Fabrication method of silicon-on-insulator wafer and silicon-on-insulator wafer

By performing densification annealing and hydrogen passivation treatment under an inert atmosphere after thermal oxidation, the problem of insufficient density of micron-sized silicon oxide films was solved, and the insulation and electrical properties of silicon wafers on insulators were improved.

CN123124772APending Publication Date: 2026-11-17XIAN ESWIN MATERIAL TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611623276.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies for preparing micron-sized silicon oxide films suffer from insufficient density and inadequate local structural rearrangement during the thermal oxidation process, which affects the electrical isolation performance of silicon wafers on insulators.

Method used

By densifying annealing in an inert atmosphere after thermal oxidation, combined with hydrogen passivation treatment, the density and interface state of the buried oxide layer are improved. The silicon-oxygen network structure is further adjusted by high-temperature high-purity nitrogen annealing and hydrogen-containing mixed atmosphere treatment.

Benefits of technology

It improves the density and structural stability of the buried oxide layer, reduces leakage current, improves insulation performance and interface states, and enhances the electrical performance of silicon wafers on insulators.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123124772A_ABST
    Figure CN123124772A_ABST
Patent Text Reader

Abstract

This application relates to a method for fabricating silicon-on-insulator (SiI) wafers and the SiI wafers themselves. The method includes: providing a support substrate; thermally oxidizing the support substrate by introducing an oxidizing atmosphere into a heat treatment furnace tube to form a buried oxide layer with a thickness of not less than 1.5 μm on the surface of the support substrate; after thermal oxidation, introducing an inert atmosphere into the heat treatment furnace tube and holding the buried oxide layer at an annealing temperature not lower than the highest oxidation temperature for a first preset time to densify the buried oxide layer; and forming a top silicon layer on the side of the buried oxide layer away from the support substrate. The density of the buried oxide layer is improved through post-film formation heat treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of semiconductor processing and manufacturing technology, specifically to a method for preparing silicon-on-insulator (SiI) wafers and the SiI wafers themselves. Background Technology

[0002] A silicon-on-insulator (SiIn) wafer includes a supporting substrate, a buried oxide layer, and a top silicon layer. The buried oxide layer provides electrical isolation between the supporting substrate and the top silicon layer. During fabrication, a silicon oxide film of the desired thickness can be formed by thermally oxidizing the supporting substrate. Subsequently, the top silicon layer is formed on this silicon oxide film, leaving the silicon oxide film as the buried oxide layer in the resulting SiIn wafer.

[0003] For silicon oxide films with a thickness in the micrometer range, thermal oxidation typically requires a long growth time. Although its overall composition is close to silicon dioxide, the local silicon-oxygen network may still exhibit insufficient rearrangement. Achieving the desired thickness through continuous oxidation does not simultaneously guarantee that the local network structure will be adequately adjusted. Therefore, silicon oxide films formed by thermal oxidation may still suffer from insufficient density. Summary of the Invention

[0004] This section provides a general summary of the application, rather than a full disclosure of the entire scope or all features of the application.

[0005] This application provides a method for preparing silicon-on-insulator wafers to improve the density of the buried oxide layer formed by thermal oxidation.

[0006] According to one aspect of this application, a method for fabricating a silicon-on-insulator (SiI) wafer is provided. The method includes: providing a support substrate; placing the support substrate inside a heat treatment furnace tube, introducing an oxidizing atmosphere into the heat treatment furnace tube to thermally oxidize the support substrate, forming a buried oxide layer on the surface of the support substrate, the thickness of the buried oxide layer being not less than 1.5 μm; after the thermal oxidation is completed, introducing an inert atmosphere into the heat treatment furnace tube and holding at an annealing temperature for a first preset time to densify the buried oxide layer, the annealing temperature being not lower than the highest oxidation temperature used in the thermal oxidation; and forming a top silicon layer on the side of the buried oxide layer away from the support substrate, thereby fabricating a SiI wafer.

[0007] According to another aspect of this application, a silicon-on-insulator (SCI) wafer prepared according to the above-described preparation method is provided. The SCI wafer includes a supporting substrate, a buried oxide layer on the supporting substrate, and a top silicon layer on the buried oxide layer. The thickness of the buried oxide layer is not less than 1.5 μm, and the refractive index of the buried oxide layer, measured using an ellipsometer, is 1.460~1.464.

[0008] According to the above technical solution, a densification and heat preservation stage under an inert atmosphere is set after thermal oxidation film formation, so that the formed buried oxide layer continues to be subjected to heat treatment at a temperature not lower than the maximum oxidation temperature, promoting further adjustment of the silicon-oxygen network structure, thereby improving the density and structural stability of the buried oxide layer. The treated buried oxide layer is then retained in the silicon-on-insulator wafer. In an embodiment with additional hydrogen-containing atmosphere passivation, the interface state between the buried oxide layer and the supporting substrate can be further improved. Attached Figure Description

[0009] The features and advantages of embodiments of this application will become more readily understood from the following description with reference to the accompanying drawings. In the drawings: Figure 1 This is a process flow diagram of the fabrication process of silicon-on-insulator wafers according to embodiments of this application.

[0010] Figure 2 This is a partial structural schematic diagram of a support substrate with a buried oxide layer formed according to an embodiment of this application.

[0011] Figure 3 This is a partial structural schematic diagram of a silicon-on-insulator wafer according to an embodiment of this application.

[0012] In the accompanying drawings, the same or corresponding technical features, parts or components are represented by the same or corresponding reference numerals. Detailed Implementation

[0013] The present application will now be described in detail with reference to the accompanying drawings and exemplary embodiments. It should be noted that the following detailed description of the present application is for illustrative purposes only and is not intended to limit the scope of the application.

[0014] In this application, the buried oxide (BOX) layer is a silicon oxide film formed on the surface of the support substrate through thermal oxidation. After the top silicon layer is subsequently formed, it remains between the support substrate and the top silicon layer, serving an electrical isolation function. For consistency, before the formation of the top silicon layer, it is also referred to as the buried oxide layer according to its purpose in the final wafer. At this time, the surface of the buried oxide layer away from the support substrate is not yet covered by the top silicon layer; the intermediate wafer consisting of the support substrate and the buried oxide layer thereon is referred to as an oxide wafer. In the following discussion of the structure and test results of the oxide wafer, the buried oxide layer is always in the corresponding processing stage before the formation of the top silicon layer.

[0015] When fabricating oxide wafers for silicon-on-insulator (SOI) wafers, a buried oxide layer can be formed on the surface of a supporting substrate through thermal oxidation. Even after reaching the desired thickness, micron-sized buried oxide layers obtained through prolonged growth may still exhibit localized structural looseness, high fixed charge, and increased trapped charge. The interface between the buried oxide layer and the supporting substrate may also have a high interface state density. These issues affect the insulating performance of the buried oxide layer and its subsequent use in SOI wafers.

[0016] Here, film thickness refers to the dimension of the buried oxide layer along the thickness direction, while density reflects the state of the internal structure of the buried oxide layer. During thermal oxidation, the growth of the buried oxide layer and the local network rearrangement are simultaneously affected by process conditions; obtaining the required thickness does not mean that the internal structure has been fully adjusted. For buried oxide layers that have reached the required thickness, their internal structure can be further improved through subsequent heat treatment.

[0017] Interfacial state density, denoted by Dit, describes the number of interfacial states per unit interfacial area and per unit energy interval, and is expressed in cm². 2 ·eV 1 Fixed charges, trapped charges, and interface states within the buried oxide layer are evaluated separately. The Dit measured in the following section pertains to the contact interface between the support substrate and the buried oxide layer formed by thermal oxidation. This original interface is retained after the formation of the top silicon layer and constitutes the support-side interface of the SOI wafer.

[0018] In response, this application provides a method for fabricating a silicon-on-insulator (SOI) wafer. This method involves forming a buried oxide layer on a supporting substrate through thermal oxidation, densifying the buried oxide layer, and then forming a top silicon layer to obtain an SOI wafer having a supporting substrate, a buried oxide layer, and a top silicon layer.

[0019] Reference Figure 1 A support substrate is provided and placed inside a heat treatment furnace tube, where an oxidizing atmosphere is introduced for thermal oxidation. Thermal oxidation forms a buried oxide layer with a thickness of not less than 1.5 μm on the surface of the support substrate. After thermal oxidation, an inert atmosphere is introduced into the same heat treatment furnace tube, and the buried oxide layer is densified by holding at the annealing temperature for a first preset time. The annealing temperature is not lower than the highest oxidation temperature used in the thermal oxidation. A top silicon layer is formed on the side of the treated buried oxide layer away from the support substrate, completing the fabrication of the SOI wafer.

[0020] Figure 1Step S102 represents the thermal oxidation to form a buried oxide layer, and step S103 represents the inert atmosphere densification annealing after film formation. Upon entering step S103, the contact interface between the buried oxide layer and the supporting substrate has already been formed during thermal oxidation. Annealing heats the entire oxide wafer, ensuring that the buried oxide layer and the area in contact with the supporting substrate undergo the post-film formation heat treatment together.

[0021] The aforementioned film thickness of not less than 1.5 μm is measured from the contact surface between the supporting substrate and the buried oxide layer to the surface of the buried oxide layer facing away from the supporting substrate. This thickness corresponds to the state after thermal oxidation is completed. For example, the thickness of the formed buried oxide layer is 1.5 μm, but a larger micrometer-level thickness can also be selected according to the film formation requirements. The film thickness of subsequent products is determined after the corresponding processing is completed.

[0022] The maximum oxidation temperature is the highest value among the temperatures used in each thermal oxidation stage to form the buried oxide layer. When thermal oxidation includes multiple stages, the annealing temperature is compared with the highest temperature among them. For example, when the wet oxidation temperature is 1100℃ and the dry oxidation temperature is 1130℃, the maximum oxidation temperature is 1130℃, and the densification annealing can be carried out at 1130℃. When the maximum oxidation temperature is 1150℃, the subsequent densification annealing temperature is selected accordingly to be no lower than 1150℃.

[0023] In some embodiments, the densification annealing temperature is 1100°C to 1150°C, and is selected according to the oxidation temperature used when forming the buried oxide layer, so that the densification annealing temperature is not lower than the highest oxidation temperature used in this thermal oxidation.

[0024] By setting a separate densification and holding stage after thermal oxidation, the already formed buried oxide layer continues to undergo heat treatment in a modified processing atmosphere. The annealing temperature is maintained at a level no lower than the previous highest oxidation temperature, and the first preset time provides the duration for further structural adjustments after film formation. The oxidation stage mainly forms the buried oxide layer and its thickness, while the densification stage further improves the network structure of this buried oxide layer; both stages act sequentially on the same buried oxide layer.

[0025] Specifically, although the overall composition of the thick buried oxide layer formed by thermal oxidation is close to that of silicon dioxide, the local Si-O-Si network formed over a long period of growth may not be fully rearranged. In the specific implementation of high-temperature, high-purity nitrogen annealing, heat treatment promotes further reconstruction of this network, reduces low-density areas and structural defects, and makes the buried oxide layer denser and more structurally stable.

[0026] The first preset time is the holding time of the oxide wafer at the set annealing temperature and inert atmosphere, excluding the heating and cooling processes. For example, when using an annealing temperature of 1130℃, the first preset time is 3 hours. Timing starts after the set holding conditions are reached, and the cooling process begins after the holding period ends.

[0027] An inert atmosphere is used to provide a gaseous environment for the densification process after film formation. For example, under the processing conditions, high-purity nitrogen is used as the inert atmosphere, with a purity of 6N or higher, i.e., not less than 99.9999%. After thermal oxidation is completed, the oxidizing atmosphere in the furnace tube is switched to this high-purity nitrogen atmosphere, and then the set heat preservation treatment is implemented.

[0028] For example, an oxide wafer sample with a buried oxide layer thickness of 1.5 μm upon completion of oxidation was subjected to high-purity nitrogen at 1130 °C for 3 hours and compared with a sample that did not undergo densification annealing. The above sample was tested before the formation of the top silicon layer. The refractive index of the buried oxide layer in the control sample was 1.457–1.459, and the distance between the support substrate and the buried oxide layer was approximately 1.2 × 10⁻⁶. 11 cm 2 ·eV 1 The refractive index stabilized at 1.462±0.002 after nitrogen annealing, and the Dit was 7×10⁻⁶. 10 cm 2 ·eV 1 And a significant decrease in leakage current was observed.

[0029] The aforementioned refractive index results are used to evaluate the optical state of the buried oxide layer. Combined with the film formation and annealing processes, they provide an optical basis for improving the state of the buried oxide layer. Refractive index and actual material density are different physical quantities. Therefore, the refractive index change can be evaluated in conjunction with interface and electrical test results, avoiding the direct use of a single optical value as a density measurement.

[0030] Dit was approximately 1.2 × 10⁻⁶ units from the control sample. 11 cm 2 ·eV 1 Reduced to 7 × 10⁻⁶ for nitrogen-annealed samples 10 cm 2 ·eV 1 This reflects an improvement in the interface state of the evaluated contact interface. The interface, along with the buried oxide layer, underwent heat treatment; the decrease in leakage current provides test results indicating improved insulation performance.

[0031] Thus, the inert atmosphere insulation stage after film formation allows the buried oxide layer to undergo structural adjustment before the formation of the top silicon layer. The specific results of the above-mentioned high-purity nitrogen treatment illustrate its role in the optical state, interface state, and leakage current performance of the buried oxide layer. The densified buried oxide layer is then retained in the fabricated SOI wafer.

[0032] Figure 1Step S106 in the diagram represents the formation of the top silicon layer. For example, a donor wafer is provided as the silicon source, hydrogen ion implantation is performed on the donor wafer, and then the donor wafer is bonded to a buried oxide layer on a support substrate. After subsequent annealing and silicon layer transfer, a top silicon layer from the donor wafer is left on the side of the buried oxide layer away from the support substrate. The support substrate and its original buried oxide layer are retained in the finished product, and the resulting three-layer structure can be used as an SOI substrate for subsequent device fabrication.

[0033] After the densification annealing described above and before the formation of the top silicon layer, the interface between the supporting substrate and the buried oxide layer can also be passivated.

[0034] Specifically, after densification and heat treatment, the oxide wafer is cooled to a passivation temperature below the annealing temperature at a set cooling rate. A hydrogen-containing mixed atmosphere is introduced into the heat treatment furnace tube, and the wafer is held at the passivation temperature for a second preset time. This process performs hydrogen passivation on the interface between the buried oxide layer and the supporting substrate. The second preset time represents the holding time at the passivation temperature and the corresponding atmosphere, excluding the previous cooling time.

[0035] This further processing corresponds to Figure 1 Step S104 is described in the text. For processes without additional hydrogen passivation, step S106 can be performed after step S103; for processes with additional hydrogen passivation, step S104 is performed first, followed by the formation of the top silicon layer. Step S105 represents the process evaluation to be carried out as needed, and the evaluation information can be used for parameter selection of subsequent samples.

[0036] The interface passivation here involves treating the contact interface between the buried oxide layer and the supporting substrate to reduce the interface state density. The initial high-temperature inert atmosphere annealing is used for densification, while the subsequent process further improves the interface in a lower-temperature hydrogen-containing environment. Through cooling and atmosphere change, the already densified interface undergoes further treatment suitable for hydrogen passivation. These two processes together improve the buried oxide layer and interface state of the oxide wafer.

[0037] Both the Dit (distillation substrate) before and after hydrogen treatment target the interface between the original supporting substrate and the buried oxide layer. By comparing the Dit after the initial annealing and after the additional passivation, the changes brought about by the subsequent passivation can be observed; this interface and the interface on one side of the subsequently formed top silicon layer are located on opposite sides of the buried oxide layer.

[0038] In some embodiments, the passivation temperature is 390°C to 500°C. For example, after densification at 1130°C, the furnace temperature is lowered to 420°C and held in a hydrogen-containing mixed atmosphere for 40 minutes. This temperature and time, together with the gas composition described later, determine the interface treatment conditions in this specific embodiment.

[0039] A hydrogen-containing mixed atmosphere can be a mixture of nitrogen and hydrogen, with hydrogen comprising 5% to 12% by volume and the remainder being nitrogen, corresponding to a nitrogen gas fraction of 88% to 95%. The proportions of the two gases correspond to each other, and the sum is 100%. For example, the volume fraction of hydrogen is 8%, and the volume fraction of nitrogen is 92%. The hydrogen gas fraction is the proportion of hydrogen volume to the total volume of the mixed gas, which is also called the forming gas.

[0040] For example, using the same film formation method as the aforementioned nitrogen-treated samples, an oxide wafer with a buried oxide layer thickness of 1.5 μm was prepared upon completion of oxidation. After holding at 1130°C for 3 hours in high-purity nitrogen, the furnace temperature was lowered to 420°C, and a nitrogen-hydrogen mixture with a hydrogen gas fraction of 8% was introduced and held for 40 minutes. Before forming the top silicon layer, the oxide wafer sample that had undergone the above combined treatment was subjected to interface state, leakage current, and breakdown field strength tests.

[0041] Under these combined processing conditions, the Dit between the supporting substrate and the buried oxide layer was measured to be 2.8 × 10⁻⁶. 10 cm -2 ·eV -1 The leakage current is further reduced compared to the sample that only underwent nitrogen densification.

[0042] Compared with the aforementioned 7×10 10 cm -2 ·eV -1 Compared with the results of nitrogen treatment, the interface state density continued to decrease after additional hydrogen treatment, indicating that the contact interface that has already undergone high-temperature nitrogen treatment can still be further improved through subsequent passivation.

[0043] The above results correspond to a complete treatment combination: annealing at 1130℃ for 3 hours in high-purity nitrogen, followed by passivation at 420℃ for 40 minutes with a hydrogen integral of 8%. Reducing the interface states helps decrease charge trapping and leakage channels associated with the contact interface, providing a material basis for substrates used in high-voltage, high-reliability SOI power devices.

[0044] The above thermal oxidation film formation process will be further explained below.

[0045] In some embodiments, thermal oxidation includes sequential wet oxidation and dry oxidation. Wet oxidation uses an oxidizing atmosphere containing water vapor, while dry oxidation uses a dry oxygen atmosphere. Both processes thermally oxidize the support substrate to form a buried oxide layer for subsequent densification.

[0046] First, the main body thickness of the buried oxide layer is grown through wet oxygen oxidation, and then the area near the supporting substrate and the contact interface are further grown and modified through dry oxygen oxidation. The portions formed in both stages together constitute the same buried oxide layer. After film formation, densification and thermal insulation are performed so that the main body of the formed buried oxide layer and the area near the interface can undergo post-processing together.

[0047] The wet oxidation temperature can be 950℃~1130℃, and the dry oxidation temperature can be 1050℃~1150℃. For example, if the wet oxidation temperature is 1100℃ and the dry oxidation temperature is 1130℃, the total film thickness after the two stages is 1.5μm, followed by densification annealing at 1130℃. When other oxidation temperatures are selected, the subsequent annealing temperature is still determined according to the highest temperature in each oxidation stage.

[0048] In one specific film formation method, the wet oxygen oxidation temperature is 1050℃~1120℃, and oxygen carrying water vapor is introduced at a flow rate of 1L / min~2L / min. The thickness grown in the wet oxygen stage accounts for 85%~92% of the target total film thickness, making this stage the main body for the growth of the buried oxygen layer.

[0049] The process is then switched to a pure dry oxygen atmosphere and dry oxygen oxidation is performed at 1100℃~1150℃ for 30min~120min to complete the growth of the remaining thickness and improve the interface quality between the buried oxide layer and the supporting substrate. The furnace pressure is maintained at atmospheric pressure throughout the oxidation process. In terms of film formation capability, this combined oxidation method can obtain silicon oxide films with a thickness of not less than 1μm, for example, 2μm~3μm; when used in the aforementioned SOI preparation scheme, the thickness of the buried oxide layer at the completion of thermal oxidation is selected to be not less than 1.5μm.

[0050] In the specific film formation method described above, the time ratio of the wet oxygen stage to the dry oxygen stage can be approximately 1:1. This time ratio, along with the proportion of the wet oxygen stage to the total film thickness (85%–92%), describes the processing time and growth result, respectively. Within the aforementioned process range, reducing the proportion of the wet oxygen stage in the total processing time of the two stages is beneficial for improving interface quality, but it also reduces production capacity. Therefore, the processing time for the two stages can be allocated based on the target film thickness, interface requirements, and production cycle time.

[0051] For example, the 1.5 μm mentioned is the overall film thickness after both the wet oxygen and dry oxygen stages are completed, and the portions formed in both stages are included in this total thickness. Although the dry oxygen stage and the subsequent nitrogen densification can use the same temperature, their processing atmospheres and uses are different, and the 3-hour holding time indicated by the first preset time does not include the time of the previous dry oxygen oxidation.

[0052] In some implementations, the heating and cooling processes are performed at rates of 2.5°C / min to 4.5°C / min, for example, 3°C / min, within a temperature range of 400°C to 1150°C. This rate represents the amount of temperature change per unit time within the corresponding heating or cooling segment. Selecting a slower temperature change within this range is beneficial for controlling the impact of thermal stress on the wafer and buried oxide layer.

[0053] Too low a heating / cooling rate will prolong processing time and reduce throughput; when the rate exceeds 4.5℃ / min, the wafer may deform due to thermal stress, increasing the risk of buried oxide layer defects. Therefore, the above implementation method of 2.5℃ / min to 4.5℃ / min takes into account both the processing cycle and the quality risks caused by temperature changes.

[0054] For example, within the stated temperature range, the temperature is increased to 1130℃ at a rate of 3℃ / min; after the densification holding period, the temperature is decreased at a rate of 3℃ / min. For the passivation process at 420℃, the temperature is reduced to 420℃ before entering the holding period. The heating and cooling rates correspond to the temperature change process; the holding period is not included in this heating and cooling interval.

[0055] 400℃~1150℃ indicates the temperature range applicable to the above rate settings, and does not mean that each process goes through both ends of this range. For example, when the annealing temperature is 1130℃ and the passivation temperature is 420℃, the aforementioned cooling section is located within this temperature range.

[0056] Thermal oxidation and densification annealing can be carried out sequentially in the same heat treatment furnace tube. First, an oxidizing atmosphere is introduced into the furnace tube to form an oxygen-buried layer. After thermal oxidation is completed, the atmosphere is switched to high-purity nitrogen, so that the same furnace tube can be used for film formation and subsequent densification treatment.

[0057] For example, a vertical furnace tube is used to complete a combination of wet and dry oxygen oxidation to obtain a buried oxide layer with a total thickness of 1.5 μm. Then, the atmosphere is switched, and the layer is held at 1130 °C for 3 hours in high-purity nitrogen. If necessary, the furnace temperature is further reduced, and a nitrogen-hydrogen mixed gas is introduced at 420 °C and held for 40 minutes. The obtained oxide wafer is then used to form an SOI wafer.

[0058] The above stages are connected by temperature and atmosphere settings, and while retaining the mainstream manufacturing route of SOI substrate, the buried oxide layer and the support side interface before the formation of the top silicon layer are strengthened.

[0059] The supporting substrate can be a single-crystal silicon substrate, and its crystal orientation is not particularly limited. For example, the specific experiment mentioned above used... <100> A single-crystal silicon substrate with a specific crystal orientation. This substrate provides the surface for the buried oxide layer and undergoes annealing together with the buried oxide layer after film deposition.

[0060] Prior to thermal oxidation, a complete RCA cleaning is performed on the support substrate to pre-treat the silicon surface that will subsequently undergo oxidation. The above substrate preparation and cleaning correspond to... Figure 1 In step S101, after cleaning, the process proceeds to the thermal oxidation process.

[0061] Figure 1Step S105 indicates that the processing results are evaluated. For example, ellipsometry, capacitance-voltage (CV) testing, and current-voltage (IV) testing are used to obtain optical and electrical information of the buried oxide layer. The evaluation of the oxide wafer is carried out after the corresponding densification or passivation treatment is completed and before the formation of the top silicon layer, and the records obtained are used to compare the process conditions and their results.

[0062] In addition to comparing the specific conditions mentioned above, multiple sets of correlation experiments can be conducted: changing the thermal oxidation temperature, wet oxidation time, and dry oxidation modification time; setting nitrogen annealing temperature points of 1110℃, 1130℃, and 1150℃; and setting annealing time points of 2h, 3h, and 4h. In this set of correlation experiments, the oxide wafer samples all underwent a complete densification and passivation process. Before forming the top silicon layer, the refractive index, fixed charge Qf, leakage current, and breakdown field strength of the buried oxide layer, as well as the Dit between the buried oxide layer and the supporting substrate, were measured.

[0063] The sampling points mentioned above are used to examine the impact of changes in process parameters and may also include comparative conditions. For the conditions intended for use in the aforementioned preparation method, the annealing temperature should not be lower than the highest oxidation temperature at which the sample group formed a film. For example, if the highest oxidation temperature is 1130°C, sampling points annealed at 1110°C can be used for comparison with sampling points that satisfy the above temperature relationship.

[0064] The following four comparative tests used RCA-cleaned materials. <100> A silicon substrate with crystal orientation underwent a combined wet and dry oxygen thermal oxidation process within a vertical furnace tube. The wet oxygen oxidation temperature was 1100℃, and the dry oxygen oxidation temperature was 1130℃, resulting in a buried oxide layer thickness of 1.5 μm at the end of oxidation. After oxidation, a high-purity nitrogen atmosphere was switched, and densification annealing was performed at 1130℃ for 3 hours, with a heating / cooling rate of 3℃ / min. Ellipsometry, CV, and IV measurements were performed on the sample after nitrogen annealing and before the formation of the top silicon layer.

[0065] Under the above baseline conditions, keeping the holding time at 3 hours and other conditions unchanged, the annealing temperature was varied. The refractive index corresponding to 1100℃ was 1.458, and the Dit was less than 6.1 × 10⁻⁶. 10 cm -2 ·eV -1 The refractive index at 1150℃ is 1.465, and Dit is less than 5 × 10⁻⁶. 10 cm -2 ·eV -1 Keeping the annealing temperature at 1130℃ and other conditions constant, the holding time was varied. For 2 hours, the refractive index was 1.457 and the Dit was less than 5.5 × 10⁻⁶. 10 cm -2 ·eV -1 The refractive index corresponding to 4h is 1.461, and Dit is less than 5 × 10⁻⁴.10 cm -2 ·eV -1 .

[0066] The annealing temperature of the 1100℃ annealing group was lower than that of the dry oxygen oxidation group at 1130℃. As a comparison condition, it was used to examine the effect of annealing temperature changes on the properties of the buried oxide layer and interface.

[0067] These records can be used to observe the correspondence between annealing conditions and optical and electrical results. Different indicators reflect different states of the buried oxide layer or interface; when selecting process conditions, a comprehensive evaluation based on the target performance can be conducted. The results of each group are recorded together with the corresponding film-forming conditions, annealing, and passivation processes to distinguish between results from nitrogen treatment alone and results from the complete combined treatment.

[0068] When establishing the correlation, the oxidation temperature, wet oxygen and dry oxygen time, annealing temperature and holding time of each group were correlated with the measured performance of that group, and the changes of each index under different conditions were compared. Through these correlation records, a process-performance correlation model was established between oxidation conditions, annealing parameters, refractive index and electrical properties, which was used to select applicable process conditions.

[0069] The aforementioned correlation model can be used for process replication between equipment and convergence of mass production process windows. In the subsequent sample preparation, the thermal oxidation and densification annealing parameters are selected based on the evaluation results, and the process conditions that meet the corresponding performance requirements are determined step by step. Figure 1 The dashed line pointing to steps S102 and S103 indicates this information usage relationship. This evaluation arrangement provides a replicable and quantifiable process development path for the domestic manufacturing of micron-scale buried oxide layer SOI wafers.

[0070] Densification and interface passivation of the buried oxide layer help reduce fixed and trapped charges, decrease scattering and leakage current paths associated with the treated interface, and improve insulation breakdown performance and long-term reliability of subsequent devices. These effects can be evaluated by combining fixed charge, trapped charge, leakage current, and breakdown tests, with each result examined separately according to the corresponding treatment stage and evaluation object.

[0071] Before forming the top silicon layer, an oxide wafer processed as described above can be obtained.

[0072] Reference Figure 2 The oxide wafer 100 includes a support substrate 120 and a buried oxide layer 140, the buried oxide layer 140 being located on the surface of the support substrate 120 and in direct contact with the support substrate 120. This contact point is the interface evaluated by Dit in the aforementioned oxide wafer test.

[0073] The buried oxide layer and interface state of oxide wafer 100 are determined by the actual processing performed. For example, the buried oxide layer 140 has undergone densification insulation at 1130°C for 3 hours with high-purity nitrogen, or it has undergone further nitrogen-hydrogen passivation at 420°C. Oxide wafers in both processing states can be used as support wafers for subsequent SOI wafer formation.

[0074] The buried oxide layer 140 can be formed by sequential wet oxidation and dry oxidation. Wet oxidation mainly forms the bulk thickness, while dry oxidation continues to grow and modify the area near the support substrate 120 and the contact interface. The resulting buried oxide layer 140 is then subjected to subsequent densification treatment as a whole. Figure 2 The buried oxygen layer 140 is represented as the overall structure.

[0075] The wet oxygen-formed portion and the dry oxygen-modified portion do not have a clearly distinguishable intrafilm boundary through direct observation. Differences between these portions can be evaluated or differentiated using techniques such as etching ratio. The names used here are to describe the film formation process and its function, and do not represent two independent material layers with different chemical compositions.

[0076] In some embodiments, before the formation of the top silicon layer, the refractive index of the buried oxide layer 140 in the processed oxide wafer 100 is 1.460 to 1.464, corresponding to the fluctuation range of 1.462 ± 0.002 in the aforementioned experiment. This fluctuation is used to represent the range of variation in the refractive index result.

[0077] The buried oxide layer 140 in the aforementioned oxide wafer was evaluated using spectral ellipsometry (SE). The spectral scanning wavelength range was 190 nm to 1700 nm, and the reported refractive index was the average refractive index at different measurement points under the same wavelength. When comparing different samples, consistent measurement and value-taking methods were used to ensure the comparability of results across groups. The object evaluated by spectral ellipsometry was the entire buried oxide layer 140.

[0078] In the case of further hydrogen passivation, the distance between the support substrate 120 and the buried oxide layer 140 can be no greater than 5 × 10⁻⁶. 10 cm -2 ·eV -1 .

[0079] Dit was calculated using the high- and low-frequency CV method to obtain the distribution of interface state density as a function of surface potential, and the average value of this distribution was used to characterize the interface state density. For example, after annealing at 1130℃ for 3 hours in high-purity nitrogen, passivation was performed at 420℃ for 40 minutes with a hydrogen gas integral of 8%, and the measured Dit was 2.8 × 10⁻⁶. 10 cm -2 ·eV -1This result corresponds to the contact interface between the support substrate 120 and the buried oxide layer 140.

[0080] The oxide wafer 100 can also be characterized by the thickness of the buried oxide layer 140 after processing. In some oxide wafer fabrication methods, the thickness of the buried oxide layer after processing is 0.8 μm to 3.5 μm; in the aforementioned SOI wafer embodiment where the thickness of the finished buried oxide layer is not less than 1.5 μm, an oxide wafer with a buried oxide layer thickness of not less than 1.5 μm after processing is selected, for example, in the case where the thickness of the buried oxide layer after processing is 1.5 μm to 3.5 μm.

[0081] For oxide wafers that have only undergone nitrogen densification, the buried oxide layer thickness is determined after this process; for oxide wafers that have undergone additional hydrogen passivation, the buried oxide layer thickness is determined after the subsequent processing. For example, for a sample with a nominal buried oxide layer thickness of 1.5 μm, the film thickness fluctuation after processing is less than 5 nm.

[0082] Figure 2 In this context, 't' represents the total dimension of the buried oxide layer 140 along its thickness direction, with its two ends located at the contact surface between the supporting substrate 120 and the buried oxide layer 140, and at the surface of the buried oxide layer 140 facing away from the supporting substrate 120, respectively. The film thickness at the completion of oxidation and the thickness after processing correspond to different process points, and the range of buried oxide layer thickness in the product is determined according to the thickness after the corresponding processing.

[0083] On the other hand, this application also provides a silicon-on-insulator (SOI) wafer 200 prepared according to the above-described preparation method. This wafer can also be referred to as an SOI substrate and is used for subsequent semiconductor device manufacturing.

[0084] Reference Figure 3 The silicon-on-insulator wafer 200 includes a support substrate 120, a buried oxide layer 140, and a top silicon layer 220 stacked sequentially. The support substrate 120 and the buried oxide layer 140 are the support substrate and buried oxide layer retained from the aforementioned oxide wafer 100, respectively, and the buried oxide layer in the finished product is solely composed of the original buried oxide layer on the support side. The top silicon layer 220 is located on the side of the buried oxide layer 140 facing away from the support substrate 120.

[0085] Specifically, the original oxide wafer 100 is retained as the support wafer. After hydrogen ion implantation, the donor wafer is bonded to the buried oxide layer 140, and after subsequent annealing and silicon layer transfer, the top silicon layer 220 is left on the buried oxide layer 140. Thus, the original buried oxide layer 140 is retained between the support substrate 120 and the top silicon layer 220, and serves as electrical isolation.

[0086] In some embodiments, the thickness of the buried oxide layer 140 on the silicon-on-insulator wafer 200 is not less than 1.5 μm, and the refractive index of the buried oxide layer, measured using an ellipsometer, is 1.460~1.464. The interface state density between the buried oxide layer 140 and the supporting substrate 120 may not exceed 5 × 10⁻⁶. 10 cm -2 ·eV -1 These parameters respectively characterize the size, optical state, and electrical state of the embedded oxide layer and the support-side interface in the corresponding products.

[0087] The original interface between the supporting substrate 120 and the buried oxide layer 140 is retained after the formation of the top silicon layer 220, forming the support-side interface of the SOI wafer. The interface between the top silicon layer 220 and the buried oxide layer 140 is formed during subsequent bonding and layer transfer processes, with the two interfaces located on opposite sides of the buried oxide layer 140.

[0088] In the above preparation method, the subsequent processes for forming the top silicon layer retain the original buried oxide layer, and no separate special processing steps are set for the buried oxide layer, allowing the buried oxide layer, which has undergone densification treatment in the early stage, to continue to serve its electrical isolation function in the finished product. During the above preparation process, after bonding, the thickness and refractive index of the buried oxide layer meet the aforementioned product parameter requirements; subsequent processes do not include process conditions that affect the thickness of the buried oxide layer and the interface state density on the support side. Annealing after donor bonding is a heat treatment process during the formation of the top silicon layer, and the aforementioned oxide wafer test data are still recorded according to their actual measurement stages.

[0089] Throughout this application, the terms "first," "second," etc., are used merely for descriptive purposes and should not be considered restrictive. Furthermore, although this application has been described with reference to exemplary embodiments, it should be understood that this application is not limited to the specific embodiments described and shown herein. Various modifications to the exemplary embodiments can be made by those skilled in the art without departing from the scope defined by the claims of this application.

[0090] The features mentioned and / or shown in the above description of exemplary embodiments of this application may be combined in the same or similar manner with one or more other embodiments, combined with features in other embodiments, or substituted for corresponding features in other embodiments. Such combinations or substitutions should also be considered as including within the scope of protection of this application.

Claims

1. A method for fabricating a silicon-on-insulator wafer, characterized in that, The preparation method includes: Provide a supporting substrate; The supporting substrate is placed inside a heat treatment furnace tube, and an oxidizing atmosphere is introduced into the heat treatment furnace tube to thermally oxidize the supporting substrate, thereby forming a buried oxide layer on the surface of the supporting substrate. The thickness of the buried oxide layer is not less than 1.5 μm. After the thermal oxidation is completed, an inert atmosphere is introduced into the heat treatment furnace tube, and the oxide layer is densified by holding it at the annealing temperature for a first preset time. The annealing temperature is not lower than the highest oxidation temperature used in the thermal oxidation. A top silicon layer is formed on the side of the buried oxide layer away from the supporting substrate to prepare the silicon-on-insulator wafer.

2. The method for fabricating silicon-on-insulator wafers according to claim 1, characterized in that, After densification annealing and before the formation of the top silicon layer, the process further includes an interface passivation step: cooling the support substrate on which the buried oxide layer is formed to the passivation temperature at a set cooling rate, introducing a hydrogen-containing mixed atmosphere into the heat treatment furnace tube, and holding at the passivation temperature for a second preset time to perform hydrogen passivation treatment on the interface between the buried oxide layer and the support substrate.

3. The method for preparing a silicon-on-insulator wafer according to claim 2, characterized in that, The passivation temperature is 390℃~500℃, and the second preset time is 40min.

4. The method for fabricating silicon-on-insulator wafers according to claim 3, characterized in that, The hydrogen-containing mixed atmosphere is a mixture of nitrogen and hydrogen, wherein the volume fraction of hydrogen in the mixed gas is 5% to 12%, and the remainder is nitrogen.

5. The method for fabricating silicon-on-insulator wafers according to claim 1, characterized in that, The thermal oxidation includes wet oxidation and dry oxidation. The wet oxidation is used to grow the main body of the buried oxide layer on the surface of the supporting substrate, and the dry oxidation is used to perform interface modification on the interface between the buried oxide layer and the supporting substrate after the main body of the buried oxide layer is formed.

6. The method for fabricating a silicon-on-insulator wafer according to claim 5, characterized in that, The temperature for wet oxidation is 950℃~1130℃, and the temperature for dry oxidation is 1050℃~1150℃.

7. The method for fabricating silicon-on-insulator wafers according to claim 1, characterized in that, The densification annealing temperature is 1130℃, the first preset time is 3h, and within the temperature range of 400℃ to 1150℃, the heating rate before densification annealing is 2.5℃ / min to 4.5℃ / min, and the cooling rate after the densification annealing holding is 2.5℃ / min to 4.5℃ / min.

8. The method for fabricating silicon-on-insulator wafers according to claim 1, characterized in that, The inert atmosphere is a nitrogen atmosphere, and the purity of the nitrogen is not less than 99.9999%. After the thermal oxidation is completed, the oxidizing atmosphere in the heat treatment furnace tube is switched to the nitrogen atmosphere to carry out the densification annealing.

9. The method for fabricating silicon-on-insulator wafers according to claim 1, characterized in that, The supporting substrate has a crystal orientation of <100> The single-crystal silicon substrate, prior to the thermal oxidation, also includes an RCA cleaning step for the supporting substrate.

10. A silicon-on-insulator wafer, characterized in that, The silicon-on-insulator wafer is prepared by the method for preparing a silicon-on-insulator wafer according to any one of claims 1 to 9, wherein the silicon-on-insulator wafer comprises: Support substrate; The buried oxide layer located on the supporting substrate; and The top silicon layer located on the buried oxide layer, The thickness of the buried oxide layer is not less than 1.5 μm, and the refractive index of the buried oxide layer is measured to be 1.460~1.464 using an ellipsometer.

11. The silicon-on-insulator wafer according to claim 10, characterized in that, The interface state density between the buried oxide layer and the supporting substrate is no greater than 5 × 10⁻⁶. 10 cm -2 ·eV -1 .