Electrode contact structure and solar cell
By defining polished areas and rough areas on the silicon wafer, and setting metal electrodes in the rough areas, the problem of insufficient contact between the metal electrodes and the doped polysilicon layer in TOPCon cells is solved, and the ohmic contact effect and passivation of the solar cells are improved. performance.
Patent Information
- Application Number
- CN202322969938.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-03
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2033-11-03
AI Technical Summary
The ohmic contact between the metal electrode of existing TOPCon solar cells and the doped polysilicon layer is weak, resulting in a small contact area and high resistance, which affects cell performance.
The polished area and rough area are defined on the silicon wafer, and a pyramid texturing morphology is formed through laser scanning processing. The tunnel oxide layer, n-type doped polysilicon layer and passivation layer are sequentially deposited, and metal electrodes are set up in the rough area. , improve the contact area and passivation effect.
By setting the rough area, the contact area between the n-type doped polysilicon layer and the metal electrode is increased, and the ohmic contact effect is improved. At the same time, a good passivation effect is maintained in the polished area, and the overall performance of the solar cell is improved.
Smart Images

Figure CN221928095U_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of new energy, and in particular to solar cells. Background Art
[0002] At present, TOPCon (tunneling oxide passivation contact) technology, as the mainstream representative of passivation contact technology, has entered the stage of large-scale mass production. The back passivation contact structure of TOPCon batteries generally includes: a silicon substrate, the back of the silicon substrate is sequentially covered with a tunneling oxide layer, a doped polysilicon layer, and a passivation layer, and a metal electrode protruding from the surface of the passivation layer is provided in the doped polysilicon layer. Usually, the tunneling oxide layer, the doped polysilicon layer, and the passivation layer are generally deposited in sequence after polishing the back of the silicon substrate under alkaline conditions. After alkaline polishing, the back surface of the silicon substrate is relatively flat and has a small specific surface area, which is conducive to the passivation of the surface by the tunneling oxide layer, the doped polysilicon layer, and the passivation layer. However, the flat surface is not conducive to the metal electrode and the doped polysilicon layer to form a large contact area, and the ohmic contact is weak. Utility Model Content
[0003] The embodiments of the present application provide an electrode contact structure and a preparation method thereof, and a solar cell to solve the technical problem of weak ohmic contact between a metal electrode and a doped polysilicon layer.
[0004] In a first aspect, an embodiment of the present application provides an electrode contact structure, the electrode contact structure comprising:
[0005] A silicon wafer, wherein one side of the silicon wafer comprises a polishing area and a rough area, wherein one side of the silicon wafer is a polished surface in the polishing area, and one side of the silicon wafer is a rough surface having a pyramid textured morphology in the rough area;
[0006] a tunneling oxide layer covering one side of the silicon wafer, wherein the surface of the tunneling oxide layer is a polished surface in the polishing area and the surface of the tunneling oxide layer is a rough surface in the rough area;
[0007] an n-type doped polysilicon layer covering the surface of the tunnel oxide layer, wherein the surface of the n-type doped polysilicon layer is a polished surface in the polishing area, and the surface of the n-type doped polysilicon layer is a rough surface in the rough area;
[0008] A passivation layer covering the surface of the n-type doped polysilicon layer in the polishing area;
[0009] A first metal electrode is disposed on the n-type doped polysilicon layer in the rough area, and a surface of the first metal electrode protrudes from the passivation layer.
[0010] In some embodiments of the present application, the material of the passivation layer includes at least one of silicon nitride, aluminum oxide, titanium oxide, and silicon dioxide.
[0011] In some embodiments of the present application, the electrode contact structure further includes a boron-doped oxide layer, and the boron-doped oxide layer is disposed on the other side of the silicon wafer.
[0012] In some embodiments of the present application, the electrode contact structure further includes a second metal electrode disposed on the boron-doped oxide layer, the boron-doped oxide layer consists of a heavily doped region and a lightly doped region, and the second metal electrode is disposed on the heavily doped region.
[0013] In some embodiments of the present application, in the n-type doped polysilicon layer, the doping atom is P.
[0014] In a second aspect, an embodiment of the present application provides a method for preparing an electrode contact structure, the method comprising the following steps:
[0015] Provide silicon wafers;
[0016] Defining a polished area and a rough area on one side of the silicon wafer, and performing laser scanning treatment on the rough area in an oxygen atmosphere;
[0017] Performing alkali polishing on the silicon wafer to polish the polishing area;
[0018] Depositing a tunneling oxide layer, an n-type doped polysilicon layer and a passivation layer in sequence on one side of the silicon wafer after alkali polishing;
[0019] In the rough area, electrode slurry is disposed on the passivation layer, and the electrode slurry is sintered to obtain the electrode contact structure.
[0020] In some embodiments of the present application, the wavelength of the laser is 300 to 1500 nm; and / or,
[0021] The power of the laser is 10 to 100 W; and / or,
[0022] The scanning width of the laser is 30 to 100 μm; and / or,
[0023] The scanning rate of the laser is 1-100 m / s.
[0024] In some embodiments of the present application, the duration of the alkali polishing is 100 to 300 seconds.
[0025] In some embodiments of the present application, before defining the polishing area and the roughening area on one side of the silicon wafer, the method further includes the following steps:
[0026] boron-doping the other side of the silicon wafer by high-temperature boron diffusion to form a boron-doped oxide layer;
[0027] The borosilicate glass material formed on one side of the silicon wafer during the high-temperature boron diffusion process is removed.
[0028] In a third aspect, an embodiment of the present application provides a solar cell, wherein the solar cell comprises the electrode contact structure described in any embodiment of the first aspect, or the electrode contact structure prepared by the method described in any embodiment of the second aspect.
[0029] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0030] The electrode contact structure provided in the embodiment of the present application sets a rough area, so that the surface of the n-type doped polysilicon layer is a rough surface in the rough area. The contact area between the rough surface and the first metal electrode is larger, which can improve the ohmic contact effect; while the polishing area still maintains a relatively smooth polishing surface, which is conducive to maintaining a good passivation effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0032] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0033] Figure 1 A schematic structural diagram of an electrode contact structure provided in an embodiment of the present application. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0035] Unless otherwise specified, the terms used herein should be understood as commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which this application belongs. In the event of a conflict, this specification takes precedence.
[0036] The English abbreviations used in this application have the following meanings:
[0037] TOPCon: Tunnel Oxide Passivated Contact solar cell (TOPcon)
[0038] BSG: Boro-silicate Glass
[0039] PECVD: Plasma Enhanced Chemical Vapor Deposition
[0040] LPCVD: Low Pressure Chemical Vapor Deposition
[0041] ALD: atomic layer deposition
[0042] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0043] The existing metal electrode has a technical problem of weak ohmic contact with the doped polysilicon layer.
[0044] The technical solution provided by the embodiments of the present application is to solve the above technical problems, and the overall idea is as follows:
[0045] In a first aspect, an embodiment of the present application provides an electrode contact structure, the electrode contact structure comprising:
[0046] A silicon wafer 1, wherein one side of the silicon wafer 1 comprises a polishing area 11 and a rough area 12, wherein the polishing area 11 on one side of the silicon wafer 1 is a polished surface, and the rough area 12 on one side of the silicon wafer 1 is a rough surface having a pyramid textured morphology;
[0047] A tunneling oxide layer 2 is covered on one side of the silicon wafer 1, wherein the surface of the tunneling oxide layer 2 is a polished surface in the polishing area 11, and the surface of the tunneling oxide layer 2 is a rough surface in the rough area 12;
[0048] an n-type doped polysilicon layer 3 covering the surface of the tunnel oxide layer 2, wherein the surface of the n-type doped polysilicon layer 3 is a polished surface in the polishing area 11, and the surface of the n-type doped polysilicon layer 3 is a rough surface in the rough area 12;
[0049] In the polishing area 11, a passivation layer 4 covering the surface of the n-type doped polysilicon layer 3;
[0050] In the rough area 12 , a first metal electrode 5 is disposed on the n-type doped polysilicon layer 3 , and a surface of the first metal electrode 5 protrudes from the passivation layer 4 .
[0051] It is easy to understand that the polished surface refers to a relatively smooth surface, which can be prepared by a polishing process.
[0052] Those skilled in the art can understand that the pyramid texturing morphology is a conventional silicon wafer surface morphology in the art and can be formed by alkali texturing.
[0053] Those skilled in the art will appreciate that the tunneling oxide layer 2 is a conventional structure in the art. The function of the tunneling oxide layer 2 is to reduce the interface state density between the silicon wafer 1 substrate and the doped polysilicon layer by chemical passivation. The majority carrier concentration is much higher than the minority carrier concentration, which reduces the probability of electron-hole recombination while increasing the resistivity to form selective contact for majority carriers. In the tunneling oxide layer 2, electrons pass through the oxide layer from the metal surface to the metal surface on the other side. This phenomenon only occurs in very thin oxide layers, usually less than a few nanometers. In this case, the wavelength of the electrons is comparable to the thickness of the tunneling oxide layer 2, so the electrons can pass through the tunneling oxide layer 2. Preparing the tunneling oxide layer 2 is a conventional technical solution in the art. As an example, the tunneling oxide layer 2 can be prepared by methods such as PECVD, LPCVD, and the deposition atmosphere can include, for example, N2O and SiH4, oxygen, and the like.
[0054] Those skilled in the art can understand that the doped polysilicon layer is a conventional structure in the art and is often abbreviated as poly in the art. Since the electrode contact structure described in the present application is mainly used on the back side of a solar cell, the present application uses an n-type doped polysilicon layer.
[0055] Those skilled in the art can understand that the passivation layer 4 is a conventional structure in the art, and the passivation layer 4 can also be called an insulating layer, and can be made of silicon nitride, aluminum oxide, titanium oxide or silicon oxide, or any combination thereof. The passivation layer 4 can be deposited by vapor deposition, sputtering, atomic deposition (ALD) or other methods.
[0056] Those skilled in the art will appreciate that metal electrodes are conventional structures in the art, and the material of the metal electrodes is generally formed by a conductive electrode slurry, and the electrode slurry may, for example, use a metallized silver paste used for p-type crystalline silicon cells on the market, such as a silver paste containing Pb-Te-O glass powder. As an exemplary preparation method, the electrode slurry may be applied to the silicon wafer 1 by screen printing in a desired patterned form, and may be subjected to post-processing such as sintering after drying. The conductive layer formed by the electrode slurry forms an electrical contact with the silicon wafer 1 to form an electrode.
[0057] In the present application, a rough area 12 is set to make the surface of the n-type doped polysilicon layer 3 a rough surface in the rough area 12. The contact area between the rough surface and the first metal electrode 5 is larger, which can improve the ohmic contact effect; while the polishing area 11 still maintains a relatively smooth polishing surface, which is conducive to maintaining a good passivation effect.
[0058] In some embodiments of the present application, the material of the passivation layer 4 includes at least one of silicon nitride, aluminum oxide, titanium oxide, and silicon dioxide.
[0059] In some embodiments of the present application, the electrode contact structure further includes a boron-doped oxide layer 6 , and the boron-doped oxide layer 6 is disposed on the other side of the silicon wafer 1 .
[0060] Those skilled in the art can understand that the boron-doped oxide layer 6 is a conventional structure in the art, and its material is mainly borosilicate glass (BSG), which is generally prepared by high-temperature boron diffusion.
[0061] In some embodiments of the present application, the electrode contact structure also includes a second metal electrode 7 arranged on the boron-doped oxide layer 6, the boron-doped oxide layer 6 consists of a heavily doped region 61 and a lightly doped region 62, and the second metal electrode 7 is arranged on the heavily doped region 61.
[0062] Those skilled in the art can understand that the heavily doped region 61 refers to a region with a high degree of boron doping, which can be prepared by local laser propulsion. The heavily doped region 61 and the lightly doped region 62 with different doping degrees are arranged on the boron-doped oxide layer 6, and the metal electrode is arranged on the heavily doped region 61. The heavily doped region 61 is conducive to reducing the metal semiconductor contact resistance and reducing contact recombination; the lightly doped region 62 is an illumination region, which is conducive to reducing surface Auger recombination, improving carrier collection rate, improving short-wave response, and improving passivation effect.
[0063] In some embodiments of the present application, the doping atoms in the n-type doped polysilicon layer 3 are P.
[0064] Using P as the doping atom is a general implementation method of performing n-type doping on a polysilicon layer.
[0065] In a second aspect, an embodiment of the present application provides a method for preparing an electrode contact structure, the method comprising the following steps:
[0066] S1: Provide silicon wafer after alkali texturing;
[0067] S2: defining a polishing area and a rough area on one side of the silicon wafer, and performing laser scanning treatment on the rough area in an oxygen atmosphere;
[0068] S3: performing alkali polishing on the silicon wafer to polish the polishing area;
[0069] S4: depositing a tunneling oxide layer, an n-type doped polysilicon layer and a passivation layer in sequence on one side of the silicon wafer after alkali polishing;
[0070] S5: in the rough area, placing electrode slurry on the passivation layer, and sintering the electrode slurry to obtain the electrode contact structure.
[0071] Those skilled in the art will appreciate that the method described in the second aspect of the present application can be used to prepare the electrode contact structure described in the first aspect.
[0072] Those skilled in the art can understand that texturing is a conventional technical means in this field, which can form special morphologies on the surface of silicon wafers. For example, a pyramid-like morphology can be obtained by alkali texturing, and a wormhole-like morphology can be obtained by acid texturing. Texturing can improve the light trapping effect of silicon wafers. In the field of Topcon batteries, alkali texturing is generally used.
[0073] It is easy to understand that laser scanning treatment in an oxygen atmosphere can oxidize the treated area to a certain extent. The oxidized area is more resistant to alkali polishing and is not easily corroded by the polishing liquid, so that the pyramid texturing morphology can be retained during the alkali polishing process.
[0074] The preparation of the tunnel oxide layer is a conventional technical solution in the art. As an example, the tunnel oxide layer can be prepared by PECVD, LPCVD and the like, and the deposition atmosphere can include N2O, SiH4, oxygen and the like.
[0075] It is a conventional technical solution in the art to prepare a doped polysilicon layer. As an example, it can be prepared by magnetron sputtering.
[0076] The preparation of the passivation layer is a conventional technical solution in the art. As an example, the passivation layer can be deposited by vapor deposition, sputtering, atomic layer deposition (ALD) or other methods.
[0077] Those skilled in the art will appreciate that, during the sintering process, the electrode slurry will penetrate the passivation layer and form the first metal electrode on the surface of the n-type doped polysilicon layer.
[0078] Since the tunneling oxide layer and the n-type doped polysilicon layer are very thin, both at the nanometer level, depositing the tunneling oxide layer and the n-type doped polysilicon layer on the silicon wafer in the rough area will also form a rough surface on the n-type doped polysilicon layer.
[0079] The present application processes the rough area with a laser so that the silicon wafer forms a rough surface in the rough area, and then sequentially deposits a tunneling oxide layer and an n-type doped polysilicon layer so that the n-type doped polysilicon layer also forms a rough surface in the rough area, and finally prepares a passivation layer and an electrode to obtain an electrode contact structure with a good ohmic contact effect.
[0080] In some embodiments of the present application, the wavelength of the laser is 300 to 1500 nm; and / or,
[0081] The power of the laser is 10 to 100 W; and / or,
[0082] The scanning width of the laser is 30 to 100 μm; and / or,
[0083] The scanning rate of the laser is 1-100 m / s.
[0084] In some embodiments of the present application, the duration of the alkali polishing is 100 to 300 seconds.
[0085] The beneficial effect of the duration of the alkali polishing being selected from the above range is that the polishing area can be fully polished without substantially affecting the morphology of the rough area.
[0086] In some embodiments of the present application, before defining the polishing area and the roughening area on one side of the silicon wafer, the method further includes the following steps:
[0087] S11: boron-doping the other side of the silicon wafer by high-temperature boron diffusion to form a boron-doped oxide layer;
[0088] S12: removing the boron dopants formed on one side of the silicon wafer during the high-temperature boron diffusion process.
[0089] Those skilled in the art will appreciate that high temperature boron diffusion is a conventional process in the art, and high temperature boron diffusion is usually performed in an oxygen atmosphere including at least one of BCl 3 and BBr 3 gases.
[0090] In a third aspect, an embodiment of the present application provides a solar cell, wherein the solar cell comprises the electrode contact structure described in any embodiment of the first aspect, or the electrode contact structure prepared by the method described in any embodiment of the second aspect.
[0091] Since the solar cell described in the third aspect is realized based on the electrode contact structure described in the first aspect or the preparation method of the electrode contact structure described in the second aspect, the implementation of its technology can be based on any embodiment of the first aspect or the second aspect and the common knowledge in the field of solar cells. Therefore, the solar cell described in the third aspect has all the achievable beneficial effects of the first aspect or the second aspect, which will not be repeated here.
[0092] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0093] Example 1
[0094] The present invention provides a method for preparing an electrode contact structure, the method comprising the following steps:
[0095] Sa: Provides silicon wafers after alkali texturing;
[0096] Sb: defining a polished area and a rough area on one side of the silicon wafer;
[0097] Sc: boron-doping the other side of the silicon wafer by high-temperature boron diffusion to form a boron-doped oxide layer;
[0098] Sd: removing the borosilicate glass material formed on one side of the silicon wafer during the high-temperature boron diffusion process;
[0099] Se: performing laser scanning treatment on the rough area in an oxygen atmosphere;
[0100] Sf: performing alkali polishing on the silicon wafer to polish the polishing area;
[0101] Sg: a tunnel oxide layer, a P-doped polysilicon layer and a passivation layer are sequentially deposited on one side of the silicon wafer after alkali polishing;
[0102] Sh: in the rough area, placing electrode slurry on the passivation layer, and sintering the electrode slurry to obtain the electrode contact structure.
[0103] Wherein, the wavelength of the laser is 355nm; the power of the laser is 60W; the scanning width of the laser is 80μm; and the scanning speed of the laser is 30m / s.
[0104] The duration of the alkali polishing is 100s.
[0105] Example 2
[0106] The difference between this embodiment and embodiment 1 is that:
[0107] The wavelength of the laser is 300 nm; the power of the laser is 1 W; the scanning width of the laser is 100 μm; and the scanning speed of the laser is 1 m / s.
[0108] The duration of the alkali polishing is 300s.
[0109] Example 3
[0110] The difference between this embodiment and embodiment 1 is that:
[0111] The wavelength of the laser is 1500nm; the power of the laser is 100W; the scanning width of the laser is 30μm; and the scanning speed of the laser is 1m / s.
[0112] The duration of the alkali polishing is 80s.
[0113] Example 4
[0114] The difference between this embodiment and embodiment 1 is that:
[0115] The wavelength of the laser is 1000 nm; the power of the laser is 40 W; the scanning width of the laser is 60 μm; and the scanning speed of the laser is 20 m / s.
[0116] The duration of the alkali polishing is 120s.
[0117] Example 5
[0118] The difference between this embodiment and embodiment 1 is that:
[0119] The wavelength of the laser is 1200 nm; the power of the laser is 50 W; the scanning width of the laser is 90 μm; and the scanning speed of the laser is 80 m / s.
[0120] The duration of the alkali polishing is 70s.
[0121] Comparative Example
[0122] The difference between this comparative example and Example 1 is only that:
[0123] Step Se is not performed;
[0124] Since it is not performed, the alkali polishing step in step Sf will polish both the polished area and the rough area.
[0125] Related experiments and effect data:
[0126] The open circuit voltage (uoc), short circuit current (isc), fill factor (ff), conversion efficiency (eta), and series resistance (rs) of Example 1 and the comparative example were tested by an IV tester, and the back gate line resistance and back contact resistance of Example 1 and the comparative example were tested by a TLM contact resistance tester. The results are shown in Table 1:
[0127] Comparative Example Example 1 uoc(mV) 717.41 718.45 isc(mA) 13.69 13.73 ff 84.13 84.32 eta(%) 25.026 25.192 rs(mΩ) 1.16 1.13 Back grid line resistance (Ω / cm) 1.9 1.5 Back contact resistance(Ω) 0.6 0.3
[0128] Table 1
[0129] It is easy to find from Table 1 that, compared with the comparative example, since the rough area is laser scanned in Example 1, the back grid line resistance and back contact resistance are significantly reduced compared with the comparative example, and the overall data is better in terms of open circuit voltage (UOC), short circuit current (ISC), fill factor (FF), conversion efficiency (ETA), series resistance (RS), etc. This shows that the processing method of Example 1 can effectively improve the comprehensive performance of solar cells.
[0130] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0131] In the present application, in the absence of any contrary description, the directional words used, such as "upper" and "lower", are specifically the directions of the drawings in the accompanying drawings. In addition, in the description of the present application specification, the terms "including", "comprising", etc. refer to "including but not limited to". Moreover, the terms "including", "comprising" or any other variants thereof are intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements not only includes those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of further restrictions, the elements defined by the sentence "including..." do not exclude the existence of other identical elements in the process, method, article or equipment including the elements. In this article, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that there can be three relationships, for example, A and / or B, which can represent: A exists alone, A and B exist at the same time, and B exists alone. For the association relationship of more than three associated objects described by "and / or", it means that any one of these three associated objects can exist alone, or any at least two of them exist at the same time. For example, for A, and / or B, and / or C, it can be represented that any one of A, B, and C exists alone, or any two of them exist at the same time, or three of them exist at the same time. In this article, "at least one" refers to one or more, and "multiple" refers to two or more. "At least one", "the following at least one (individual)" or similar expressions refer to any combination of these items, including any combination of single (individual) or plural (individual). For example, "at least one (individual) of a, b, or c", or "at least one (individual) of a, b, and c", can all represent: a, b, c, ab (i.e. a and b), ac, bc, or abc, wherein a, b, and c can be single or multiple, respectively.
[0132] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. An electrode contact structure, characterized in that: The electrode contact structure comprises: A silicon wafer, wherein one side of the silicon wafer comprises a polishing area and a rough area, wherein one side of the silicon wafer is a polished surface in the polishing area, and one side of the silicon wafer is a rough surface having a pyramid textured morphology in the rough area; a tunneling oxide layer covering one side of the silicon wafer, wherein the surface of the tunneling oxide layer is a polished surface in the polishing area and the surface of the tunneling oxide layer is a rough surface in the rough area; an n-type doped polysilicon layer covering the surface of the tunnel oxide layer, wherein the surface of the n-type doped polysilicon layer is a polished surface in the polishing area, and the surface of the n-type doped polysilicon layer is a rough surface in the rough area; A passivation layer covering the surface of the n-type doped polysilicon layer in the polishing area; A first metal electrode is disposed on the n-type doped polysilicon layer in the rough area, and a surface of the first metal electrode protrudes from the passivation layer.
2. The electrode contact structure according to claim 1, characterized in that: The material of the passivation layer includes any one of silicon nitride, aluminum oxide, titanium oxide and silicon dioxide.
3. The electrode contact structure according to claim 1, characterized in that: The electrode contact structure further includes a boron-doped oxide layer, and the boron-doped oxide layer is arranged on the other side of the silicon wafer.
4. The electrode contact structure according to claim 3, characterized in that: The electrode contact structure further includes a second metal electrode disposed on the boron-doped oxide layer, the boron-doped oxide layer consists of a heavily doped region and a lightly doped region, and the second metal electrode is disposed on the heavily doped region.
5. The electrode contact structure according to claim 1, characterized in that: In the n-type doped polysilicon layer, the doping atoms are P.
6. A solar cell, characterized in that: The solar cell comprises the electrode contact structure according to any one of claims 1 to 5.
Citation Information
Cited By
Electrode contact structure, preparation method thereof and solar cell
CN117238983A