Thick product made of aluminum-copper-lithium alloys with improved toughness and manufacturing process

The described process for manufacturing aluminum copper lithium alloy sheets addresses the challenge of balancing elastic limit and toughness by optimizing composition and rolling conditions, resulting in improved mechanical properties for aircraft structures.

FR3147815A1Pending Publication Date: 2024-10-18CONSTELLIUM ISSOIRE +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
FR2023003680
Authority / Receiving Office
FR · FR
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing aluminum copper lithium alloys struggle to achieve a balanced compromise between elastic limit in the longitudinal direction (Rp0.2(L)) and toughness in the L-T direction (Kic (L-T)) for thick sheets used in aircraft wing structures, particularly for products with thicknesses greater than 25 mm.

Method used

A manufacturing process involving casting, homogenization, hot rolling, solution treatment, quenching, and tempering of aluminum alloy plates with specific compositions, including controlled end-of-rolling temperatures and texture management, to produce sheets with improved Rp0.2(L) and Kic (L-T) properties.

Benefits of technology

The process results in sheets with enhanced elastic limit and toughness, achieving Rp0.2(L) greater than 505 MPa and Kic (L-T) greater than 45.5 MPa·m^0.5 without compromising thermal stability or corrosion resistance, suitable for aircraft structural elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

Laminated product exhibiting an improved Rp0.2 (L) – K1c (LT) compromise, with a thickness of 25 mm to 50 mm, made of aluminium alloy with the following composition by weight: Cu 2.2-3.9 - Li 0.7-1.2 - Mg 0.1-0.8 - Mn 0.1-0.6 - Zr 0.07-0.15 - Ti 0.01-0.15 - Fe <0.1 - Si <0.1% - Ag ≤ 0.40 - Zn ≤ 0.70, Other elements <0.05 each and <0.15 in total, remaining aluminium, as it appears at mid-thickness, a volume fraction of grains having a brass texture is less than 21%. This product is obtained by a process comprising a casting step, homogenization, hot rolling, solution quenching, and tempering, such that during the hot rolling step the outlet temperature is between 395 and 445°C. Abbreviated figure: 1
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Thick product made of aluminum copper lithium alloys with improved toughness and method for obtaining same Technical field

[0001] The invention relates to thick products made of aluminum-copper-lithium alloys, more particularly, such products with a thickness of between 25 mm and 50 mm, their manufacturing and use methods, intended in particular for aeronautical and space construction. PREVIOUS ART

[0002] Most structural applications in the aeronautical industry require a high level of strength, as well as a high level of toughness. Products are therefore sought that offer the best static-toughness compromise.

[0003] Products intended for aircraft wing structures are mainly made from thick sheets according to the definition given in EN 12258-1. For products intended for aircraft wing structures, it is advantageous to focus on the compromise between yield strength in the longitudinal direction (Rp0.2(L)) and toughness in the LT direction (Kic(LT)). This is particularly the case for wing skins, central box panels or spars. In this case, where the main stress is along the largest dimension of the sheet, the tensile properties in the L direction (rolling direction) are of prime importance, as well as the toughness in the LT direction, this term meaning that the stress is applied in the L direction and the crack propagates in the T direction (longitudinal).

[0004] Lithium aluminum alloys are considered in the metallic design of aircraft structural elements, and in particular aircraft wing structures because they offer an excellent compromise between density, mechanical characteristics, toughness, fatigue and corrosion resistance.

[0005] Among the aluminum-lithium based alloys, aluminum copper lithium alloys are well known in the prior art for their interesting properties. Specifically, US patent 7,229,509 describes an alloy comprising (% by weight): 2.5-5.5 Cu; 0.1-2.5 Li; 0.2-1.0 Mg; 0.2-0.8 Ag; 0.2-0.8 Mn; 0.4 max Zr or other grain refining agents such as Cr, Ti, Hf, Sc, V, having in particular a toughness KiC (LT)>37.4 MPa / Vm for a yield strength Rp0j2(L) > 448.2 MPa (products with a thickness greater than 76.2 mm) and in particular a toughness K1C(L)>38.5 MPa'Vm for a yield strength RpO,2(L) > 489.5 MPa (products with a thickness less than 76.2 mm).

[0006] EP2235224 discloses an essentially non-recrystallized rolled product obtained from from a sheet of at least 30 mm thickness, comprising: 2.2 to 3.9 wt% Cu, 0.7 to 2.1 wt% Li; 0.2 to 0.8 wt% Mg; 0.2 to 0.5 wt% Mn; 0.04 to 0.18 wt% Zr; less than 0.05 wt% Zn and, optionally, 0.1 to 0.5 wt% Ag, the remainder being aluminium and unavoidable impurities, having a low propensity for crack bifurcation during a fatigue test in the LS direction. The product according to EP2235224 has a crack deflection angle T of at least 20° under an equivalent stress intensity factor Keffmax 10 MPa / Vm for a cracked specimen SL subjected to mixed mode I and II stress, in which the angle W between a plane perpendicular to the crack direction and the stress direction is 75°.

[0007] EP3384061 discloses a rolled and / or forged product made of an aluminum-based alloy comprising, in wt%, Cu: 3.2 - 4.0; Li: 0.80 - 0.95; Zn: 0.45 - 0.70; Mg: 0.15 - 0.7; Zr: 0.07 - 0.15; Mn: 0.1 - 0.6; Ag: < 0.15; Fe + Si < 0.20; at least one element from Ti: 0.01 - 0.15; Sc: 0.02 - 0.1; Cr: 0.02 - 0.1; Hf: 0.02 - 0.5; V: 0.02 - 0.1 other elements < 0.05 each and < 0.15 in total, remainder aluminum. The products according to EP3384061 are obtained from a process in which a bath of liquid metal based on aluminum alloy according to the invention is prepared, a raw form is cast from said bath of liquid metal; said raw form is homogenized at a temperature between 450°C and 550°; said raw form is hot deformed and optionally cold deformed, preferably to a thickness of at least 15 mm: said product is dissolved between 490 and 530°C for 15 min to 8 h and is quenched; said product is pulled in a controlled manner with a permanent deformation of 1 to 7% and said product is tempered.The product is advantageous for the manufacture of aircraft structural elements.

[0008] EP2675933 discloses wrought products made of lithium aluminum alloy of a thickness of at least 12.7 mm and containing from 3.00 to 3.80 wt% Cu, from 0.05 to 0.35 wt% Mg, from 0.975 to 1.385 wt% Li, where -0.3*Mg-0.15Cu +1.65 = Li = -0.3*Mg-0.15Cu +1.85, from 0.05 to 0.50 wt% of at least one element for controlling grain structure selected from the group consisting of Zr, Sc, Cr, V, Hf, other rare earth elements, and combinations thereof, up to 1.0 wt% Zn, up to 1.0 wt% Mn, up to 0.12 wt% Si, up to 0.15 wt% Fe, up to 0.15 wt% weight of Ti, up to 0.10% by weight of any other element, the total of such other elements not exceeding 0.35% by weight, the remainder being aluminum.

[0009] There is a need for sheets with a thickness greater than 25 mm of aluminum copper lithium alloy having an improved Rpo.2(L))- K[c (LT) compromise compared to existing products while retaining properties of thermal stability, corrosion resistance and fatigue endurance. Statement of the invention

[0010] The subject matter of the patent relates to a method for manufacturing a rolled product in which an aluminum alloy plate is cast, the composition of which, in % by weight, is: Cu 2.2-3.9; Li 0.7-1.2; Mg 0.1-0.8; Mn 0.1-0.6; Zr 0.07-0.15; Ti 0.01-0.15; Fe <0.1; Si <0.1%; Ag <0.40; Zn <0.70; other elements <0.05 each and <0.15 in total, remainder aluminum.

[0011] Preferably, the Zn content is from 0.05 to 0.25% by weight and the Ag content is from 0.20 to 0.40% by weight.

[0012] In another preferred embodiment, the Zn content is from 0.45 to 0.70% by weight and the Ag content is less than or equal to 0.15% by weight.

[0013] Said cast plate is then homogenized at a temperature of from 510°C to 540°C for 5 to 50 hours. Preferably, the homogenization temperature is from 515°C to 540°C.

[0014] Said homogenized plate is hot-deformed by rolling, so as to obtain a rolled product, such that the final hot-deformation temperature is between 395°C and 445°C to obtain a rolled product whose thickness is between 25 mm and 50 mm. Preferably, the final thickness of the product is between 30 mm and 40 mm. Preferably, the rolling outlet temperature is between 410°C and 445°C.

[0015] Said rolled product having a thickness of 25 mm to 50 mm is solution-treated at a temperature of 490°C to 530°C for 15 minutes to 8 hours. Said solution-treated product is quenched with water. Preferably, the quenching water is at room temperature. Said quenched product is then pulled in a controlled manner with a permanent deformation of 1 to 6%. Said product is then tempered by heating at a temperature of 120°C to 170°C for 5 to 100 hours.

[0016] The invention also relates to a rolled product whose thickness is from 25 mm to 50 mm, preferably from 30 mm to 40 mm, made of aluminum alloy of composition in % by weight, Cu 2.2-3.9; Li 0.7-1.2; Mg 0.1-0.8; Mn 0.1-0.6; Zr 0.07-0.15; Ti 0.01-0.15; Fe <0.1; Si <0.1%; Ag <0.40; Zn <0.70; other elements <0.05 each and <0.15 in total, remainder aluminum and such that at mid-thickness, the volume fraction of grains having a brass texture is less than 21%, preferably less than 20%, even more preferably less than 19%.

[0017] Preferably, the mid-thickness rolled product is such that at mid-thickness the sum of the volume fractions of the grains having a copper, brass and S texture is less than or equal to 60%, preferably less than or equal to 55%.

[0018] Preferably, the composition of the product comprises a Zn content of from 0.05 to 0.25% by weight and an Ag content of from 0.20 to 0.40% by weight.

[0019] In another preferred embodiment, the composition of the product comprises a Zn content of from 0.45 to 0.70% by weight and an Ag content of from 0.05 to 0.15% by weight.

[0020] Preferably, the rolled product has a mid-thickness elastic limit in the long direction Rp0.2(L) at least equal to 505 MPa and a toughness Kic (LT) of at least 45.5 MPa.'Vm. FIGURES

[0021] [Fig. 1] shows the evolution of the stress intensity factor K[c (TL) as a function of the final hot rolling temperature of the products of example 1.

[0022] [Fig.2] shows the compromise yield strength Rp0.2 - direction L - stress intensity factor Kic (LT) (LT) of the products of example 1.

[0023] [Fig.3] shows the evolution of the stress intensity factor Kic (LT) as a function of the final hot rolling temperature of the products of example 2. DETAILED DESCRIPTION OF THE INVENTION

[0024] Unless otherwise stated, all statements regarding the chemical composition of alloys are expressed as a percentage by weight based on the total weight of the alloy. Designation of alloys is in accordance with the regulations of The Aluminium Association, known to those skilled in the art. Density depends on the composition and is determined by calculation rather than by a weight measurement method. Values ​​are calculated in accordance with the procedure of The Aluminium Association, which is described on pages 2-12 and 2-13 of "Aluminum Standards and Data". Definitions of metallurgical tempers are given in European Standard EN 515.

[0025] Unless otherwise stated, the static mechanical characteristics, in other words the breaking strength Rm, the tensile strength Rp0>2 and the elongation at break A, are determined by a tensile test according to standard EN 10002-1 or NF EN ISO 6892-1, the location at which the parts are taken and their direction being defined by standard EN 485-1.

[0026] The stress intensity factor (KQ) is determined according to ASTM E 399. Thus, the proportion of specimens defined in paragraph 7.2.1 of this standard is always verified as well as the general procedure defined in paragraph 8. ASTM E 399 gives in paragraphs 9.1.3 and 9.1.4 criteria which make it possible to determine whether KQ is a valid value of KiC. Thus, a K[C value is always a KQ value, the converse not being true.

[0027] Unless otherwise stated, the definitions of standard EN 12258 apply. The crystallographic texture can be described by a 3-dimensional mathematical function. This function is known in the art as the Orientation Density Function (ODF). It is defined as the volume fraction of the material dV / V having an orientation g to within dg: where (q>l, ¢, q>2) are the Euler angles describing the orientation g.

[0028] The present inventors calculated the FDO of each sheet by the spherical harmonics method from four pole figures measured by X-ray diffraction on a traditional texture goniometer. In the context of the invention, the measurements of the pole figures were carried out on samples cut at mid-thickness of the sheets. Similarly, in order to obtain statistically representative measurements, the size of the samples was adapted to the grain size. Preferably, the size of the samples is chosen so as to be able to analyze at least 3000 grains, preferably 5000.

[0029] It is possible to simplify the information contained in the FDO. This is commonly done in the art to describe selected aspects of the distribution of orientations in the material. An example of this practice is the calculation of the volume fraction of crystallites that have a specific orientation. To do this, the reference orientation is arbitrarily defined, along with an angle of maximum misorientation around this orientation. The FDO is then integrated into the domain thus defined, which makes it possible to deduce the relative volume of orientations contained in this domain compared to the total volume.

[0030] The present inventors used a tolerance of 15° around the orientations “copper”, “brass”, “S” in order to describe the texture obtained. The crystallographic orientations “copper”, “brass”, “S” are known to those skilled in the art and described for example in the reference document by UF Kocks, CN Tomé, and H.-R. Wenk, “Texture and anisotropy: preferred orientations in polycrystals and their effect on materials properties”. Cambridge University Press, 2000.

[0031] The orientations “copper”, “brass”, “S” are reproduced in the table below. Name Indices Bunge (ç>i,C>, ç>2) Kocks (^,0,0) Copper {112}<1H> 90,35,45 0,35,45 Brass {110} <il2>35,45,0 55,45,0 S {123} <634> 59,37,63 149,37,27

[0032] The inventors have found that it is possible to improve the compromise Rpo.2(L) - K[c (LT), on rolled products with a thickness of 25 mm to 50 mm, preferably at least 30 mm, and at most 45 mm or 40 mm if a mid-thickness texture is maintained such that the volume fraction of grains having a brass texture is less than 21%, preferably less than 20%, or 19%. Preferably, it is possible to improve the compromise Rp0.2 (L) - Kk (LT), on rolled products with a thickness of 25 mm to 50 mm, if the sum of the volume fractions of the grains having a compression texture, that is to say the sum of the volume fractions of the grains with copper, brass, and S texture, is less than or equal to 60%, preferably less than or equal to 55%.

[0033] Preferably, the rolled products with a thickness of 25 mm to 50 mm, preferably at least 30 mm, and at most 40 mm or 45 mm according to the invention have a mid-thickness yield strength in the long direction Rp0.2(L) of at least 505 MPa and a toughness Kk (LT) of at least 45.5 MPa.'Vm.

[0034] Preferably, the rolled products for which the composition is such that the Zn content is less than or equal to 0.25% by weight, preferably between 0.05% and 0.25% and the Ag content is between 0.20 and 0.40% by weight have a yield strength in the long direction Rp0.2(L) of at least 510 MPa and a toughness Kic (LT) of at least 46 MPa.'Vm.

[0035] The rolled products according to the invention are obtained by a process comprising the steps of casting, homogenization, hot rolling, solution treatment, stress relief, and tempering.

[0036] An aluminum alloy plate according to the invention is cast.

[0037] The aluminum alloy according to the invention comprises in % by weight Cu 2-3.9, Li 0.7-1.2, Mg 0.1-0.8, Mn 0.1-0.6, Zr 0.07-0.15, Ti 0.01-0.15, Fe <0.1, Si <0.1%, Ag <0.40, Zn <0.70, other impurities <0.05, total 0.15, remainder aluminum.

[0038] The copper content is from 2% to 3.9% by weight. In an advantageous embodiment, the copper content is at least 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%. In another advantageous embodiment, the copper content is at most 3.8%, 3.7%. Any combination of the Cu values ​​previously described constitutes an advantageous embodiment of the invention.

[0039] The lithium content is from 0.7% to 1.2% by weight. In an advantageous embodiment, the lithium content is at least 0.80%, 0.85%, 0.90%. In another advantageous embodiment, the lithium content is at most 1.15%, 1.10%, 1.05%, 1.0%. Any combination of the previously described Li values ​​constitutes an advantageous embodiment of the invention.

[0040] The magnesium content is from 0.1 to 0.8% by weight. In an advantageous embodiment, the magnesium content is at least 0.2%, 0.3%, 0.35%, 0.40%. In another advantageous embodiment, the magnesium content is at most 0.6%, 0.5%. Any combination of the previously described Mg values ​​constitutes an advantageous embodiment of the invention.

[0041] The silver content is less than or equal to 0.40% by weight. In an advantageous embodiment, the silver content is at least 0.05%, 0.10%, 0.15%, 0.20%. In another advantageous embodiment, the silver content is at most 0.35%, 0.30%, 0.25%, 0.20%, 0.15%. Any combination of the Mg values ​​previously described constitutes an advantageous embodiment of the invention.

[0042] The zinc content is less than or equal to 0.70% by weight. In an advantageous embodiment, the zinc content is at least 0.05%, 0.10%, 0.15%, 0.20%, 0.25%, 0.30%, 0.35%, 0.40%, 0.45%, 0.50%. In another advantageous embodiment, the zinc content is at most 0.65%, 0.60%, 0.55%, 0.50%, 0.45%, 0.40%, 0.35%, 0.30%, 0.25%, 0.20%, 0.15%.

[0043] Advantageously, the Zn content is less than or equal to 0.25% by weight, preferably from 0.05% to 0.25% and the Ag content is from 0.20 to 0.40% by weight. In another advantageous embodiment, the Zn content is from 0.45% to 0.70% by weight and the Ag content is less than or equal to 0.15%, preferably from 0.05% to 0.15% by weight.

[0044] The zirconium content is between 0.07 and 0.15% and preferably between 0.09 and 0.12%.

[0045] The manganese content is between 0.1 and 0.6% by weight. Advantageously, the manganese content is between 0.2 and 0.4% in order to improve toughness without compromising mechanical strength. In the absence of manganese addition, the desired compromise is not achieved.

[0046] The titanium content is between 0.01 and 0.15% by weight. Preferably, between 0.02 and 0.10% by weight of titanium is chosen.

[0047] It is preferable to limit the content of impurities in the alloy. These elements include iron and silicon and any other unavoidable impurities. The iron content and the silicon content are each at most 0.1% by weight. Preferably, the iron and silicon contents are each at most 0.08% by weight. In an advantageous embodiment of the invention, the iron and silicon contents are at most 0.06% and 0.04% by weight, respectively. The other impurities have a content of less than 0.05% by weight each and 0.15% by weight in total. The remainder corresponds to aluminum.

[0048] The cast plate is then homogenized. The homogenization temperature is preferably between 510°C and 540°C for 5 to 50 hours. Preferably, the temperature is at least 515°C. Preferably, the temperature is at most 530°C, or 525°C. In another preferred embodiment, the homogenization is carried out in two stages, with at least one of the two stages at a temperature between from 510°C to 540°C or from 510°C to 525°C or from 515°C to 525°C.

[0049] After homogenization, the plate is usually cooled to room temperature before being reheated in order to be hot rolled. The purpose of reheating is to allow the hot deformation of the product. However, it is possible not to carry out this reheating if the homogenized plate can be rolled without it being cooled. Preferably, the initial hot rolling temperature is between 420°C and 520°C, preferably, the initial rolling temperature is at most 510°C, 500°C, or 490°C.

[0050] The plate is then hot rolled so as to obtain a rolled product with a thickness of between 25 mm and 50 mm, preferably at least 30 mm, and at most 40 mm or 45 mm.

[0051] The inventors have found that by controlling the end-of-rolling temperature from 395°C to 445°C for this final thickness range of 25 to 50 mm, preferably at least 30 mm, and at most 40 mm or 45 mm, it is possible to increase the toughness Klc (LT), also called critical stress intensity factor, and to improve the compromise between the elastic limit at mid-thickness in the long direction Rpo.2(L) and the toughness K[c (LT).

[0052] The end of rolling temperature is between 395°C and 445°C. The end of rolling temperature is preferably at least 400°C, or 405°C or 410°C or 415°C or 420°C or 425°C or 435°C. Preferably, the end of rolling temperature is at most 440°C. There are several means of controlling the final rolling temperature. For example, it is possible to act on the rolling speed or the reduction rate per pass, or the waiting time between passes or the cooling / reheating means such as the temperature of the working rolls of the rolling mill or the quantity of emulsion supplied, or even by sprinkling. The measurement of the rolling temperature can be done by infrared pyrometers. It is also possible to use a rolling model.The rolling forces and torques are linked to the temperature of the rolled product, so that by knowing the deformations and deformation rates imposed during a rolling pass, the forces measured on the rolling mill make it possible to deduce the temperature of the metal, using a model implemented in the rolling mill control software.

[0053] The product thus obtained is then put into solution, preferably by heat treatment at 490 to 530°C for 15 min to 8 h, then typically quenched with water.

[0054] The inventors have found that the total equivalent time for homogenization and dissolution t(eq) can exceed 40h, preferably 50h, where T (in Kelvin) is the instantaneous treatment temperature, which changes with time t (in hours), and Tref is a reference temperature set at 773 K. The equivalent time at 500°C (773K) is defined by the formula | exp(-26100 / T) dt = ---——---— exp{-2b!00 ; TW)

[0055] in which T is the instantaneous temperature expressed in Kelvin which evolves with time t (in hours) and Tref is a reference temperature of 500 °C (773 K). t(eq) is expressed in hours. The constant Q / R = 26100 K is derived from the activation energy for the diffusion of Mn, Q = 217000 J / mol.

[0056] The product put into solution then undergoes a controlled traction of 1 to 6% and preferably at least 2%, or 3%, typically around 4%.

[0057] An income is carried out on the pulled product at a temperature of 120 to 170°C for 5 to 100 h, preferably 140 to 160°C for 10 to 60 h. EXAMPLES

[0058] Example 1

[0059] Five Al-Cu-LI alloy plates referenced A, B, C, D, E were cast. Their composition is given in Table 1

[0060] [Table 1] - Composition (% by weight) of the different plates. Ref. 0.34 C 0.03 0.05 3.59 0.38 0.31 0.13 0.03 0.08 0.89 0.35 D 0.03 0.05 3.65 0.38 0.33 0.12 0.03 0.08 0.88 0.35 E 0.03 0.05 3.59 0.38 0.33 0.15 0.03 0.08 0.90 0.35

[0061] The plates were homogenized for 12 hours at 508°C + 15 hours 30 minutes at 518°C. They were then hot rolled after being reheated to a temperature of 525°C for a period of approximately 20 hours to reach a final thickness of approximately 31 mm. The initial and final rolling thickness, the initial and final hot rolling temperature of each of the plates are indicated in Table 2.

[0062] [Table 2] - Rolling conditions Ref. Initial temperature (°C) Final temperature (°C) Initial thickness (mm) Final thickness (mm) A Inv. 490 419 362 31 B Inv. 480 432 365 31 C Inv. 488 441 363 31 D Ref. 477 452 366 31 E Ref. 499 492 366 31

[0063] The sheets thus obtained were then solution-treated for 2 hours at 515°C and quenched with cold water. The sheets thus solution-treated and quenched were pulled in a controlled manner, with a permanent elongation of 3.75% and were subjected to 18 hours of tempering at 155°C. Thick sheets A, B, C are produced according to the invention. Thick sheets D and E correspond to reference examples.

[0064] The thick sheets were mechanically tested in such a way as to determine their static mechanical properties in the long rolling direction (L) and their stress intensity factor (KiC) in the LT direction according to standard E 399 (see Table 3).

[0065] [Table 3] - Static mechanical properties and stress intensity factor (Kæ) measured at mid-thickness (T / 2) Rm L Rp02 LA% L Kic LT MPa MPa MPa MPa.'Vm A Inv. 552 525 11.7 46.9 B Inv. 550 524 11.1 46.2 C Inv. 545 516 11.7 47.6 D Ref. 555 524 11.1 44.7 E Ref. 551 519 10.7 44.6

[0066] [Fig. 1] shows the evolution of the stress intensity factor as a function of the final hot rolling temperature. [Fig. 2] shows the compromise yield strength (L direction) - stress intensity factor (LT stress), i.e. the compromise (Rpo.2-L) - K1C (LT). These tests show that the stress intensity factor K1C (LT) increases if the end of rolling temperature is between 395°C and 445°C, preferably between 410°C and 445°C. This increase in the stress intensity factor is obtained without degradation of the yield strength of the product. The products according to the invention A, B, C have a yield strength greater than 505 MPa in the longitudinal direction and a toughness Kk (LT) greater than 45.5 MPa.'Vm.

[0067] Example 2

[0068] Two plates made of the same H alloy were cast. The H composition is shown in Table 4. The plates were homogenized in two 12-hour stages. 508°C then 15h30 525°C. They were then hot rolled after being reheated to a temperature of 525°C for a period of approximately 20 hours to reach a final thickness of approximately 40 mm. The thick sheet H1 was hot rolled to reach a final temperature of 480°C. The sheet H-2 was hot rolled to reach a final rolling temperature of 403°C.

[0069] [Table 4] - Composition (% by weight) of the different plates. Reference Si Fe Cu Mn Mg Zn Ti Zr Li Ag H 0.02 7 0.03 9 3.42 0.33 0.36 0.58 0.03 3 0.08 6 0.9 0.09

[0070] The sheets thus obtained were solution-treated for 2 hours at 515°C and quenched with cold water. The sheets thus solution-treated and quenched were tensile in a controlled manner, with a permanent elongation of 3.75% and were subjected to 18 hours of tempering at 155°C.

[0071] The thick sheets were mechanically tested in such a way as to determine their static mechanical properties in the long rolling direction (L) and their stress intensity factor (KiC) in the LT direction according to standard E 399 (see Table 5).

[0072] [Table 5] - Static mechanical properties and stress intensity factor (K[C) measured at mid-thickness (T / 2) Rm L Rp02 LA% L Kic LT MPa MPa MPa MPa.'Vm Hl Ref. 550 517 11.8 41.1 H-2 Inv. 536 507 11.3 45.7

[0073] These tests show that the stress intensity factor K1C (LT) increases if the end of rolling temperature is between 395°C and 445°C ([Fig.3]). The product according to the invention H-2 has an elastic limit greater than 505 MPa in the long direction and a toughness Kic (LT) greater than 45.5 MPa.'Vm.

[0074] A texture measurement by X-ray diffractometry was carried out on the H1 and H-2 sheets at mid-thickness. The analyzed surface is approximately 50 x 50 mm2. The volume fraction in % of the orientations, brass, copper and S, for each of the samples is given in Table 6.

[0075] [Table 6] - Volume fraction of the components Copper, Brass and S measured at mid- thickness Copper Brass S Sum (Copper+Brass+S) % % % % Hl Ref. 9.9 22.7 33.5 66.1 H-2 Inv. 7.4 17.7 26.1 51.2

[0076] It is observed that the product H-2 according to the invention has a brass texture of less than 21%, precisely less than or equal to 18%. The sum of the copper, brass and S textures is less than or equal to 60%, precisely less than or equal to 51%.

Claims

Claims

1. A method of manufacturing a rolled product in which: a) an aluminum alloy plate is cast having the composition in % by weight, Cu 2.2-3.9 Li 0.7-1.2 Mg 0.1-0.8 Mn 0.1-0.6 Zr 0.07-0.15 Ti 0.01-0.15 Fe <0.1 Si <0.1% Ag <0.40 Zn <0.70 Other elements <0.05 each and <0.15 in total, remaining aluminum, b) said plate is homogenized at a temperature of 510°C to 540°C for 5 to 50 hours, c) said homogenized plate is hot deformed by rolling such that the final hot deformation temperature is between 395°C and 445°C to obtain a rolled product whose thickness is between 25 mm and 50 mm, d) said product is solution-treated at a temperature of 490°C to 530°C for 15 minutes to 8 hours, e) quenching with water, f) said product is tensile in a controlled manner with a permanent deformation of 1 to 6%, g) said product is tempered by heating at a temperature of 120°C to 170°C for 5 to 100 hours.

2. A method of manufacturing a rolled product according to claim 1 wherein the Zn content is 0.05 to 0.25% by weight and the Ag content is 0.20 to 0.40% by weight.

3. A method of manufacturing a rolled product according to claim 1 wherein the Zn content is from 0.45 to 0.70% by weight and the Ag content is less than or equal to 0.15% by weight.

4. A method of manufacturing a rolled product according to any one of claims 1 to 3 wherein in step c) the rolling outlet temperature is between 410°C and 445°C.

5. A method of manufacturing a rolled product according to any one of claims 1 to 4 wherein during step c) the final thickness of the product is between 30 mm and 40 mm.

6. Rolled product with a thickness of 25 mm to 50 mm made of an aluminum alloy of composition in % by weight, Cu 2.2-3.9 Li 0.7-1.2 Mg 0.1-0.8 Mn 0.1-0.6 Zr 0.07-0.15 Ti 0.01-0.15 Fe <0.1 Si <0.1% Ag < 0.40 Zn < 0.70 Other elements <0.05 each and <0.15 in total, remainder aluminum, characterized in that at mid-thickness, the volume fraction of grains having a brass texture is less than 21%.

7. Rolled product according to claim 6 characterized in that at mid-thickness the sum of the volume fractions of the grains having a copper, brass and S texture is less than or equal to 60%.

8. Rolled product according to claim 6 or 7 characterized in that the Zn content is from 0.05 to 0.25% by weight and the Ag content is from 0.20 to 0.40% by weight.

9. Rolled product according to claim 6 or 7 characterized in that the Zn content is from 0.45 to 0.70% by weight and the Ag content is from 0.05 to 0.15% by weight.

10. Rolled product according to any one of claims 6 to 9 characterized in that the elastic limit at mid-thickness in the long direction RpO.2(L) is at least equal to 505 MPa and in that the toughness Klc (LT) is at least 45.5 MPa.'Vm.

Citation Information

Patent Citations

  • Rolled product made of aluminum-lithium alloy for aeronautical applications

    EP2235224A1

  • 2xxx series aluminum lithium alloys

    EP2675933A2

  • Aluminium-copper-lithium alloy having improved mechanical strength and improved toughness

    EP3384061A1

  • Al-Cu-Li-Mg-Ag-Mn-Zr alloy for use as structural members requiring high strength and high fracture toughness

    US7229509B2

  • Rolled product made of aluminum-lithium alloy for aeronautical applications

    WO2009103899A1