Perovskite solar cell

By introducing an alkali metal halide intermediate layer and a protective layer into a perovskite solar cell, the problem of insufficient binding force between the perovskite layer and the electron transport layer is solved, and the stability and aging resistance of the perovskite solar cell are significantly improved.

CN221930601UActive Publication Date: 2024-10-29WUXI UTMOST LIGHT TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202420544289.2
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2024-03-19
Publication Date
2024-10-29
Estimated Expiration
2034-03-19

AI Technical Summary

Technical Problem

In perovskite solar cells, the bonding force between the perovskite layer and the electron transport layer is insufficient, and the electron transport layer lacks a protective structure, resulting in poor stability and vulnerability to damage.

Method used

Introducing an intermediate layer and a protective layer into the perovskite solar cell structure, using the same alkali metal halide (such as cesium iodide) to enhance the binding force between the perovskite layer and the electron transport layer, and forming the intermediate layer and protective layer through an annealing process Protective layer to provide protection.

Benefits of technology

It improves the binding force between the perovskite layer and the electron transport layer, reduces the risk of damage to the electron transport layer in the subsequent deposition process, and improves the overall stability and aging resistance of the perovskite solar cell.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221930601U_ABST
    Figure CN221930601U_ABST
Patent Text Reader

Abstract

The utility model relates to the field of perovskite solar cells, and discloses a perovskite solar cell. The perovskite solar cell comprises a perovskite layer, an intermediate layer, an electron transport layer and a protective layer, wherein the protective layer and the intermediate layer use alkali metal halide. According to the utility model, the intermediate layer and the protective layer are additionally arranged in an original perovskite solar cell structure, so that the binding force of the perovskite layer and the electron transport layer is improved, and the structure of the electron transport layer is effectively protected.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to the field of perovskite solar cells, in particular to a perovskite solar cell. Background Art

[0002] The photovoltaic cell industry is an important part of the new energy technology industry. Perovskite solar cells, as a new photovoltaic technology, are expected to be widely used in daily life and have received widespread attention. Therefore, how to prepare efficient and stable solar cells is crucial.

[0003] The common perovskite solar cells currently have insufficient bonding between the perovskite layer and the organic electron transport layer due to their own structure and film deposition method, and the electron transport layer may be damaged by subsequent deposition processes. In summary, the current perovskite solar cells have the problem of insufficient bonding between the perovskite layer and the electron transport layer, and the lack of a protective structure for the electron transport layer. Utility Model Content

[0004] In view of this, the utility model provides a perovskite solar cell to solve the problem of insufficient bonding between the perovskite layer and the electron transport layer and lack of a protective structure for the electron transport layer.

[0005] The utility model provides a perovskite solar cell, comprising:

[0006] A perovskite layer, an intermediate layer, an electron transport layer and a protective layer, wherein the intermediate layer is arranged on a surface of the electron transport layer close to the perovskite layer, and the protective layer is arranged on a surface of the electron transport layer away from the perovskite layer, and the protective layer and the intermediate layer use the same alkali metal halide.

[0007] Due to the structure of the perovskite solar cell itself and the film deposition method, the perovskite layer and the organic electron transport layer not only have average bonding strength but also poor stability. The utility model adds a protective layer and an intermediate layer to the conventional perovskite solar cell structure, and the protective layer and the intermediate layer use alkali metal halides, which improves the bonding strength between the perovskite layer and the electron transport layer, reduces the possibility of the electron transport layer being damaged by subsequent deposition processes, and improves the overall stability of the perovskite solar cell.

[0008] In an alternative embodiment, the alkali metal halide is selected from cesium iodide.

[0009] In an optional embodiment, the material of the electron transport layer is selected from C 60 , C 70 And one of PCBM.

[0010] In an optional embodiment, the thickness of the intermediate layer is 1 nm to 5 nm.

[0011] In an optional embodiment, the thickness of the electron transport layer is 5 nm to 50 nm.

[0012] In an optional embodiment, the thickness of the protective layer is 1 nm to 5 nm.

[0013] In an optional embodiment, the solar cell further comprises a buffer layer, which is arranged on a surface of the protective layer on a side away from the electron transport layer, and has a thickness of 7 nm to 25 nm.

[0014] In an optional embodiment, the material of the buffer layer is selected from tin dioxide.

[0015] In an optional embodiment, the solar cell further includes a substrate layer, a bottom electrode layer, a hole transport layer and a back electrode layer; the hole transport layer is arranged on a surface of the perovskite layer on a side away from the electron transport layer, the bottom electrode layer is arranged on a surface of the hole transport layer on a side away from the perovskite layer, the substrate layer is arranged on a surface of the bottom electrode layer on a side away from the hole transport layer, and the back electrode layer is arranged on a surface of the buffer layer on a side away from the electron transport layer; the material of the back electrode layer is selected from indium tin oxide or copper, and the thickness of the back electrode layer is 60nm to 130nm.

[0016] In an optional embodiment, the thickness of the intermediate layer is 2 nm to 4 nm, and the thickness of the protective layer is 2 nm to 4 nm.

[0017] In the utility model, a halide intermediate layer is added to connect the perovskite layer and the electron transport layer, thereby solving the problem of poor bonding between the perovskite layer and the electron transport layer in the perovskite battery. By adding a halide protective layer between the electron transport layer and the back electrode layer, the problem that the electron transport layer is easily damaged during the preparation of the back electrode layer is solved. Among them, the materials of the intermediate layer and the protective layer are both selected from cesium iodide. Since cesium iodide belongs to metal iodide and is an inorganic compound, and the formation of the cesium iodide layer uses an annealing process, in the process of annealing to form the intermediate layer and the protective layer, the perovskite layer, the intermediate layer, the organic electron transport layer, and the protective layer can be combined to increase the bonding force between the perovskite layer and the electron transport layer. In addition, cesium iodide as a constituent material of the protective layer can effectively protect the organic electron transport layer from damage during the subsequent deposition process. Because cesium iodide is an inorganic compound, it can block air vapor to a certain extent, thereby protecting the perovskite layer and the organic electron transport layer. Since the organic electron transport layer is sandwiched between the intermediate layer and the protective layer, the intermediate layer and the protective layer can also serve as the skeleton of the organic electron transport layer to a certain extent and play a supporting role, making the perovskite solar cell structure including the intermediate layer and the protective layer more stable. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the specific implementation methods of the utility model or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the utility model. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0019] Figure 1 It is a schematic structural diagram of a perovskite solar cell according to an embodiment of the utility model. DETAILED DESCRIPTION

[0020] In order to make the purpose, technical solution and advantages of the embodiment of the utility model clearer, the technical solution in the embodiment of the utility model will be clearly and completely described below in conjunction with the drawings in the embodiment of the utility model. Obviously, the described embodiment is a part of the embodiment of the utility model, not all the embodiments. Based on the embodiment of the utility model, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the utility model.

[0021] In one embodiment, Figure 1 As shown, the utility model provides a perovskite solar cell, comprising:

[0022] A perovskite layer, an intermediate layer, an electron transport layer and a protective layer, wherein the intermediate layer is arranged on a surface of the electron transport layer close to the perovskite layer, and the protective layer is arranged on a surface of the electron transport layer away from the perovskite layer, and the protective layer and the intermediate layer use the same alkali metal halide.

[0023] Due to the structure of the perovskite solar cell itself and the film deposition method, the perovskite layer and the organic electron transport layer not only have average bonding strength but also poor stability. The utility model adds a protective layer and an intermediate layer to the conventional perovskite solar cell structure, and the protective layer and the intermediate layer use alkali metal halides, which improves the bonding strength between the perovskite layer and the electron transport layer, reduces the possibility of the electron transport layer being damaged by subsequent deposition processes, and improves the overall stability of the perovskite solar cell.

[0024] It should be noted that for the substrate layer, bottom electrode layer, hole transport layer, perovskite layer, intermediate layer, electron transport layer, protective layer, buffer layer, back electrode layer and other film layers in the perovskite solar cell, if not specifically limited in the present disclosure, those skilled in the art can select appropriate materials according to actual needs. For example, the substrate material can be glass or an organic transparent material, the hole transport layer material can be nickel oxide or poly (3,4-ethylenedioxythiophene), and the perovskite layer material can be CsPbI3, MAPbI3, FAPbI3, Cs 0.5 MA0.5 PbI3、FA 0.5 MA 0.5 PbI 2.5 Br 0.5 or FA 0.5 MA 0.5 PbI 1.5 Br 1.5 , this disclosure does not limit this.

[0025] Optionally, in one embodiment, the alkali metal halide is selected from cesium iodide, and the selection from cesium iodide means that the corresponding film layer material is cesium iodide, that is, a cesium iodide layer is formed.

[0026] Optionally, in one embodiment, the material of the electron transport layer is selected from C 60 , C 70 and PCBM (fullerene derivative), that is, the electron transport layer material only includes C 60 , C 70 And one of PCBM.

[0027] Optionally, in one embodiment, the thickness of the intermediate layer is 1 nm to 5 nm (nanometers), for example, 1 nm, 3 nm or 5 nm.

[0028] Optionally, in one embodiment, the thickness of the electron transport layer is 5 nm to 50 nm, for example, 5 nm, 10 nm, 20 nm or 50 nm.

[0029] Optionally, in one embodiment, the thickness of the protective layer is 1 nm to 5 nm, for example, 1 nm, 3 nm or 5 nm.

[0030] Optionally, in one embodiment, the solar cell further includes a buffer layer, which is disposed on a surface of the protective layer away from the electron transport layer, and the thickness of the buffer layer is 7 nm to 25 nm, for example, 7 nm, 10 nm, 15 nm or 25 nm.

[0031] Optionally, in one embodiment, the material of the buffer layer is selected from tin dioxide, that is, the buffer layer is specifically a tin dioxide layer.

[0032] Optionally, in one embodiment, the solar cell further includes a substrate layer, a bottom electrode layer, a hole transport layer and a back electrode layer; the hole transport layer is arranged on a surface of the perovskite layer on a side away from the electron transport layer, the bottom electrode layer is arranged on a surface of the hole transport layer on a side away from the perovskite layer, the substrate layer is arranged on a surface of the bottom electrode layer on a side away from the hole transport layer, and the back electrode layer is arranged on a surface of the buffer layer on a side away from the electron transport layer; the material of the back electrode layer is selected from indium tin oxide or copper, that is, the material of the back electrode layer is indium tin oxide or copper, and the thickness of the back electrode layer is 60nm to 130nm, for example 60nm, 100nm or 130nm.

[0033] The alkali metal halide in the utility model is selected from cesium iodide, which is a metal iodide and an inorganic compound. The protective layer and the intermediate layer composed of cesium iodide are formed by an annealing process. The intermediate layer and the protective layer formed by the annealing process have the function of causing each film layer to crystallize and grow again, so that the intermediate layer and the protective layer are combined with the perovskite layer and the organic electron transport layer, and the bonding force between the perovskite layer and the electron transport layer is increased. Cesium iodide as a component material of the protective layer and the intermediate layer can effectively protect the organic electron transport layer from damage during the subsequent deposition process. Because cesium iodide is an inorganic compound, it can block air vapor to a certain extent, thereby protecting the perovskite layer and the organic electron transport layer. Since the organic electron transport layer is sandwiched between the intermediate layer and the protective layer, the intermediate layer and the protective layer can also serve as the skeleton of the organic electron transport layer to a certain extent, playing a supporting role, so that the perovskite solar cell structure including the intermediate layer and the protective layer is more stable. For example, when the electron transport layer material is C 60 The material is prone to agglomeration when the intermediate layer and protective layer are present. 60 reunion.

[0034] In one embodiment, based on the description of the above perovskite solar cell structure and materials, a method for preparing an inverted perovskite solar cell using the above description is provided.

[0035] The inverse perovskite solar cell preparation method is as follows:

[0036] A substrate layer is provided, for example a transparent glass substrate.

[0037] A bottom electrode layer is formed on the substrate layer. The bottom electrode layer is made of fluorine-doped tin dioxide with a thickness of 150 nm.

[0038] A hole transport layer is deposited on the cleaned bottom electrode layer. The hole transport layer is made of nickel oxide with a thickness of 40 nm.

[0039] On the hole transport layer, a perovskite layer can be deposited by scraping, spin coating, rolling coating, etc., and the perovskite layer is annealed to form a perovskite cell. The material of the perovskite layer is FA 0.5 MA 0.5 PbI3, thickness is 450nm.

[0040] The prepared perovskite cell was placed in the transition chamber of the PVD (Physical Vapor Deposition) vacuum evaporation equipment and evacuated to 8.0×10^-5Torr. When the vacuum degree of the evaporation source chamber was better than 3×10^-6Torr, the cesium iodide crucible was heated to 530°C to stabilize the deposition rate. The cell is sent into the evaporation source chamber for deposition, 3nm cesium iodide is deposited to form an intermediate layer, and 14nm C is deposited. 60 An electron transport layer is formed, and 3 nm of cesium iodide is deposited to form a protective layer.

[0041] A buffer layer is formed on the protective layer. Specifically, the buffer layer is deposited by using an ALD (Atomic Layer Deposition) device to form a tin dioxide buffer layer with a thickness of 7 nm.

[0042] The cell after the buffer layer is deposited is placed on a hot plate and annealed at 140°C for 1 hour.

[0043] A back electrode layer is formed on the buffer layer. Specifically, the back electrode layer is formed by depositing 150 nm copper on the surface of the buffer layer by using PVD / electron beam sputtering / magnetron sputtering.

[0044] In one embodiment, a reference example is provided, in which the structure of the perovskite solar cell is the same as the structure of the perovskite solar cell in the above method embodiment, including a substrate layer, a bottom electrode layer, a hole transport layer, a perovskite layer, an intermediate layer, an electron transport layer, a protective layer, a buffer layer and a back electrode layer, wherein the substrate layer is made of glass; the bottom electrode is 150nm thick, and the material used is fluorine-doped tin dioxide; the hole transport layer is deposited 40nm, and the material used is nickel oxide; the perovskite layer is deposited 450nm, and the material used is FA 0.5 MA 0.5 PbI3; the intermediate layer and protective layer are deposited at 3nm, and the material used is cesium iodide; the electron transport layer is deposited at 14nm, and the material used is C 60 The buffer layer is deposited at 7nm and the material used is tin dioxide; the back electrode layer is deposited at 150nm and the material used is copper.

[0045] Optionally, in one embodiment, a comparative example 1 is also provided: comparative example 1 provides another perovskite solar cell, which has a substrate layer, a bottom electrode layer, a hole transport layer, a perovskite layer, an electron transport layer, a buffer layer, and a back electrode layer compared to the above embodiment, wherein the substrate layer is made of glass; the bottom electrode is 150nm thick, and the material used is fluorine-doped tin dioxide; the hole transport layer is deposited to 40nm, and the material used is nickel oxide; the perovskite layer is deposited to 450nm, and the material used is FA 0.5 MA 0.5 PbI3; electron transport layer deposition 14nm, the material used is C 60 The buffer layer is deposited at 7nm and the material used is tin dioxide; the back electrode layer is deposited at 150nm and the material used is copper; there is no intermediate layer or protective layer.

[0046] Optionally, in one embodiment, a comparative example 2 is also provided: comparative example 2 provides another perovskite solar cell, which has a substrate layer, a bottom electrode layer, a hole transport layer, a perovskite layer, an intermediate layer, an electron transport layer, a buffer layer, and a back electrode layer compared to the above embodiment, wherein the substrate layer is made of glass; the bottom electrode is 150nm thick, and the material used is fluorine-doped tin dioxide; the hole transport layer is deposited 40nm, and the material used is nickel oxide; the perovskite layer is deposited 450nm, and the material used is FA 0.5 MA 0.5 PbI3; the middle layer is deposited 3nm, the material used is cesium iodide; the electron transport layer is deposited 14nm, the material used is C 60 ; The buffer layer is deposited at 7nm, and the material used is tin dioxide; the back electrode layer is deposited at 150nm, and the material used is copper; there is no protective layer.

[0047] Optionally, in one embodiment, a comparative example 3 is also provided: comparative example 3 provides another perovskite solar cell, which has a substrate layer, a bottom electrode layer, a hole transport layer, a perovskite layer, an electron transport layer, a protective layer, a buffer layer, and a back electrode layer compared to the above embodiments, wherein the substrate layer is made of glass; the bottom electrode is 150nm thick, and the material used is fluorine-doped tin dioxide; the hole transport layer is deposited 40nm, and the material used is nickel oxide; the perovskite layer is deposited 450nm, and the material used is FA 0.5 MA 0.5 PbI3; the protective layer is deposited at 3nm, and the material used is cesium iodide; the electron transport layer is deposited at 14nm, and the material used is copper; the buffer layer is deposited at 7nm, and the material used is tin dioxide; the back electrode layer is deposited at 150nm, and the material used is copper; there is no intermediate layer.

[0048] The perovskite solar cells provided in the reference example, comparative example 1, comparative example 2, and comparative example 3 were subjected to performance tests, and the test methods were as follows:

[0049] Photoelectric conversion efficiency test: Use a solar simulator to emit a standard sunlight (spectrum AM1.5G, incident power 100mW / cm 2 , temperature 25°C). At the same time, the components were aged (85°C, 15% RH, 300 hours of illumination under a standard sun) and then tested. The component area is 4.1 square centimeters.

[0050] The test results are shown in the following table:

[0051]

[0052] Compared with the comparative example, the efficiency of the perovskite component in the reference example is improved after aging, while the perovskite components in the comparative example all have different degrees of attenuation after aging. Specifically, the perovskite component of the reference example in which the intermediate layer and the protective layer are deposited has an efficiency increase of 1.77% after aging; the efficiency of the perovskite component of the comparative example 2 in which only the intermediate layer is deposited is attenuated by 14.31% after aging, and the efficiency of the perovskite component of the comparative example 3 in which only the protective layer is deposited is attenuated by 12.49% after aging; the efficiency of the perovskite component of the comparative example 1 in which the intermediate layer and the protective layer are not deposited is attenuated by 13.07% after aging.

[0053] According to the above, the utility model adds a protective layer and an intermediate layer, increases the bonding force between the perovskite layer and the electron transport layer, effectively protects the electron transport layer structure, and improves the aging resistance of the perovskite solar cell.

[0054] In the description of this specification, the description with reference to the terms "this embodiment", "one embodiment", "some embodiments", "example", "specific example", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the utility model. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, unless they are contradictory.

[0055] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present utility model, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0056] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0057] Although the embodiments of the present invention are described in conjunction with the accompanying drawings, those skilled in the art may make various modifications and variations without departing from the spirit and scope of the present invention, and such modifications and variations are all within the scope defined by the appended claims.

Claims

1. A perovskite solar cell, characterized in that: include: A perovskite layer, an intermediate layer, an electron transport layer and a protective layer, wherein the intermediate layer is arranged on a surface of the electron transport layer close to the perovskite layer, and the protective layer is arranged on a surface of the electron transport layer away from the perovskite layer, and the protective layer and the intermediate layer use the same alkali metal halide.

2. The solar cell according to claim 1, characterized in that: The alkali metal halide is selected from cesium iodide.

3. The solar cell according to claim 1, characterized in that The material of the electron transport layer is selected from C 60 , C 70 And one of PCBM.

4. The solar cell according to claim 1, characterized in that The thickness of the intermediate layer is 1 nm to 5 nm.

5. The solar cell according to claim 1, characterized in that: The thickness of the electron transport layer is 5 nm to 50 nm.

6. The solar cell according to claim 1, characterized in that The thickness of the protective layer is 1 nm to 5 nm.

7. The solar cell according to claim 1, characterized in that: Also includes: A buffer layer is provided on a surface of the protective layer away from the electron transport layer, and the thickness of the buffer layer is 7 nm to 25 nm.

8. The solar cell according to claim 7, characterized in that: The material of the buffer layer is selected from tin dioxide.

9. The solar cell according to claim 8, characterized in that Also includes: A substrate layer, a bottom electrode layer, a hole transport layer and a back electrode layer; the hole transport layer is arranged on a side surface of the perovskite layer away from the electron transport layer, the bottom electrode layer is arranged on a side surface of the hole transport layer away from the perovskite layer, the substrate layer is arranged on a side surface of the bottom electrode layer away from the hole transport layer, and the back electrode layer is arranged on a side surface of the buffer layer away from the electron transport layer; the material of the back electrode layer is selected from indium tin oxide or copper, and the thickness of the back electrode layer is 60nm to 130nm.

10. The solar cell according to claim 2, characterized in that: The thickness of the intermediate layer is 2nm-4nm, and the thickness of the protective layer is 2nm-4nm.