment is used, with a deposition thickness of 200nm to 800nm.

[0048] Photolithography patterning:

[0049] Photoresist: Positive photoresist is selected.

[0050] Patterning process: The mask window is formed using standard ultraviolet lithography. Key patterning parameters are: window width 10µm, mask strip width 5µm. These dimensions can be precisely achieved through photolithography.

[0051] Etching process:

[0052] Reactive ion etching (RIE) is employed.

[0053] Example 1

[0054] Cleaning a 10×10mm piece 2 An Ir(100) / Sapphire(11-20) heteroepitaxial substrate was placed in an MPCVD chamber. A mixture of methane and hydrogen was introduced, with the volume concentration of methane in the mixture controlled at 1.5%. Unhindered planar bias-enhanced nucleation was performed at 800°C for 15 min under a DC bias of -250V. Subsequently, the bias was turned off, and a mixture of CH4 and hydrogen was introduced, with the volume percentage of CH4 in the mixture at 4%. The growth was carried out at 850~900°C for 6 h under a pressure of 10 kPa to obtain a continuous initial diamond film with a thickness of 60 μm.

[0055] The sample was removed and placed in a magnetron sputtering apparatus. Using a high-purity SiO2 target, a 500nm thick SiO2 dielectric layer was deposited on the diamond surface. The sample was then annealed in a 400℃ oven for 1 hour to densify it and form a hard mask. Positive photoresist was spin-coated, and the Ir film was developed and set using a photolithography machine. <110> An array of circular holes with a diameter of 10 μm and a center-to-center distance of 20 μm was formed. Deep reactive ion etching (DRIE) was performed on the exposed SiO2 using an etching machine, with a mixture of CF4 and Ar gas introduced. The etching stopped when the laser endpoint indicated the carbon layer had been reached. The photoresist was then washed away, completing the fabrication of the patterned nucleation template. This template was then placed back into the MPCVD chamber for unbiased lateral epitaxial growth. A mixture of CH4 and hydrogen gas (CH4 volume percentage 5%) was introduced, along with 0.02 sccm N2 and 2 sccm O2. Growth was carried out at 880°C and 11.3 kPa for 20 hours until fusion. After growth, the microwave source was cut off, and the CH4 supply was stopped. The sample was cooled to 400°C at a rate of 50°C / min using a water-cooled tray. Utilizing the significant thermal stress caused by Sapphire contraction, the high-quality diamond film at the top layer automatically fractured at the neck of the micro-hole connection, achieving self-supporting separation from the primary nucleation layer, ultimately yielding a self-supporting wafer with a thickness of 250 µm. The wafer was systematically characterized for crystal quality and mechanical properties, and the results are as follows:

[0056] Raman spectroscopy: The characteristic peak of diamond is located at 1332.5 cm⁻¹. -1 Its half-width at half-height (FWHM) is only 4.0cm. -1 X-ray diffraction (XRD) rocking curve:

[0057] Diamond (004) crystal face: half width at half maximum (FWHM) of the rocking curve is 0.39°.

[0058] Diamond (311) crystal plane: Half-width at half-maximum (FWHM) of 0.69°. Dislocation density: Dislocation density is effectively filtered and reduced through the ELO lateral growth mechanism. The estimated dislocation density of the diamond wafer obtained in this embodiment is approximately 1.0 × 10⁻⁶. 7 cm -2 Residual stress: Calculated by Raman spectral peak shift, the residual stress inside the wafer is extremely low, only 0.002 GPa.

[0059] Example 2: High-energy-resolution single-crystal diamond detector for nuclear radiation detection.

[0060] This embodiment is basically the same as Embodiment 1, except that after lateral epitaxial growth, the obtained self-supporting single-crystal diamond is cut, polished, and fabricated into a detector. Specific supplementary steps are as follows:

[0061] Preparation of self-supporting diamond: Following the parameters of Example 1, in a 10×10 mm...2 Diamond films were prepared on Ir(100) / Sapphire(11-20) substrates, with the growth time controlled to 5h. Finally, self-supported single-crystal diamond with a thickness of about 50μm was obtained by thermal stress self-exfoliation.

[0062] Detector fabrication: Self-supporting diamond was cut into 4.5mm × 4.5mm square samples and polished on both sides. Au (200nm) / Cr (50nm) electrode layers were deposited on the upper and lower surfaces of the diamond using magnetron sputtering to form a sandwich-structured MSM (metal-semiconductor-metal) detector. The electrode area was 4mm × 4mm.

[0063] Test conditions: using 241 The Amα particle source was used to test the detector's performance.

[0064] Measured performance parameters:

[0065] Dark current: At a bias voltage of 300V, the dark current is 0.35nA.

[0066] Energy resolution: at a bias voltage of 300V, for 241 The energy resolution of Amα particles reached 4.5%.

[0067] Charge collection efficiency: At a bias voltage of 300V, the charge collection efficiency reaches 93.5%.

[0068] Time response: Under a 300V bias voltage, the rise time of the pulse signal is 1.7ns and the fall time is 2.5ns.

[0069] Pulse amplitude: At a bias voltage of 200V, the pulse amplitude reaches 92mV.

[0070] Example 3: High-performance detector for 14.1 MeVD-T fusion neutron detection

[0071] This embodiment is basically the same as Embodiment 2, but adopts a different electrode structure design to optimize neutron detection performance.

[0072] Preparation of self-supporting diamond: Following the parameters of Example 1, except that the growth time was controlled to 50h, a self-supporting single crystal diamond with a thickness of about 500μm was prepared and cut into square samples of 4.5mm×4.5mm.

[0073] Detector fabrication: A sandwich structure is constructed using a flat gold electrode and an orbital gold electrode. One electrode covers the entire lower surface, while the other electrode is designed as an orbital on the upper surface to optimize the electric field distribution and improve charge collection efficiency.

[0074] Test conditions: Tested at a 14.1 MeVD-T fusion neutron source, with a flux of approximately 7.5 × 10⁻⁶. 5 / (s·cm 2 The applied bias electric field strength is 30kV / cm.

[0075] Measured performance parameters:

[0076] Dark current: Under an electric field of 30 kV / cm, the dark current is less than 0.15 nA.

[0077] Energy resolution: for ¹²C(n,α0) 9 The energy resolution of the Be reaction characteristic peak (center energy approximately 8.28 MeV) is better than 2.5%.

[0078] Characteristic peak clarity: A clear and independent 8.28 MeV characteristic peak was successfully observed, with an intensity much higher than that of the neutron elastic / inelastic scattering peak, indicating that the detector has excellent particle discrimination capability.

[0079] Comparative Example 1: Nucleation directly on a patterned Ir substrate using the traditional BEN method

[0080] The difference from Example 1 is that all other conditions are exactly the same as in Example 1, but in the preparation process, the step of first growing a planar diamond film and then depositing a SiO2 dielectric layer is not used. Instead, bias-enhanced nucleation (BEN) is performed directly on an Ir / Sapphire substrate with a circular hole array nucleation template according to the conventional method.

[0081] result:

[0082] Nucleation failure: In the circular aperture array region, due to electric field distortion, the plasma distribution is extremely uneven, resulting in low diamond nucleation density and disordered distribution, making it impossible to form a uniform and continuous epitaxial layer.

[0083] Impurities and contamination: A large number of unexpected polycrystalline diamond or non-diamond carbon phases also appeared on the SiO2 mask in the non-circular hole area, which made subsequent lateral epitaxial growth impossible.

[0084] Low process tolerance: Repeated experiments have confirmed that the process is extremely sensitive to parameters such as bias voltage, power, and gas pressure, making it difficult to stably reproduce and resulting in an extremely narrow process window.

Claims

1. A method for preparing large-size self-supporting diamond, characterized in that: A diamond film was grown on an Ir / Sapphire heteroplanar substrate, followed by the deposition of a SiO2 dielectric layer on the diamond film surface; then, a boundary layer was defined along the Ir direction on the SiO2 dielectric layer. <110> A circular hole array region with periodically arranged crystal orientation is used to etch the SiO2 dielectric layer in the defined circular hole array region to obtain a circular hole array nucleation template. Then, diamond is grown laterally on the circular hole array nucleation template to obtain a large-size self-supporting diamond.

2. The method for preparing large-size self-supporting diamond according to claim 1, characterized in that: In the Ir / Sapphire heteroplanar substrate, the thickness of the bottom metal Ir film is 100nm to 300nm.

3. A method for preparing large-size self-supporting diamond according to claim 1 or 2, characterized in that: The process of growing diamond films on Ir / Sapphire heteroplanar substrates is as follows: The Ir / Sapphire heteroplanar substrate is placed in an MPCVD chamber, and a mixed atmosphere of methane and hydrogen is introduced. The volume concentration of methane in the mixed atmosphere is controlled to be 0.5% to 5%. First, bias-enhanced nucleation is performed for 5 to 60 minutes under a negative bias voltage of -200V to -300V. Then, the bias voltage is turned off, and the volume concentration of methane in the mixed atmosphere is adjusted to 0.5% to 8%. Then, diamond films are grown under the conditions of microwave power of 1.5 to 6kW, gas pressure of 5 to 15kPa, and growth time of 3 to 10h. The thickness of the diamond film is 40~80μm.

4. The method for preparing large-size self-supporting diamond according to claim 1, characterized in that: A SiO2 dielectric layer was deposited on the surface of a diamond thin film using a pure SiO2 target via magnetron sputtering. The thickness of the SiO2 dielectric layer is 200nm to 800nm.

5. The method for preparing a large-size self-supporting diamond according to claim 4, characterized in that: After magnetron sputtering, anneal at 300℃~400℃ for 30min~2h.

6. The method for preparing a large-size self-supporting diamond according to claim 1, characterized in that: The etching process uses a mixture of fluorine-containing gas and Ar gas, wherein the fluorine-containing gas is selected from CF4 and / or CHF3.

7. The method for preparing large-size self-supporting diamond according to claim 1, characterized in that: In the circular hole array core template, the line connecting the centers of any adjacent holes is parallel to the underlying metal Ir film. <110> Crystal orientation; In the circular hole array nucleation template, the diameter of a single circular hole is 5μm to 15μm, and the center-to-center distance between adjacent circular holes is 15μm to 30μm.

8. The method for preparing large-size self-supporting diamond according to claim 1, characterized in that: During the lateral epitaxial growth of diamond, the MPCVD process is used, the microwave power is controlled at 3-5kW, the cavity gas pressure is controlled at 10-20kPa, and a mixture of hydrogen and methane is introduced, with the volume concentration of methane in the mixture controlled at 2-8%.

9. A method for preparing large-size self-supporting diamond according to claim 1 or 8, characterized in that: After the transverse epitaxial growth of diamond is completed, the CH4 supply is stopped, and the diamond is cooled at a rate of ≥40℃ in a pure H2 plasma atmosphere. When the temperature drops to 200-600℃, large-size self-supporting diamonds with cleavage separation are obtained.

10. A large-size self-supporting diamond prepared by the preparation method according to claim 1 or 2.

11. The application of a large-size self-supporting diamond prepared by the preparation method according to claim 1 or 2, characterized in that: The large-size self-supporting diamond is used as a semiconductor material in at least one of deep ultraviolet / solar-blind ultraviolet detectors, nuclear radiation detectors, and electronic devices.