Methods to enhance bonding strength, back-illuminated chips and their fabrication methods, integrated chips

By forming a reinforced metal layer on the back side of the back-illuminated chip and electrically connecting it to the pads, the reliability problem of back-illuminated chips during wire bonding is solved, and the mechanical strength of the pads is significantly improved and the structural reliability is enhanced.

CN123124471APending Publication Date: 2026-11-17THE 44TH INST OF CHINA ELECTRONICS TECH GROUP CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611427283.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-15
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In back-illuminated chips, insufficient metal thickness during wire bonding leads to reliability issues such as pad burn-through, cracking, solder ball detachment, and pad peeling, which existing technologies have not been able to effectively resolve.

Method used

A reinforcing metal layer electrically connected to the pads is formed on the back side of the wafer to form a reinforcing pad structure. The oxide layer and primary metal of the pad area are exposed by local etching, and a reinforcing metal layer is formed on it to enhance the mechanical strength of the pad.

Benefits of technology

It significantly improves the tensile strength of wire bonding of pads, solves reliability problems such as pad burn-through, tearing, solder ball detachment and pad peeling, ensures structural reliability, and is highly compatible with existing mass production processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124471A_ABST
    Figure CN123124471A_ABST
Patent Text Reader

Abstract

This invention discloses a method for enhancing bonding strength, a back-illuminated chip and its fabrication method, and an integrated chip. The method for enhancing bonding strength involves forming a reinforcing metal layer electrically connected to the pads on the back side of the wafer. The reinforcing metal layer and the pads together constitute reinforced pads with enhanced bonding strength. By forming a reinforcing metal layer electrically connected to the pads on the back side of the wafer, this invention significantly increases the thickness and mechanical strength of the pads, improves the tensile strength of the pad-to-pad bonding, and fundamentally solves reliability problems such as pad burn-through, tearing, solder ball detachment, and pad peeling during wire bonding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of semiconductor technology, and in particular to a method for enhancing bonding strength, a back-illuminated chip and its fabrication method, and an integrated chip. Background Technology

[0002] To expand the functionality and improve the performance of individual chips, the current mainstream technology employs inter-chip interconnection and integration. This involves using specific integration methods to interconnect and integrate different functional chips, forming integrated chips with expanded functionality and higher performance. Inter-chip interconnection and integration is a trend in semiconductor development, with image sensors representing a particularly strong demand and rapid technological advancement. For image sensor interconnection and integration, the photosensitive chip needs to be integrated with other functional chips (such as ADCs (analog-to-digital converters), memory, etc.) in a back-illuminated manner.

[0003] In traditional back-illuminated chips, during the back-side fabrication process, the front side of the target wafer is temporarily bonded to a carrier wafer using adhesive (serving as a support). This way, after the target wafer is thinned to the epitaxial layer thickness, the carrier wafer provides fixation and mechanical support. To achieve packaging, the epitaxial layer, several tens of micrometers thick, is etched away from the bond pads on the target wafer, exposing the primary metal on the front side to serve as the bonding pads for wire bonding.

[0004] The primary metal on the front side of the target wafer, which serves as the bonding pad, has a thickness of approximately 0.5-1.5 μm due to process limitations. Furthermore, the front side is fixed to the carrier wafer using temporary bonding adhesive. During wire bonding of the target wafer, failures such as the primary metal bonding pad being crushed by the cleaver bonding force, the bonding pad being torn when the cleaver retracts, the bonding pad being torn during tensile testing, and solder ball detachment may occur. These failures result in reliability issues such as low chip package connectivity, pad peeling, and insufficient bonding strength.

[0005] Because the aforementioned back-illumination process has potential reliability issues during wire bonding of bonding pads, existing technologies typically improve connectivity by reducing wire bonding force and performing multiple resoldering operations after desoldering. However, these methods fail to fundamentally solve the problem of the limitation of primary metal force on bonding pads. Summary of the Invention

[0006] In view of the shortcomings of the prior art, the technical problem to be solved by the present invention is to provide a method and structure for enhancing the bonding strength of back-illuminated chips that can fundamentally solve the problem of primary metal stress limitation of the pads.

[0007] To solve the above-mentioned technical problems, one technical solution adopted by the present invention is to provide a method for enhancing bonding strength: forming a reinforcing metal layer electrically connected to the pads on the back side of the wafer, wherein the reinforcing metal layer and the pads together constitute a reinforcing pad with enhanced bonding strength.

[0008] Furthermore, this includes the following steps: The epitaxial layer on the back side of the wafer is partially etched to expose the oxide layer in the pad area; The oxide layer is partially etched to expose the primary metal of the solder pads; A reinforcing metal layer is formed on the exposed area of ​​the primary metal, and the reinforcing metal layer and the primary metal together constitute the reinforcing structure of the reinforcing pad.

[0009] Furthermore, in the step of locally etching the oxide layer to expose the primary metal of the pad: the etching area of ​​the oxide layer is smaller than the area of ​​the primary metal, and an oxide layer of a predetermined width is retained in the edge region of the primary metal; the central region of the primary metal serves as an exposed area for electrical connection with the reinforcing metal layer.

[0010] Furthermore, the step of forming a reinforcing metal layer on the exposed area of ​​the primary metal includes the following sub-steps: A metal layer is formed on the back side of the wafer; The metal layer is partially etched to retain the metal layer located on the exposed area of ​​the primary metal, which serves as the reinforcing metal layer.

[0011] Furthermore, the reinforcing metal layer is at least one layer.

[0012] Furthermore, the preset width of the oxide layer retained in the edge region of the primary metal is 2μm to 10μm, and the thickness of the reinforcing metal layer is 1μm to 3μm.

[0013] Furthermore, the thickness of the reinforcing structure is greater than or equal to 3 μm, and the wire bonding tensile strength of the reinforcing pad is greater than or equal to 10 gf.

[0014] To solve the above-mentioned technical problems, another technical solution adopted by the present invention is: to provide a method for fabricating a back-illuminated chip, comprising the following steps: A target wafer is provided, wherein the front-side manufacturing process has been completed and pads are formed on the front side; The front side of the target wafer is bonded to the support carrier using an adhesive layer; The back side of the target wafer is thinned to remove the substrate; The method described above for enhancing bonding strength is used to form a reinforcing metal layer electrically connected to the pads on the back side of the target wafer.

[0015] To solve the above-mentioned technical problems, another technical solution adopted by the present invention is to provide a back-illuminated chip, which is prepared by the back-illuminated chip preparation method.

[0016] To solve the above-mentioned technical problems, another technical solution adopted by the present invention is to provide an integrated chip, including the back-illuminated chip.

[0017] The method for enhancing bonding strength, the back-illuminated chip and its fabrication method, and the integrated chip of the present invention have at least the following beneficial effects: (i) Significantly improved mechanical strength of the pads. By forming a reinforced metal layer on the back of the wafer that is electrically connected to the primary metal, the tensile strength of the pad wire bonding is improved, fundamentally solving reliability problems such as pad burn-through, tearing, solder ball detachment, and pad peeling during wire bonding.

[0018] (ii) Dual reinforcement mechanism ensures structural reliability. On the one hand, the reinforcement metal layer and the primary metal are stacked and bonded together in the vertical direction to form a reinforcement structure, which greatly increases the ability of the pad to withstand bonding pressure. On the other hand, the edge area of ​​the primary metal is covered and clamped by the oxide layer, which effectively constrains the displacement of the primary metal edge and prevents it from lifting or peeling off during bonding. The two mechanisms work together to enhance the pad's resistance to damage.

[0019] (iii) Strong process compatibility, suitable for mass production. This method is implemented based on the existing back-illuminated chip process flow. Each step adopts mature etching, deposition and photolithography technologies in the wafer field, which are highly compatible with existing mass production processes, have low implementation costs and are easy to promote and apply. Attached Figure Description

[0020] The accompanying drawings, which are included to provide a further understanding of this application and form part of this application, illustrate exemplary embodiments and are used to explain this application, but do not constitute an undue limitation of this application. In the drawings: Figure 1 This is a flowchart of one embodiment of the method for enhancing bond strength according to the present invention.

[0021] Figure 2 This is a cross-sectional schematic diagram of the wafer to be processed in one embodiment of the method for enhancing bonding strength according to the present invention.

[0022] Figure 3 This is a cross-sectional schematic diagram of the structure obtained in step S410 of one embodiment of the method for enhancing bond strength of the present invention.

[0023] Figure 4 This is a cross-sectional schematic diagram of the structure obtained in step S420 of one embodiment of the method for enhancing bond strength of the present invention.

[0024] Figure 5 for Figure 1 Flowchart of step S430.

[0025] Figure 6 This is a cross-sectional schematic diagram of the structure obtained in step S431 of one embodiment of the method for enhancing bond strength of the present invention.

[0026] Figure 7 This is a cross-sectional schematic diagram of the structure obtained in step S432 of one embodiment of the method for enhancing bond strength of the present invention.

[0027] Figure 8 This is a flowchart of one embodiment of the back-illuminated chip fabrication method of the present invention.

[0028] Figure 9 This is a cross-sectional schematic diagram of the structure obtained in step S100 in one embodiment of the back-illuminated chip fabrication method of the present invention.

[0029] Figure 10 This is a cross-sectional schematic diagram of the structure obtained in step S200 in one embodiment of the back-illuminated chip fabrication method of the present invention.

[0030] Figure 11 This is a cross-sectional schematic diagram of the structure obtained in step S300 in one embodiment of the back-illuminated chip fabrication method of the present invention.

[0031] Figure 12 This is a cross-sectional schematic diagram of one embodiment of the back-illuminated chip of the present invention.

[0032] The meanings of the labels in the attached diagram are as follows: Substrate 101, epitaxial layer 102, oxide layer 103, primary metal 104, metal hole 105, top metal 106, adhesive layer 201, support carrier 202, first cavity 501, second cavity 601, metal layer 701, and reinforcing metal layer 801. Detailed Implementation

[0033] The following disclosure provides various different embodiments or examples for implementing different features of the invention. Specific examples will be described below to simplify the invention. Of course, these are merely examples and are not intended to limit the invention. For example, in the following description, forming a first component above or on a second component may include embodiments where the first and second components are in direct contact, or embodiments where other components may be formed between the first and second components such that the first and second components are not in direct contact. Furthermore, reference numerals and / or characters may be repeated in various instances of the invention. Such repetition is for simplification and clarity and does not in itself indicate a relationship between the various embodiments and / or configurations.

[0034] Furthermore, spatial relation terms such as "below," "under," "below," "above," and "above" may be used herein to readily describe the relationship between one element or component and another element (or component) or component (or component) as shown in the figure. In addition to the orientations shown in the figure, spatial relation terms will encompass various different orientations of the device in use or operation. The device may be positioned in other ways (rotated 90 degrees or in other orientations) and will be interpreted accordingly through the spatial relation descriptors used herein.

[0035] Although the numerical ranges and parameter settings presented in this invention are approximations, the numerical settings in specific instances are reported as precisely as possible. Any numerical value, however, inherently contains certain inevitable errors arising from the standard deviation found in the respective test measurements. Similarly, as used herein, the term "about" generally refers to within 10%, 5%, 1%, or 0.5% of a given value or range. Alternatively, the term "about" means within an acceptable average standard error that can be conceived by one of ordinary skill in the art. Except in instances of operation / work, or unless expressly stated otherwise, all numerical ranges, totals, values, and percentages, such as those for material quantities, durations, temperatures, operating conditions, amounts, and other similarities disclosed herein, should be understood to be modified by the term "about" in all cases. Therefore, unless otherwise stated, the numerical parameter settings set forth in this invention and the appended claims are approximations that can be changed upon request. At a minimum, each numerical parameter should be interpreted based on the number of significant figures reported and the application of ordinary rounding techniques. A range herein may be expressed as from one endpoint to another or between two endpoints. All scopes disclosed herein include endpoints unless otherwise stated.

[0036] Furthermore, the technical parts described in this invention and the appended claims are primarily the improved technical parts of this invention, and do not limit the object protected by this invention to only having these technical parts. Other known essential components (structures and / or methods) and / or non-essential components of the object protected, besides the technical parts described in this invention and the appended claims, are not included in this invention and the appended claims because they do not fall within the scope of improvements of this invention; however, this does not mean that the object protected by this invention does not possess these known components.

[0037] In this invention, for ease of description and understanding, it should first be noted that the pad refers to a conductive structure located on the front side of a semiconductor, used to achieve electrical and mechanical connections between the chip and external circuits. In the back-illuminated chip of this invention, the pad includes a primary metal, a metal via, and a top metal. The primary metal is the outermost layer of the pad, and its top surface is the bonding surface of the pad. Before being reinforced by the method of this invention, the primary metal itself serves as the bonding pad.

[0038] The method for enhancing bonding strength according to the present invention is as follows: forming a reinforcing metal layer electrically connected to the pads on the back side of the wafer, wherein the reinforcing metal layer and the pads together constitute a reinforcing pad with enhanced bonding strength.

[0039] Please see Figure 1 This is a flowchart of an embodiment of the method for enhancing bond strength according to the present invention. This embodiment includes the following steps: S410, perform partial etching on the epitaxial layer 102 on the back side of the wafer to expose the oxide layer 103 in the pad area.

[0040] For details, please refer to Figure 2 The wafer has completed front-side fabrication, temporary bonding with adhesive, and back-side thinning processes. After back-side thinning, the thinned wafer is flipped so that the back side is facing upwards. Please refer to [further details to be added]. Figure 3 The epitaxial layer 102 on the back side of the wafer is locally etched, specifically at the location corresponding to the area where the front pads are located. The etching depth must penetrate the entire thickness of the epitaxial layer 102 until the oxide layer 103 beneath the pad area is exposed. After etching, a layer is formed as shown... Figure 3 The first cavity 501 shown (i.e., the epitaxial layer etching cavity) has its sidewalls exposed to the subsequent processing environment. It should be noted that the etching endpoint must be precisely controlled during the etching process to avoid over-etching and damaging the underlying oxide layer 103, thereby ensuring the insulating and protective function of the oxide layer 103 for the primary metal 104.

[0041] S420. The oxide layer 103 is partially etched to expose the primary metal 104 of the pad.

[0042] After step S410 is completed, the oxide layer 103 is exposed at the bottom of the first cavity 501. Further details can be found in the following sections. Figure 4The oxide layer 103 is locally etched to expose at least a portion of the surface of the underlying primary metal 104. In this embodiment, the etched area of ​​the oxide layer 103 is controlled to be smaller than the area of ​​the primary metal 104, that is, an oxide layer 103 of a predetermined width is retained to cover the edge region of the primary metal 104, while the central region of the primary metal 104 serves as the exposed area for subsequent electrical connection with the reinforcing metal layer 801. For example, the predetermined width of the oxide layer 103 retained at the edge region of the primary metal 104 is 2 μm to 10 μm.

[0043] Etching forms as Figure 4 The second cavity 601 (i.e., the oxide etching cavity) shown is connected to the first cavity 501 and located at the bottom of the first cavity 501. The bottom of the second cavity 601 exposes the central region of the primary metal 104. This design has at least the following technical effects: On the one hand, the oxide layer 103 covers and holds the edge region of the primary metal 104. During subsequent wire bonding, the oxide layer 103 can effectively constrain the displacement of the edge of the primary metal 104, preventing the primary metal 104 from lifting or peeling off from the edge, enhancing the mechanical strength of the primary metal 104, and improving the ability of the pads to resist external mechanical forces. On the other hand, the retained oxide layer 103, as an insulating isolation layer, can effectively prevent short circuits between the subsequently generated reinforcing metal layer 801 and the conductive structure in the non-pad area, thereby improving the reliability of the chip from both electrical isolation and mechanical reinforcement dimensions.

[0044] S430, A reinforcing metal layer 801 is formed on the exposed area of ​​the primary metal 104, and the reinforcing metal layer 801 and the primary metal 104 together constitute a reinforcing structure for the reinforcing pad.

[0045] Please see Figure 5 This step S430 includes the following sub-steps: S431. A metal layer 701 is formed on the back side of the wafer.

[0046] Please see Figure 6 After completing step S420, a metal layer 701 is formed on the entire back side of the wafer (including the sidewalls of the first cavity 501 and the second cavity 601, the exposed surface of the primary metal 104, and the exposed upper surfaces of the epitaxial layer 102 and the oxide layer 103), so that the back metal layer 701 is in direct contact with and electrically connected to the exposed area of ​​the primary metal 104. The back metal layer 701 can be formed by any of the following processes: physical vapor deposition, chemical vapor deposition, electroplating, etc.

[0047] It should be noted that, in the extended embodiments of the present invention, the material of the metal layer 701 can be the same as or different from the material of the primary metal 104. For example, when the primary metal 104 is aluminum, the metal layer 701 can be copper or gold, as long as a reliable ohmic contact can be formed between the two. Different materials can be flexibly configured according to specific packaging requirements.

[0048] S432. The metal layer 701 is partially etched to retain the metal layer 701 located on the exposed area of ​​the primary metal 104, which serves as the reinforcing metal layer 801.

[0049] Please see Figure 7 After step S431 is completed, the metal layer 701 formed in step S431 is partially etched away, removing the metal layer outside the exposed area of ​​the primary metal 104, leaving only the metal layer 701 on the exposed area of ​​the primary metal 104. This retained portion serves as the reinforcing metal layer 801. The reinforcing metal layer 801 and the underlying primary metal 104 together constitute the reinforcing structure of the reinforcing pad. In this embodiment, the thickness of the reinforcing metal layer 801 is approximately 1 μm to 3 μm, preferably 2 μm.

[0050] After processing in steps S431 and S432, the reinforcing metal layer 801 and the primary metal 104 are stacked and tightly bonded in the vertical direction, resulting in a reinforced structure thickness greater than or equal to 3 μm, a significant increase compared to the original primary metal's 0.5 μm to 1.5 μm. Since there is a positive correlation between metal layer thickness and mechanical strength, the compressive and tensile strength of the reinforced pads are significantly improved. In a verification embodiment of the present invention, tests showed that the wire bonding tensile strength of the pads reinforced using the method of the present invention increased from less than 3 gf in the prior art to greater than or equal to 10 gf.

[0051] It should be noted that the scope of protection of this invention is not limited to a single reinforcing metal layer 801. In another extended embodiment, steps S431 and S432 can be repeated once or multiple times to form multiple stacked reinforcing metal layers 801 on the exposed area of ​​the primary metal 104. Each reinforcing metal layer 801 can be made of the same or different metal materials, and the thickness of each layer can be independently set according to specific requirements. The design of multiple reinforcing metal layers 801 can further increase the total thickness of the reinforced structure within a limited process space, thereby obtaining higher mechanical strength.

[0052] Please see Figure 8 This is a flowchart of an embodiment of the back-illuminated chip fabrication method of the present invention. This embodiment includes the following steps: S100. Provide a target wafer, wherein the target wafer has completed the front-side manufacturing process and has pads formed on its front side.

[0053] Please see Figure 9 The wafer has completed the front-side manufacturing process, and pads have been formed on the front side. These pads are metal pads located on the front side of the target wafer, comprising primary metal 104, metal vias 105, and a top metal layer 106. It should be noted that the front-side manufacturing process refers to all the micro-processing completed on the front side of the wafer substrate during the front-end manufacturing process, including but not limited to shallow trench isolation, well implantation, gate oxide growth, polysilicon gate deposition, source / drain ion implantation, contact hole etching, multilayer metal interconnects, and passivation layer deposition. After completing the front-side manufacturing process, transistors, logic circuits, and the outermost front-side metal layer (i.e., primary metal 104) have been formed on the wafer. The thickness of the primary metal 104 is limited by the front-side process conditions, typically approximately 0.5 μm to 1.5 μm, and its mechanical strength is insufficient to withstand the wedge pressure during subsequent wire bonding.

[0054] S200, the front side of the target wafer is bonded to the support carrier 202 through the adhesive layer 201.

[0055] Please see Figure 10 To support subsequent back-side thinning and back-side processing, the front side of the target wafer needs to be temporarily bonded to a support carrier 202 via an adhesive layer 201. The support carrier 202 provides fixation and mechanical support for subsequent processes. The adhesive layer 201 is made of bonding adhesive, and the support carrier 202 is made of a material with a coefficient of thermal expansion close to that of the target wafer (e.g., a supporting silicon wafer) to reduce the risk of warping or cracking due to thermal stress in subsequent processes. Specifically, bonding adhesive is applied to the front side of the wafer, and the wafer is bonded to the support carrier 202 using the bonding adhesive.

[0056] S300, Thin the back side of the target wafer and remove the substrate 101.

[0057] Please see Figure 11 After step S200 is completed, the back side of the target wafer is thinned to remove the wafer substrate 101, leaving only the epitaxial layer 102. The thinning method can employ one or more combinations of mechanical polishing, chemical mechanical polishing, or wet etching. In this embodiment, a two-step thinning process combining mechanical polishing and chemical mechanical polishing is preferred. First, mechanical polishing is used to quickly remove the bulk thickness of the substrate, and then chemical mechanical polishing is used for fine finishing and surface planarization to obtain an epitaxial layer 102 with uniform thickness and a smooth surface, meeting the precision requirements of subsequent photolithography and etching processes.

[0058] S400, A reinforcing metal layer 801 electrically connected to the pads is formed on the back side of the target wafer.

[0059] Please see Figures 2 to 7 After step S300 is completed, the thinned target wafer is flipped so that the back side of the target wafer faces upwards, and then step S400 is performed. The specific implementation of step S400 refers to any of the implementations of steps S410 to S430 in the method for enhancing bonding strength described above, and will not be repeated here. In short, this step involves locally etching the epitaxial layer 102 on the back side of the target wafer to form a cavity 501, locally etching the oxide layer 103 to form a cavity 601, forming a metal layer 701 on the back side of the wafer, and locally etching the metal layer 701 to retain the reinforcing metal layer 801, etc., to finally form a reinforcing metal layer 801 that is electrically connected to the primary metal 104 of the front pad, so that the reinforcing metal layer 801 and the primary metal 104 together constitute a reinforcing pad with enhanced bonding strength.

[0060] By completing steps S100 to S400, the back-illuminated chip of the present invention can be obtained. Please refer to... Figure 7 The back-illuminated chip has a reinforced metal layer 801 formed on the back side that is electrically connected to the front pads. The reinforced metal layer 801 and the primary metal 104 together form a reinforced structure. The thickness of this reinforced structure is greater than or equal to 3μm. The tensile strength of the bonded pads after reinforcement can reach greater than or equal to 10 gf, which fundamentally solves the reliability problems such as pressure penetration, tearing, and desoldering caused by insufficient thickness of the primary metal 104.

[0061] Please see Figure 12 This is a cross-sectional schematic diagram of an embodiment of the back-illuminated chip of the present invention. The back-illuminated chip is prepared by the above-described back-illuminated chip preparation method.

[0062] The back-illuminated chip includes a support carrier 202, an adhesive layer 201 above the support carrier, an oxide layer 102 above the adhesive layer 201, an epitaxial layer 102 above the oxide layer, a primary metal 104 for the front pads, metal vias 105, a top metal 106, and a reinforcing metal layer 801 electrically connected to the primary metal 104. In this embodiment, the thickness of the reinforcing metal layer 801 is approximately 1 μm to 3 μm, the total thickness of the reinforcing structure (i.e., the composite structure of the primary metal 104 and the reinforcing metal layer 801) is greater than or equal to 3 μm, and the wire bonding tensile strength of the reinforced pads is greater than or equal to 10 gF.

[0063] This invention also discloses an integrated chip, including the back-illuminated chip as described above. Exemplarily, when the back-illuminated chip is a back-illuminated image sensor chip, its back side is the photosensitive surface. The integrated chip also includes at least one functional chip, which is electrically connected to the back-illuminated chip via reinforced pads. The functional chip can be at least one of an analog-to-digital converter chip, a memory chip, and a digital signal processing chip, but is not limited thereto. In the actual packaging structure, the functional chip is electrically connected to the reinforced pads of the back-illuminated chip via interconnection methods such as wire bonding. Because the reinforced pads have significantly enhanced mechanical strength, they can withstand greater wedge pressure during wire bonding without causing crushing or tearing, thereby greatly improving the package connectivity and long-term reliability of the integrated chip.

[0064] This invention significantly increases the thickness and mechanical strength of the pads by forming a reinforcing metal layer electrically connected to the primary metal on the back side of the wafer, thereby improving the tensile strength of the pad wire bonding and fundamentally solving reliability problems such as pad burn-through, tearing, solder ball detachment, and pad peeling during wire bonding. The reinforcing metal layer and the primary metal are stacked vertically to form a reinforced structure, greatly increasing the pad's ability to withstand bonding pressure. The edge region of the primary metal is covered and held by an oxide layer, effectively constraining the displacement of the primary metal edge and preventing it from lifting or peeling during bonding. These two mechanisms work synergistically to enhance the pad's resistance to damage. This method is implemented based on existing back-illuminated chip manufacturing processes, and each step uses mature etching, deposition, and photolithography technologies in the semiconductor field, making it highly compatible with existing mass production processes, low in implementation cost, and easy to promote and apply. This invention significantly improves the pad robustness and packaging reliability of back-illuminated chips, providing strong support for high-density, high-reliability inter-chip interconnect integration.

Claims

1. A method for enhancing bond strength, characterized in that: A reinforcing metal layer electrically connected to the pads is formed on the back side of the wafer. The reinforcing metal layer and the pads together constitute a reinforcing pad with enhanced bonding strength.

2. The method for enhancing bond strength as described in claim 1, characterized in that, Includes the following steps: The epitaxial layer on the back side of the wafer is partially etched to expose the oxide layer in the pad area; The oxide layer is partially etched to expose the primary metal of the solder pads; A reinforcing metal layer is formed on the exposed area of ​​the primary metal, and the reinforcing metal layer and the primary metal together constitute the reinforcing structure of the reinforcing pad.

3. The method for enhancing bond strength as described in claim 2, characterized in that, In the step of locally etching the oxide layer to expose the primary metal of the pad: the etching area of ​​the oxide layer is smaller than the area of ​​the primary metal, and an oxide layer of a predetermined width is retained in the edge region of the primary metal; the central region of the primary metal serves as an exposed area for electrical connection with the reinforcing metal layer.

4. The method for enhancing bond strength as described in claim 2, characterized in that, The step of forming a reinforced metal layer on the exposed area of ​​the primary metal includes the following sub-steps: A metal layer is formed on the back side of the wafer; The metal layer is partially etched to retain the metal layer located on the exposed area of ​​the primary metal, which serves as the reinforcing metal layer.

5. The method for enhancing bond strength as described in claim 2, characterized in that: The reinforcing metal layer is at least one layer.

6. The method for enhancing bond strength as described in claim 3, characterized in that: The preset width of the oxide layer retained in the edge region of the primary metal is 2μm to 10μm, and the thickness of the reinforcing metal layer is 1μm to 3μm.

7. The method for enhancing bond strength as described in claim 2, characterized in that: The thickness of the reinforcement structure is greater than or equal to 3 μm, and the wire bonding tensile strength of the reinforcement pad is greater than or equal to 10 gf.

8. A method for fabricating a back-illuminated chip, characterized in that, Includes the following steps: A target wafer is provided, wherein the front-side manufacturing process has been completed and pads are formed on the front side; The front side of the target wafer is bonded to the support carrier using an adhesive layer; The back side of the target wafer is thinned to remove the substrate; A reinforcing metal layer electrically connected to the pads is formed on the back side of the target wafer using the method for enhancing bonding strength as described in any one of claims 1 to 7.

9. A back-illuminated chip, characterized in that: It is prepared by the back-illuminated chip preparation method according to claim 8.

10. An integrated chip, characterized in that: Including the back-illuminated chip as described in claim 9.