A stepwise HF etching method for antimony-implanted oxide layers
By employing a stepwise HF etching method, utilizing a strategy of concentrated HF pre-etching and dilute HF fine etching, the problem of uneven corrosion in antimony implanted oxide layers was solved, achieving high-quality interfaces and high-yield removal of antimony implanted oxide layers, which is suitable for semiconductor manufacturing.
Patent Information
- Application Number
- CN202611344587.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-01
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies, the etching process of the oxide layer after antimony implantation cannot simultaneously guarantee the requirements of appearance consistency and electrical parameters coordination. The BOE process is costly and incompatible with mass production, while the conventional HF process has problems with color difference and interface damage.
The stepwise HF etching method is adopted. First, a concentrated HF solution is used to pre-etch and remove the defective loose oxide layer in the antimony injection area. Then, a dilute HF solution is used to finely etch and completely remove the oxide layer. Pure water is used for rinsing in between, and finally, the area is rinsed and dried.
It completely eliminates the color difference caused by corrosion of the oxide layer in the antimony implantation area, optimizes interface quality, and significantly improves device breakdown voltage and electrical yield, while requiring no new equipment and being compatible with existing production lines.
Smart Images

Figure CN123124694A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of semiconductor technology, and specifically relates to a stepwise HF etching method for antimony implantation oxide layers in semiconductor devices. Background Technology
[0002] In semiconductor ion implantation processes, antimony (Sb) is a typical heavily doped donor impurity, commonly used in processes such as device channel tuning, field oxygen doping, and high voltage buffer layer doping. After Sb ion implantation, ion bombardment causes lattice damage, density changes, and impurity enrichment in the surface silicon dioxide (SiO2) film, resulting in differences in the microstructure of the oxide layer in the Sb implantation region and the non-implantation region, which in turn affects the uniformity and consistency of subsequent wet etching processes of the oxide layer.
[0003] In existing technologies, the following two methods are commonly used to remove the oxide layer after Sb implantation: Firstly, there is the BOE (buffered hydrofluoric acid) one-step etching process. The BOE solution is prepared by mixing hydrofluoric acid and ammonium fluoride. It exhibits a mild etching rate and uniform etching selectivity, and is insensitive to micro-density differences in the oxide layer caused by Sb doping. Therefore, the surface consistency between the Sb-injected and non-injected areas after etching is good, with no visible color difference. However, BOE chemical reagents are expensive and require a separate tank, making it incompatible with pre-furnace cleaning processes. This increases equipment costs and process complexity, limiting its widespread application in mass production lines.
[0004] Secondly, the conventional one-step HF etching process (single etching with concentrated or dilute HF). In industrial mass production, HF solution is often used to rapidly remove the oxide layer after implantation. However, in the Sb implantation region, the oxide layer experiences increased lattice defects, higher oxygen vacancy concentration, and Sb impurity segregation and enrichment due to ion implantation, resulting in a significantly higher HF etching rate than ordinary thermal oxide layers. With single-step HF etching, the oxide layer in the implantation region is removed prematurely due to the rapid etching rate, and the HF solution continues to etch the exposed silicon substrate, causing interface depressions and micro-damage. Meanwhile, the oxide layer in the non-implanted region is not completely removed, resulting in a lighter etching morphology. This inconsistent etching progress between the two regions leads to light and dark color differences and uneven regional textures on the wafer surface. Simultaneously, the defect density at the interface depressions increases significantly, increasing device leakage current, significantly degrading breakdown voltage, and reducing stability.
[0005] In summary, while the BOE process produces no color difference after etching, it suffers from poor process compatibility and cannot meet the requirements of mass production lines. The conventional HF process, although highly compatible, suffers from severe color differences, significant interface damage, and low breakdown voltage. Neither of these two solutions satisfies the synergistic requirements of appearance consistency and electrical parameters. Summary of the Invention
[0006] To address the aforementioned problems in the prior art, this invention provides a stepwise HF etching method for antimony-implanted oxide layers. The technical problem to be solved by this invention is achieved through the following technical solution: This invention proposes a stepwise HF etching method for antimony-implanted oxide layers, comprising the following steps: Step 1: Use HF solution of the first concentration to pre-etch the wafer after Sb implantation to remove the defective and loose oxide layer on the surface of the Sb implantation area, while retaining part of the oxide layer; Step 2: Use a second concentration of HF solution to perform fine etching on the pre-etched wafer to completely remove the remaining oxide layer in the implanted area and the oxide layer in the non-implanted area; wherein, the first concentration is greater than the second concentration; Step 3: Rinse and dry the finely etched wafer to complete the stepwise HF etching of the antimony implanted oxide layer.
[0007] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. Completely eliminate color difference caused by corrosion of the oxide layer in the Sb injection area.
[0008] This invention utilizes concentrated HF pre-etching to pre-consume the highly reactive, porous oxide layer in the Sb implantation region, followed by the simultaneous removal of the oxide layer in both regions using dilute HF at a low rate and with high uniformity. This two-stage synergistic approach eliminates the difference in etching rates between the implantation and non-implantation regions, resulting in a wafer surface free of visible color differences and achieving the highest standards of mass production uniformity.
[0009] 2. Significantly optimizes the Si / SiO2 interface quality.
[0010] This invention employs a step-by-step etching strategy. Pre-etching with concentrated HF retains a portion of the oxide layer, preventing direct contact between HF and the silicon substrate. Then, fine etching with dilute HF gently and uniformly removes the remaining oxide layer, avoiding interface damage caused by one-step over-etching. The resulting interface is smooth with a significantly reduced defect density, providing a high-quality interface foundation for subsequent device fabrication.
[0011] 3. Significantly improves device breakdown voltage and electrical yield.
[0012] This invention suppresses the formation of leakage channels by smoothing the low-defect interface, reducing the interface state density and leakage current, increasing the average breakdown voltage of the device by 8% to 15%, and significantly enhancing batch consistency, effectively improving the electrical yield and reliability of high-voltage and power devices.
[0013] 4. It has strong process compatibility and requires no additional equipment investment.
[0014] This invention employs a fully wet, room-temperature process, which can be achieved by simply splitting the existing single HF etching process into two steps. It requires no new equipment and does not change the original wafer fabrication structure. It is seamlessly compatible with existing Sb implantation processes, high-voltage devices, and power device mass production lines, and is easy to promote in engineering.
[0015] 5. The process is simple, the cost is low, and the yield is significantly improved.
[0016] This invention solves long-standing process pain points by simply splitting the HF etching process into two steps and adding an intermediate pure water rinse. It has a wide process window, is easy to operate, and has extremely high mass production value. While improving appearance consistency and electrical parameters, it effectively reduces yield losses caused by color difference and breakdown voltage degradation.
[0017] The present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description
[0018] Figure 1 This is a schematic flowchart of a stepwise HF etching method for an antimony-implanted oxide layer provided in an embodiment of the present invention. Detailed Implementation
[0019] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the embodiments described below are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0020] This invention provides a stepwise HF etching method for antimony implanted oxide layers. Through a segmented control strategy of concentrated HF pre-etching and dilute HF precise re-etching, it avoids the deposition of Sb oxide and HF-generated SbF5 / HSbF6 on the Si surface in the implanted region, thereby completely eliminating color difference, significantly optimizing interface state, and significantly improving device BV performance. It is also compatible with existing furnace cleaning equipment and processes.
[0021] Please see Figure 1 , Figure 1 This is a schematic flowchart of a stepwise HF etching method for an antimony-implanted oxide layer provided by an embodiment of the present invention. The method includes the following steps: Step 1: Use HF solution of the first concentration to pre-etch the wafer after Sb implantation to remove the defective and loose oxide layer on the surface of the Sb implantation area, while retaining part of the oxide layer.
[0022] In this step, the antimony (Sb)-implanted wafer refers to a semiconductor wafer that has undergone the antimony ion implantation process. Sb, as a typical heavily doped donor impurity, is commonly used in processes such as device channel tuning, field oxygen doping, and high-voltage buffer layer doping. During ion implantation, high-energy Sb ions bombard the wafer surface, causing lattice damage, density changes, and Sb impurity segregation and enrichment in the surface silicon dioxide (SiO2) film. This results in significant differences in the microstructure and corrosion characteristics of the oxide layer in the Sb-implanted region compared to the non-implanted region.
[0023] A defective, porous oxide layer refers to an oxide layer in the Sb-implanted region that exhibits numerous lattice distortions, oxygen vacancies, and dangling bonds due to ion bombardment. This layer has a loose structure and high corrosion activity. It also contains byproducts such as Sb₂O₃ generated during Sb implantation. In contrast, the thermal oxide layer in the non-implanted region has a dense structure, fewer defects, and a more uniform and lower corrosion rate.
[0024] Specifically, the Sb-implanted wafer is placed in an etching bath containing a first-concentration HF solution for pre-etching. Optionally, the first-concentration HF solution is a concentrated HF solution with a mass concentration ranging from 5% to 49%. Concentrated HF solution has a faster etching rate on the porous oxide layer with defects in the Sb-implanted region, effectively removing the highly defective surface layer generated by ion implantation and removing Sb₂O₃ generated by Sb implantation. The pre-etching time can be determined based on the concentration of the HF solution and the initial thickness of the oxide layer, generally ranging from 5 to 300 seconds.
[0025] For example, when using a concentrated HF solution with a mass concentration of 10%, the pre-corrosion time is preferably 60 s.
[0026] Furthermore, it should be noted that excessive etching of the oxide layer during the pre-etching stage can lead to the inability to remove SbF5 / HSbF6 deposits, while insufficient etching will result in excessively long etching times in the subsequent fine etching stage. Therefore, in this embodiment, the thickness of the oxide layer retained in the Sb implantation region after pre-etching is set to 5~20nm. This thickness range ensures that the HF solution does not penetrate the oxide layer and directly contact the silicon substrate, while also providing a suitable process window for the subsequent fine etching steps.
[0027] The core function of this step is to rapidly etch the highly reactive surface layer and Sb₂O₃ byproducts in the Sb-implanted region using a concentrated HF solution, while retaining part of the oxide layer to prevent direct contact between HF and the silicon substrate. This operation consumes most of the highly reactive oxide layer in the implanted region, reducing its corrosive activity and bringing it closer to the dense oxide layer of the non-implanted region, thus creating conditions for the simultaneous removal of the implanted and non-implanted regions in the second step.
[0028] Step 2: Use a second concentration of HF solution to perform fine etching on the pre-etched wafer to completely remove the remaining oxide layer in the implanted area and the oxide layer in the non-implanted area; wherein, the first concentration is greater than the second concentration.
[0029] It is understandable that after completing the pre-etching in step 1 and before proceeding to the fine etching in step 2, the following steps are also included: The pre-etched wafer is rinsed with pure water for 120-300 seconds, preferably 180 seconds.
[0030] By rinsing the pre-etched wafer with pure water, the residual concentrated HF solution and reaction products generated during the pre-etching process (such as SbF5, HSbF6, etc.) on the wafer surface can be removed, preventing these residues from interfering with the corrosion uniformity in the subsequent fine etching step. At the same time, it avoids bringing high-concentration HF into the low-concentration HF fine etching tank, ensuring precise control of the fine etching concentration.
[0031] After cleaning, the second step of corrosion can be carried out.
[0032] Specifically, the wafer, after being rinsed with pure water, is placed in an etching tank containing a second concentration of HF solution for fine etching. Optionally, the second concentration of HF solution is a dilute HF solution with a mass concentration ranging from 0.5% to 2%, preferably 1%. The fine etching time is matched according to the thickness of the remaining oxide layer to ensure complete removal of the remaining oxide layer. For example, when using a 1% dilute HF solution, the fine etching time is typically 60 to 180 seconds.
[0033] After the first pre-etching step, the injected area retains a portion of the oxide layer, while the non-injected area maintains a complete and dense oxide layer, with the oxide layer states in both areas becoming increasingly similar. Due to its low concentration, gentle etching rate, and good uniformity, the dilute HF solution exhibits minimal difference in etching rate between the remaining oxide layer in the injected area and the dense oxide layer in the non-injected area. Therefore, the oxide layers in both areas are simultaneously and uniformly removed under the gentle etching of dilute HF, exposing the silicon surface at the same time without any height or color difference. Furthermore, the concentration of the reaction products (SbF5 / HSbF6) in the dilute HF solution is extremely low, allowing for complete removal through subsequent rinsing.
[0034] The core function of this step is to utilize the low concentration, slow and uniform corrosion rate of dilute HF solution to simultaneously and completely remove the remaining oxide layer in both areas, thus avoiding the problem of over-etching in the injected area and insufficient corrosion in the non-injected area in one-step HF corrosion.
[0035] This invention fundamentally solves the problem of inconsistent corrosion rates between the implanted and non-implanted regions by employing a rate difference cancellation mechanism through a first-step fast-rate corrosion and a second-step slow-rate corrosion. Simultaneously, by avoiding interface depressions and rough layers caused by a single strong HF corrosion, the interface state density is significantly reduced, leakage current channels are suppressed, and the device breakdown voltage is improved.
[0036] Step 3: Rinse and dry the finely etched wafer to complete the stepwise HF etching of the antimony implanted oxide layer.
[0037] First, the finely etched wafers are rinsed with pure water to remove residual HF solution and reaction products from the wafer surface, preventing the residues from causing contamination or corrosion in subsequent processes.
[0038] Then, the rinsed wafers are placed in SC1 cleaning solution for cleaning to remove particle and metal ion contamination from the wafer surface.
[0039] Specifically, the rinsed wafers are placed in SC1 cleaning solution (usually a mixed solution of NH4OH:H2O2:H2O=1:2:50) for cleaning to remove particle and metal ion contamination from the wafer surface. SC1 cleaning is a standard step in semiconductor wet cleaning processes to ensure wafer surface cleanliness.
[0040] Next, the wafers cleaned with SC1 were rinsed again with pure water to remove any residue of the SC1 cleaning solution.
[0041] Finally, the rinsed wafers are dried, which can be done by spin drying, nitrogen blowing, or baking, to complete the process of removing the antimony implanted oxide layer.
[0042] In summary, the stepwise HF etching method for antimony implanted oxide layers provided by this invention first pre-etches the Sb-implanted wafer with a concentrated HF solution to remove the defective and loose oxide layer on the surface of the Sb-implanted region, while retaining a portion of the oxide layer. Then, a dilute HF solution is used to finely etch the pre-etched wafer, completely removing the remaining oxide layer in the implanted region and the oxide layer in the non-implanted region. Finally, the finely etched wafer is rinsed and dried, thus achieving stepwise HF etching of the antimony implanted oxide layer. This method offers the following advantages: 1. Completely eliminate color difference caused by corrosion of the oxide layer in the Sb injection area.
[0043] This invention utilizes concentrated HF pre-etching to pre-consume the highly reactive, porous oxide layer in the Sb implantation region, followed by the removal of the oxide layer in both regions using dilute HF at a low rate and with high uniformity. This two-stage process eliminates the adsorption of byproducts due to the difference in etching rates between the implantation and non-implantation regions, resulting in a wafer surface free of visible color differences and achieving the highest standards of mass production uniformity.
[0044] 2. Significantly optimizes the Si / SiO2 interface quality.
[0045] This invention employs a step-by-step etching strategy. Pre-etching with concentrated HF retains a portion of the oxide layer, preventing direct contact between HF and the silicon substrate. Then, fine etching with dilute HF gently and uniformly removes the remaining oxide layer, avoiding interface damage caused by one-step over-etching. The resulting interface is smooth with a significantly reduced defect density, providing a high-quality interface foundation for subsequent device fabrication.
[0046] 3. Significantly improves device breakdown voltage and electrical yield.
[0047] This invention suppresses the formation of leakage channels by smoothing the low-defect interface, reducing the interface state density and leakage current, increasing the average breakdown voltage of the device by 8% to 15%, and significantly enhancing batch consistency, effectively improving the electrical yield and reliability of high-voltage and power devices.
[0048] 4. It has strong process compatibility and requires no additional equipment investment.
[0049] This invention employs a fully wet, room-temperature process, which can be achieved by simply splitting the existing single HF etching process into two steps. It requires no new equipment and does not change the original wafer fabrication structure. It is seamlessly compatible with existing Sb implantation processes, high-voltage devices, and power device mass production lines, and is easy to promote in engineering.
[0050] 5. The process is simple, the cost is low, and the yield is significantly improved.
[0051] This invention solves long-standing process pain points by simply splitting the HF etching process into two steps and adding an intermediate pure water rinse. It has a wide process window, is easy to operate, and has extremely high mass production value. While improving appearance consistency and electrical parameters, it effectively reduces yield losses caused by color difference and breakdown voltage degradation.
[0052] Furthermore, the method provided by this invention can be applied to the oxide layer removal process after Sb implantation in high-voltage or power devices. After completing the rinsing and drying process, subsequent semiconductor manufacturing processes can proceed. The entire process is a room-temperature wet operation, requiring no additional equipment and seamlessly compatible with existing Sb implantation processes, high-voltage devices, and power device mass production lines.
[0053] The beneficial effects of the present invention will be verified and explained through comparative experiments below.
[0054] Experiment 1: Antimony implantation oxide layer removal was performed using the distributed HF etching method of the present invention.
[0055] Specifically, the experimental procedure is as follows: The first step is pre-etching with concentrated HF solution. The Sb-implanted wafer is placed in a 10% concentrated HF solution and etched for 60 seconds. This removes the defective and loose oxide layer and Sb₂O₃ from the surface of the Sb-implanted region, leaving an oxide layer of approximately 5–20 nm thickness.
[0056] The second step is intermediate rinsing. The pre-etched wafer is rinsed with pure water for 180 seconds to remove residual HF solution and reaction products from the surface.
[0057] The third step is fine etching with dilute HF solution. The rinsed wafer is placed in a 1% dilute HF solution and etched for 90 seconds to completely remove the remaining oxide layer in the implanted area and the oxide layer in the non-implanted area.
[0058] The fourth step is rinsing and drying. The finely etched wafers are then rinsed with pure water, cleaned with SC1, rinsed again with pure water, and dried to obtain wafers with the antimony-implanted oxide layer removed.
[0059] Experimental results show that the implanted and non-implanted regions of the wafer exhibit no color difference, and the surface has a uniform mirror finish; the interface roughness is significantly reduced. Testing revealed that the breakdown voltage of the fabricated devices increased by an average of 8%–15%, and the leakage current decreased by an order of magnitude.
[0060] Experiment 2: Antimony implantation oxide layer removal was performed using the traditional one-step HF etching method.
[0061] Specifically, the experimental procedure is as follows: The Sb-implanted wafer was directly placed in a 49% concentrated HF solution for one-time etching until the oxide layer was completely removed.
[0062] Because the Sb-implanted oxide layer has more lattice defects, a looser structure, and higher corrosion reactivity, its corrosion rate is significantly faster than that of the dense oxide layer in the non-implanted region. When the oxide layer in the implanted region is removed prematurely, the HF solution continues to etch the exposed silicon substrate, causing interface depressions and micro-damage; meanwhile, the oxide layer in the non-implanted region has not yet been completely removed. The resulting wafer surface exhibits light and dark color differences and uneven regional textures, a significantly increased interface defect density, increased device leakage current, and a marked deterioration in breakdown voltage.
[0063] This verifies that, compared with existing technologies, the present invention can completely eliminate color difference, significantly optimize interface state, and significantly improve the BV performance of the device.
[0064] The above description, in conjunction with specific preferred embodiments, provides a further detailed explanation of the present invention. It should not be construed that the specific implementation of the present invention is limited to these descriptions. For those skilled in the art, various simple deductions or substitutions can be made without departing from the concept of the present invention, and all such modifications and substitutions should be considered within the scope of protection of the present invention.
Claims
1. A stepwise HF etching method for an antimony-implanted oxide layer, characterized in that, Includes the following steps: Step 1: Use HF solution of the first concentration to pre-etch the wafer after Sb implantation to remove the defective and loose oxide layer on the surface of the Sb implantation area, while retaining part of the oxide layer; Step 2: Use a second concentration of HF solution to perform fine etching on the pre-etched wafer to completely remove the remaining oxide layer in the implanted area and the oxide layer in the non-implanted area; wherein, the first concentration is greater than the second concentration; Step 3: Rinse and dry the finely etched wafer to complete the stepwise HF etching of the antimony implanted oxide layer.
2. The method according to claim 1, characterized in that, In step 1, the first concentration HF solution is a concentrated HF solution with a mass concentration of 5% to 49%.
3. The method according to claim 1, characterized in that, In step 1, the pre-corrosion time is 5~300s.
4. The method according to claim 1, characterized in that, In step 1, the first concentration HF solution is a 10% (w / w) concentrated HF solution, and the pre-corrosion time is 60 seconds.
5. The method according to claim 1, characterized in that, In step 1, after pre-etching, the thickness of the oxide layer retained in the Sb implantation region is 5~20nm.
6. The method according to claim 1, characterized in that, After completing the pre-etching in step 1 and before proceeding to the fine etching in step 2, the process also includes: The pre-etched wafers are rinsed with pure water for 120-300 seconds.
7. The method according to claim 1, characterized in that, In step 2, the second concentration HF solution is a dilute HF solution with a mass concentration of 0.5% to 2%.
8. The method according to claim 1, characterized in that, In step 2, the fine etching time is matched according to the thickness of the remaining oxide layer to ensure complete removal of the remaining oxide layer.
9. The method according to claim 1, characterized in that, Step 3 includes: The finely etched wafers are rinsed with pure water to remove residual HF solution and reaction products from the wafer surface. After rinsing, the wafers are placed in SC1 cleaning solution for cleaning to remove particle and metal ion contamination from the wafer surface. The wafers cleaned with SC1 were rinsed again with pure water; The rinsed wafers are then dried.
10. The method according to claim 1, characterized in that, The method is applied to the oxide layer removal process after Sb implantation in high-voltage or power devices.