Continuous method gas-liquid countercurrent fixed bed reactor system device
Through the continuous gas-liquid counterflow fixed bed reactor system using antimony-silver-titanium catalyst in trimethylaluminum synthesis, the problems of low selectivity and many by-products in the existing process are solved, and high efficiency and low cost are achieved Trimethylaluminum is prepared to improve production efficiency and separation convenience.
Patent Information
- Application Number
- CN202420648223.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-29
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2034-03-29
AI Technical Summary
The existing trimethylaluminum synthesis process has problems such as low selectivity, many by-products, high production costs, and high separation difficulty, especially in industrial applications.
The continuous gas-liquid countercurrent fixed bed reactor system device is used to use three metal oxides of antimony-silver-titanium as catalyst active components to carry out alkyl exchange reactions through two or more stage temperature-controlled reactors to realize trimethylaluminum efficient preparation.
It improves the selectivity and conversion rate of trimethylaluminum, reduces energy consumption, improves the operational efficiency of mass production, increases the production capacity to 96%, and simplifies the separation process.
Smart Images

Figure CN222057302U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to a continuous method gas-liquid countercurrent fixed bed reactor system device, belonging to the technical field of organic metal compound synthesis. Background Art
[0002] Trimethylaluminum (TMA) is an important organometallic compound, which is widely used in important fields such as polymer chemistry, electronic materials, photovoltaic materials, national defense science and technology, organic catalysis, and organic synthesis. In recent years, with the rapid development of metallocene catalyst systems, trimethylaluminum (TMA) is used as the starting material for the cocatalysts in the synthesis of metallocene catalyst systems, such as methylaluminoxane (MAO) and modified methylaluminoxane (MMAO). It plays an increasingly important role in the polymer chemical industry, especially in catalytic materials. At the same time, trimethylaluminum is also an extremely dangerous organometallic compound. It will burn violently when it comes into contact with air and will undergo violent chemical reactions when it comes into contact with water. There are very high requirements for its production, transfer, storage, and transportation.
[0003] 1. Application of TMA
[0004] 1. Application of TMA in the emerging organic polymer industry
[0005] TMA is the core raw material for producing metallocene catalyst cocatalysts - MAO and MMAO. Since the 1990s, metallocene catalysts have developed rapidly in the organic polymer industry. Compared with traditional Ziegler-Natta catalysts, the polymers formed under the action of metallocene catalyst systems have many excellent properties such as narrow molecular weight distribution, high stereoregularity, good optical transparency, good radiation resistance, low signal / noise ratio, high strength, high melting point, chemical resistance, water resistance, and steam resistance. The catalyst system is composed of an organic metal complex formed by transition metal zirconium (Zr) (or titanium or hafnium) and two cyclopentadienyl or cyclopentadiene substituents and two chlorine atoms (or methyl, etc.) and a cocatalyst methylaluminoxane (MAO, Methylaluminoxane) or modified methylaluminoxane (MMAO). In the next 5-10 years, metallocene catalysts will be more widely used in polyethylene, polypropylene, POE, PAO, COC, high-end a-olefins and other fields.
[0006] 2. Application of TMA in the electronic information industry
[0007] Ultra-high purity TMA is used as a MO source in the semiconductor industry, which is the basis for manufacturing nanochips and developing the electronic information industry. Ultra-high purity is defined in the industry as: containing impurities of 100ppm-100ppb, that is, purity 4-9N (nines). TMA is an important source of organic metals in aluminum-containing semiconductors (such as AlAs, AlN, AlP, AlSb, AlGaAs, AlInGaAs, AlInGaP, AlGaN, AlInGaN, AlInGaNP, etc.). TMA is a precursor for the manufacture of TMGa (trimethylgallium) and TMIn (trimethylindium), etc. Trimethylaluminum (CH3)3Al and gallium trichloride GaCl3 undergo a methyl group exchange reaction to obtain trimethylgallium ((CH3)3Ga). TMA is used as an Al (aluminum) source high dielectric constant dielectric film in LED and OLED manufacturing. For example, TMA is used with oxygen or ammonia to obtain Al2O3 or AlN (aluminum nitride) as a buffer layer for silicon wafer substrates, which has important applications in related products.
[0008] 3. Application of TMA in the photovoltaic industry
[0009] Rear passivation of crystalline silicon solar cells is seen as a key technology being deployed by PV manufacturers to improve cell efficiency and PERC and MWT technologies. A specific solar grade trimethylaluminum produced from aluminum oxide as raw material for rear passivation of crystalline silicon solar cells can reduce the cost of photovoltaic cells and significantly improve photovoltaic efficiency.
[0010] 4. Application of TMA in organic synthesis
[0011] Trimethylaluminum can react with ethylene to form high-carbon alkyl aluminum, which, after oxidation and hydrolysis, forms straight-chain higher primary alcohols and higher α-olefins. Among metal organic compounds, organic aluminum is not only cheap but also highly reactive, so it is often used to prepare other metal organic compounds. For example, methyl tin can be prepared by reacting trimethylaluminum with tin chloride. If methyl tin chloride is to be obtained, trimethylaluminum can also be used as a raw material. As long as an excess of tin chloride is added, methyl tin monochloride and dichloride can be obtained. In the synthesis reaction of organic compounds, trimethylaluminum can be used as a reaction reagent with high stereoselectivity. In addition, trimethylaluminum can also be used as a mild reducing agent for the synthesis of drugs such as vitamins and hormones.
[0012] 4. Brief Introduction to the Synthesis Process of Trimethylaluminum
[0013] There are many methods for synthesizing trimethylaluminum, which are reported in the literature: sodium reduction method, aluminum reduction method, magnesium-aluminum alloy reduction method, Grignard reagent method, ultrasonic radiation method, alkyl exchange method, etc. However, these methods all have their own shortcomings. Among them, the more industrially valuable ones are the sodium reduction method and the alkyl exchange method under the catalysis of bismuth-based catalysts.
[0014] 1. Sodium reduction method
[0015] Aluminum with a purity of more than 95% is made into shavings, particles or powders, and reacted with methyl halide under strict anhydrous and oxygen-free conditions, and a small amount of iodine or methylaluminum chloride is added as an initiator of the reaction. After the reaction is completed, an equimolar equilibrium mixture of monomethylaluminum halide, dimethylaluminum halide and their dimers is generated. The process is expressed as follows:
[0016] 3CH3X+2Al—→(CH3)3Al2X3(CH3)2AlX+CH3AlX2
[0017] This mixture composed of (CH3)3Al2X3 or CH3AlX2·(CH3)2AlX is called methyl sesquihalide (semihalide for short).
[0018] Methyl sesquihalide is further treated with metallic sodium to generate trimethylaluminum. Sodium metal with 10% excess over theoretical amount is placed in an organic solvent and a small amount of stearic acid is added. Sodium sand is prepared by high-speed stirring at 90-100°C. Methyl sesquihalide is dropped into the suspension under stirring. After the reaction is completed, the product is evaporated and the residue is disposed outdoors.
[0019] 3(CH3)2AlCl+3Na→3NaCl+Al+2Al(CH3)3
[0020] 3CH3AlCl2+6Na→6NaCl+2Al+Al(CH3)3
[0021] This method was once used as a classic method for producing trimethylaluminum. However, the dehalogenation coupling reaction between two molecules of methyl chloride and aluminum often produces ethane, and the byproduct sodium tetramethylaluminide is produced during the reaction, which reduces the selectivity of the reaction. In addition, since aluminum participates in the reaction as a reactant, and aluminum is produced when the intermediate product is treated with sodium, the reaction is difficult to proceed. At the same time, the aluminum precipitates on the surface of sodium, which further reduces the reaction rate, thereby greatly reducing the conversion rate of the reaction.
[0022] 2. Aluminum reduction method
[0023] Trimethylaluminum can be prepared by direct reduction of methylmercury with aluminum:
[0024] 2Al+3(CH3)2Hg→2(CH3)3Al+3Hg
[0025] This method produces a high yield of trimethylaluminum, but the reaction has no practical value due to the instability and high toxicity of alkylmercury. In addition, the generation of mercury makes the product difficult to handle.
[0026] Trimethylaluminum can also be prepared by aluminum reduction of methyl halides (mainly methyl iodide):
[0027] 3CH3I+Al→(CH3)3Al+3I
[0028] The reaction temperature of this method is between 69° C. and 72° C., and the theoretical conversion rate is 50% to 65%. However, the long reaction time (more than 20 hours) and the high price of iodomethane limit the practicability of the reaction.
[0029] 3. Magnesium-aluminum alloy reduction method
[0030] Trimethylaluminum can also be prepared by reacting magnesium-aluminum alloy with alkyl halides:
[0031] Al2Mg3+6CH3Cl→2(CH3)3Al+3MgCl2
[0032] The main problems with this method are: low aluminum conversion rate, complicated recovery process of by-product MgCl2, nearly two tons of residue for every ton of trimethylaluminum produced, the residue is doped with metallic magnesium and aluminum, magnesium oxide and aluminum oxide, as well as magnesium hydroxide and aluminum hydroxide in addition to MgCl2, and is generally not recovered but discarded as waste.
[0033] 4. Green's reagent method
[0034] This method uses ether as solvent and produces trimethylaluminum by reacting Grignard's reagent with aluminum halide or metallic aluminum:
[0035] 3CH3MgX+AlX3→(CH3)3Al+3MgX2
[0036] Or 6CH3MgI+2Al→2(CH3)3Al+3MgI2
[0037] Since this method uses ether as solvent, the trimethylaluminum generated is difficult to evaporate from the reaction solution after etherification, so it is not practical.
[0038] 5. Ultrasonic radiation method
[0039] Ultrasonic radiation has a promoting effect on organic synthesis, especially multiphase reactions. However, it was not until the mid-1980s that ultrasonic radiation was used for the synthesis of metal organics. This is a method for preparing trimethylaluminum by ultrasonic radiation. Methyl iodide and aluminum powder react at room temperature under an iodine atmosphere to generate methylaluminum sesquiiodine, which then reacts with triethylaluminum to generate trimethylaluminum. The first step reaction time is 2 hours, the second step reaction time is 0.5 hours, the reaction yield is 86%, and the purity of the product trimethylaluminum is 98%.
[0040] This method has a short reaction cycle and a high reaction yield, but because it requires two steps of reaction, the process flow is complicated and the separation is cumbersome, so it is still in the laboratory research stage.
[0041] 6. Alkyl exchange reaction
[0042] Alkyl exchange reactions using bismuth-based compounds as catalysts:
[0043] 3CH3X+R3Al→(CH3)3Al+3RX
[0044] Where R=C2H5-C4H9
[0045] X=Br、Cl
[0046] The catalyst is generally a bismuth-containing compound. Alkyl bismuth, aryl bismuth, inorganic bismuth salts and any bismuth-containing compound that can be converted into alkyl or aryl bismuth can form the catalyst active component.
[0047] In the early 1980s, US Pat. No. 4,364,872 disclosed a relatively economical method for preparing trimethylaluminum, namely, the alkyl exchange method, in which the reactants trialkylaluminum, methyl halide and a bismuth compound as a catalyst are put into a closed autoclave to react and generate trimethylaluminum. The main problem with this method is that the bismuth compound is very expensive. Although the laboratory yield has been improved, it is still difficult to industrialize it. The reason is that the reaction is completed in a closed autoclave. As the reaction proceeds, the ratio of halogenated hydrocarbon to trialkylaluminum in the reaction system gradually increases, and halogenated hydrocarbon and trialkylaluminum can react to generate various halogenated alkylaluminums, which increases the difficulty of separation and purification, and the violent reaction of trialkylaluminum and halogenated hydrocarbon has the risk of explosion.
[0048] In view of the above defects, US4925962 proposed an improved process, that is, while controlling the feed amount of methyl halide, halogenated hydrocarbons are evaporated from the reactor, thereby controlling the amount of the two compounds in the reactor and avoiding explosion. However, the process still uses bismuth compounds as catalysts, the production cost remains high, and the product yield is not very ideal.
[0049] ZL98106736.0 proposed a method for preparing TMA using a relatively cheap catalytic system, an iron-antimony based catalyst. Although the yield was significantly improved (the yield reached 92%), due to the inherent defects of the kettle stirring reaction, various by-products still existed and were difficult to separate. Utility Model Content
[0050] The technical problem to be solved by the utility model is to provide a new synthesis process of trimethylaluminum and a catalyst matched therewith.
[0051] In order to solve the above problems, the utility model provides a continuous gas-liquid countercurrent fixed bed reactor system device, which includes a fixed bed reactor, a liquid phase nozzle is provided on the top of the fixed bed reactor, a gas phase nozzle is provided on the bottom, the fixed bed reactor is axially divided into multiple sections and the reaction temperature is controlled in sections by a temperature control system, and the top of the fixed bed reactor is connected to a separation unit.
[0052] Preferably, the separation unit comprises a lightness removal tower and a separation tower and a heavyness removal tower respectively connected to the top and bottom of the lightness removal tower.
[0053] Preferably, the top of the fixed bed reactor is connected to the middle of the lightness removal tower, the top of the lightness removal tower is connected to the middle of the separation tower, the bottom of the separation tower is connected to the third storage tank, and the gas phase nozzle is connected to the first storage tank and the top of the separation tower; the bottom of the lightness removal tower is connected to the middle of the weight removal tower, the top of the weight removal tower is connected to the fourth storage tank, and the liquid phase nozzle is connected to the second storage tank and the bottom of the weight removal tower.
[0054] When in use, the first storage tank is filled with alkyl halide, the second storage tank is filled with alkyl aluminum, and the fixed bed reactor is filled with honeycomb filler containing catalyst active components; liquid alkyl aluminum with a higher boiling point flows uniformly from the top of the fixed bed reactor to the bottom through the liquid phase nozzle through the multi-stage temperature control zone of the fixed bed reactor, and reaches the bottom of the fixed bed reactor to participate in azeotropic and reaction; alkyl halide with a lower boiling point enters the fixed bed reactor from the gas phase nozzle, most of the alkyl halide participates in the alkyl exchange reaction in the lower section of the fixed bed reactor, and a small part flows upstream, and after a partial alkyl exchange reaction occurs with the descending high-boiling-point alkyl aluminum, it escapes from the top of the fixed bed reactor together with the trimethyl aluminum obtained by the reaction and the alkyl halide with a higher boiling point produced by the reaction, and enters the separation unit for separation and recovery.
[0055] Preferably, the fixed bed reactor is divided into two sections, the upper section is a low-temperature section, and the lower section is a high-temperature section.
[0056] More preferably, the temperature of the high temperature section is 140-210°C, the temperature of the low temperature section is 90-140°C; the space velocity of the halogenated alkane in the fixed bed reactor is 1-100 / h. The temperature of the high temperature section is 160-190°C, preferably 170-180°C; the temperature of the low temperature section is 100-130°C, preferably 125-128°C; the space velocity of the halogenated alkane in the fixed bed reactor is 10-50 / h, preferably 20-30 / h.
[0057] Preferably, the honeycomb filler is made by grinding the active components of the catalyst, kneading them with porous materials in water, shaping them, and calcining them.
[0058] More preferably, the active components of the catalyst include antimony trioxide, silver oxide, and titanium dioxide.
[0059] Furthermore, the mass ratio of antimony trioxide, silver oxide, titanium dioxide and porous material is (0.5-30):(0.1-10):(1-50):(1-95), preferably (2-10):(0.5-2):(2-5):(10-90).
[0060] Preferably, the alkyl group of the alkyl aluminum is any alkyl group with a carbon number of not less than 2; the alkyl aluminum is at least one of fluoromethane, chloromethane, bromomethane and iodomethane.
[0061] Specifically, the utility model provides a catalyst and process for preparing trimethylaluminum in a continuous gas-liquid countercurrent fixed bed reactor, and more particularly relates to a process for preparing trimethylaluminum by a countercurrent reaction of methyl bromide and triethylaluminum in a fixed bed reactor composed of a honeycomb catalyst containing three metal oxides of antimony, silver and titanium, with gaseous methyl bromide reacting from bottom to top and liquid triethylaluminum reacting from top to bottom.
[0062] Firstly, the honeycomb catalyst with antimony, silver and titanium three metal oxides as the active components of the catalyst greatly improves the selectivity of the target product; secondly, the temperature control mode of the two-stage or multi-stage fixed bed reactor enables the reaction products to be separated from the high-boiling point raw materials and intermediates in the low-temperature section of the fixed bed reactor, and escape from the reactor in time, reducing the probability of the alkyl exchange reaction to proceed in reverse, thereby effectively improving the single-pass conversion rate of the reaction.
[0063] The combined effect of increased product selectivity and main raw material conversion rate has increased the reaction yield of trimethylaluminum prepared by alkyl exchange reaction to 96% compared with the value reported in the literature (92%, intermittent kettle catalyst slurry reaction), thereby increasing the reaction capacity, reducing the reaction energy consumption, and providing good operational efficiency for mass production of trimethylaluminum.
[0064] The detailed process and catalyst preparation method are briefly described as follows:
[0065] Preparation of catalyst components: After fully grinding, three metal oxides (antimony trioxide, silver oxide, titanium dioxide) and porous materials (such as 4A molecular sieve) are kneaded, shaped, and calcined with the porous materials (such as 4A molecular sieve) in a proper amount of water in the following ratio range (0.5-30): (0.1-10): (1-50): (1-95) to form a honeycomb catalyst component that meets the requirements of filling a fixed bed reactor;
[0066] The preparation process of trimethylaluminum is as follows: the catalyst assembly prepared by the above method is placed in a fixed bed reactor with a two-stage or multi-stage temperature control system to form a catalytic system. The high-boiling point liquid phase alkyl aluminum flows uniformly from the top of the fixed bed reactor through a rotatable nozzle, through the two or more temperature control zones of the reactor, and reaches the bottom of the fixed bed reactor (high temperature section, the temperature of the high temperature section of the fixed bed reactor is: 140-210°C) to participate in azeotropic and reaction; the low-boiling point methyl halide enters the high temperature section of the reactor from the bottom of the fixed bed reactor through a gas phase nozzle, and most of the methyl halide participates in the alkyl exchange reaction in the high temperature section, and a small part of it flows upstream, and after a partial alkyl exchange reaction with the descending high-boiling point alkyl aluminum, it quickly escapes from the top of the fixed bed reactor (the temperature of the low temperature section is: 90-140°C) together with the trimethyl aluminum obtained by the reaction and the high-boiling point halogenated alkanes produced by the reaction, and enters the separation unit of the process flow. The space velocity of the halogenated alkanes in the fixed bed reactor is controlled to be: 1-100 / h. The alkyl group of the trialkylaluminum participating in the reaction may be any alkyl group with a carbon number of not less than 2, and the methyl halide participating in the reaction may be methyl fluoride, methyl chloride, methyl bromide, or methyl iodide;
[0067] Product separation process: As shown in the attached drawings of this patent, the gaseous material escaping from the top of the reactor is cooled by the heat exchanger and enters the light-removing tower. In the light-removing tower, the halogenated hydrocarbons are separated from all other components. The gaseous component (mixed halogenated hydrocarbons) escapes from the top of the light-removing tower and enters the separation tower. In the separation tower, the methyl halide is separated from other halogenated alkanes. The halogenated hydrocarbons escape from the top of the separation tower and are sent back to the reactor inlet to continue to participate in the reaction. The high-boiling halogenated alkanes are discharged from the bottom of the separation tower and enter the by-product tank; the liquid-phase material discharged from the bottom of the light-removing tower is sent to the de-weighting tower. In the de-weighting tower, the product escapes from the top of the tower, enters the product tank after condensation, and other high-boiling-point components are discharged from the bottom of the de-weighting tower and are sent back to the alkyl aluminum feeding system to participate in the reaction again.
[0068] In summary, the utility model uses a honeycomb catalyst assembly made of three metal oxides of antimony, silver and titanium as active components, and allows alkyl aluminum with not less than two carbon atoms and alkyl halide to undergo continuous countercurrent reaction in a two-stage or multi-stage temperature-controlled fixed bed reactor. The catalyst dosage is small, the selectivity of the target product is good, the conversion rate of the main raw materials is high, and the yield of the product can reach 96% relative to the dosage of the alkyl aluminum. The utility model is an ideal method for batch preparation of alkyl aluminum, especially trimethyl aluminum. BRIEF DESCRIPTION OF THE DRAWINGS
[0069] Figure 1 This is a schematic diagram of a continuous gas-liquid countercurrent fixed bed reactor system device provided by the utility model. DETAILED DESCRIPTION
[0070] In order to make the present invention more clearly understood, a preferred embodiment is described in detail below with reference to the accompanying drawings. Figure 1 As shown, a continuous gas-liquid countercurrent fixed bed reactor system device provided by the utility model includes a fixed bed reactor R1, a liquid phase nozzle N2 is provided on the top of the fixed bed reactor R1, and a gas phase nozzle N1 is provided on the bottom. The fixed bed reactor R1 is axially divided into multiple sections, and the reaction temperature is controlled in sections by a temperature control system. The top of the fixed bed reactor R1 is connected to the separation unit.
[0071] The separation unit includes a light-removing tower T1 and a separation tower T3 and a de-weighting tower T2 which are respectively connected to the top and bottom of the light-removing tower T1. The top of the fixed bed reactor R1 is connected to the middle of the light-removing tower T1, the top of the light-removing tower T1 is connected to the middle of the separation tower T3, the bottom of the separation tower T3 is connected to the third storage tank V3, the gas phase nozzle N1 is connected to the first storage tank V1 and the top of the separation tower T3; the bottom of the light-removing tower T1 is connected to the middle of the de-weighting tower T2, the top of the de-weighting tower T2 is connected to the fourth storage tank V4, and the liquid phase nozzle N2 is connected to the second storage tank V2 and the bottom of the de-weighting tower T2.
[0072] A preparation method for a catalyst for preparing trimethylaluminum, specifically comprising: a first storage tank V1 is filled with a halogenated alkane, a second storage tank V2 is filled with an alkyl aluminum, and a fixed bed reactor R1 is filled with a honeycomb filler containing a catalyst active component; a liquid phase alkyl aluminum with a higher boiling point flows uniformly from the top of the fixed bed reactor R1 through a liquid phase nozzle N2 from top to bottom through the multi-stage temperature control zone of the fixed bed reactor R1, and reaches the bottom of the fixed bed reactor R1 to participate in azeotropic and reaction; a halogenated alkane with a lower boiling point enters the fixed bed reactor R1 from a gas phase nozzle N1, most of the halogenated alkane participates in an alkyl exchange reaction in the lower section of the fixed bed reactor R1, and a small part flows upstream, undergoes a partial alkyl exchange reaction with the descending high-boiling-point alkyl aluminum, and then escapes from the top of the fixed bed reactor R1 together with the trimethyl aluminum obtained by the reaction and the halogenated alkane with a higher boiling point produced by the reaction, and enters a separation unit for separation and recovery (the product in the third storage tank V3 is a halogenated alkane, and the product in the fourth storage tank V4 is an alkyl aluminum).
[0073] The fixed bed reactor R1 is divided into two sections, the upper section is a low temperature section, and the lower section is a high temperature section. The temperature of the high temperature section is 140-210°C, and the temperature of the low temperature section is 90-140°C; the space velocity of the halogenated alkane in the fixed bed reactor R1 is 1-100 / h (technical personnel in the field can adjust it according to actual conditions).
[0074] The honeycomb filler is made by grinding the active components of the catalyst, kneading them with porous materials in water, shaping them, and calcining them. The active components of the catalyst include antimony trioxide, silver oxide, and titanium dioxide. The mass ratio of antimony trioxide, silver oxide, titanium dioxide, and porous materials is (0.5-30): (0.1-10): (1-50): (1-95).
[0075] The alkyl group of the alkyl aluminum is any alkyl group with a carbon number of not less than 2; the alkyl aluminum is at least one of fluoromethane, chloromethane, bromomethane and iodomethane.
[0076] Example 1
[0077] Preparation of catalyst: Weigh 150 g of chemically pure antimony trioxide, 50 g of chemically pure silver oxide, 750 g of chemically pure titanium dioxide and 9050 g of 4A molecular sieve crushed by a pulverizer, put these four materials into a ball mill with a capacity of 15 L, and continue ball milling for 5 hours under medium frequency vibration. Pour the obtained powdered solid mixture from the ball mill and put it into a kneading machine with a capacity of 10 L. Add 1800 mL of deionized water to the kneading machine, turn on the kneading machine, and fully mix the powdered material with the deionized water to form a semi-solid paste without fluidity. All of these semi-solid pastes are put into a cylindrical cross-sectional inner diameter of 80 mm and a height of 400 mm. 16 metal round rods with a diameter of 10 mm are evenly distributed at the bottom of the cylinder (referred to as a honeycomb catalyst). The catalyst forming mold is made of a pore-forming rod, and the outer shell of the catalyst forming mold is gently tapped with a rubber hammer so that the semi-solid paste can be evenly distributed to all corners of the catalyst forming mold. After standing for 60 minutes, the shaped catalyst is gently poured out from the upper mouth of the forming mold. According to the size of the fixed bed reactor, this cylindrical catalyst with uniform pore distribution can be cut into several sections (for easy installation inside the fixed bed reactor). Finally, the cut cylindrical honeycomb catalyst is placed in a roasting furnace, which is replaced with high-purity nitrogen. The temperature of the roasting furnace is raised from room temperature to 600°C within 2 hours by programmed temperature increase, and the temperature is kept constant at 600°C for 4 hours. Then, under the protection of high-purity nitrogen, the temperature of the honeycomb catalyst is reduced to 40°C, and it can be installed in the fixed bed reactor. At this point, the preparation and installation of the catalyst assembly are completed.
[0078] Synthesis of trimethylaluminum by fixed-bed alkyl exchange reaction: 500 mL of dry decane was added to the fixed-bed reactor containing the honeycomb catalyst constructed by the above method, and the temperature of the lower end (high temperature section) of the fixed-bed reactor was first raised to about 170°C using the fixed-bed two-stage temperature control mode. Then, the alkyl aluminum feeding system at the top (low temperature section) of the fixed-bed reactor was opened to allow the liquid alkyl aluminum to pass through the feeding nozzle and evenly enter the reactor. After 10 minutes, the heating system of the low temperature section of the fixed-bed reactor was opened to allow the bed temperature to reach 125°C. Then, the methyl halide feeding system at the bottom of the fixed-bed reactor was carefully opened to allow the gaseous methyl halide to enter the fixed-bed reactor through the nozzle at the bottom of the reactor. The high temperature section of the bed reactor participates in the reaction, and the feed amount of the alkyl aluminum and the feed amount of the methyl halide are appropriately adjusted to control the molar ratio of the two entering the reactor to about 1:3.5 (keeping the methyl halide in excess). The reaction enters a steady state after 2 hours. The yield of the reaction is calculated to be 93.5% from the feed amount of the alkyl aluminum per unit time (reading the value of the liquid mass flowmeter used for alkyl aluminum metering) and the mass increment of the trimethyl aluminum product tank (V4) per unit time; 1g of the sample is taken through the sampling port on the product tank (V4) under the protection of high-purity nitrogen, placed in a 100mL three-necked flask replaced with high-purity nitrogen, first diluted with 20mL of dry decane, and then, in an ice-water bath, diluted with 10mL of 20% dilute sulfuric acid causes the trimethylaluminum in the solution to hydrolyze. After the intense reaction stage is basically over, it can be heated appropriately to allow the hydrolysis reaction to proceed to the end. All gases produced by the hydrolysis reaction are collected by the water discharge gas collection method. The composition of the collected gas is analyzed by gas chromatography: methane 99%, ethane 0.5%, and other gases 0.5%. The chlorine in the water phase is analyzed by the chlorine element analysis method, and the obtained value is back-calculated to the chlorine content in trimethylaluminum as 15PPM.
[0079] Example 2
[0080] Except that chemically pure antimony trioxide is adjusted to 100 grams and chemically pure silver oxide is adjusted to 100 grams, other conditions and steps are exactly the same as those in Example 1, and the reaction yield is calculated to be 96%; the gas phase composition obtained after decomposition with dilute sulfuric acid is: methane 99.4%, ethane 0.2%, and other gases 0.4%. The chlorine in the water phase is analyzed by the chlorine element analysis method, and the obtained value is back-calculated to the chlorine content in trimethylaluminum, which is 12PPM.
[0081] Example 3
[0082] Except that chemically pure antimony trioxide is adjusted to 200 grams, chemically pure silver oxide is adjusted to 200 grams, chemically pure titanium dioxide is 950 grams, and 4A molecular sieve crushed by a pulverizer is 8650 grams, the other conditions are exactly the same as the method and steps of Example 1, and the calculated reaction yield is 87%; the gas phase composition obtained after decomposition with dilute sulfuric acid is: methane 98.8%, ethane 0.9%, and other gases 0.3%. The chlorine in the water phase is analyzed by the chlorine element analysis method, and the obtained value is back-calculated to the chlorine content in trimethylaluminum, which is 55PPM.
[0083] Example 4
[0084] Except that the amount of chemically pure silver oxide added was reduced to 2 grams and the amount of 4A molecular sieve crushed by a pulverizer was adjusted to 9100 grams, the other conditions were exactly the same as the method and steps of Example 1, and the calculated reaction yield was 78%; the gas phase composition obtained after decomposition with dilute sulfuric acid was: methane 97.8%, ethane 1.8%, and other gases 0.4%. The chlorine in the water phase was analyzed by the chlorine element analysis method, and the obtained value was back-calculated to the chlorine content in trimethylaluminum, which was 85PPM.
[0085] Example 5
[0086] Except that the temperature of the low temperature section of the fixed bed reactor was adjusted to 140°C, the other conditions were exactly the same as the method and steps of Example 1, and the calculated reaction yield was 95.5%; the gas phase composition obtained after decomposition of dilute sulfuric acid was: methane 98.8%, ethane 0.6%, and other gases 0.6%. The chlorine in the water phase was analyzed by the chlorine element analysis method, and the obtained value was back-calculated to the chlorine content in trimethylaluminum, which was 35PPM.
[0087] Example 6
[0088] Except that the temperature of the low temperature section of the fixed bed reactor was adjusted to 100°C, the other conditions were exactly the same as the method and steps of Example 1, and the calculated reaction yield was 85%; the gas phase composition obtained after decomposition of dilute sulfuric acid was: methane 99.4%, ethane 0.3%, and other gases 0.3%. The chlorine in the water phase was analyzed by the chlorine element analysis method, and the obtained value was back-calculated to the chlorine content in trimethylaluminum, which was 17PPM.
[0089] Example 7
[0090] Except that the temperature of the high temperature section of the fixed bed reactor was adjusted to 180°C and the temperature of the low temperature section was adjusted to 135°C, the other conditions were exactly the same as the method and steps of Example 1, and the calculated reaction yield was 92%; the gas phase composition obtained after decomposition of dilute sulfuric acid was: methane 98.5%, ethane 1.1%, and other gases 0.4%. The chlorine in the water phase was analyzed by the chlorine element analysis method, and the obtained value was back-calculated to the chlorine content in trimethylaluminum, which was 65PPM.
[0091] Example 8
[0092] Except that the fixed bed reactor is divided into four sections for temperature control, the four sections are controlled from low to high (in the fixed bed reactor, from the top of the reactor to the bottom of the reactor), namely: 120°C, 140°C, 160°C, 180°C, and the other conditions are exactly the same as the method and steps of Example 1, and the calculated reaction yield is 96.5%; the gas phase composition obtained after decomposition of dilute sulfuric acid is: methane 99.6%, ethane 0.2%, other gases 0.2%, and the chlorine in the water phase is analyzed by the chlorine element analysis method. The obtained value is back-calculated to the chlorine content in trimethylaluminum, which is 22PPM.
[0093] Comparative Example 1
[0094] Except for deleting the addition of chemically pure silver oxide, the other conditions and steps are exactly the same as those of Example 1, and the calculated reaction yield is 55%; the gas phase composition obtained after decomposition with dilute sulfuric acid is: methane 95.8%, ethane 3.3%, and other gases 0.9%. The chlorine in the water phase is analyzed by the chlorine element analysis method, and the obtained value is back-calculated to the chlorine content in trimethylaluminum, which is 90PPM.
[0095] Comparative Example 2
[0096] Except that the temperature of the low temperature section of the fixed bed reactor was adjusted to 170°C, the other conditions were exactly the same as the method and steps of Example 1, and the calculated reaction yield was 45%; the gas phase composition obtained after decomposition of dilute sulfuric acid was: methane 92.6%, ethane 6.5%, and other gases 0.9%. The chlorine in the water phase was analyzed by the chlorine element analysis method, and the obtained value was back-calculated to the chlorine content in trimethylaluminum of 150PPM.
[0097] Comparative Example 3
[0098] Except that the temperature of the low temperature section of the fixed bed reactor was adjusted to 120°C and the temperature of the high temperature section was adjusted to 120°C, the other conditions were exactly the same as the method and steps of Example 1, and the calculated reaction yield was 38%; the gas phase composition obtained after decomposition of dilute sulfuric acid was: methane 96.7%, ethane 2.8%, and other gases 0.5%. The chlorine in the water phase was analyzed by the chlorine element analysis method, and the obtained value was back-calculated to the chlorine content in trimethylaluminum, which was 19PPM.
Claims
1. A continuous gas-liquid countercurrent fixed bed reactor system, characterized in that: The invention comprises a fixed bed reactor (R1), wherein a liquid phase nozzle (N2) is arranged at the top of the fixed bed reactor (R1), and a gas phase nozzle (N1) is arranged at the bottom. The fixed bed reactor (R1) is axially divided into multiple sections, and the reaction temperature is controlled in sections by a temperature control system. The top of the fixed bed reactor (R1) is connected to a separation unit.
2. The continuous gas-liquid countercurrent fixed bed reactor system device according to claim 1, characterized in that: The separation unit comprises a lightness removal tower (T1), a separation tower (T3) and a heavyness removal tower (T2) which are respectively connected to the top and the bottom of the lightness removal tower (T1).
3. The continuous gas-liquid countercurrent fixed bed reactor system device according to claim 1, characterized in that: The top of the fixed bed reactor (R1) is connected to the middle of the lightness removal tower (T1), the top of the lightness removal tower (T1) is connected to the middle of the separation tower (T3), the bottom of the separation tower (T3) is connected to the third storage tank (V3), the gas phase nozzle (N1) is connected to the first storage tank (V1) and the top of the separation tower (T3); the bottom of the lightness removal tower (T1) is connected to the middle of the weight removal tower (T2), the top of the weight removal tower (T2) is connected to the fourth storage tank (V4), and the liquid phase nozzle (N2) is connected to the second storage tank (V2) and the bottom of the weight removal tower (T2).
Citation Information
Cited By
Preparation method and device of trimethyl aluminum
CN118371194A