Non-stick pan
By forming a microporous structure and a micro-nano structure on the surface of the base layer of non-stick cookware, and combining the reinforced transition layer and the non-stick layer, the problem of the non-stick layer of existing non-stick cookware being easy to fall off is solved, and the non-stick property and use are improved. life, and enhanced oil and stain resistance.
Patent Information
- Application Number
- CN202420523008.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-18
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2034-03-18
AI Technical Summary
The connection between the non-stick layer and the base layer of existing non-stick cookware is weak, resulting in a weakened non-stick effect and possible health problems.
Several parallel non-stick patterns are formed on the surface of the base layer. Each non-stick pattern includes a microporous structure, forming micron-scale protrusions and depressions, and a transition layer and micro-nano structure are formed in these depressions to increase the connection between the transition layer and the base layer. The bonding strength of the base layer, while the non-stick layer extends to the sidewalls of the transition layer to improve overall non-stick properties.
Significantly improves the non-stick property and service life of the pot, reduces the probability of the non-stick layer falling off, and enhances hydrophobicity and anti-fouling properties with oil.
Smart Images

Figure CN221903303U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to the technical field of kitchenware, in particular to a non-stick cookware. Background Art
[0002] In the prior art, non-stick cookware is usually composed of a base layer and a non-stick coating. Since the surface structure of the base layer is smooth, after the non-stick coating is formed on its surface, the connection between the non-stick coating and the base layer is weak, so that when the non-stick cookware is used, kitchen utensils such as shovels and steel wool will accelerate the shedding of the non-stick layer. On the one hand, the non-stick effect of the non-stick cookware is greatly weakened, and on the other hand, it is easy to cause health problems caused by human body accidentally ingesting the detached coating. Utility Model Content
[0003] In view of this, the purpose of the present invention is to provide a non-stick cookware, which is used to overcome the problems of easy detachment of the coating and poor non-stick effect in the prior art.
[0004] In order to achieve the above-mentioned purpose, the utility model provides the following technical solution: a non-stick cookware, comprising:
[0005] A base layer, wherein a plurality of parallel non-stick lines are formed on the inner surface of the base layer, each of the non-stick lines comprises a plurality of spaced microporous structures, and the microporous structures form a plurality of micron-scale protrusions and depressions on the inner surface of the base layer;
[0006] A transition layer, the transition layer is formed at the convex part of the inner surface of the base layer and at the concave part of the inner surface of the base layer, and a plurality of micro-nano structures are formed on the surface of the transition layer at the concave part;
[0007] The non-stick layer is formed on the surface of the transition layer at the protrusion and extends to the upper part of the transition layer at the side wall of the concave part.
[0008] The above technical solution is adopted, by setting a number of parallel non-stick lines on the inner surface of the base layer, each non-stick line includes a number of spaced microporous structures, and the microporous structure forms a number of protrusions and depressions on the surface of the base layer, thereby forming a micron-level concave-convex structure on the surface of the base layer. The transition layer is formed on the concave-convex structure, which can increase the bonding force between the transition layer and the base layer compared to the smooth surface of the prior art. In addition, a micro-nano structure is further set on the transition layer located at the depression, and the micro-nano structure can play a role of hydrophobic oil blocking. In addition, a non-stick layer is further formed on the surface of the transition layer located at the protrusion, and extends to the upper part of the transition layer located at the side wall of the depression. On the one hand, the micro-nano structure at the depression is combined with the non-stick layer at the protrusion, which can greatly improve the overall non-stickiness of the pot body. On the other hand, the non-stick layer at the protrusion extends to the upper part of the depression, so that the non-stick layer forms an integral structure, which can reduce the probability of the non-stick layer being damaged along the edge of the protrusion during use, thereby extending the service life of the pot.
[0009] Furthermore, the ratio of the bottom diameter to the top diameter of the depression of the microporous structure is 0.4-0.6, the depression depth is 0.03-0.06 mm, and the top diameter of the depression is greater than the depression depth.
[0010] Furthermore, the distance between two adjacent non-stick lines is 0.5 mm to 1 mm.
[0011] Furthermore, the distance between the center points of two adjacent microporous structures is 0.01 mm to 0.05 mm.
[0012] Furthermore, a plurality of micro-nano structures are formed on the surface of the transition layer located at the protrusion.
[0013] Furthermore, the micro-nano structures formed on the transition layer on the surface of the depression are arranged in a periodic and orderly manner.
[0014] Furthermore, the area of the non-stick layer located on the upper side wall of the depression accounts for 20-50% of the total area of the side wall of the depression.
[0015] Furthermore, the thickness of the transition layer is 0.3-3 μm.
[0016] Furthermore, the thickness of the non-stick layer is 0.5-3 μm.
[0017] Furthermore, the base layer is a pure titanium layer or a stainless steel composite layer; the transition layer is a pure titanium layer or a pure chromium layer; the non-stick layer is a titanium-chromium alloy layer; and the base layer, the transition layer and the non-stick layer are all metallurgically connected. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a schematic diagram of the structure of a non-stick pan according to an embodiment of the utility model;
[0019] Figure 2 This is a schematic diagram of the microporous structure on the surface of a non-stick pan in an embodiment of the utility model;
[0020] Figure 3 This is a schematic diagram of the microporous structure after the transition layer and the non-stick layer are formed in the embodiment of the utility model;
[0021] Figure 4 for Figure 3 A magnified view of part A in FIG.
[0022] Figure 5 It is another schematic diagram of a microporous structure after forming a transition layer and a non-stick layer in an embodiment of the utility model;
[0023] Figure 6 for Figure 5 Enlarged view of part A in . DETAILED DESCRIPTION
[0024] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0025] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it can be directly on the other element or indirectly on the other element. When an element is referred to as being "connected to" another element, it can be directly connected to the other element or indirectly connected to the other element.
[0026] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present utility model, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined. The meaning of "several" is one or more, unless otherwise clearly and specifically defined.
[0027] In the description of the present invention, it should be understood that the terms "upper", "lower", "front", "back", "left", "right", etc. indicate directions or positional relationships based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore should not be understood as a limitation on the present invention.
[0028] In the description of the present utility model, it should be noted that, unless otherwise clearly specified and limited, the terms "installation", "connection" and "connection" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present utility model can be understood according to specific circumstances.
[0029] See also Figures 1 to 3 The present invention provides a non-stick cookware, comprising:
[0030] The base layer 1 should be understood that the base layer is the pot body of the non-stick cookware. The base layer material can be selected as a pure titanium plate or a stainless steel composite plate. The exemplary stainless steel composite plate can be a titanium / aluminum / stainless steel composite plate, or a stainless steel / aluminum / stainless steel composite plate, etc.
[0031] See also Figures 1 to 3 The inner surface of the base layer 1 is formed with a plurality of parallel non-stick lines 11, each of which includes a plurality of spaced microporous structures 12, and the microporous structures 12 form a plurality of micron-sized protrusions 121 and depressions 122 on the inner surface of the base layer. It should be understood that the inner surface of the base layer 1 is formed with a plurality of microporous structures 12, and the periodic arrangement of the microporous structures 12 constitutes the non-stick line shape on the inner surface of the base layer 1. In addition, it should be understood that the microporous structures 12 on the inner surface of the base layer 1 can be formed by an etching process.
[0032] The transition layer 2 is formed at the protrusion 121 on the inner surface of the base layer 1 and the depression 122 on the inner surface of the base layer 1. The transition layer 2 is also formed with a plurality of micro-nano structures 21 on the surface of the depression 122. Of course, the micro-nano structure can also be formed at the protrusion at the same time. When the protrusion and the depression have micro-nano structures at the same time, the connection stability between the non-stick layer and the transition layer can be further improved. It should be understood that the transition layer 2 covers the protrusion 121 and the depression 122 of the base layer 1. The thickness of the transition layer can be 0.3 to 3 μm. For example, the thickness of the transition layer can be selected as 0.3 μm, 0.7 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm or 3 μm, etc. Further, the material of the transition layer can be selected as a pure titanium layer, a pure chromium layer or a chromium-titanium alloy layer, etc. These transition layers can be formed by the PVD process in the prior art.
[0033] The non-stick layer 3 is formed on the surface of the transition layer 2 located at the protrusion 121, and extends to the upper part of the transition layer 2 located at the side wall of the recess 122. It should be understood that the thickness of the non-stick layer can be 0.5 to 3 μm. For example, the thickness of the non-stick layer can be selected to be 0.3 μm, 0.7 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm or 3 microns. In addition, the sum of the thickness of the transition layer and the non-stick layer is preferably not more than 4 microns. Further, the material of the non-stick layer can be selected as a chromium-titanium alloy layer. The non-stick layer can also be formed by PVD and other processes in the prior art. It should also be understood that the non-stick layer is formed into an alloy layer by PVD and other processes, which can further ensure that the base layer, the transition layer and the non-stick layer are all metallurgically connected.
[0034] The above technical solution is adopted, by setting a number of parallel non-stick lines on the inner surface of the base layer, each non-stick line includes a number of spaced microporous structures, and the microporous structure forms a number of protrusions and depressions on the surface of the base layer, thereby forming a micron-level concave-convex structure on the surface of the base layer. The transition layer is formed on the concave-convex structure, which can increase the bonding force between the transition layer and the base layer compared to the smooth surface of the prior art. In addition, a micro-nano structure is further set on the transition layer located at the depression, and the micro-nano structure can play a role of hydrophobic oil blocking. In addition, a non-stick layer is further formed on the surface of the transition layer located at the protrusion, and extends to the upper part of the transition layer located at the side wall of the depression. On the one hand, the micro-nano structure at the depression is combined with the non-stick layer at the protrusion, which can greatly improve the overall non-stickiness of the pot body. On the other hand, the non-stick layer at the protrusion extends to the upper part of the depression, so that the non-stick layer forms an integral structure, which can reduce the probability of the non-stick layer being damaged along the edge of the protrusion during use, thereby extending the service life of the pot. In addition, the transition layer and the non-stick layer can be formed by processes such as PVD, which further ensures that the base layer, the transition layer and the non-stick layer are all metallurgically connected, thereby improving the stability of the connection between the film layers.
[0035] Further, in combination with the above-mentioned embodiments, in this embodiment, the ratio of the bottom diameter to the top diameter of the depression 122 of the microporous structure 12 is 0.4 to 0.6, the depression depth of the depression 122 is 0.03 to 0.06 mm, and the top diameter of the depression 122 is greater than the depression depth of the depression 122. It should be understood that at this time, the bottom diameter of the depression 122 is smaller than the top diameter, so that the depression 122 can form an inverted trapezoidal cross-sectional structure with a small bottom opening and a large top opening. This structure is conducive to the transition layer 2 to further form a micro-nano structure 21 in the depression, and the micro-nano structure 21 can play a role in hydrophobic oil blocking. The depression depth of the depression 122 is set to 0.03 to 0.06 mm, and it is also defined that the top diameter of the depression 122 is greater than the depression depth of the depression 122. Since the depth of the microporous structure 12 is shallow, it can be ensured that when making food, it is not easy to store food in the microporous structure 12. Furthermore, the microporous structure 12 on the inner surface of the base layer 1, combined with the micro-nano structure 21 formed on the surface of the recess 122, can greatly increase the specific surface area of the inner surface of the cookware and reduce the contact between food and the inner surface of the cookware.
[0036] Further, in combination with the above embodiment, the distance between two adjacent non-stick patterns 11 is further limited to 0.5mm to 1mm in this embodiment. For example, the distance between two adjacent non-stick patterns 11 can be 0.5mm, 0.6mm, 0.7mm, 0.8mm, 0.9mm or 1mm, etc. The distance between the center points of two adjacent microporous structures 12 is 0.01mm to 0.05mm. For example, the distance between the center points of two adjacent microporous structures 12 can be 0.01mm, 0.02mm, 0.03mm, 0.04mm or 0.05mm, etc. By limiting the distance between adjacent non-stick patterns 11 and the distance between adjacent microporous structures 12, the micron-scale convex / concave structures in the microporous structure 12 are arranged in a certain pattern to form an array-like structure on the surface of the base layer 1, which is reflected on the surface of the base layer as a non-stick pattern shape. This shape can improve the surface performance of the base layer, such as improving the non-stick properties of non-stick cookware.
[0037] Further, refer to Figure 5 and Figure 6 As shown, the surface of the transition layer 2 located at the protrusion 121 can also form a micro-nano structure, which can further enhance the bonding strength between the transition layer 2 and the non-stick layer 3.
[0038] Further, in combination with the above embodiments, Figure 3 and Figure 4 In this embodiment, the micro-nano structures 21 formed on the transition layer 2 on the surface of the recess 122 are further defined as being arranged periodically. That is, the micro-nano structures 21 on the surface of the transition layer 2 on the surface of the recess 122 are arranged periodically, and this structure can make its surface have hydrophobic and oleophobic properties, thereby improving the waterproof and oil-proof, self-cleaning, and anti-fouling functions of the non-stick cookware. Furthermore, the micro-nano structures 21 combined with the non-stick layer 3 on the protrusion 121 can make the inner surface of the cookware non-stick as a whole, greatly improving the non-stick, self-cleaning, and anti-fouling properties of the cookware.
[0039] Further, in combination with the above embodiment, the area of the non-stick layer 3 located on the side wall of the recess 122 is further limited to 20-50% of the total area of the side wall of the recess 122. It should be understood that the area of the non-stick layer 3 located on the side wall of the recess 122 may be 20%, 30%, 40% or 50% of the total area of the side wall of the recess 122. By limiting the area occupied by the non-stick layer 3 on the side wall of the recess 122, it can be ensured that the contact area between the non-stick layer 3 and the transition layer 2 can be attached more stably.
[0040] The above-mentioned non-stick cookware is applied to kitchen utensils such as frying pans, rice cookers, and electric baking pans that need to have non-stick properties.
[0041] Test example
[0042] The non-stick cookware in the present invention can be prepared by referring to the following preparation method, specifically:
[0043] S1. Pretreatment of the substrate layer. The substrate layer is selected as a pure titanium plate. A number of periodically arranged microporous structures are formed on the surface of the substrate layer by laser etching. The microporous structures constitute a number of parallel non-stick lines. The distance between adjacent non-stick lines is 0.5 mm. The ratio of the bottom diameter to the top diameter of the depression of the microporous structure is 0.5. In this test example, the bottom diameter of the depression of the microporous structure is 0.03 mm, the top diameter of the depression is 0.06 mm, the depth of the depression is 0.04 mm, the distance between the center points of adjacent microporous structures is 0.03 mm, and the microporous structures form a number of parallel non-stick lines on the surface of the substrate layer:
[0044] S2. Install the target material. Install the target material required for pot coating in the vacuum coating chamber. The transition layer target material is a titanium target and the non-stick layer target material is a titanium-chromium alloy target;
[0045] S3, vacuum wash the target. After installing the target, close the chamber door and vacuumize to 9x10 -3 The target was washed at 1.5 Pa. The process gas was introduced into the chamber to make the working pressure in the chamber reach 1 Pa, and the sputtering power supply was turned on to wash the target. The process gas for target washing was highly inert argon gas, and the target washing power supply was a sputtering DC power supply with a power density of 3W / cm 2 , target washing time is 60min.
[0046] S4, coating of pots. After the target is washed, the cavity is opened to release the gas to break the vacuum. After the pot is placed on the sample rack, the process is introduced and vacuum is started. The vacuum degree should not be less than 9ⅹ10 -3 Pa, the chamber is heated up, and the preset temperature is 220°C. When the substrate reaches the preset temperature and vacuum degree of the process, a certain amount of process gas is introduced to start coating. The specific coating process is as follows: first, plasma cleaning is performed, and then a transition layer and a non-stick layer are formed on the substrate layer in sequence.
[0047] The plasma cleaning bias voltage is 600 V, the process gas is Ar, the working gas pressure is 1 Pa, and the plasma cleaning time is 15 min.
[0048] The transition layer material is titanium. When the transition layer material is coated on the recessed part of the concave-convex structure, the substrate bias is 300V, the thickness of the coated film is controlled at 0.8μm, the process gas is Ar, and the working gas pressure is 1Pa; when the transition layer material of the micro-nano structure is coated on the raised part of the concave-convex structure, the substrate bias is 300V, the thickness of the coated film is controlled at 0.8μm, the process gas is Ar, and the working gas pressure is 1Pa.
[0049] The non-stick layer material is a titanium-chromium alloy layer. When the non-stick layer material is plated, the substrate bias is 200V, the plated film thickness is controlled at 0.7μm, the process gas is Ar, O2, N2, C2H2, and the working gas pressure is 2Pa.
[0050] S5, the pot is taken out of the cavity. After the coating is completed, the cavity is cooled down, the cavity is opened and taken out of the oven, and a non-stick pot is prepared.
[0051] Test Case
[0052] Furthermore, the present invention also performs non-stick and surface wear resistance tests on the non-stick cookware in the above embodiment. The specific test methods are as follows:
[0053] 1. The specific test method for non-stick properties shall refer to the provisions of 4.2.1 in GB / T 32095.2-2015 "Performance and Test Specifications for Non-stick Surfaces of Metal Cooking Utensils for Household Food".
[0054] The non-stick test method includes the following steps:
[0055] A: Pour an appropriate amount of vegetable oil on the surface of the substrate and wipe the non-stick surface with a soft cloth until it is evenly coated;
[0056] B: Wash with warm water above 60℃ and neutral detergent, then rinse with clean water and wipe dry;
[0057] C: Heat the cooking utensil on an electric stove with a rated voltage of 220V and an output power of 1kw. Use a surface thermometer with an accuracy of not less than 2.5 to measure. When the surface temperature of the inner coating reaches 150℃-170℃, break a fresh egg that meets the requirements of SB / T10277-1997, Grade 2 (weight 50g-60g), and put it into the cooking utensil. Wait until the egg white is basically coagulated (during the entire cooking process, the surface temperature of the inner coating shall not exceed 210℃;
[0058] D: Use a plastic spatula with a cutting edge thickness of 0.2mm-0.5mm to completely remove the egg. If there is any egg residue attached, gently wipe it off with a wet sponge or gauze.
[0059] Test 1: Set up three experimental groups, each with 50 non-stick pans, repeat steps C and D, observe, and judge the non-stick effect according to Table 1.
[0060] Test 2: Set up three experimental groups, each with 50 non-stick pans, repeat steps C and D, measure the number of eggs that can be fried continuously in a non-stick pan without oil, and calculate the average number of eggs fried.
[0061] 2. The plane wear resistance test method shall comply with 4.3.1 plane wear resistance test in GB / T 32095.2-2015 "Performance and Test Specifications for Non-stick Surfaces of Metal Cooking Utensils for Household Food".
[0062] The grade judgment criteria are shown in Table 1.
[0063] Table 1 Fried egg non-stick test results and plane wear test structure evaluation
[0064]
[0065] Table 2 Non-stick test results of examples and comparative examples
[0066]
[0067] The non-stick level of the non-stick pan in the embodiment of the utility model can reach level I, and the number of eggs fried can reach 6.12 to 6.47 eggs fried continuously without oil, and the wear resistance level can also reach level I, which greatly improves the non-stickiness and wear resistance of the non-stick pan.
[0068] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention is described in detail with reference to the above embodiments, those skilled in the art can still modify the technical solutions described in the above embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A non-stick cookware, characterized in that: include: A base layer, wherein the inner surface of the base layer is formed with a plurality of parallel non-stick lines, each of the non-stick lines comprises a plurality of spaced microporous structures, and the microporous structures form a plurality of micrometer-level protrusions and depressions on the inner surface of the base layer; A transition layer, wherein the transition layer is formed at a protrusion on the inner surface of the base layer and at a depression on the inner surface of the base layer, and a plurality of micro-nano structures are formed on the surface of the transition layer located at the depression; A non-stick layer is formed on the surface of the transition layer at the protrusion and extends to the upper portion of the transition layer at the side wall of the recess.
2. The non-stick cookware according to claim 1, characterized in that: The ratio of the bottom diameter to the top diameter of the depression of the microporous structure is 0.4-0.6, the depression depth is 0.03-0.06 mm, and the top diameter of the depression is greater than the depression depth.
3. The non-stick cookware according to claim 1, characterized in that: The distance between two adjacent non-stick lines is 0.5 mm to 1 mm.
4. The non-stick cookware according to any one of claims 1 to 3, characterized in that: The distance between the center points of two adjacent microporous structures is 0.01 mm to 0.05 mm.
5. The non-stick cookware according to claim 1, characterized in that: A plurality of micro-nano structures are formed on the surface of the transition layer located at the protrusion.
6. The non-stick cookware according to claim 1, characterized in that: The micro-nano structures formed on the transition layer on the surface of the depression are arranged in a periodic and orderly manner.
7. The non-stick cookware according to claim 1, characterized in that: The area of the non-stick layer located on the side wall of the depression accounts for 20-50% of the total area of the side wall of the depression.
8. The non-stick cookware according to claim 1, characterized in that: The thickness of the transition layer is 0.3-3 μm.
9. The non-stick cookware according to claim 1, characterized in that: The thickness of the non-stick layer is 0.5-3 μm.
10. The non-stick cookware according to claim 1, characterized in that: The base layer is a pure titanium layer or a stainless steel composite layer; the transition layer is a pure titanium layer or a pure chromium layer; the non-stick layer is a titanium-chromium alloy layer; and the base layer, the transition layer and the non-stick layer are all metallurgically connected.