Methods for manufacturing epitaxial wafers

By using hydrogen peroxide aqueous solution for cleaning and appropriate temperature control, the problem of surface roughness deterioration during oxygen atom layer formation was solved, enabling the manufacture of high-quality epitaxial wafers and improving the crystallinity and gettering effect of epitaxial growth.

CN123126074APending Publication Date: 2026-11-17SHIN ETSU HANDOTAI CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202580024200.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-03-29
Filing Date
2025-02-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies can easily lead to a deterioration in wafer surface roughness when forming oxygen atom layers, and improper control of oxygen concentration can affect the quality of epitaxial growth, resulting in a decline in the quality of epitaxial wafers.

Method used

A cleaning method containing hydrogen peroxide aqueous solution was adopted. By adjusting the cleaning conditions, the oxygen concentration of the oxygen atom layer was controlled while suppressing the surface roughness, thus forming a high-quality oxygen atom layer, which was then epitaxially grown at an appropriate temperature.

Benefits of technology

It effectively suppressed the deterioration of wafer surface roughness, achieved efficient formation of oxygen atom layers and appropriate control of oxygen concentration, produced high-quality epitaxial wafers, and improved crystallinity and gettering effect after epitaxial growth.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123126074A_ABST
    Figure CN123126074A_ABST
Patent Text Reader

Abstract

This invention discloses a method for manufacturing epitaxial wafers, specifically a method for forming a single-crystal silicon layer on a single-crystal silicon wafer. The method is characterized by comprising the following steps: a hydrofluoric acid cleaning step, in which the native oxide film on the surface of the single-crystal silicon wafer is removed using a cleaning solution containing hydrofluoric acid; an oxygen atom layer formation step, in which an oxygen atom layer is formed on the surface of the single-crystal silicon wafer after the native oxide film has been removed, through cleaning; and an epitaxial growth step, in which the single-crystal silicon layer is epitaxially grown on the surface of the single-crystal silicon wafer on which the oxygen atom layer has been formed using a vapor phase growth method; and, in the oxygen atom layer formation step, the cleaning solution uses a cleaning solution containing at least water containing hydrogen peroxide. Therefore, a method for manufacturing epitaxial wafers is provided that does not deteriorate the surface roughness of the wafer and can efficiently form and control the oxygen atom layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for manufacturing epitaxial wafers. Background Technology

[0002] For silicon substrates used to form semiconductor devices such as solid-state imaging elements and other transistors, the ability to getter elements, such as heavy metals, that can interfere with device characteristics is required. Regarding gettering, the following methods have been proposed and put into practical use: methods that create a polycrystalline silicon (Poly-Si) layer on the back side of the silicon substrate, methods that form a damaged layer through sandblasting, and various methods such as using silicon substrates with high boron concentrations or forming precipitates. Gettering via oxygen evolution refers to the process of capturing metals with a high ionization tendency (low electronegativity) to getter oxygen with high electronegativity.

[0003] In addition, so-called proximity gettering has been proposed, which involves forming a getter layer near the active region of a device. Examples include substrates obtained by epitaxial growth of silicon on ion-implanted carbon substrates. During gettering, elements need to diffuse to the getter sites (compared to the state where metals exist in elemental form, the overall energy of the system decreases through metal bonding or clustering at these sites). The diffusion coefficient of the metal elements contained in silicon varies depending on the element, and considering the recent trend of increasingly lower process temperatures preventing metals from diffusing to the getter sites, a proximity gettering method has been proposed. Existing technical documents Patent documents

[0004] Patent Document 1: Japanese Patent Application Publication No. 2022-146664 Patent Document 2: Japanese Patent Application Publication No. 2021-111696 Patent Document 3: International Publication No. 2022 / 158148 Patent Document 4: Japanese Patent Application Publication No. 2024-007890 Patent Document 5: Japanese Patent Application Publication No. 2009-016637 Summary of the Invention The technical problem that the invention aims to solve

[0005] It is believed that if oxygen can be used for near-neighbor gettering, silicon substrates with very powerful getter layers can be created. In particular, if the epitaxial wafer has an oxygen atom layer in the middle of the epitaxial layer, it can reliably getter metal impurities even in recent low-temperature processes. In addition to gettering, it is also expected to suppress the diffusion of dopants such as boron and phosphorus.

[0006] As described above, epitaxial wafers with an oxygen atom layer in the middle of the epitaxial layer exhibit improved device performance compared to general epitaxial wafers without an oxygen atom layer. Furthermore, this state of high-concentration doping with a thickness of several atomic layers is called Delta doping (also known as "δ doping"). For example, when the doping element is oxygen, it is called oxygen δ doping. That is, an epitaxial wafer with an oxygen atom layer in the middle of the epitaxial layer is an oxygen δ-doped epitaxial wafer. Hereinafter, in this invention, oxygen atom layer and oxygen δ-doped layer have the same meaning.

[0007] Next, prior art methods for manufacturing oxygen-δ-doped epitaxial wafers will be described. Patent Document 1 discloses a method for manufacturing oxygen-δ-doped epitaxial wafers, which includes: performing a process of removing the natural oxide film on the surface of a silicon wafer at a temperature below 700°C, followed by performing one or more processes to form an oxygen atom layer and a single-crystal silicon layer, thereby manufacturing an oxygen-δ-doped epitaxial wafer. The oxygen atom layer and single-crystal silicon layer formation process involves forming a planar concentration of 1×10⁻⁶ on the surface of the single-crystal silicon wafer using nitric oxide. 15 atoms / cm 2 The following oxygen atom layer is formed, and a single-crystal silicon layer is formed on the oxygen atom layer by epitaxial growth.

[0008] Patent document 2 describes a method for manufacturing an oxygen-δ-doped epitaxial wafer: after removing the natural oxide film on the wafer surface composed of group IV elements including silicon in a hydrogen-containing atmosphere, an oxygen atom layer is formed by oxidation treatment, and a single-crystal silicon layer is further epitaxially grown on the oxygen atom layer, thereby manufacturing an oxygen-δ-doped epitaxial wafer.

[0009] Patent document 3 describes a method for manufacturing an oxygen-δ-doped epitaxial wafer: after removing the natural oxide film on the surface of a single-crystal silicon wafer with fluoric acid, the wafer is rinsed with pure water or placed in an oxygen-containing atmosphere to form an oxygen atom layer. Then, a single-crystal silicon layer is epitaxially grown on the oxygen atom layer, thereby manufacturing an oxygen-δ-doped epitaxial wafer. Furthermore, it discloses a method for setting the oxygen planar concentration of the oxygen atom layer to 1×10⁻⁶. 15 atoms / cm 2 The following method enables the growth of single-crystal silicon layers without the formation of dislocations or stacking faults on the oxygen atom layer. On the other hand, if the oxygen concentration is too low, the gettering function may not be effective.

[0010] Patent document 4 describes a method for manufacturing an epitaxial wafer doped with oxygen δ: after forming an oxide film on the surface of a silicon wafer using an oxidizing solution, the oxide film is thinned to form an oxygen atom layer, and then a single-crystal silicon layer is epitaxially grown on the oxygen atom layer, thereby manufacturing an epitaxial wafer doped with oxygen δ.

[0011] Patent document 5 describes a method in which an oxide film is formed on a silicon substrate using an oxidizing aqueous solution, followed by the formation of an epitaxial film to create an SOI structure. Alternatively, this method involves forming a silicon layer on a chemical oxide film of at least 1 nm in size, rather than on a layer of oxygen atoms.

[0012] Here, the comparative example of Patent Document 4 describes the following results: For oxide films formed using oxidizing solutions, when a Si epitaxial film is deposited on an oxide film without thin-film treatment, the number of defects reaches the upper limit of measurement (approximately 20,000) (paragraph

[0120] ). In contrast, it is also described that in Example 1, where thin-film treatment was performed in a hydrogen atmosphere, the number of defects is 27 or less, and a single-crystal silicon epitaxial layer can be formed on the oxygen atom layer without defects. In addition, paragraph

[0103] describes that when the amount of oxidation (the planar concentration of oxygen in the oxygen atom layer) is low, the crystallinity of the single-crystal silicon wafer is maintained, so it is possible to prevent the formation of defects in the epitaxial layer caused by the oxygen atom layer. Therefore, it can be anticipated that the reason why the number of defects reaches the upper limit of measurement when thin-film treatment is not performed is due to excessive oxidation. Furthermore, Patent Document 5 does not disclose the evaluation results of dislocations and stacking faults in the Si film layer. Based on Patent Documents 1 to 4, it can be inferred that the quality of dislocations, stacking faults, etc., may be deteriorated. Therefore, to manufacture high-quality epitaxial wafers doped with oxygen δ, it is necessary to properly control the planar concentration of oxygen in the oxygen atom layer.

[0013] Here, the inventors investigated the technique for forming an oxygen atom layer by rinsing with pure water as described in Patent Document 3, but found that the reactivity was low at room temperature and the oxygen concentration of the formed oxygen atom layer was low. They then discovered that rinsing with heated pure water (i.e., warm pure water) increased the reactivity and allowed for efficient control of the oxygen concentration, but it was also clarified that the Si itself was etched during the formation of this oxygen atom layer, leading to a significant deterioration in surface roughness. Thus, if the surface roughness is already poor before epitaxial growth, the quality after epitaxial growth will further deteriorate.

[0014] Based on the above, it is believed that the higher the oxygen concentration of the oxygen atomic layer, the rougher the surface before epitaxial growth, and the worse the quality after epitaxial growth. That is, if the oxygen concentration of the oxygen atomic layers is relatively uniform, the better the surface roughness before epitaxial growth, the better the quality after epitaxial growth. Therefore, good surface roughness before epitaxial growth is preferable.

[0015] In addition, the method in Patent Document 4 has the following technical problem compared with Patent Document 3: a thinning process is required to make the oxide film thinner, which increases the number of processes.

[0016] Therefore, a method is sought that does not worsen the surface roughness of the wafer and can efficiently form and control oxygen atom layers.

[0017] The present invention is made to solve the above-mentioned problems and aims to provide a method for manufacturing an epitaxial wafer, which in particular can appropriately control the planar concentration of oxygen in the oxygen atom layer in a manner that does not deteriorate the quality of the silicon layer after epitaxial growth. More specifically, it provides a method for manufacturing an epitaxial wafer that does not deteriorate the surface roughness of the wafer and can efficiently form and control the oxygen atom layer. Technical means to solve the problem

[0018] In order to achieve the above-mentioned objective, the inventors conducted an in-depth investigation into whether an oxygen atom layer could be formed on the surface of a silicon wafer by cleaning it with an aqueous solution containing hydrogen peroxide. As a result, they made a novel discovery that by adjusting the cleaning conditions, it is possible to control the planar concentration of oxygen in the oxygen atom layer while suppressing the deterioration of surface roughness, thereby completing the present invention.

[0019] That is, the present invention was made to achieve the above-mentioned objective, and provides a method for manufacturing an epitaxial wafer, which is a method for manufacturing an epitaxial wafer on which a single-crystal silicon layer is formed, characterized by comprising the following steps: a hydrofluoric acid cleaning step, in which the native oxide film on the surface of the single-crystal silicon wafer is removed by a cleaning solution containing hydrofluoric acid; an oxygen atom layer formation step, in which an oxygen atom layer is formed on the surface of the single-crystal silicon wafer on which the native oxide film has been removed by cleaning; an epitaxial growth step, in which the single-crystal silicon layer is epitaxially grown on the surface of the single-crystal silicon wafer on which the oxygen atom layer has been formed by vapor phase growth; and, in the oxygen atom layer formation step, the cleaning uses a cleaning solution containing at least water containing hydrogen peroxide.

[0020] According to this epitaxial wafer manufacturing method, the surface of a single-crystal silicon wafer can be oxidized using hydrogen peroxide in an aqueous solution while suppressing the deterioration of surface roughness, thereby efficiently forming an oxygen atom layer with appropriately controlled oxygen planar concentration. Furthermore, by performing epitaxial growth on such a single-crystal silicon wafer, high-quality epitaxial wafers can be manufactured.

[0021] In this case, it can be set that no process to thin the oxygen atom layer is performed after the oxygen atom layer formation process.

[0022] Therefore, there is no need to add an additional thinning process for the oxygen atom layer; the oxygen concentration of the oxygen atom layer can be appropriately controlled simply through the cleaning process.

[0023] At this point, the pH value of the cleaning solution containing hydrogen peroxide water can be set in the range of 4 to 7.

[0024] If the pH value is within this range, the oxygen atom layer can be formed more stably.

[0025] At this point, in the oxygen atom layer formation process, the planar concentration of oxygen in the oxygen atom layer can be set to 1×10⁻⁶. 15 atoms / cm 2 the following.

[0026] This reduces stacking faults and dislocations in epitaxially grown single-crystal silicon layers, resulting in layers with higher crystallinity.

[0027] At this time, in the epitaxial growth process, epitaxial growth can be carried out at a temperature above 450°C and below 800°C.

[0028] By growing at such a temperature, epitaxial growth can be carried out more stably without defects.

[0029] At this point, CMP processing can be performed on the surface of the single-crystal silicon layer after the epitaxial growth process.

[0030] This can improve the surface defects and roughness of the epitaxial layer.

[0031] At this time, the oxygen atom layer formation process and the epitaxial growth process can be alternated multiple times.

[0032] By setting up multiple layers of oxygen atoms in this way, it is possible to manufacture epitaxial wafers with higher gettering effect and dopant diffusion suppression effect than in the case of a single layer. Invention Effects

[0033] As described above, the epitaxial wafer manufacturing method according to the present invention can oxidize the surface of a single-crystal silicon wafer using hydrogen peroxide in an aqueous solution while suppressing the deterioration of surface roughness, thereby efficiently forming an oxygen atom layer with appropriately controlled oxygen planar concentration. Furthermore, by performing epitaxial growth on such a single-crystal silicon wafer, high-quality epitaxial wafers can be manufactured. Attached Figure Description

[0034] Figure 1 This is a flowchart illustrating an example of a method for manufacturing an epitaxial wafer according to the present invention. Figure 2 This is a diagram showing an epitaxial wafer manufactured by the epitaxial wafer manufacturing method of the present invention. Figure 3 This is a diagram showing an epitaxial wafer, which is fabricated by the epitaxial wafer manufacturing method of the present invention, having multiple layers of alternating oxygen atom layers and single-crystal silicon layers. Figure 4 This is a graph showing the relationship between the hydrogen peroxide concentration and the plane concentration of oxygen in the oxygen atom layer when cleaning is carried out under the conditions of cleaning solution temperature of 80°C and cleaning time of 3 minutes. Figure 5 This is a graph showing the relationship between the hydrogen peroxide concentration and the plane concentration of oxygen in the oxygen atom layer when cleaning is performed under the conditions of cleaning solution temperature of 25°C and cleaning time of 3 minutes. Figure 6 This is a graph showing the relationship between cleaning time and the plane concentration of oxygen in the oxygen atom layer when cleaning is performed under conditions of cleaning solution temperature of 25°C and hydrogen peroxide concentration of 10000 ppm (1% by mass). Figure 7 This is a graph showing the relationship between hydrogen peroxide concentration and surface roughness (Haze value) and etching rate when cleaning is performed with varying hydrogen peroxide concentrations. Figure 8 This is a graph showing the relationship between hydrogen peroxide concentration and surface roughness (Haze value) when cleaning is performed under conditions of cleaning solution temperature of 25°C and cleaning time of 3 minutes. Figure 9 This is a graph showing the relationship between hydrogen peroxide concentration and pH at a temperature of 25°C. Figure 10 This is a graph showing the evolution of Haze values ​​of Examples 1 and Comparative Examples 1-4 before cleaning, after cleaning, and after film formation. Figure 11 This is a graph showing the evolution of Haze values ​​of Examples 2 and Comparative Examples 5-8 before cleaning, after cleaning, and after film formation. Figure 12 This is a graph showing the oxygen concentration of the oxygen atom layer in Examples 3 and Comparative Examples 9-12. Figure 13 This is a TEM image showing a cross-sectional view of the epitaxial wafer of Example 3. Detailed Implementation

[0035] The present invention will now be described in detail, but the invention is not limited to these descriptions.

[0036] As mentioned above, in the fabrication of epitaxial wafers, there is a need for a method that can efficiently form and control oxygen atom layers without deteriorating the surface roughness of the wafer.

[0037] The inventors, through repeated and meticulous research into the aforementioned technical problems, discovered that a method for manufacturing epitaxial wafers, as described below, can oxidize the surface of a single-crystal silicon wafer while suppressing the deterioration of surface roughness, thereby efficiently forming an oxygen atom layer with appropriately controlled oxygen planar concentration. This manufacturing method is a method for manufacturing epitaxial wafers with a single-crystal silicon layer formed on a single-crystal silicon wafer, characterized by comprising the following steps: a hydrofluoric acid cleaning step, in which the native oxide film on the surface of the single-crystal silicon wafer is removed using a cleaning solution containing hydrofluoric acid; an oxygen atom layer formation step, in which an oxygen atom layer is formed on the surface of the single-crystal silicon wafer after the native oxide film has been removed through cleaning; and an epitaxial growth step, in which the single-crystal silicon layer is epitaxially grown on the surface of the single-crystal silicon wafer on which the oxygen atom layer has been formed using a vapor phase growth method; and, in the oxygen atom layer formation step, the cleaning uses a cleaning solution containing at least water containing hydrogen peroxide. Furthermore, it was discovered that by performing epitaxial growth on such a single-crystal silicon wafer, high-quality epitaxial wafers can be manufactured, thus completing this invention.

[0038] [Epipolar wafer] Figure 2 This diagram illustrates an epitaxial wafer manufactured by the epitaxial wafer manufacturing method of the present invention. The epitaxial wafer 10A according to the present invention has a single-crystal silicon layer 3 on a single-crystal silicon wafer 1, and an oxygen atom layer 2 between the single-crystal silicon layer 3 and the single-crystal silicon wafer 1.

[0039] Here, it is preferable that the oxygen planar concentration of the oxygen atom layer 2 in the epitaxial wafer 10A involved in the present invention is 1×10⁻⁶. 15 atoms / cm 2 The following applies. If an epitaxial wafer possesses an oxygen atom layer with such a range of oxygen planar concentrations, the epitaxially grown single-crystal silicon layer will have fewer stacking faults and dislocations, thus enabling the fabrication of a layer with higher crystallinity. It should be noted that there is no lower limit to the oxygen planar concentration, as long as it is greater than 0. It should also be noted that for stable gettering capability, a concentration of 1 × 10⁻⁶ is preferred. 13 atoms / cm 2 Of the above, 1×10 is a more preferred option. 14 atoms / cm 2 above.

[0040] The single-crystal silicon wafer 1 can be fabricated in any manner. For example, a CZ wafer fabricated using the Czochralski method (hereinafter referred to as the "CZ method") or an FZ wafer fabricated using the Floating Zone method (hereinafter referred to as the "FZ method") can be used. Alternatively, an epitaxial wafer formed by epitaxially growing single-crystal silicon on a single-crystal silicon wafer fabricated using the CZ method or the FZ method can also be used.

[0041] in addition, Figure 3 This diagram illustrates an epitaxial wafer 10B formed by alternating layers of oxygen atoms and single-crystal silicon on a single-crystal silicon wafer using the epitaxial wafer manufacturing method of the present invention. Figure 3 As shown, the epitaxial wafer manufacturing method of the present invention can produce an epitaxial wafer formed by repeatedly stacking an oxygen atom layer 2 and a single-crystal silicon layer 3 on a single-crystal silicon wafer 1. The uppermost surface is the single-crystal silicon layer 3.

[0042] [Epipolar wafer manufacturing methods] Figure 1 The diagram shows a flowchart of an example of a method for manufacturing an epitaxial wafer that forms a monocrystalline silicon layer on a monocrystalline silicon wafer, as described in this invention. Figure 1 The S1 process is the process of preparing the monocrystalline silicon wafer. Here, there is no particular limitation on the manufacturing method of the monocrystalline silicon wafer used as the substrate. It can be a monocrystalline silicon wafer manufactured by the CZ method or a monocrystalline silicon wafer manufactured by the FZ method. Alternatively, an epitaxial wafer formed by epitaxially growing monocrystalline silicon on a monocrystalline silicon wafer manufactured by the CZ or FZ methods can also be used.

[0043] [Hydrofluoric acid cleaning process] Figure 1 The S2 step is a hydrofluoric acid cleaning step, in which the natural oxide film is removed by a cleaning solution containing hydrofluoric acid (fluoric acid) (hereinafter referred to as "fluoric acid cleaning solution"). In this invention, what needs to be formed is not a natural oxide film, but an oxygen atom layer. Since the natural oxide film is too thick, it is necessary to completely remove the natural oxide film first, and then form an oxygen atom layer through the oxygen atom layer formation step in S3.

[0044] At this point, as long as the natural oxide film can be removed by hydrofluoric acid, the liquid agent used can be hydrofluoric acid alone, or a liquid agent containing other components, such as buffered hydrofluoric acid, can be used. The concentration of hydrofluoric acid only needs to be sufficient to remove the natural oxide film; for example, it can be set to 0.001% by mass or more and 60% by mass or less. More preferably, it can be set to 0.1% by mass or more and 10% by mass or less. The temperature of the hydrofluoric acid cleaning solution can be set to 10°C or more and 50°C or less. More preferably, it can be set to 20°C or more and 30°C or less.

[0045] The time for natural oxide film removal (cleaning) using hydrofluoric acid can be set until hydrophobicity is confirmed, for example, it can be set to 10 seconds or more but less than 1 hour. A time of 10 seconds or more allows for more reliable removal of the natural oxide film. Furthermore, setting it to less than 1 hour effectively maintains productivity. A time of 30 seconds or more but less than 360 seconds is more preferably preferred. Hydrofluoric acid treatment (cleaning) can be performed using batch cleaning equipment or single-plate cleaning equipment. Alternatively, hydrofluoric acid vapor can also be used to remove the oxide film.

[0046] [Oxygen Atom Layer Formation Process] Figure 1 The S3 process is an oxygen atom layer formation process as follows: an oxygen atom layer is formed on the silicon surface by cleaning the monocrystalline silicon wafer, which has had its native oxide film removed, with an aqueous solution containing at least hydrogen peroxide (hereinafter referred to as "H2O2 cleaning solution"). In monocrystalline silicon, oxygen atoms are stable at the bond centers between silicon atoms and their nearest silicon atoms; therefore, assuming the presence of a 1-atom-layer oxygen, the planar concentration of oxygen is 1.36 × 10⁻⁶. 15 atoms / cm 2 The oxygen concentration in the plane is 1×10⁻⁶. 15 atoms / cm 2 In this case, it is equivalent to 0.74 atomic layers.

[0047] Hydrogen peroxide acts as an oxidant, enabling an oxidation reaction on the silicon surface to form an oxygen atom layer. The planar concentration of oxygen can be determined, for example, by SIMS (Secondary Ion Mass Spectrometry). When measuring Si containing an oxide layer using SIMS, an oxygen peak is formed at the depth where the oxide layer is formed. The planar concentration can be determined by integrating the product of the volume concentration generated by each sputtering near the peak and the depth.

[0048] At this point, the oxygen concentration of the oxygen atom layer can be controlled by adjusting the temperature of the H2O2 cleaning solution, the hydrogen peroxide concentration, and the cleaning time. Figure 4 The figure shows the planar concentration of oxygen in the oxygen atom layer after cleaning with H2O2 cleaning solution at a temperature of 80℃ / 3 minutes, using H2O2 cleaning solution with hydrogen peroxide concentrations of 0, 100, 250, and 500 ppm and epitaxial growth in S4. Figure 5 The figure shows the planar concentration of oxygen in the oxygen atom layer after cleaning with H2O2 cleaning solution at a temperature of 25℃ / 3 minutes, using H2O2 cleaning solution with hydrogen peroxide concentrations of 0, 10000, 30000, and 50000 ppm (0, 1, 3, and 5% by mass, respectively) and epitaxial growth in S4. Figure 6 The paper shows the planar oxygen concentration of the oxygen atom layer after epitaxial growth in S4 under the conditions of H2O2 cleaning solution temperature of 25°C, hydrogen peroxide concentration of 10000 ppm (1% by mass), and cleaning time of 3, 10, and 20 minutes. These results show that the oxygen concentration of the oxygen atom layer can be controlled by adjusting the H2O2 cleaning solution temperature, hydrogen peroxide concentration, and cleaning time, especially within a range of 1×10⁻⁶. 14 ~1×10 15atoms / cm 2 The scope is controlled.

[0049] If the planar concentration of oxygen in the oxygen atom layer is 1×10 15 atoms / cm 2 The following method can reduce stacking faults and dislocations in the epitaxially grown monocrystalline silicon layer, thereby enabling the fabrication of a layer with higher crystallinity, and is therefore preferred.

[0050] Next, the surface roughness of the wafer after cleaning with H2O2 cleaning solution will be described. Figure 7 The diagram shows the relationship between hydrogen peroxide concentration and surface roughness (Haze) and etching rate after cleaning with H2O2 cleaning solution temperature and cleaning time set to 80℃ / 3 minutes and hydrogen peroxide concentration varied in the range of 0 to 300 ppm.

[0051] A higher Haze value indicates a more severe deterioration in surface roughness. Haze is determined using a particle counter SP3 manufactured by KLA. The etching rate is calculated based on the wafer thickness before and after cleaning. Figure 7 It is known that the higher the hydrogen peroxide concentration, the smaller the haze becomes, and the surface roughness is improved. It is also known that the addition of hydrogen peroxide reduces the etching rate, thereby reducing the amount of Si etched, and thus improving the surface roughness. This is likely because the oxygen atom layer plays a protective role for Si.

[0052] Figure 8 The paper shows the surface roughness (Haze) of wafers after cleaning with H2O2 cleaning solution at a temperature of 25°C for 3 minutes and varying hydrogen peroxide concentration within the range of 0–30,000 ppm (0–3% by mass). The results show that the Haze value is not correlated with the hydrogen peroxide concentration, exhibiting nearly identical values ​​across all concentration levels. Furthermore, the Haze value is lower than... Figure 7 Setting the cleaning temperature and time to 80℃ / 3 minutes resulted in better surface roughness. This is believed to be because etching of Si is difficult to occur at temperatures as low as 25℃. Therefore, from the perspective of surface roughness, processing at room temperature, such as around 25℃, is more ideal.

[0053] The results above show that, compared to conventional cleaning with warm pure water without hydrogen peroxide, cleaning with an aqueous solution containing hydrogen peroxide can effectively control the planar concentration of oxygen in the oxygen atom layer while suppressing the deterioration of surface roughness. Furthermore, the cleaning process can be performed using either batch cleaning equipment or single-piece cleaning equipment.

[0054] Next, the H2O2 cleaning solution will be described in more detail. In this invention, the oxidizing effect of hydrogen peroxide is utilized. More specifically, the oxidation reaction is carried out through the oxygen released by the decomposition reaction of hydrogen peroxide (2H2O2→2H2O+O2).

[0055] The decomposition reaction varies depending on the pH (Potential Hydrogen) of the aqueous solution. pH represents the concentration of hydrogen ions in the aqueous solution; 7 is neutral, less than 7 is acidic, and greater than 7 is alkaline. Figure 9 The table shows the pH values ​​of aqueous H2O2 solutions when the hydrogen peroxide concentration is varied from 0 to 50,000 ppm (0 to 5% by mass) at a temperature of 25°C. Figure 9 As shown, the addition of hydrogen peroxide creates a weakly acidic environment. Under this weakly acidic environment, the decomposition reaction of hydrogen peroxide proceeds relatively stably, and therefore can be controlled by adjusting the temperature, concentration, and washing time of the aqueous solution.

[0056] When the pH is below 7, the formation of a thicker oxygen atom layer, which would otherwise occur due to the decomposition of hydrogen peroxide and the promotion of oxidation at pH above 7, can be effectively prevented. Furthermore, if the pH is above 4, the decomposition reaction becomes more stable, allowing for reproducible and more stable formation of the oxygen atom layer. Therefore, in this invention, it is preferable to set the pH of the cleaning solution containing hydrogen peroxide in the range of 4 to 7. Additionally, the H2O2 cleaning solution contains at least hydrogen peroxide, and may also contain other chemicals, additives, etc.

[0057] Furthermore, in this invention, since the oxygen concentration of the oxygen atom layer can be appropriately controlled during the oxygen atom layer formation process, it is unnecessary to perform a process to thin the oxygen atom layer as described in Patent Document 4. In other words, it is possible to omit the process of thinning the oxygen atom layer after the oxygen atom layer formation process. Therefore, there is no need to add an additional thinning process for the oxygen atom layer, thus improving productivity.

[0058] [Epithelial Growth Process] Figure 1 S4 is an epitaxial growth process that grows a single-crystal silicon layer on the surface of a silicon single-crystal wafer with an oxygen atom layer formed by vapor phase growth. Monosilane or disilane can be used as the gas used in the growth. Nitrogen or hydrogen can be used as the carrier gas. Furthermore, the pressure in the chamber where epitaxial growth is performed is only required to prevent the formation of tiny silicon crystals in the gas phase. For example, a pressure of 133 Pa or higher and 13300 Pa or lower can be used. Both batch and single-wafer epitaxial growth apparatuses can be used.

[0059] In addition, epitaxial growth of single-crystal silicon can be carried out at temperatures above 450°C and below 800°C. By growing at such a temperature, it is possible to effectively prevent the formation of dislocations and stacking faults in the epitaxial layer.

[0060] Higher temperatures result in higher epitaxial growth rates, so film deposition at high temperatures allows for the formation of thicker epitaxial layers in a shorter time. Conversely, to form thinner epitaxial layers, film deposition can be performed at lower temperatures. Thus, the growth temperature can be adjusted according to the desired epitaxial layer thickness. Furthermore, the deposition time can be adjusted to control the epitaxial layer thickness.

[0061] It should be noted that during the epitaxial growth of single-crystal silicon, hydrogen baking is typically performed just before epitaxial growth to remove the native oxide film on the substrate surface and clean it. However, in the epitaxial growth process involved in this invention, hydrogen baking is preferably not performed, and epitaxial growth begins when the specified growth temperature is reached. This is to prevent the oxygen atom layer from disappearing. Hydrogen baking, as mentioned here, refers to holding the single-crystal silicon wafer at a temperature above 800°C for a specified time in a hydrogen atmosphere. Since the oxygen atom layer does not disappear below 800°C, as long as the temperature is below 800°C, introducing hydrogen as a carrier gas before epitaxial growth will not cause any problems.

[0062] By performing the S1 to S4 processes described above, it is possible to manufacture products such as... Figure 2 The epitaxial wafer formed by δ-doping of oxygen can also control the oxygen concentration of the oxygen atom layer.

[0063] Alternatively, depending on the purpose, CMP processing (S5) can be performed on the wafer surface after the S4 process. This can improve the surface defects and roughness of the epitaxial layer.

[0064] In this case, by making the amount removed by CMP processing less than the thickness of the silicon layer formed in epitaxial growth, it is possible to leave the silicon layer, thereby manufacturing an epitaxial wafer with an oxygen atom layer.

[0065] This invention can also manufacture, by alternating the formation of at least an oxygen atom layer with the epitaxial growth process multiple times, a product such as... Figure 3 Epitaxial wafers with multiple oxygen atom layers. By forming multiple layers of oxygen atoms in this way, the getter absorption and dopant suppression capabilities are significantly improved compared to a single layer.

[0066] At this point, the spacing of the oxygen atom layers is not limited, and the oxygen concentration and layer spacing can be adjusted according to the application. However, as... Figure 7As shown, especially in a high temperature region where the temperature of the H2O2 cleaning solution is 80°C or the like, Si on the outermost surface is etched. Therefore, to reliably form multiple layers, it is preferable to adjust the conditions of steps S3 and S4 such that the silicon etching amount in the oxygen atom layer formation step of S3 < the silicon film formation amount (also referred to as silicon film formation thickness) in the epitaxial growth step of S4. In this way, by performing the treatment multiple times such that the silicon etching amount in the oxygen atom layer formation step of S3 < the silicon film formation amount in the epitaxial growth step of S4, a multilayer oxygen atom layer can be reliably formed. [Examples]

[0067] Hereinafter, the present invention will be specifically described with reference to Examples, but the present invention is not limited to these Examples.

[0068] (Example 1) One piece of monocrystalline silicon wafer having a diameter of 300 mm, a crystal plane orientation of (100), a p-type conductivity, and a resistivity of 10 Ωcm was prepared. The prepared wafer was inspected using SP5 manufactured by KLA Corporation, and the Haze value indicating the surface roughness was obtained.

[0069] Next, the prepared monocrystalline silicon wafer was cleaned using a batch-type cleaning machine. After cleaning for 3 minutes with an HF cleaning solution having a temperature of 25°C and a concentration of 5.0 mass% to remove the natural oxide film, cleaning was performed for 3 minutes with 1 mass% hydrogen peroxide water at 25°C. At this time, the pH of the hydrogen peroxide water cleaning solution was 5.88.

[0070] The cleaned wafer was inspected using SP5 manufactured by KLA Corporation, and the Haze value was obtained. Next, epitaxial growth of monocrystalline silicon was performed in a single-wafer type epitaxial furnace without performing hydrogen baking. At this time, the growth temperature was set to 700°C, and the time was set to 2 seconds. The wafer after film formation was inspected using SP5 manufactured by KLA Corporation, and the Haze value was obtained.

[0071] (Comparative Examples 1 to 4) The cleaning solution after HF cleaning was changed from hydrogen peroxide water to pure water, and otherwise, the epitaxial wafer was manufactured and the Haze value was acquired under all the same conditions as in Example 1. At this time, the temperature of the pure water and the cleaning time were set as follows: Comparative Example 1 was 80°C / 10 minutes, Comparative Example 2 was 80°C / 3 minutes, Comparative Example 3 was 50°C / 3 minutes, and Comparative Example 4 was 25°C / 3 minutes.

[0072] (Example 2) Except that the film formation time during epitaxial growth was changed to 5 seconds, the epitaxial wafer was manufactured and the Haze value was acquired under the same conditions as in Example 1.

[0073] (Comparative Examples 5 to 8) The film formation time during epitaxial growth was changed to 5 seconds. Otherwise, epitaxial wafers were manufactured and Haze values ​​were obtained under the same conditions as Comparative Examples 1 to 4.

[0074] (Example 3) The film formation time during epitaxial growth was changed to 60 seconds, but the epitaxial wafer was fabricated under the same conditions as in Example 1. Here, the oxygen atom concentration of the oxygen atom layer was evaluated using SIMS. Furthermore, the crystallinity of the film layer was evaluated using cross-sectional TEM (Transmission Electron Microscopy).

[0075] (Comparative Examples 9-12) The film formation time during epitaxial growth was changed to 60 seconds, but otherwise, epitaxial wafers were fabricated under the same conditions as Comparative Examples 1-4. Here, the oxygen atom concentration of the oxygen atom layer was evaluated by SIMS.

[0076] Figure 10 The evolution of Haze values ​​for Examples 1 and Comparative Examples 1-4 before, after, and after film formation is shown. In Comparative Examples 1-4, the higher the temperature and the longer the pure water rinsing conditions, the worse the Haze after rinsing, and this also affects the Haze after film formation. In particular, compared with Comparative Examples 1 and 2, the Haze of Example 1 is good.

[0077] Figure 11 The text shows the evolution of Haze values ​​for Examples 2 and Comparative Examples 5-8 before cleaning, after cleaning, and after film formation. (Compared to...) Figure 10 Similarly, in Comparative Examples 5-8, the higher the temperature and the longer the duration of the pure water rinsing, the worse the haze became after rinsing, and this also affected the haze of the film formed. In particular, compared with Comparative Examples 5 and 6, the haze of Example 2 was good. The degree of haze after film formation in Comparative Examples 7 and 8 was comparable to that of Example 2, but as will be described later, it is believed that Example 2 obtained an oxygen atom layer with a high oxygen concentration.

[0078] Figure 12 The oxygen concentrations of the oxygen atom layers in Examples 3 and Comparative Examples 9-12 are shown. In Comparative Examples 9-12, the higher the temperature and the longer the pure water cleaning conditions, the higher the oxygen concentration. In contrast, the oxygen concentration in Example 3 is higher than that in Comparative Examples 9-12. That is, by using a hydrogen peroxide cleaning solution, an oxygen atom layer can be formed efficiently while suppressing the deterioration of surface roughness. As described above, Figure 11 The degree of haze after film formation in Example 2 is comparable to that in Comparative Examples 7 and 8, but as... Figure 12As shown, the oxygen concentration of the oxygen atom layer in Example 3 (cleaning conditions with hydrogen peroxide water were the same as in Example 2) was higher than that in Comparative Examples 11 and 12 (cleaning conditions with pure water were the same as in Comparative Examples 7 and 8, respectively). Based on this, by performing cleaning with hydrogen peroxide water, even with comparable haze levels in the epitaxial films, a high oxygen concentration oxygen atom layer can still be obtained. That is, it can be said that an oxygen atom layer was obtained efficiently. Furthermore, in Figure 10 The same situation can also be found in the comparison of Example 1 with Comparative Examples 3 and 4.

[0079] Figure 13 The image shows a cross-sectional TEM image of the epitaxial wafer of Example 3. A contrast variation caused by the oxygen atom layer was observed. Since the contrast levels of the substrate and the film layer were comparable, it was confirmed that the film layer was a single-crystal layer.

[0080] In summary, according to embodiments of the present invention, it is possible to manufacture epitaxial wafers with oxygen atom layers and good Haze values ​​while controlling the oxygen concentration of the oxygen atom layer.

[0081] This instruction manual includes the following methods. [1] A method for manufacturing an epitaxial wafer, which is a method for forming a single-crystal silicon layer on a single-crystal silicon wafer, characterized in that it includes the following steps: a hydrofluoric acid cleaning step, in which the natural oxide film on the surface of the single-crystal silicon wafer is removed by a cleaning solution containing hydrofluoric acid; an oxygen atom layer formation step, in which an oxygen atom layer is formed on the surface of the single-crystal silicon wafer on which the natural oxide film has been removed by cleaning; an epitaxial growth step, in which the single-crystal silicon layer is epitaxially grown on the surface of the single-crystal silicon wafer on which the oxygen atom layer has been formed by vapor phase growth; and, in the oxygen atom layer formation step, the cleaning uses a cleaning solution containing at least water containing hydrogen peroxide. [2] The method for manufacturing an epitaxial wafer as described in [1] above includes the following process: after the oxygen atom layer formation process, no process is performed to thin the oxygen atom layer. [3] The method for manufacturing an epitaxial wafer as described in [1] or [2] above includes the following process: setting the pH value of the cleaning solution containing hydrogen peroxide water in the range of 4 to 7. [4] The method for manufacturing an epitaxial wafer as described in [1], [2] or [3] above includes the following process: in the oxygen atom layer formation process, the planar concentration of oxygen in the oxygen atom layer is set to 1×10⁻⁶. 15 atoms / cm 2 the following. [5] The method for manufacturing an epitaxial wafer as described above [1], [2], [3] or [4] includes the following process: in the epitaxial growth process, epitaxial growth is performed at a temperature of 450°C or higher and 800°C or lower. [6] The method for manufacturing an epitaxial wafer as described in [1], [2], [3], [4] or [5] above includes the following process: performing CMP processing on the surface of the single crystal silicon layer after the epitaxial growth process. [7] The method for manufacturing an epitaxial wafer as described in [1], [2], [3], [4], [5] or [6] above includes the following process: alternating the oxygen atom layer formation process with the epitaxial growth process multiple times.

[0082] It should be noted that this invention is not limited to the embodiments described above. The embodiments described above are illustrative examples. As long as they have a substantially identical structure and perform the same function as the technical concept described in the patent claims of this invention, all solutions are included within the technical scope of this invention.

Claims

1. A method for manufacturing an epitaxial wafer, comprising forming a single-crystal silicon layer on a single-crystal silicon wafer, characterized in that, It includes the following processes: The hydrofluoric acid cleaning process removes the natural oxide film on the surface of the monocrystalline silicon wafer using a cleaning solution containing hydrofluoric acid. The oxygen atom layer formation process involves forming an oxygen atom layer on the surface of the single-crystal silicon wafer, after the natural oxide film has been removed, through cleaning. as well as, The epitaxial growth process involves epitaxially growing a single-crystal silicon layer on the surface of the single-crystal silicon wafer on which the oxygen atom layer has been formed, using a vapor phase growth method; and... In the oxygen atom layer formation process, the cleaning process uses a cleaning solution containing at least water containing hydrogen peroxide.

2. The method for manufacturing an epitaxial wafer according to claim 1, characterized in that, After the oxygen atom layer formation process, no process is performed to thin the oxygen atom layer.

3. The method for manufacturing an epitaxial wafer according to claim 1, characterized in that, The pH value of the cleaning solution containing hydrogen peroxide is set in the range of 4 to 7.

4. The method for manufacturing an epitaxial wafer according to claim 1, characterized in that, In the oxygen atom layer formation process, the planar concentration of oxygen in the oxygen atom layer is set to 1×10⁻⁶. 15 atoms / cm 2 the following.

5. The method for manufacturing an epitaxial wafer according to claim 1, wherein, In the epitaxial growth process, epitaxial growth is carried out at a temperature above 450°C and below 800°C.

6. The method for manufacturing an epitaxial wafer according to claim 1, characterized in that, After the epitaxial growth process, the surface of the single-crystal silicon layer is subjected to CMP processing.

7. The method for manufacturing an epitaxial wafer according to any one of claims 1 to 6, characterized in that, The oxygen atom layer formation process and the epitaxial growth process are performed alternately multiple times.

Citation Information

Patent Citations

  • Method of manufacturing semiconductor substrate

    JP2009016637A

  • Manufacturing method for epitaxial wafer, and epitaxial wafer

    JP2021111696A

  • Epitaxial wafer manufacturing method

    JP2022146664A

  • Manufacturing method for epitaxial wafer

    JP2024007890A

  • Method for manufacturing epitaxial wafer

    WO2022158148A1