Reflective film
By introducing a light-transmitting insulating layer and ultraviolet-resistant layer into the photovoltaic gap reflective film, the problems of poor UV protection effect of polyester film and short-circuit corrosion of metal coating are solved, and the conversion efficiency and service life of photovoltaic modules are improved.
Patent Information
- Application Number
- CN202420272376.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-04
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2034-02-04
AI Technical Summary
The existing photovoltaic gap reflective films have poor UV protection effect, resulting in a short service life, and the metal coating is prone to short circuits and corrosion, reducing the power of photovoltaic modules.
A reflective film is designed, including a light-transmitting insulating layer, a reflective structure layer, a base film layer and an ultraviolet-resistant layer. The light-transmitting insulating layer blocks the contact between the reflective structure layer and the battery cell, and the ultraviolet-resistant layer prevents external factors from eroding, reducing short-circuit phenomenon. And improve service life.
It effectively reduces the occurrence of short circuit phenomenon, improves the service life of the reflective film and the conversion efficiency of photovoltaic modules, and enhances its durability and corrosion resistance.
Smart Images

Figure CN221946205U_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a reflective material, and in particular to a reflective film. Background Art
[0002] In photovoltaic modules, there are gaps between cells or cell strings. The sunlight passing through these gaps cannot be utilized, which results in low energy density of photovoltaic modules. Photovoltaic gap reflective film is a reflective film product specially used in photovoltaic power generation systems. It can reuse the sunlight in these gaps, thereby increasing the power of photovoltaic modules and ultimately achieving higher energy density of photovoltaic modules. In practical applications, photovoltaic gap reflective film is usually installed in the gaps between photovoltaic panels to increase light intensity and improve power generation efficiency. As one of the important means to improve the power generation efficiency of photovoltaic modules, photovoltaic gap reflective film has been increasingly applied and promoted, and has broad application prospects and market potential.
[0003] In the prior art, such as Figure 1 As shown, the photovoltaic gap reflective film is mainly composed of a base layer 10 and a reflective layer 20. The base layer 10 is generally a polyester film, and the reflective layer 20 is composed of a multi-layer reflective microstructure, and the multi-layer reflective microstructure is composed of at least one prism structure and a reflective layer for reflecting light. The anti-ultraviolet effect of polyester film is not good. The reflective film made of polyester film is exposed to sunlight for a long time, which will reduce the service life of the reflective film, increase the frequency of users replacing the reflective film, cause economic damage to users, and is not conducive to the use of users.
[0004] The utility model patent with patent number CN108010981A discloses a reflective film for improving photovoltaic conversion efficiency and a preparation method thereof. The reflective film includes a substrate layer, an adhesive layer arranged on the lower layer of the substrate layer, a microstructure layer arranged on the upper layer of the substrate layer, and a reflective layer arranged on the upper layer of the microstructure layer. The reflective layer is a metal coating, which is generally an aluminum coating or a silver coating. Although the reflective film of this structure can improve the photovoltaic conversion efficiency to a certain extent, it is easy for the metal coating to directly contact the battery cell and conductive solder and other materials, resulting in a short circuit, thereby reducing the power of the photovoltaic module. In addition, the metal coating is easily scratched and corroded during the application process.
[0005] Therefore, it is urgent to provide a new reflective film to solve the above problems. Utility Model Content
[0006] The utility model aims to solve at least one of the technical problems existing in the prior art. To this end, the utility model provides a reflective film that can reduce the occurrence of short circuits and prevent external factors from corroding the reflective film, thereby increasing its service life.
[0007] The utility model provides a reflective film, comprising: a light-transmitting insulating layer, a reflective structural layer, a base film layer, an ultraviolet-resistant layer and an adhesive film layer, wherein the reflective structural layer is arranged on one side of the base film layer, the light-transmitting insulating layer is arranged on a side of the reflective structural layer away from the base film layer, the ultraviolet-resistant layer is arranged on a side of the base film layer away from the reflective structural layer, and the adhesive film layer is arranged on a side of the ultraviolet-resistant layer away from the base film layer.
[0008] Furthermore, the material of the light-transmitting insulating layer includes at least one of UV adhesive, thermosetting adhesive, and hot melt adhesive.
[0009] Furthermore, the thickness of the light-transmitting insulating layer is 1-50 μm.
[0010] Preferably, the thickness of the light-transmitting insulating layer is 2-10 μm.
[0011] Furthermore, the reflective structure layer includes a first base layer and a first coating arranged on the first base layer, the first base layer is composed of a plurality of triangular prisms, the first coating includes at least one of a first metal coating and a first metal oxide coating, and the first coating is a triangular corrugated shape that matches the shape of the first base layer.
[0012] Furthermore, the top angle of the triangular corrugation is 90-150 degrees, and the angle between the extending direction of the triangular corrugation and the preset direction of the base film layer is 10-90 degrees.
[0013] Furthermore, the UV-resistant layer includes at least one of a second metal coating, a second metal oxide coating, a polyester polyurethane coating, an acrylic coating, a siloxane coating, a fluorocarbon coating, a ceramic coating, and a mica coating.
[0014] Furthermore, the material of the first metal coating layer and the second metal coating layer includes at least one of aluminum and silver;
[0015] and / or,
[0016] The materials of the first metal oxide coating layer and the second metal oxide coating layer include at least one of titanium dioxide and zinc oxide.
[0017] Furthermore, the UV-resistant layer includes a second base layer and a second coating disposed on the second base layer, the second coating includes at least one of the second metal coating and the second metal oxide coating, and the second base layer is composed of a plurality of triangular prisms.
[0018] Furthermore, the top of the triangular prism is at least one of a pointed angle structure, an arc angle structure, a platform structure, and a wave structure.
[0019] Furthermore, the material of the base film layer includes polyethylene terephthalate and UV-resistant material.
[0020] Furthermore, the UV-resistant material includes at least one of mica powder and titanium dioxide.
[0021] One or more of the above embodiments of the present invention have at least one or more of the following beneficial effects:
[0022] The utility model can reduce the occurrence of short circuit phenomenon and prevent the erosion of the reflective film by external factors by arranging a light-transmitting insulating layer on the side of the reflective structure layer away from the base film layer, and arranging a UV-resistant layer on the side of the base film layer away from the reflective structure layer, thereby improving its service life. Specifically, the light-transmitting insulating layer can block the direct contact between the reflective structure layer and conductive materials such as the battery cell and the photovoltaic welding strip, reduce the occurrence of short circuit phenomenon, thereby achieving a good insulation effect, and ultimately improving the service life of the reflective film. The UV-resistant layer can effectively prevent the erosion of the reflective film by external factors, thereby improving its service life.
[0023] Additional aspects and advantages of the present invention will be given in part in the following description and in part will become apparent from the following description or will be learned through the practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The disclosure of the present invention will become easier to understand with reference to the accompanying drawings. It is easy for those skilled in the art to understand that these drawings are only for illustrative purposes and are not intended to limit the scope of protection of the present invention. In addition, similar numbers in the drawings are used to represent similar components, among which:
[0025] Figure 1 It is a schematic diagram of the structure of the photovoltaic gap reflective film provided by the background technology of this application;
[0026] Figure 2 It is a schematic diagram of the structure of a reflective film provided in an embodiment of the present application;
[0027] Figure 3 It is a schematic diagram of the structure of another reflective film provided in an embodiment of the present application.
[0028] Description of Reference Numerals
[0029] The base layer 10 , the reflective layer 20 , the light-transmitting insulating layer 100 , the reflective structural layer 200 , the base film layer 300 , the UV-resistant layer 400 and the adhesive film layer 500 . DETAILED DESCRIPTION
[0030] Some embodiments of the present invention are described below with reference to the accompanying drawings. It should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the present invention and are not intended to limit the protection scope of the present invention.
[0031] As shown in the background technology, the reflective film is mainly composed of a base layer and a reflective layer. The base layer is mainly composed of polyester film. Since the anti-ultraviolet effect of polyester film is not good, the reflective film made of polyester film will be exposed to the sun for a long time, which will reduce the service life of the reflective film. In addition, the reflective layer is mainly a metal coating. During the use of the reflective film, the metal coating will directly contact the battery cell and conductive solder and other materials, resulting in a short circuit, thereby reducing the power of the photovoltaic module.
[0032] In this regard, the utility model creatively proposes a reflective film, which can reduce the occurrence of short circuits and prevent external factors from corroding the reflective film, thereby increasing its service life by arranging a light-transmitting insulating layer on the side of the reflective structure layer away from the base film layer and a UV-resistant layer on the side of the base film layer away from the reflective structure layer.
[0033] like Figure 2 As shown, the reflective film provided by the utility model includes a light-transmitting insulating layer 100, a reflective structural layer 200, a base film layer 300, an ultraviolet-resistant layer 400 and an adhesive film layer 500. The reflective structural layer 200 is arranged on one side of the base film layer 300, the light-transmitting insulating layer 100 is arranged on the side of the reflective structural layer 200 away from the base film layer 300, the ultraviolet-resistant layer 400 is arranged on the side of the base film layer 300 away from the reflective structural layer 200, and the adhesive film layer 500 is arranged on the side of the ultraviolet-resistant layer 400 away from the base film layer 300.
[0034] The reflective structure layer 200 includes a first substrate layer and a first coating layer disposed on the first substrate layer, wherein the first substrate layer is composed of a plurality of triangular prisms arranged, the first coating layer includes at least one of a first metal coating layer and a first metal oxide coating layer, and the first coating layer is a triangular corrugated shape adapted to the shape of the first substrate layer. The first substrate layer composed of a plurality of triangular prisms arranged and the first coating layer adapted to the shape thereof can reflect sunlight at different incident angles to the cell through the triangular prisms, thereby improving the utilization rate of solar energy and thus improving the photovoltaic conversion efficiency. In the embodiment of the present application, the top of the triangular prism is at least one of a sharp angle structure, a rounded angle structure, a platform structure, and a wave structure.
[0035] As a preferred embodiment, the vertex angle of the triangular corrugation is 90-150 degrees, and the angle between the corrugation extension direction of the triangular corrugation and the preset direction of the base film layer 300 is 10-90 degrees, and the preset direction is the length direction of the base film layer 300. As a schematic illustration, Figure 2 , Figure 3As shown, the X direction is the length direction of the base film layer 300, and the Y direction is the width direction of the base film layer 300. The vertex angle of the triangular corrugation is set to 90-150 degrees, and the angle between the corrugation extension direction of the triangular corrugation and the preset direction of the base film layer 300 is set to 10-90 degrees to ensure that light sources from different lighting directions can be reflected onto the battery sheet, thereby improving the utilization rate of solar energy under different solar incident angles, making the photovoltaic module applicable to areas with different lighting directions, and increasing the versatility of the reflective film.
[0036] In a specific embodiment, the material of the first substrate layer is a polymer material, preferably polyethylene terephthalate. Polyethylene terephthalate has good transparency and weather resistance, which can ensure the service life and stability of the reflective film. Polyethylene terephthalate also has a low density and a high elastic modulus, which can reduce the weight of the reflective film and improve the flexibility and plasticity of the reflective film. In addition, polyethylene terephthalate also has good processing performance and low cost, and a triangular prism structure can be prepared through a simple process, thereby reducing the difficulty of producing the reflective film.
[0037] In the embodiment of the present application, the material of the first metal coating layer includes at least one of aluminum and silver, and the material of the first metal oxide coating layer includes at least one of titanium dioxide and zinc oxide. The thickness of the first coating layer is 10-1000nm. The use of the first coating layer of the above thickness can improve the reflectivity of the first coating layer, so that more sunlight is reflected onto the battery cell, increasing the conversion efficiency of the photovoltaic module, and also taking into account the thickness of the first coating layer, thereby reducing the production cost of the reflective film.
[0038] In the prior art, the reflective layer of the reflective film is mainly a metal coating. During use, the metal coating will directly contact materials such as battery cells and conductive solder, resulting in a short circuit, thereby reducing the power of the photovoltaic module. In order to overcome this defect, the present application is provided with a light-transmitting insulating layer 100 on one side of the reflective structure layer 200. The material of the light-transmitting insulating layer 100 includes at least one of UV glue, thermosetting glue, and hot melt glue. The light-transmitting insulating layer 100 prepared by UV glue, thermosetting glue, and hot melt glue has a low hardness and is resistant to high temperatures. In actual use, it can block the direct contact between the first coating in the reflective structure layer 200 and conductive materials such as battery cells and photovoltaic welding strips, reduce the occurrence of short circuits, thereby achieving a good insulation effect, and ultimately improving the service life of the reflective film.
[0039] In a specific embodiment, the thickness of the light-transmitting insulating layer 100 is 1-50 μm. Preferably, the thickness of the light-transmitting insulating layer 100 is 2-10 μm. The thickness in the above range can not only achieve a good insulating effect of the reflective film, but also take into account the weight of the reflective film, thereby improving the production efficiency of the reflective film and reducing the production cost of the reflective film.
[0040] In another specific embodiment, the shape of the light-transmitting insulating layer 100 is adapted to the shape of the first coating layer, and the light-transmitting insulating layer 100 rises and falls with the rise and fall of the first coating layer structure. This design can reduce the amount of the light-transmitting insulating layer 100 while ensuring that the reflective film has a good insulation effect, thereby reducing the production cost of the reflective film.
[0041] The base film layer 300 is generally a polyester film, which is a transparent, glossy film with excellent mechanical properties, high rigidity, hardness and toughness, puncture resistance, friction resistance, high and low temperature resistance, good air tightness and other advantages. However, the anti-ultraviolet effect of polyester film is not good. The reflective film prepared by polyester film is exposed to the sun for a long time, which will reduce the service life of the reflective film, increase the frequency of users replacing the reflective film, cause economic damage to users, and be unfavorable for users to use. In response to this problem, the present application is provided with an ultraviolet-resistant layer 400 on the side of the base film layer 300 away from the reflective structure layer 200. The ultraviolet-resistant layer 400 can effectively prevent external factors from eroding the reflective film, thereby increasing its service life.
[0042] In the embodiment of the present application, the UV-resistant layer 400 includes at least one of a second metal coating, a second metal oxide coating, a polyester polyurethane coating, an acrylic coating, a siloxane coating, a fluorocarbon coating, a ceramic coating, and a mica coating.
[0043] The use of the second metal coating as the UV-resistant layer 400 can not only prevent external factors from corroding the reflective film, but also increase the reflective effect of the back of the reflective film, thereby improving the double-sidedness of the photovoltaic module. The double-sidedness of a photovoltaic module refers to the ratio of the ability of both sides of the photovoltaic module to generate electricity to the total area. Specifically, the double-sidedness refers to the ratio of the total amount of solar radiation received by the back of the photovoltaic module to the total amount of solar radiation received by the front, usually expressed as a percentage. The calculation formula for the double-sidedness is: double-sidedness = (back power / front power) × 100%. This ratio reflects the degree to which both sides of the photovoltaic module can absorb solar energy, which is directly related to the power generation efficiency of the photovoltaic module. The importance of the bifaciality of photovoltaic modules to photovoltaic systems is reflected in the following aspects: 1) Improved power generation efficiency: Bifacial modules can use both sides to absorb sunlight, thereby improving power generation efficiency, which is unmatched by single-sided modules; 2) Improved load capacity: Since bifacial modules can generate electricity on two sides, they can withstand more loads than single-sided modules; 3) Higher environmental adaptability: In certain special environments, such as steep mountainous areas, snowy areas or water surfaces with strong light, bifacial modules can better cope with such environments; 4) Longer service life: Since bifacial modules can generate electricity on two sides, they can better ensure the balance of module surface temperature, thereby increasing the service life of the modules.
[0044] As a preferred embodiment, the material of the second metal coating includes at least one of aluminum and silver. The aluminum layer or silver layer made of aluminum or silver has a high reflectivity, which can more effectively reflect sunlight onto the cell, thereby effectively improving the conversion efficiency of the photovoltaic module. In addition, the aluminum layer and the silver layer also have good weather resistance and corrosion resistance, which can increase the service life of the reflective film.
[0045] The material of the second metal oxide coating includes at least one of titanium dioxide and zinc oxide. These metal oxide coatings have high transparency and can effectively reflect light without affecting the visible light transmission performance of the reflective film.
[0046] In addition, other types of UV-resistant layers 400 provided in the present application also have their own advantages. For example, polyester polyurethane coatings have excellent weather resistance and UV resistance; acrylic coatings have excellent weather resistance and corrosion resistance, and can also effectively resist damage from environmental factors such as UV rays and ozone; siloxane coatings have excellent weather resistance and high temperature resistance, and can effectively resist damage to the reflective film by UV rays, while also improving the anti-fouling performance of the reflective film; fluorocarbon coatings have excellent weather resistance, high temperature resistance, and chemical resistance.
[0047] In a specific embodiment, the thickness of the UV-resistant layer 400 is 1-20 μm. The thickness in the above range can not only improve the UV resistance of the reflective film, but also take into account the weight of the reflective film, thereby improving the production efficiency of the reflective film and reducing the production cost of the reflective film.
[0048] As a preferred implementation method, Figure 3 As shown, the UV-resistant layer 400 includes a second substrate layer and a second coating disposed on the second substrate layer, the second coating includes at least one of a second metal coating and a second metal oxide coating, and the second substrate layer is composed of a plurality of triangular prisms. This design can make the upper and lower surfaces of the reflective film reflective. When the reflective film is applied to a photovoltaic module, the light from the illuminated surface and the backlight surface can be effectively reflected to the surface of the photovoltaic module, thereby improving the double-sidedness of the module. In addition, the second substrate layer composed of a plurality of triangular prisms and the second coating adapted to the shape thereof can reflect sunlight of different incident angles to the battery cell through the triangular prisms, thereby improving the utilization rate of solar energy and thus improving the photovoltaic conversion efficiency. Similarly, the top of the triangular prism is at least one of a sharp angle structure, a rounded angle structure, a platform structure, and a wave structure.
[0049] In addition, in order to further improve the service life of the reflective film, the material of the base film layer 300 provided in the present application includes, in addition to polyethylene terephthalate, a UV-resistant material, and the UV-resistant material includes at least one of mica powder and titanium dioxide.
[0050] In the embodiment of the present application, the adhesive film layer 500 is arranged on the side of the UV-resistant layer 400 away from the adhesive film layer 500. The adhesive film layer 500 is to facilitate the connection between the reflective film and the photovoltaic module and ensure the stability of the reflective film during use. The material of the adhesive film layer 500 includes but is not limited to polyurethane, ethylene-vinyl acetate copolymer (EVA), copolyamide, copolyester, etc. Users can choose according to actual needs, and no specific limitation is made here.
[0051] The following is described by specific examples:
[0052] Example 1
[0053] A reflective film comprises a light-transmitting insulating layer 100, a reflective structural layer 200, a base film layer 300, an ultraviolet-resistant layer 400 and an adhesive film layer 500 which are arranged in sequence.
[0054] The material of the light-transmitting insulating layer 100 is high-transmittance UV glue, and the thickness is 5 μm.
[0055] The reflective structure layer 200 includes a first substrate layer and a first coating layer disposed on the first substrate layer. The material of the first substrate layer is UV structural adhesive, the material of the first coating layer is metal aluminum, the reflectivity of the first coating layer to the visible light spectrum is 95%, and the optical density is 4.6. The first substrate layer is composed of a plurality of triangular prisms arranged, and the first coating layer is a triangular corrugated shape adapted to the shape of the first substrate layer, the vertex angle of the triangular corrugated shape is 120 degrees, and the angle between the corrugated extension direction of the triangular corrugated shape and the length direction of the base film layer 300 is 18 degrees. The thickness of the first coating layer is 50nm.
[0056] The material of the base film layer 300 is polyethylene terephthalate, and the thickness of the base film layer 300 is 35 μm.
[0057] The UV-resistant layer 400 is a metal coating made of aluminum. The reflectivity of the metal coating to the visible light spectrum is 96%, and the optical density is 4.6.
[0058] The material of the adhesive film layer 500 is EVA, and the thickness thereof is 90 μm.
[0059] Example 2
[0060] The difference between Example 2 and Example 1 lies in that the UV-resistant layer 400 and the adhesive film layer 500 are different.
[0061] The UV-resistant layer 400 in Example 2 includes a second substrate layer and a second coating disposed on the second substrate layer. The material of the second substrate layer is UV structural adhesive, the material of the second coating is metal aluminum, the reflectivity of the second coating to the visible light spectrum is 95%, and the optical density is 4.6. The second substrate layer is composed of a plurality of triangular prisms arranged, and the second coating is a triangular corrugated shape that matches the shape of the first substrate layer, the vertex angle of the triangular corrugated shape is 120 degrees, and the angle between the corrugated extension direction of the triangular corrugated shape and the length direction of the base film layer 300 is 18 degrees. The thickness of the second coating is 50nm.
[0062] The adhesive film layer 500 in Example 2 is in a triangular corrugated shape that matches the shape of the second coating layer.
[0063] Comparative Example 1
[0064] The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 does not have the light-transmitting insulating layer 100 .
[0065] Comparative Example 2
[0066] The difference between Comparative Example 2 and Example 1 is that Comparative Example 2 does not have the UV resistant layer 400 .
[0067] Comparative Example 3
[0068] The difference between Comparative Example 3 and Example 1 is that Comparative Example 3 does not have the light-transmitting insulating layer 100 and the UV-resistant layer 400 .
[0069] The following experiments were conducted on the reflective films prepared in Examples 1-2 and Comparative Examples 1-3.
[0070] A 570W standard photovoltaic module was used as a blank group, and the reflective films prepared in Examples 1-2 and Comparative Examples 1-3 were pasted between the gaps of the solar panels, and the adhesive film layer 500 was bonded to the glass back panel of the photovoltaic module. The test time span was 1 hour, and the test results are shown in Table 1.
[0071] Table 1
[0072] Power(W) Power increase percentage Blank Group 570 0 Example 1 580 1.75% Example 2 582 2.10% Comparative Example 1 581 1.92% Comparative Example 2 577 1.22% Comparative Example 3 578 1.40%
[0073] Test results:
[0074] 1) From the test results of Example 1, Comparative Examples 1-3 and the blank group, it can be seen that the UV-resistant layer provided on the side of the base film layer away from the reflective structure layer can increase the power of the photovoltaic module. This is because the UV-resistant layer can effectively prevent the erosion of the reflective film by external factors, increase the reflectivity of the reflective film, enhance its reflective effect, and thus increase the power of the photovoltaic module.
[0075] 2) From the test results of Example 1 and Example 2, it can be seen that when the UV-resistant layer includes a second substrate layer and a second coating disposed on the second substrate layer, the second substrate layer is composed of a plurality of triangular prisms, and the second coating is a triangular corrugated shape that matches the shape of the first substrate layer, the power of the photovoltaic module is increased more. This is because the second substrate layer composed of a plurality of triangular prisms and the second coating that matches the shape can reflect sunlight at different incident angles to the battery cell through the triangular prisms, thereby improving the utilization rate of solar energy and thus improving the photovoltaic conversion efficiency.
[0076] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the utility model. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0077] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present utility model, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0078] Although the embodiments of the present invention have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations of the present invention. Ordinary technicians in the field can change, modify, replace and modify the above embodiments within the scope of the present invention.
Claims
1. A reflective film, characterized in that: include: A light-transmitting insulating layer, a reflective structural layer, a base film layer, a UV-resistant layer and an adhesive film layer, wherein the reflective structural layer is arranged on one side of the base film layer, the light-transmitting insulating layer is arranged on a side of the reflective structural layer away from the base film layer, the UV-resistant layer is arranged on a side of the base film layer away from the reflective structural layer, and the adhesive film layer is arranged on a side of the UV-resistant layer away from the base film layer.
2. The reflective film according to claim 1, characterized in that: The material of the light-transmitting insulating layer is one of UV glue, thermosetting glue and hot melt glue.
3. The reflective film according to claim 1, characterized in that: The thickness of the light-transmitting insulating layer is 1-50 μm.
4. The reflective film according to claim 1, characterized in that: The reflective structure layer includes a first base layer and a first coating arranged on the first base layer, the first base layer is composed of a plurality of triangular prisms, the first coating is one of a first metal coating and a first metal oxide coating, and the first coating is a triangular corrugated shape that matches the shape of the first base layer.
5. The reflective film according to claim 4, characterized in that: The top angle of the triangular corrugation is 90-150 degrees, and the angle between the corrugation extension direction of the triangular corrugation and the preset direction of the base film layer is 10-90 degrees.
6. The reflective film according to claim 1, characterized in that: The UV-resistant layer is one of a second metal coating, a second metal oxide coating, a polyester polyurethane coating, an acrylic coating, a siloxane coating, a fluorocarbon coating, a ceramic coating, and a mica coating.
7. The reflective film according to claim 4, characterized in that: The material of the first metal coating layer is one of aluminum and silver, and the material of the first metal oxide coating layer is one of titanium dioxide and zinc oxide.
8. The reflective film according to claim 6, characterized in that: The material of the second metal coating layer is one of aluminum and silver, and the material of the second metal oxide coating layer is one of titanium dioxide and zinc oxide.
9. The reflective film according to claim 6, characterized in that: The UV-resistant layer includes a second base layer and a second coating layer disposed on the second base layer, the second coating layer is one of the second metal coating layer and the second metal oxide coating layer, and the second base layer is composed of a plurality of triangular prisms arranged.
10. The reflective film according to claim 4 or 9, characterized in that: The top of the triangular prism is at least one of a pointed angle structure, an arc angle structure, a platform structure, and a wave structure.