Sample for evaluating fracture toughness of wire rod

By designing a specimen made of a long strip of metal cut from wire with a notch in its thickness direction, the problem of difficulty in evaluating the fracture toughness of fastener wire notches in the prior art is solved, and the fatigue resistance and end forming performance of fasteners are improved.

CN222013750UActive Publication Date: 2024-11-15CHINALCO MATERIALS APPL RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202323418336.3
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-12-14
Publication Date
2024-11-15
Estimated Expiration
2033-12-14

AI Technical Summary

Technical Problem

Existing technologies make it difficult to quickly and effectively assess the notch fracture toughness of fastener wires, which affects the fatigue resistance and service life of fasteners.

Method used

A specimen for evaluating the fracture toughness of wire is designed by cutting a long strip of metal from the wire and making a notch in its thickness direction. The notch is located at the center of the length, and the cross-section is I-shaped or triangular with a circular arc at the root. The material is aluminum alloy, titanium alloy or nickel-based high-temperature alloy, and it is used for dynamic/static loading tests on a bending testing machine.

Benefits of technology

It enables efficient and convenient assessment of wire notch fracture toughness, improves the end forming performance and fatigue resistance of fasteners, and reduces evaluation costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN222013750U_ABST
    Figure CN222013750U_ABST
Patent Text Reader

Abstract

The utility model provides a sample for evaluating the fracture toughness of a wire rod, which comprises a main body, the main body is a strip-shaped metal sheet obtained by cutting the wire rod, the main body is provided with a notch along the thickness direction of the main body, and the notch is arranged at the length center of the main body. By adopting the scheme, the main body is the strip-shaped metal sheet obtained by cutting the wire rod, so that the main body is convenient for testing the fracture toughness, and the main body is provided with the notch along the thickness direction of the main body, so that the notch fracture toughness of different wire rods can be evaluated. The mode of cutting the metal sheet from the wire to form the notch is adopted, operation is easy and convenient, the construction period is short, and efficiency is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to the technical field of wire material testing, in particular to a test specimen for evaluating the fracture toughness of a wire material. Background Art

[0002] Fasteners are usually formed from wire. The processing deformation and service load generated by fasteners during processing, manufacturing and application are directly related to their processing formability, thread loading and tightening force, and defect sensitivity of fasteners and notch fracture toughness, which will also directly affect the fatigue resistance of fasteners and connection structures of fastener products, as well as the stiffness performance and service life of the products.

[0003] In industrial production applications, metal wires or bars are generally processed into fastener parts, and the end failure evaluation of the finished fasteners is used. The evaluation cost is high and the technical threshold is high, making it difficult to quickly and effectively develop high-performance fasteners and wires and bars. Therefore, a specimen is needed to efficiently evaluate the notch fracture toughness of wires. Utility Model Content

[0004] The utility model provides a sample for evaluating the fracture toughness of a wire material, so as to achieve the purpose of evaluating the notch fracture toughness of the wire material with high efficiency.

[0005] In order to solve the above problems, the utility model provides a specimen for evaluating the fracture toughness of a wire, comprising a main body, which is a long metal sheet cut from a wire, and a notch is opened along the thickness direction of the main body, and the notch is set at the length center of the main body.

[0006] Furthermore, the cross section of the wire is polygonal or circular.

[0007] Furthermore, the depth of the notch is 0.1 to 0.5 times the thickness of the main body.

[0008] Furthermore, the longitudinal cross section of the notch in the length direction of the main body is in a straight line shape.

[0009] Furthermore, a longitudinal cross section of the notch in the length direction of the main body is a triangle.

[0010] Furthermore, the root of the notch is arc-shaped.

[0011] Furthermore, the radius of the root of the notch is 0.05-0.5 mm.

[0012] Further, the thickness of the body is the radius of a cylindrical fastener, which is processed from a wire; or the thickness of the body is the thickness of a hollow fastener, which is processed from a wire.

[0013] Furthermore, the length range of the main body is greater than 10 mm.

[0014] Furthermore, the material of the main body is aluminum alloy, titanium alloy or nickel-based high-temperature alloy.

[0015] By applying the technical solution of the utility model, a test specimen for evaluating the fracture toughness of wires is provided, including a main body, which is a long metal sheet cut from a wire, and a notch is provided in the thickness direction of the main body, and the notch is arranged at the length center of the main body. With this solution, the main body is a long metal sheet cut from a wire, so that the main body is convenient for testing the fracture toughness, and the main body is notched in the thickness direction of the main body, so that the notch fracture toughness of different wires can be evaluated. The method of notching the metal sheet cut from the wire is simple and convenient to operate, with a short construction period and high efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] The drawings constituting part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation on the present invention. In the drawings:

[0017] Figure 1 The schematic diagram of the structure of the sample for evaluating the fracture toughness of a wire provided in the first embodiment of the utility model is shown;

[0018] Figure 2 The test curve of the sample in the first embodiment of the present utility model is shown.

[0019] The above drawings include the following reference numerals:

[0020] 10. Main body; 11. Gap. DETAILED DESCRIPTION

[0021] The following will be combined with the drawings in the embodiments of the utility model to clearly and completely describe the technical solutions in the embodiments of the utility model. Obviously, the described embodiments are only part of the embodiments of the utility model, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means a limitation on the utility model and its application or use. Based on the embodiments in the utility model, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the utility model.

[0022] like Figure 1 to Figure 2 As shown, an embodiment of the utility model provides a specimen for evaluating the fracture toughness of a wire, including a main body 10, the main body 10 is a long metal sheet cut from a wire, the main body 10 is provided with a notch 11 along the thickness direction of the main body 10, and the notch 11 is arranged at the length center of the main body 10.

[0023] In this solution, the main body 10 is a long metal sheet cut from a wire, so that the main body 10 is convenient for testing the fracture toughness. The main body 10 is provided with a notch 11 along the thickness direction of the main body 10, so that the notch fracture toughness of different wires can be evaluated. The method of cutting the metal sheet from the wire to provide the notch 11 is simple and convenient to operate, with a short construction period and high efficiency.

[0024] Furthermore, the cross section of the wire is polygonal or circular. In this way, the specimens for evaluating the fracture toughness of the wire provided in the present application are mainly sampled for polygonal and circular wires.

[0025] like Figure 1 As shown, the depth of the notch 11 is 0.1 to 0.5 times the thickness of the main body 10. This arrangement enables the depth of the notch 11 to meet the requirements of the fracture toughness test of the main body 10.

[0026] In the first embodiment of the present invention, the longitudinal cross section of the notch 11 in the length direction of the main body 10 is in the shape of a straight line. In this way, the cross section of the notch 11 is in the shape of a straight line, so that the sample for evaluating the fracture toughness of the wire has a straight notch in the thickness direction, and the fracture toughness of the sample is tested on the basis of the straight notch.

[0027] In the sixth embodiment of the present invention, the longitudinal cross section of the notch 11 in the length direction of the main body 10 is triangular. In this way, the cross section of the notch 11 is triangular, so that the sample for evaluating the fracture toughness of the wire has a triangular notch in the thickness direction, and the fracture toughness of the sample is tested on the basis of the triangular notch.

[0028] like Figure 1 As shown, the root of the notch 11 is arc-shaped. In this way, an arc-shaped chamfer is set at the root of the notch 11, so that the stress at the root of the notch 11 is small, and the fracture toughness test result of the sample for evaluating the fracture toughness of the wire is less affected by the shape of the bottom of the notch 11.

[0029] Furthermore, the radius of the root of the notch 11 is 0.05-0.5 mm. This arrangement allows the radius of the root of the notch 11 to change with the width and shape of the notch 11.

[0030] The thickness of the main body 10 is the radius of a cylindrical fastener, which is processed from a wire; or the thickness of the main body 10 is the thickness of a hollow fastener, which is processed from a wire. In this way, the thickness of the sample for evaluating the fracture toughness of the wire of a cylindrical fastener is the radius of the fastener, and the thickness of the sample for evaluating the fracture toughness of the wire of a hollow fastener is the thickness of the fastener, so that the thickness of the main body 10 of the sample for evaluating the fracture toughness of the wire changes with the shape of the fastener.

[0031] Furthermore, the length of the main body 10 is greater than 10 mm. This arrangement enables the main body 10 to overlap the two supporting points of the supporting platform, so that the supporting points support the main body 10, and the main body 10 is deformed by the load to complete the test.

[0032] In a specific embodiment of the present invention, the material of the main body 10 is aluminum alloy, titanium alloy or nickel-based high-temperature alloy.

[0033] With such arrangement, in a specific embodiment of the present invention, the wire fracture toughness can be evaluated by sampling from wires of aluminum alloy, titanium alloy or nickel-based high-temperature alloy.

[0034] The test specimen for evaluating the fracture toughness of a wire rod of the utility model is used in a testing device, and the testing device comprises a loading pressure head and two supporting rollers.

[0035] In the first embodiment of the present invention, a 7075-T6 aluminum alloy wire with a diameter*length of φ8mm*50mm is taken as a research object to study the notch 11 fracture toughness of wires prepared by different processes, specifically including the following steps:

[0036] (1) A 2.5 mm thick bow-shaped specimen was cut from a φ8 mm*50 mm 7075-T6 aluminum alloy wire, and a straight notch 11 was machined at the center of the specimen. The height of the notch 11 was 0.5 mm, and the arc radius at the root of the notch 11 was 0.1 mm.

[0037] Among them, samples of φ8mm 7075-T6 aluminum alloy wires of the original and optimized processes were taken to process the above-mentioned specimens for evaluating the fracture toughness of the wires, with the optimized process wires as test specimens and the original process wires as comparison specimens;

[0038] (2) The distance between the support rollers is set to D + 3 times the sample thickness a, that is, the diameter of the loading head is 5 mm, and the distance between the two force application points is 12.5 mm;

[0039] (3) The test specimen (including the test specimen and the comparative specimen) is placed between the loading head and the support roller of the bending test machine, and the test specimen is loaded at a dynamic / static rate through the hydraulic control system of the test machine. The dynamic / static loading and failure process of the specimen are monitored by a load sensor and a displacement sensor, wherein a force application point of the loading head on one end of the test specimen (the end of the unprocessed notch 11 of the specimen for evaluating the fracture toughness of the wire) is located at the center of the length, and two force application points of the support roller on the other end of the test specimen (the end of the processed notch 11 of the specimen for evaluating the fracture toughness of the wire) are symmetrically located on both sides of the center of the length;

[0040] (4) The bending test machine records data by means of load sensors and displacement sensors during dynamic / static loading and failure processes, and performs subsequent processing on the experimental data to evaluate the notched fracture toughness of the fastener wire and its failure mechanism.

[0041] The load-displacement curve during the test of Example 1 is as follows: Figure 2 As shown. Among them, the test specimen of the optimized process wire broke at a load of 595N and a displacement of 2.1mm, while the comparison specimen of the original process wire broke at a load of 558N and a displacement of 1.9mm, indicating that the notch 11 fracture toughness of the optimized process wire is better than that of the original process wire. The two process wires of the same batch were processed into standard fasteners, and the fastener closing forming experiment was carried out to compare the closing forming performance of the two process wires. The maximum locking torque of the fastener closing is 0.98N*m, and the maximum locking torque of the fastener closing is 0.7N*m; indicating that the closing forming performance of the optimized process wire is better than that of the original process wire.

[0042] In the second embodiment of the present invention, a 7075-T6 aluminum alloy wire with a diameter*length of φ8mm*50mm is taken as a research object to study the notch 11 fracture toughness of the alloy wire, which specifically includes the following steps:

[0043] (1) A 4 mm thick bow-shaped specimen was cut from a φ8 mm*50 mm 7075-T6 aluminum alloy wire, and a straight notch 11 was machined at the center of the specimen. The height of the notch 11 was 0.5 mm, and the arc radius at the root of the notch 11 was 0.1 mm.

[0044] (2) The distance between the support rollers is set to D + 3 times the sample thickness a, that is, the diameter of the loading head is 5 mm, and the distance between the two force application points is 17 mm;

[0045] (3) The test specimen (including the test specimen and the comparative specimen) is placed between the loading head and the support roller of the bending test machine, and the test specimen is loaded at a dynamic / static rate through the hydraulic control system of the test machine. The dynamic / static loading and failure process of the specimen are monitored by a load sensor and a displacement sensor, wherein a force application point of the loading head on one end of the test specimen (the end of the unprocessed notch 11 of the specimen for evaluating the fracture toughness of the wire) is located at the center of the length, and two force application points of the support roller on the other end of the test specimen (the end of the processed notch 11 of the specimen for evaluating the fracture toughness of the wire) are symmetrically located on both sides of the center of the length;

[0046] (4) The bending test machine records data by means of load sensors and displacement sensors during dynamic / static loading and failure processes, and performs subsequent processing on the experimental data to evaluate the notched fracture toughness of the fastener wire and its failure mechanism.

[0047] In the third embodiment of the present invention, a 7075-T6 aluminum alloy wire with a diameter*length of φ8mm*50mm is used as a research object to study the notch 11 fracture toughness of the alloy wire, which specifically includes the following steps:

[0048] (1) A 4 mm thick bow-shaped specimen was cut from a φ8 mm*50 mm 7075-T6 aluminum alloy wire, and a straight notch 11 was machined at the center of the specimen. The height of the notch 11 was 2 mm, and the arc radius at the root of the notch 11 was 0.1 mm.

[0049] (2) The distance between the support rollers is set to D + 3 times the sample thickness a, that is, the diameter of the loading head is 5 mm, and the distance between the two force application points is 17 mm;

[0050] (3) The test specimen (including the test specimen and the comparative specimen) is placed between the loading head and the support roller of the bending test machine, and the test specimen is loaded at a dynamic / static rate through the hydraulic control system of the test machine. The dynamic / static loading and failure process of the specimen are monitored by a load sensor and a displacement sensor, wherein a force application point of the loading head on one end of the test specimen (the end of the unprocessed notch 11 of the specimen for evaluating the fracture toughness of the wire) is located at the center of the length, and two force application points of the support roller on the other end of the test specimen (the end of the processed notch 11 of the specimen for evaluating the fracture toughness of the wire) are symmetrically located on both sides of the center of the length;

[0051] (4) The bending test machine records data by means of load sensors and displacement sensors during dynamic / static loading and failure processes, and performs subsequent processing on the experimental data to evaluate the notched fracture toughness of the fastener wire and its failure mechanism.

[0052] In the fourth embodiment of the present invention, a 7075-T6 aluminum alloy wire with a diameter*length of φ8mm*50mm is taken as a research object to study the notch 11 fracture toughness of the alloy wire, which specifically includes the following steps:

[0053] (1) A 4 mm thick bow-shaped specimen was cut from a φ8 mm*50 mm 7075-T6 aluminum alloy wire, and a straight notch 11 was machined at the center of the specimen. The height of the notch 11 was 2 mm, and the arc radius at the root of the notch 11 was 0.5 mm.

[0054] (2) The distance between the support rollers is set to D + 3 times the sample thickness a, that is, the diameter of the loading head is 5 mm, and the distance between the two force application points is 17 mm;

[0055] (3) The test specimen (including the test specimen and the comparative specimen) is placed between the loading head and the support roller of the bending test machine, and the test specimen is loaded at a dynamic / static rate through the hydraulic control system of the test machine. The dynamic / static loading and failure process of the specimen are monitored by a load sensor and a displacement sensor, wherein a force application point of the loading head on one end of the test specimen (the end of the unprocessed notch 11 of the specimen for evaluating the fracture toughness of the wire) is located at the center of the length, and two force application points of the support roller on the other end of the test specimen (the end of the processed notch 11 of the specimen for evaluating the fracture toughness of the wire) are symmetrically located on both sides of the center of the length;

[0056] (4) The bending test machine records data by means of load sensors and displacement sensors during dynamic / static loading and failure processes, and performs subsequent processing on the experimental data to evaluate the notched fracture toughness of the fastener wire and its failure mechanism.

[0057] In the fifth embodiment of the present invention, a 7075-T6 aluminum alloy wire with a diameter*length of φ8mm*50mm is used as a research object to study the notch 11 fracture toughness of the alloy wire, which specifically includes the following steps:

[0058] (1) A 4 mm thick bow-shaped specimen was cut from a φ8 mm*50 mm 7075-T6 aluminum alloy wire, and a straight notch 11 was machined at the center of the specimen. The height of the notch 11 was 0.5 mm, and the arc radius at the root of the notch 11 was 0.1 mm.

[0059] (2) The distance between the support rollers is set to D + 3 times the sample thickness a, that is, the diameter of the loading head is 2 mm, and the distance between the two force application points is 14 mm;

[0060] (3) The test specimen (including the test specimen and the comparative specimen) is placed between the loading head and the support roller of the bending test machine, and the test specimen is loaded at a dynamic / static rate through the hydraulic control system of the test machine. The dynamic / static loading and failure process of the specimen are monitored by a load sensor and a displacement sensor, wherein a force application point of the loading head on one end of the test specimen (the end of the unprocessed notch 11 of the specimen for evaluating the fracture toughness of the wire) is located at the center of the length, and two force application points of the support roller on the other end of the test specimen (the end of the processed notch 11 of the specimen for evaluating the fracture toughness of the wire) are symmetrically located on both sides of the center of the length;

[0061] (4) The bending test machine records data by means of load sensors and displacement sensors during dynamic / static loading and failure processes, and performs subsequent processing on the experimental data to evaluate the notched fracture toughness of the fastener wire and its failure mechanism.

[0062] In the sixth embodiment of the present invention, a 7075-T6 aluminum alloy wire with a diameter*length of φ8mm*50mm is used as a research object to study the notch 11 fracture toughness of the alloy wire, which specifically includes the following steps:

[0063] (1) A 4 mm thick bow-shaped specimen was cut from a φ8 mm*50 mm 7075-T6 aluminum alloy wire, and a triangular notch 11 was machined at the center of the specimen. The height of the notch 11 was 2 mm, and the arc radius at the root of the notch 11 was 0.5 mm.

[0064] (2) The distance between the support rollers is set to D + 3 times the sample thickness a, that is, the diameter of the loading head is 5 mm, and the distance between the two force application points is 17 mm;

[0065] (3) The test specimen (including the test specimen and the comparative specimen) is placed between the loading head and the support roller of the bending test machine, and the test specimen is loaded at a dynamic / static rate through the hydraulic control system of the test machine. The dynamic / static loading and failure process of the specimen are monitored by a load sensor and a displacement sensor, wherein a force application point of the loading head on one end of the test specimen (the end of the unprocessed notch 11 of the specimen for evaluating the fracture toughness of the wire) is located at the center of the length, and two force application points of the support roller on the other end of the test specimen (the end of the processed notch 11 of the specimen for evaluating the fracture toughness of the wire) are symmetrically located on both sides of the center of the length;

[0066] (4) The bending test machine records data by means of load sensors and displacement sensors during dynamic / static loading and failure processes, and performs subsequent processing on the experimental data to evaluate the notched fracture toughness of the fastener wire and its failure mechanism.

[0067] In the seventh embodiment of the present invention, a regular hexagonal 7075-T6 aluminum alloy wire with a size of S8mm*50mm is used as a research object to study the notch 11 fracture toughness of the alloy wire, which specifically includes the following steps:

[0068] (1) A trapezoidal specimen with a thickness of 4 mm was cut from a 7075-T6 aluminum alloy wire with a specification of S8 mm*50 mm, and a straight notch 11 was processed at the center of the specimen. The length of the notch 11 was 0.5 mm, and the arc radius at the root of the notch 11 was 0.1 mm;

[0069] (2) The distance between the support rollers is set to D + 3 times the sample thickness a, that is, the diameter of the loading head is 5 mm, and the distance between the two force application points is 17 mm;

[0070] (3) The test specimen (including the test specimen and the comparative specimen) is placed between the loading head and the support roller of the bending test machine, and the test specimen is loaded at a dynamic / static rate through the hydraulic control system of the test machine. The dynamic / static loading and failure process of the specimen are monitored by a load sensor and a displacement sensor, wherein a force application point of the loading head on one end of the test specimen (the end of the unprocessed notch 11 of the specimen for evaluating the fracture toughness of the wire) is located at the center of the length, and two force application points of the support roller on the other end of the test specimen (the end of the processed notch 11 of the specimen for evaluating the fracture toughness of the wire) are symmetrically located on both sides of the center of the length;

[0071] (4) The bending test machine records data by means of load sensors and displacement sensors during dynamic / static loading and failure processes, and performs subsequent processing on the experimental data to evaluate the notched fracture toughness of the fastener wire and its failure mechanism.

[0072] In the eighth embodiment of the present invention, a 7075-T6 aluminum alloy wire with a diameter*length of φ20mm*50mm is used as a research object to study the notch 11 fracture toughness of the alloy wire, which specifically includes the following steps:

[0073] (1) A 5 mm thick bow-shaped specimen was cut from a φ20 mm*50 mm 7075-T6 aluminum alloy wire, and a straight notch 11 was machined at the center of the specimen. The height of the notch 11 was 1 mm, and the arc radius at the root of the notch 11 was 0.1 mm.

[0074] (2) The distance between the support rollers is set to D + 3 times the sample thickness a, that is, the diameter of the loading head is 5 mm, and the distance between the two force application points is 20 mm;

[0075] (3) The test specimen (including the test specimen and the comparative specimen) is placed between the loading head and the support roller of the bending test machine, and the test specimen is loaded at a dynamic / static rate through the hydraulic control system of the test machine. The dynamic / static loading and failure process of the specimen are monitored by a load sensor and a displacement sensor, wherein a force application point of the loading head on one end of the test specimen (the end of the unprocessed notch 11 of the specimen for evaluating the fracture toughness of the wire) is located at the center of the length, and two force application points of the support roller on the other end of the test specimen (the end of the processed notch 11 of the specimen for evaluating the fracture toughness of the wire) are symmetrically located on both sides of the center of the length;

[0076] (4) The bending test machine records data by means of load sensors and displacement sensors during dynamic / static loading and failure processes, and performs subsequent processing on the experimental data to evaluate the notched fracture toughness of the fastener wire and its failure mechanism.

[0077] In the ninth embodiment of the present invention, a 7075-T6 aluminum alloy wire with a diameter*length of φ4mm*50mm is taken as a research object to study the notch 11 fracture toughness of the alloy wire, which specifically includes the following steps:

[0078] (1) A 2 mm thick bow-shaped specimen was cut from a φ4 mm*50 mm 7075-T6 aluminum alloy wire, and a straight notch 11 was machined at the center of the specimen. The height of the notch 11 was 0.5 mm, and the arc radius at the root of the notch 11 was 0.1 mm.

[0079] (2) The distance between the support rollers is set to D + 3 times the sample thickness a, that is, the diameter of the loading head is 5 mm, and the distance between the two force application points is 11 mm;

[0080] (3) The test specimen (including the test specimen and the comparative specimen) is placed between the loading head and the support roller of the bending test machine, and the test specimen is loaded at a dynamic / static rate through the hydraulic control system of the test machine. The dynamic / static loading and failure process of the specimen are monitored by a load sensor and a displacement sensor, wherein a force application point of the loading head on one end of the test specimen (the end of the unprocessed notch 11 of the specimen for evaluating the fracture toughness of the wire) is located at the center of the length, and two force application points of the support roller on the other end of the test specimen (the end of the processed notch 11 of the specimen for evaluating the fracture toughness of the wire) are symmetrically located on both sides of the center of the length;

[0081] (4) The bending test machine records data by means of load sensors and displacement sensors during dynamic / static loading and failure processes, and performs subsequent processing on the experimental data to evaluate the notched fracture toughness of the fastener wire and its failure mechanism.

[0082] In the tenth embodiment of the present invention, a 2024-T3 aluminum alloy wire with a diameter*length of φ8mm*50mm is used as a research object to study the notch 11 fracture toughness of the alloy wire, which specifically includes the following steps:

[0083] (1) A 4 mm thick bow-shaped specimen was cut from a φ8 mm*50 mm 2024-T3 aluminum alloy wire, and a straight notch 11 was machined at the center of the specimen. The height of the notch 11 was 0.5 mm, and the arc radius at the root of the notch 11 was 0.1 mm.

[0084] (2) The distance between the support rollers is set to D + 3 times the sample thickness a, that is, the diameter of the loading head is 5 mm, and the distance between the two force application points is 17 mm;

[0085] (3) The test specimen (including the test specimen and the comparative specimen) is placed between the loading head and the support roller of the bending test machine, and the test specimen is loaded at a dynamic / static rate through the hydraulic control system of the test machine. The dynamic / static loading and failure process of the specimen are monitored by a load sensor and a displacement sensor, wherein a force application point of the loading head on one end of the test specimen (the end of the unprocessed notch 11 of the specimen for evaluating the fracture toughness of the wire) is located at the center of the length, and two force application points of the support roller on the other end of the test specimen (the end of the processed notch 11 of the specimen for evaluating the fracture toughness of the wire) are symmetrically located on both sides of the center of the length;

[0086] (4) The bending test machine records data by means of load sensors and displacement sensors during dynamic / static loading and failure processes, and performs subsequent processing on the experimental data to evaluate the notched fracture toughness of the fastener wire and its failure mechanism.

[0087] In the eleventh embodiment of the present invention, a TC4 titanium alloy wire with a diameter*length of φ8mm*50mm is taken as a research object to study the notch 11 fracture toughness of the alloy wire, which specifically includes the following steps:

[0088] (1) A 4 mm thick bow-shaped specimen was cut from a φ8 mm*50 mm TC4 titanium alloy wire, and a straight notch 11 was machined at the center of the specimen. The height of the notch 11 was 0.5 mm, and the arc radius at the root of the notch 11 was 0.1 mm.

[0089] (2) The distance between the support rollers is set to D + 3 times the sample thickness a, that is, the diameter of the loading head is 5 mm, and the distance between the two force application points is 17 mm;

[0090] (3) The test specimen (including the test specimen and the comparative specimen) is placed between the loading head and the support roller of the bending test machine, and the test specimen is loaded at a dynamic / static rate through the hydraulic control system of the test machine. The dynamic / static loading and failure process of the specimen are monitored by a load sensor and a displacement sensor, wherein a force application point of the loading head on one end of the test specimen (the end of the unprocessed notch 11 of the specimen for evaluating the fracture toughness of the wire) is located at the center of the length, and two force application points of the support roller on the other end of the test specimen (the end of the processed notch 11 of the specimen for evaluating the fracture toughness of the wire) are symmetrically located on both sides of the center of the length;

[0091] (4) The bending test machine records data by means of load sensors and displacement sensors during dynamic / static loading and failure processes, and performs subsequent processing on the experimental data to evaluate the notched fracture toughness of the fastener wire and its failure mechanism.

[0092] In the twelfth embodiment of the present invention, a GH4169 high temperature alloy wire with a diameter*length of φ8mm*50mm is taken as a research object to study the notch 11 fracture toughness of the alloy wire, which specifically includes the following steps:

[0093] (1) A 4 mm thick bow-shaped specimen was cut from a φ8 mm*50 mm GH4169 high-temperature alloy wire, and a straight notch 11 was machined at the center of the specimen. The height of the notch 11 was 0.5 mm, and the arc radius at the root of the notch 11 was 0.1 mm.

[0094] (2) The distance between the support rollers is set to D + 3 times the sample thickness a, that is, the diameter of the loading head is 5 mm, and the distance between the two force application points is 17 mm;

[0095] (3) The test specimen (including the test specimen and the comparative specimen) is placed between the loading head and the support roller of the bending test machine, and the test specimen is loaded at a dynamic / static rate through the hydraulic control system of the test machine. The dynamic / static loading and failure process of the specimen are monitored by a load sensor and a displacement sensor, wherein a force application point of the loading head on one end of the test specimen (the end of the unprocessed notch 11 of the specimen for evaluating the fracture toughness of the wire) is located at the center of the length, and two force application points of the support roller on the other end of the test specimen (the end of the processed notch 11 of the specimen for evaluating the fracture toughness of the wire) are symmetrically located on both sides of the center of the length;

[0096] (4) The bending test machine records data by means of load sensors and displacement sensors during dynamic / static loading and failure processes, and performs subsequent processing on the experimental data to evaluate the notched fracture toughness of the fastener wire and its failure mechanism.

[0097] The test specimens of Examples 1 to 12 failed during the loading process.

[0098] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may be subject to various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

[0099] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0100] Unless otherwise specifically stated, the relative arrangement, numerical expressions and numerical values ​​of the parts and steps set forth in these embodiments do not limit the scope of the utility model. At the same time, it should be understood that, for ease of description, the sizes of the various parts shown in the accompanying drawings are not drawn according to the actual proportional relationship. The technology, method and equipment known to those of ordinary skill in the relevant art may not be discussed in detail, but in appropriate cases, the technology, method and equipment should be considered as a part of the specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values. It should be noted that similar reference numerals and letters represent similar items in the following drawings, and therefore, once a certain item is defined in an accompanying drawing, it does not need to be further discussed in subsequent drawings.

[0101] In the description of the present utility model, it needs to be understood that the directions or positional relationships indicated by directional words such as "front, back, up, down, left, right", "lateral, vertical, perpendicular, horizontal" and "top, bottom" are usually based on the directions or positional relationships shown in the drawings, and are only for the convenience of describing the present utility model and simplifying the description. Unless otherwise specified, these directional words do not indicate or imply that the device or element referred to must have a specific direction or be constructed and operated in a specific direction, and therefore cannot be understood as limiting the scope of protection of the present utility model; the directional words "inside and outside" refer to the inside and outside relative to the contours of each component itself.

[0102] For ease of description, spatially relative terms such as "above", "above", "on the upper surface of", "above", etc. may be used here to describe the spatial positional relationship between a device or feature and other devices or features as shown in the figure. It should be understood that spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientation described in the figure. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Thus, the exemplary term "above" can include both "above" and "below". The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatially relative descriptions used here are interpreted accordingly.

[0103] In addition, it should be noted that the use of terms such as "first" and "second" to limit components is only for the convenience of distinguishing the corresponding components. If not otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of the utility model.

Claims

1. A test specimen for evaluating the fracture toughness of a wire rod, characterized in that: include: The main body (10) is a long metal sheet cut from a wire rod. The main body (10) is provided with a notch (11) along the thickness direction of the main body (10), and the notch (11) is arranged at the length center of the main body (10).

2. The test specimen for evaluating the fracture toughness of a wire rod according to claim 1, characterized in that: The cross section of the wire is polygonal or circular.

3. The test specimen for evaluating the fracture toughness of a wire rod according to claim 1, characterized in that: The depth of the notch (11) is 0.1 to 0.5 times the thickness of the main body (10).

4. The test specimen for evaluating the fracture toughness of a wire rod according to claim 1, characterized in that: The longitudinal cross section of the notch (11) in the length direction of the main body (10) is in the shape of a straight line.

5. The test specimen for evaluating the fracture toughness of a wire rod according to claim 1, characterized in that: The longitudinal cross section of the notch (11) in the length direction of the main body (10) is triangular.

6. The test specimen for evaluating the fracture toughness of a wire rod according to claim 1, characterized in that: The root of the notch (11) is in an arc shape.

7. The test specimen for evaluating the fracture toughness of a wire rod according to claim 6, characterized in that: The radius of the root of the notch (11) is 0.05-0.5 mm.

8. The test specimen for evaluating the fracture toughness of a wire rod according to claim 1, characterized in that: The thickness of the main body (10) is the radius of a cylindrical fastener, and the cylindrical fastener is processed from the wire; or the thickness of the main body (10) is the thickness of a hollow fastener, and the hollow fastener is processed from the wire.

9. The test specimen for evaluating the fracture toughness of a wire rod according to claim 1, characterized in that: The length of the main body (10) is greater than 10 mm.

10. The test specimen for evaluating the fracture toughness of a wire rod according to claim 1, characterized in that: The material of the main body (10) is aluminum alloy, titanium alloy or nickel-based high-temperature alloy.