Methods for stripping inert metals

By combining static immersion with columnar and fan-shaped cleaning methods, the problem of metal edge burrs and debris residue in inert metal stripping was solved, achieving a highly efficient metal stripping effect. This method is suitable for bonding processes and ensures the quality of the bonding surface.

CN123124693APending Publication Date: 2026-11-17SHANGHAI IND U TECH RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202510635014.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing inert metal stripping processes suffer from metal edge burrs and debris residue, which affect the quality of subsequent processing and are difficult to adapt to the needs of large-scale production.

Method used

A static immersion method combined with columnar and fan-shaped cleaning was adopted. The cleaning solution containing photoresist dissolving components was used in conjunction with a non-uniform electric field to remove the inert metal film. The stripping process was optimized by adjusting the immersion time and cleaning method.

Benefits of technology

It effectively reduces metal burrs and debris residue, improves peeling quality, and is suitable for large-scale production, especially in bonding processes to ensure clean and flat bonding surfaces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124693A_ABST
    Figure CN123124693A_ABST
Patent Text Reader

Abstract

This application relates to a method for stripping inert metal, comprising: providing a patterned wafer to be cleaned and fixing the wafer in a cleaning apparatus, wherein the wafer includes a substrate, a photoresist layer formed on the substrate, and an inert metal film deposited above the photoresist layer, the photoresist layer forming patterned and non-patterned areas through exposure and development; statically immersing the wafer in a cleaning solution containing photoresist dissolving components to soften the photoresist in the non-patterned areas, the immersion time being 3-8 minutes; and cleaning the immersed wafer with the cleaning solution containing photoresist dissolving components, the cleaning employing a combination of columnar cleaning and fan-shaped cleaning to remove the photoresist layer and the portion of the inert metal film above the non-patterned areas. This method, while ensuring work efficiency, can also reduce metal burrs and metal debris residue, effectively improving the stripping quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the semiconductor field, and more specifically, to a method for stripping inert metals. Background Technology

[0002] In the semiconductor manufacturing field, inert metals (such as titanium, platinum, and gold) are widely used in the manufacture of microelectronic devices due to their excellent chemical stability and electrical conductivity. However, the patterning process for inert metals has long faced technical challenges. Traditional dry etching technology offers high processing precision, but the equipment is expensive and the etching rate is low; wet etching, while simple in equipment, has low resolution, and the corrosiveness of the etchant has a significant impact on the environment and equipment; electrochemical etching, while suitable for complex structures, is difficult to control. Therefore, among various metal patterning technologies, the lift-off process has become an important choice due to its lower processing cost and suitability for mass production.

[0003] Traditional metal stripping processes mainly consist of two stages: immersion and cleaning. In the immersion stage, the metal adhesion layer in the non-patterned areas is softened by dissolving the photoresist; in the cleaning stage, the softened metal in the non-patterned areas is removed using a solution. However, existing processes result in burrs and metal debris remaining at the metal edges. During the cleaning process, metal debris may re-adhere to the wafer surface, thus affecting the quality of subsequent processing. Summary of the Invention

[0004] The purpose of this invention is to provide a method for peeling inert metals that, while ensuring work efficiency, can also reduce metal burrs and metal debris residue, and effectively improve peeling quality.

[0005] To achieve the above objectives, the present invention provides the following technical solution: a method for peeling off inert metals, comprising:

[0006] A patterned wafer to be cleaned is provided and the wafer to be cleaned is fixed in a cleaning apparatus, wherein the wafer to be cleaned includes a substrate, a photoresist layer formed on the substrate and an inert metal thin film deposited on the photoresist layer, and the photoresist layer forms patterned areas and non-patterned areas through exposure and development;

[0007] The wafer to be cleaned is statically immersed in a cleaning solution containing photoresist dissolving components to soften the photoresist in the non-patterned areas for 3-8 minutes.

[0008] The wafer to be cleaned after immersion is cleaned with a cleaning solution containing photoresist dissolving components. The cleaning process combines columnar cleaning and fan-shaped cleaning to remove the photoresist layer and the inert metal film portion above the non-patterned area.

[0009] Furthermore, the cleaning solution includes N-methylpyrrolidone solution, acetone solution, or dimethyl thionamide.

[0010] Furthermore, the static immersion specifically includes: the wafer to be cleaned is statically immersed in an N-methylpyrrolidone solution at 70-90°C for 3-5 minutes.

[0011] Furthermore, the ratio of columnar cleaning to fan-shaped cleaning is 1:3.

[0012] Furthermore, the pressure values ​​set for the columnar cleaning and fan-shaped cleaning are 40-80 Bar.

[0013] Furthermore, the cleaning process includes: first, using columnar cleaning to perform overall cleaning of the wafer to be cleaned; and then using fan-shaped cleaning to perform overall cleaning of the wafer to be cleaned.

[0014] Furthermore, the stripping method also includes cleaning the wafer surface with deionized water or isopropanol to remove remaining metal debris and solution residue.

[0015] Furthermore, the stripping method further includes:

[0016] After the fan-shaped cleaning is completed, a non-uniform electric field is applied to the wafer to be cleaned to form a dielectric force.

[0017] Furthermore, the frequency of the electromagnetic field is set according to the conductivity of the inert metal film and the dielectric constant of the cleaning solution, and the frequency f of the electromagnetic field is:

[0018]

[0019] Where k represents the experimental fitting constant; σ represents the conductivity of the inert metal film; and ε represents the dielectric constant of the cleaning solution.

[0020] Furthermore, the stripping method further includes preparing the wafer to be cleaned, specifically including:

[0021] Provide substrate;

[0022] Photoresist is spin-coated onto the substrate to form a photoresist layer;

[0023] Patterned and non-patterned areas are formed on the photoresist layer through a patterning process. The morphology of the photoresist layer in the patterned area is an inverted T-shaped or vertical columnar structure.

[0024] An inert metal film is formed by deposition.

[0025] The beneficial effects of this invention are as follows: This application uses a static immersion method to immerse the wafer to be cleaned, and sets the immersion time to 3-8 minutes, breaking the conventional logic of the prior art. This helps to reduce the amount of metal debris generated during immersion and avoid the problem of uneven metal edges. Furthermore, by using a cleaning solution containing photoresist dissolving components and employing columnar and fan-shaped cleaning methods to clean the wafer to be cleaned, the problem of insufficient dissolution during immersion can be effectively compensated, improving the peeling quality. Moreover, since the generation of metal debris is reduced during immersion, the difficulty of the cleaning step is reduced. Combined with the shortened immersion time in the early stage, the overall efficiency of the process is ultimately guaranteed. Therefore, compared with the prior art, the inert metal peeling method of this application can reduce metal burrs and metal debris residue while ensuring work efficiency, effectively improving the peeling quality. This method is particularly suitable for bonding processes.

[0026] The above description is merely an overview of the technical solution of the present invention. In order to better understand the technical means of the present invention and to implement it in accordance with the contents of the specification, the preferred embodiments of the present invention are described in detail below with reference to the accompanying drawings. Attached Figure Description

[0027] Figure 1 This is a schematic flowchart of an embodiment of the method for peeling off inert metals according to this application;

[0028] Figure 2 This is a schematic diagram of the structure of an inert metal stripping method according to an embodiment of this application;

[0029] Figure 3a An optical microscope (OM) image of a wafer to be cleaned after an immersion step, as described in the prior art;

[0030] Figure 3b An optical microscope (OM) image of a wafer to be cleaned after the immersion step in one embodiment of this application;

[0031] Figure 3c This is an optical microscope (OM) image of a wafer to be cleaned after the cleaning step in one embodiment of this application.

[0032] Figure reference numerals: 10-Wafer to be cleaned; 11-Substrate; 12-Photoresist layer; 13-Inert metal thin film; 121-Patterned area; 122-Non-Patterned area. Detailed Implementation

[0033] The technical solution of the present invention will now be clearly and completely described with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0034] In the description of this invention, it should be noted that the terms "center," "upper," "lower," "left," "right," "vertical," "horizontal," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing the invention and for simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the invention. Furthermore, the terms "first," "second," and "third" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.

[0035] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances.

[0036] Furthermore, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0037] In bonding processes, the cleanliness and flatness of the bonding surface are crucial to bonding quality. The peeling method described in this application can be used in bonding processes. This peeling method can effectively improve the bonding surface contamination and unevenness caused by surface debris after metal film patterning, thereby ensuring subsequent bonding quality. Please refer to... Figure 1 and Figure 2 The method for stripping inert metal according to one embodiment of this application includes:

[0038] Step S100: Provide a patterned wafer 10 to be cleaned and fix the wafer 10 to be cleaned in a cleaning apparatus (not shown). The wafer 10 to be cleaned includes a substrate 11, a photoresist layer 12 formed on the substrate 11, and an inert metal thin film 13 deposited on the photoresist layer 12. The photoresist layer 12 forms a patterned area 121 and a non-patterned area 122 through exposure and development. The photoresist in the patterned area 121 is removed, and the photoresist in the non-patterned area 122 is retained. The inert metal thin film 13 is partially located in the patterned area 121 and partially located on top of the photoresist layer 12 in the non-patterned area 122.

[0039] Step S200: Staticly immerse the wafer 10 to be cleaned in a cleaning solution containing photoresist dissolving components to soften the photoresist in the non-patterned area 122 for 3-8 minutes.

[0040] Step S300: The wafer 10 to be cleaned after immersion is cleaned with a cleaning solution containing photoresist dissolving components. The cleaning is performed by a combination of columnar cleaning and fan-shaped cleaning to remove the photoresist layer 12 and part of the inert metal film 13 above the non-patterned area 122.

[0041] It should be noted that in semiconductor metal stripping methods, it is well known in the art that dynamic immersion (i.e., using ultrasonic vibration, bubble stirring, etc. during immersion) can improve immersion efficiency and avoid uneven softening of photoresist, thereby enhancing the contact between the solution and the photoresist and achieving rapid dissolution of the photoresist. Static immersion, lacking dynamic action, results in slower photoresist dissolution and is prone to localized insufficient or uneven dissolution. More importantly, the slow and inefficient nature of static immersion contradicts the large-scale production applications required for stripping. Therefore, in the prior art, those skilled in the art conventionally choose dynamic immersion for semiconductor stripping.

[0042] Based on the aforementioned common knowledge, the inventors initially employed a dynamic immersion method to remove the inert metal. Specifically, the wafer 10 to be cleaned was dynamically immersed in a cleaning solution containing photoresist dissolving components. This dynamic immersion included ultrasonic vibration and bubble agitation, and the immersion time was set to 30 minutes (30 minutes is the conventional immersion time used in the prior art). After immersion, the wafer 10 was cleaned. After applying the above-mentioned removal method, the inventors observed through an optical microscope that a large amount of metal debris still remained on the finally cleaned wafer. More importantly, the edges of the metal film on the wafer were uneven.

[0043] To determine the cause of this problem, the inventors observed the wafer 10 to be cleaned after each step of the stripping method using an optical microscope. Through extensive observation, the inventors discovered that the existing dynamic immersion process generates a large amount of metal debris on the wafer, such as... Figure 3a As shown, a large amount of metal debris is difficult to remove during subsequent cleaning, and the generation of this debris is the root cause of uneven metal film edges. To address this issue, the inventors lowered the parameters of ultrasonic vibration and bubble agitation. Simultaneously, to compensate for the low dissolution efficiency caused by lowering these parameters, which prevents large-scale production, the inventors also adjusted the soaking time. However, the problem of generating a large amount of metal debris and uneven metal edges still persists.

[0044] After extensive experimentation, the inventors grasped the root cause of metal debris generation and broke away from conventional thinking in existing technologies. They adopted a static soaking method instead of ultrasonic vibration and bubble agitation. However, static soaking resulted in slow peeling speeds. Initially, the inventors tried extending the soaking time to address this issue, but after multiple experiments, the number of metal debris only slightly decreased, and the uneven edges of the metal film remained. More importantly, this method could not prevent static soaking from being suitable for large-scale production. To further address this limitation, the inventors attempted to shorten the soaking time. However, insufficient soaking time led to inadequate dissolution, resulting in incomplete peeling.

[0045] As described above, the inert metal stripping method of this application can solve the problems of metal debris and uneven metal film edges while meeting the work efficiency required for large-scale production. Specifically, by immersing the wafer 10 to be cleaned in a static immersion method for 3-8 minutes, the amount of metal debris generated during immersion is reduced, and uneven metal edges are avoided. Then, by using a cleaning solution containing photoresist dissolving components and employing columnar and fan-shaped cleaning, the problem of insufficient dissolution during immersion can be effectively compensated, improving the stripping quality. The cleaning solution containing photoresist dissolving components helps soften and solvent the photoresist, reducing the adhesion of the metal film and compensating for insufficient dissolution. At the same time, the columnar and fan-shaped cleaning further accelerates the removal of photoresist through physical impact, compensating for insufficient dissolution and improving stripping efficiency. Furthermore, since the generation of metal debris is reduced during immersion, the difficulty of the cleaning step is reduced. Combined with the shortened immersion time in the early stage, the overall efficiency of the process is ultimately guaranteed. Therefore, the method for peeling off inert metals in this application can reduce metal burrs and metal debris residue while ensuring work efficiency, and effectively improve the peeling quality. This method is particularly suitable for bonding processes.

[0046] Figure 3b This image shows an optical microscope (OM) image of the wafer 10 to be cleaned after the immersion step, using the inert metal stripping method of this embodiment. Figure 3b It can be seen that the number of metal fragments is significantly reduced, with large metal fragments absent, and the edges of the metal film are... Figure 3a Compared to the metal thin film in the middle, its burrs are significantly reduced and the smoothness of the edges is significantly improved. Figure 3c This illustration shows an optical microscope (OM) image of the wafer 10 to be cleaned after the cleaning step in this embodiment. Figure 3c It can be seen that the metal fragments have been basically cleaned.

[0047] In step S100 above, the wafer to be cleaned can be obtained through procurement or through a previous preparation method. In one embodiment, the stripping method further includes preparing the wafer to be cleaned, specifically including:

[0048] Step S101: Provide a substrate;

[0049] Step S102: Spin-coat photoresist onto the substrate, and then form a photoresist layer through processes such as soft baking, exposure, and development;

[0050] Step S103: A patterned area 121 and a non-patterned area 122 are formed on the photoresist layer by a patterning process;

[0051] Step S104: An inert metal is deposited to form an inert metal film using a low-temperature metal evaporation process. The inert metal may be selected from titanium (Ti), platinum (Pt), or gold (Au).

[0052] In an alternative embodiment, during the patterning process, the process parameters can be optimized so that the morphology of the photoresist layer 12 in the patterned area is an inverted T-shaped or vertical columnar structure. This helps to reduce the accumulation of metal at the edge of the pattern in subsequent processes, thereby reducing the difficulty of cleaning.

[0053] In steps S200 and S300, the cleaning solution used is the same, which can be an N-methylpyrrolidone (NMP) solution, or a commonly used photoresist removal solution such as acetone or dimethyl thionamide (DMSO) solution. In step S200, the immersion time is shortened by limiting the immersion stop time to within 5%-20% of the amount of metal debris generated by the inert metal film 13 above the non-patterned area 122. Experiments have verified that the immersion time in this application is less than 8 minutes. In an alternative embodiment, the static immersion specifically includes: statically immersing the wafer to be cleaned in an N-methylpyrrolidone solution at 70-90°C for 3-5 minutes. The temperature of this static immersion is selected in actual operation, for example, 70°C, 80°C, or 90°C, and the immersion time is 3 minutes, 4 minutes, or 5 minutes. In other embodiments, such as when using an acetone solution, the immersion time can be 3-6 minutes.

[0054] In step S300, the cleaning process includes: first, using columnar cleaning to perform overall cleaning of the wafer 10 to be cleaned; then, using fan-shaped cleaning to perform overall cleaning of the wafer 10 to be cleaned. The columnar cleaning applies a strong impact to the wafer 10 to be cleaned, providing physical assistance to the inert metal film portions that are not completely dissolved during static immersion, thus solving the problem of difficult peeling; the fan-shaped cleaning is used to reduce metal debris after immersion. In one embodiment, the ratio of columnar cleaning to fan-shaped cleaning is 1:3. Specifically, the number of columnar cleaning cycles can be 8-32, and the number of fan-shaped cleaning cycles can be 24-96. In practical applications, the number of columnar cleaning cycles can be selected, for example, 8, 15, 20, 25, or 32, and correspondingly, the number of fan-shaped cleaning cycles can be selected, for example, 24, 45, 60, 75, or 96. The pressure values ​​set for columnar and fan-shaped cleaning are 40-80 Bar, for example, 40 Bar, 60 Bar, or 80 Bar.

[0055] In an alternative embodiment, the method for stripping inert metal further includes cleaning the wafer surface with deionized water or isopropanol to remove residual metal debris and solution residue.

[0056] To prevent secondary adhesion of metal debris and reduce contamination of the wafer surface while improving the stripping effect, in one embodiment, the stripping method further includes: after fan-shaped cleaning, applying a non-uniform electric field to the wafer 10 to be cleaned to form a dielectric force, thereby further removing residual metal particles from the surface of the wafer 10. The non-uniform electric field is generated by setting several electrode arrays within the cleaning apparatus.

[0057] The frequency of the electromagnetic field is set based on the conductivity of the inert metal thin film 13 and the dielectric constant of the cleaning solution. The frequency f of the electromagnetic field is:

[0058]

[0059] Where k represents the experimental fitting constant; σ represents the conductivity of the inert metal film 13; and ε represents the dielectric constant of the cleaning solution.

[0060] The electromagnetic field frequency is calculated using a frequency formula to optimize the effect of dielectric adhesion on metal debris, thereby enhancing the debris removal capability. In the aforementioned electromagnetic field frequency formula, conductivity σ and dielectric constant ε are inherent properties of the inert metal film 13 and the cleaning fluid. Although temperature affects conductivity σ and dielectric constant ε in practical applications, experiments have shown that this effect is negligible. Therefore, in this embodiment, conductivity σ and dielectric constant ε are the values ​​of the inert metal film 13 and the cleaning fluid at room temperature, respectively. To facilitate industrial application, the experimental fitting constant k is obtained based on experimental data and a fixed value is selected to ensure stable optimization of the electromagnetic field frequency in practical applications, thereby improving the metal debris removal efficiency.

[0061] Different metal materials and solutions will result in variations in the required motor spacing, voltage, and electromagnetic field frequency. For example, using an inert metal with low conductivity necessitates a moderate dielectric force to prevent excessive metal debris deposition; conversely, using a non-uniform electric field with higher conductivity requires a higher frequency to achieve efficient cleaning in a short time. In practical applications, the appropriate motor spacing, voltage, and electromagnetic field frequency can be determined through repeated experiments based on the specific metal materials and solutions used.

[0062] For ease of implementation, taking the 8-inch P-type silicon wafer to be cleaned (10) as an example, N-methylpyrrolidone is used. The inventors will conduct experiments using three commonly used inert metal materials: titanium, platinum, and gold, and finally obtain the following preferred implementation data. When titanium or platinum is used as the inert metal material, the electrode spacing is selected from 1 to 1.5 mm, for example, 1 mm, 1.25 mm, or 1.5 mm, and the voltage value is selected from 50 V to 100 V, for example, 50 V, 75 V, or 100 V. According to the formula for calculating the frequency of the electromagnetic field, the following can be obtained: When titanium is used, the experimental fitting constant k is 2.2, and the frequency f of the electromagnetic field is 1.5 kHz to 3.5 kHz; when platinum is used, the experimental fitting constant k is 3, and the frequency f of the electromagnetic field is 2.5 kHz to 5 kHz; when gold is used as the inert metal material, the electrode spacing is selected from 1.5 mm to 2 mm, for example, 1.5 mm, 1.75 mm, or 2 mm, and the voltage value is selected from 30 V to 70 V, for example, 30 V, 50 V, or 70 V. The experimental fitting constant k is 5, and according to the formula for calculating the frequency of the electromagnetic field, the frequency f of the electromagnetic field is 6 kHz to 10 kHz.

[0063] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0064] The above embodiments merely illustrate several implementation methods of the present invention, and their descriptions are relatively specific and detailed, but they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.

Claims

1. A method for peeling off an inert metal, characterized in that, The stripping method includes: A patterned wafer to be cleaned is provided and the wafer to be cleaned is fixed in a cleaning apparatus, wherein the wafer to be cleaned includes a substrate, a photoresist layer formed on the substrate and an inert metal thin film deposited on the photoresist layer, and the photoresist layer forms patterned areas and non-patterned areas through exposure and development; The wafer to be cleaned is statically immersed in a cleaning solution containing photoresist dissolving components to soften the photoresist in the non-patterned areas for 3-8 minutes. The wafer to be cleaned after immersion is cleaned with a cleaning solution containing photoresist dissolving components. The cleaning process combines columnar cleaning and fan-shaped cleaning to remove the photoresist layer and the inert metal film portion above the non-patterned area.

2. The method for peeling off inert metals as described in claim 1, characterized in that, The cleaning solution includes N-methylpyrrolidone solution, acetone solution, or dimethyl thionamide.

3. The method for peeling off inert metals as described in claim 2, characterized in that, The static immersion specifically includes: the wafer to be cleaned is statically immersed in an N-methylpyrrolidone solution at 70-90°C for 3-5 minutes.

4. The method for peeling off inert metals as described in any one of claims 1 to 3, characterized in that, The ratio of columnar cleaning to fan-shaped cleaning is 1:

3.

5. The method for peeling off inert metals as described in claim 4, characterized in that, The pressure values ​​set for the columnar cleaning and fan-shaped cleaning are 40-80 Bar.

6. The method for peeling off inert metals as described in claim 5, characterized in that, The cleaning process includes: first, using columnar cleaning to perform overall cleaning of the wafer to be cleaned; then using fan-shaped cleaning to perform overall cleaning of the wafer to be cleaned.

7. The method for peeling off inert metals as described in claim 1, characterized in that, The stripping method further includes cleaning the wafer surface with deionized water or isopropanol to remove remaining metal debris and solution residue.

8. The method for peeling off inert metals as described in claim 1, characterized in that, The stripping method further includes: After the fan-shaped cleaning is completed, a non-uniform electric field is applied to the wafer to be cleaned to form a dielectric force.

9. The method for peeling off inert metals as described in claim 8, characterized in that, The frequency of the electromagnetic field is set according to the conductivity of the inert metal film and the dielectric constant of the cleaning solution, and the frequency f of the electromagnetic field is: Where k represents the experimental fitting constant; σ represents the conductivity of the inert metal film; and ε represents the dielectric constant of the cleaning solution.

10. The method for peeling off inert metals as described in claim 1, characterized in that, The stripping method further includes preparing the wafer to be cleaned, specifically including: Provide substrate; Photoresist is spin-coated onto the substrate to form a photoresist layer; Patterned and non-patterned areas are formed on the photoresist layer through a patterning process. The morphology of the photoresist layer in the patterned area is an inverted T-shaped or vertical columnar structure. An inert metal film is deposited to form.