Positive electrode active material for lithium secondary battery, preparation method therefor, and lithium secondary battery comprising the same
A lithium-excess layered oxide with an ion-conductive coating layer addresses discharge capacity and voltage decay issues by stabilizing the structure and enhancing lithium ion conductivity, thereby improving battery performance.
Patent Information
- Application Number
- JP2024107739
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2020-10-19
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-02
AI Technical Summary
Lithium-excess layered oxides used in lithium secondary batteries face issues with discharge capacity reduction, voltage decay, and poor electrochemical properties due to phase transitions and Mn elution during cycling.
A lithium-excess layered oxide with a monoclinic structure and an ion-conductive coating layer composed of Ti, Al, or Zr is applied, which suppresses Mn elution and lattice changes, enhancing lithium ion conductivity and reducing resistance.
The solution improves discharge capacity, reduces overvoltage, and extends the lifespan of the battery by stabilizing the structure and increasing the rate characteristics.
Smart Images

Figure 2024133587000001_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a positive electrode active material containing a lithium-excess layered oxide, and more particularly, to a positive electrode active material for a lithium secondary battery having an ion-conductive coating layer formed on its surface, a method for manufacturing the same, and a lithium secondary battery including the same.
Background Art
[0002] With the development of portable mobile electronic devices such as smartphones, MP3 players, and tablet PCs, the demand for secondary batteries capable of storing electrical energy has increased explosively. In particular, with the emergence of electric vehicles, medium and large-sized energy storage systems, and portable devices that require high energy density, the demand for lithium secondary batteries is increasing.
[0003] In recent years, the most spotlighted material as a positive electrode active material is lithium nickel manganese cobalt oxide Li(Ni x Co y Mn z )O2 (in this case, x, y, and z are the atomic fractions of independent oxide composition elements, respectively, where 0 < x ≤ 1, 0 < y ≤ 1, 0 < z ≤ 1, and 0 < x + y + z ≤ 1). This positive electrode active material has been actively studied and used as a positive electrode active material, and is used at a higher voltage than LiCoO2, so it has the advantage of showing a high capacity, and because the Co content is relatively low, it has the advantage of being low in price. However, it has the disadvantages of poor rate capability and poor life characteristics at high temperatures.
[0004] Therefore, research is being conducted to apply a lithium-excess layered oxide that exhibits a high reversible capacity and exceeds existing Li(Ni x Co y Mn z )O2 to a lithium secondary battery.
[0005] However, such lithium-rich layered oxides have problems with discharge capacity reduction (cycle life) and voltage decay phenomena that occur during life cycling, which are caused by the phase transition from a spinel-like structure to a cubic structure due to the movement of transition metals during life cycling. The discharge capacity reduction and voltage decay phenomena of such lithium-rich layered oxides are problems that must be solved for commercialization in lithium secondary batteries.
[0006] There is also a need for solutions that can improve the electrochemical properties of lithium-rich layered oxides. Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention aims to improve the lithium ion conductivity of a positive electrode active material containing a lithium-excess layered oxide, thereby reducing the resistance, thereby reducing overvoltage generated during charge and discharge, and improving the rate characteristics.
[0008] Another objective of the present invention is to suppress the dissolution of Mn from the Mn-rich positive electrode active material and the lattice change from the spinel phase to the rock-salt phase that occurs on the surface of the positive electrode active material during cycling, thereby suppressing the decrease in discharge capacity and voltage drop and improving the life span. [Means for solving the problem]
[0009] The positive electrode active material according to the embodiment of the present invention includes a lithium-excess layered oxide represented by the following Chemical Formula 1: [Chemical formula 1]rLi2MnO3·(1-r)Li a Ni x Co y Mn z M1 1-(x+y+z) O2 (In the chemical formula 1, 0 < r ≤ 0.6, 0 < a ≤ 1, 0 ≤ x ≤ 1, 0 ≤ y < 1, 0 ≤ z < 1, and 0 < x + y + z ≤ 1, and M1 is at least one selected from Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Mg, Gd, Sm, Ca, Ce, Fe, Al, Ta, Mo, Sc, V, Zn, Cu, In, S, B, Ge, Si, and Bi.)
[0010] The lithium-excess layered oxide may be a solid solution phase in which Li2MnO3 having a monoclinic structure and LiMO2 having a rhombohedral structure are mixed. Further, M may be at least one selected from Ni, Co, Mn, and M1.
[0011] Also, in the lithium-excess layered oxide, a flat plateau due to Li2MnO3 may appear in the 4.4 V region of the initial charge-discharge profile. The lithium-excess layered oxide according to the examples of the present invention, unlike lithium during the initial charging process, the Li2MnO3 phase is electrochemically inactive up to the 4.4 V region, and a reaction in which lithium desorbs and oxygen evolution may occur in the Li2MnO3 phase at 4.4 V or higher.
[0012] The ratio (Li / Ni + Co + Mn) of the number of moles of lithium to the total number of moles of metals of Ni, Co, or Mn contained in the lithium-excess layered oxide represented by the chemical formula 1 may be 1.1 to 1.6, 1.2 to 1.6, 1.3 to 1.6, or 1.4 to 1.5.
[0013] In the chemical formula 1, the value of x may be greater than 0 and less than or equal to 0.5, greater than 0 and less than or equal to 0.4, greater than 0 and less than or equal to 0.3, greater than 0 and less than or equal to 0.2, or greater than 0 and less than or equal to 0.1.
[0014] In Chemical Formula 1, the value of y may be greater than 0 and less than 0.5, greater than 0 and less than 0.4, greater than 0 and less than 0.3, greater than 0 and less than 0.2, or 0.1 to 0.2.
[0015] In the formula 1, M1 is at least one selected from Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Mg, Gd, Sm, Ca, Ce, Fe, Al, Ta, Mo, Sc, V, Zn, Nb, Cu, In, S, B, Ge, Si, and Bi, and may be a dopant that may be included in the lithium-excess layered oxide. More preferably, M1 may be at least one selected from Ba, Sr, B, P, Y, Zr, Nb, Mo, Ta, and W, which may further grow the size of the primary particles and be appropriately adjusted according to a specific range. Most preferably, M1 may be at least one selected from Nb and Ta.
[0016] The ratio of the number of moles of Mn to the total number of moles of Ni (Mn / Ni) may be 1-4.5, 1-4, 2-4.5, 2-4, 3-4.5, or 3-4.
[0017] The oxide of the present invention has a layered structure, and can have a layered structure in which lithium atomic layers and metal atomic layers of Ni, Co, Mn, or M1 are alternately stacked with oxygen atomic layers interposed therebetween.
[0018] The planes constituting the layers of the layered structure of the positive electrode active material may have a crystal orientation perpendicular to the C-axis. In this case, the mobility of lithium ions contained in the positive electrode active material is improved, and the structural stability of the positive electrode active material is increased. When applied to a battery, the initial capacity characteristics, output characteristics, resistance characteristics, and long-term life characteristics may be improved.
[0019] The positive electrode active material according to the present invention suppresses the elution of Mn in an oxide rich in lithium and manganese by forming an ion conductive coating layer on the surface, and suppresses the lattice change from the spinel phase to the rock-salt phase that mainly occurs from the surface of the positive electrode active material during cycling, thereby suppressing the decrease in discharge capacity and voltage drop.
[0020] Further, in the present invention, since the ion conductive coating layer is coated on the particle surface of the lithium-rich layered oxide, the resistance is reduced by improving the ion conductivity. As a result, the life deterioration and voltage drop can be suppressed.
[0021] Further, in the present invention, since the ion conductive coating layer is coated on the particle surface of the lithium-rich layered oxide, the overvoltage generated during charge and discharge with the lithium-rich layered oxide can be reduced, and the rate characteristics can be improved.
[0022] To achieve the above effects, more preferably, the ion conductive coating layer can contain at least one element selected from Ti, Al, and Zr.
[0023] Further, the ion conductive coating layer can contain a substance represented by the following Chemical Formula 2. [Chemical Formula 2]Li a M2 b O c In the Chemical Formula 2, 0 < a ≤ 4, 0 < b ≤ 5, and 0 < c ≤ 12, and M2 can be at least one selected from Ti, Al, and Zr.
[0024] To achieve the above effects, the ion conductive coating layer can be contained in an amount of 0.05 mol% to 5 mol%, 0.1 mol% to 3 mol%, 0.1 mol% to 2 mol%, or 0.5 mol% to 2 mol% with respect to the lithium-rich layered oxide.
[0025] The ion-conductive coating layer may be included uniformly or non-uniformly on the surface of the lithium-excess layered oxide represented by Chemical Formula 1.
[0026] Also, as an example, the ion-conductive coating layer may be formed on the surface of each of the secondary particles or the primary particles.
[0027] In addition, for example, the ion conductive coating layer may form a concentration gradient portion of elements contained in the ion conductive coating layer on the surface of the secondary particles or the primary particles.
[0028] In the positive electrode active material according to the embodiment of the present invention, the thickness of the ion conductive coating layer may be 1 nm to 100 nm, more preferably 10 nm to 100 nm. If the coating layer is thinner than this, the improvement effect may be insignificant, while if the coating layer is thicker than this, the resistance to lithium ions may increase. If the ion conductive coating layer satisfies the above range, it is possible to suppress the Mn elution of the Mn-rich positive electrode active material of the present invention and to suppress the lattice change from the spinel phase to the rock-salt phase that starts from the surface during cycling, thereby suppressing the decrease in discharge capacity and the voltage drop and improving the lifespan.
[0029] In the positive electrode active material according to the embodiment of the present invention, the primary particles may be aggregated to form secondary particles, and the primary particles having a size of 300 nm to 10 μm may be adjusted to 50 vol% to 100 vol%, 70 vol% to 100 vol%, or 100 vol% in the primary particles constituting the secondary particles.
[0030] In addition, for example, the positive electrode active material may be adjusted such that primary particles having a size of more than 500 nm and not more than 10 μm constitute the secondary particles at 50 vol% to 100 vol%, 70 vol% to 100 vol%, or 100 vol%.
[0031] For example, the positive electrode active material may have primary particles having a size of 1 μm to 10 μm adjusted to 50 vol% to 100 vol%, 70 vol% to 100 vol%, or 100 vol% based on the total volume of the lithium-excess layered oxide.
[0032] For example, the positive electrode active material may have primary particles having a size of more than 1 μm adjusted to 50 vol% to 100 vol%, 70 vol% to 100 vol%, or 100 vol% based on the total volume of the lithium-excess layered oxide.
[0033] Also, for example, the positive electrode active material may be adjusted so that primary particles having a size of 2 μm or more are 50 vol% to 100 vol%, or 50 vol% to less than 70 vol%, based on the total volume of the lithium-excess layered oxide.
[0034] In addition, for example, the positive electrode active material may have a controlled size of primary particles, and the number of primary particles in a secondary particle may be 1 to 1,000, 1 to 100, or 1 to 10, or may be one primary particle.
[0035] The primary particle size means the maximum length of the particle.
[0036] For example, the average particle size of the primary particles of the positive electrode active material may be adjusted to be greater than 500 nm and less than or equal to 10 μm, or to be in the range of 1 μm to 10 μm.
[0037] The present invention can solve the problems of discharge capacity reduction and voltage drop caused by lithium-excess layered oxides, and can adjust the size of primary particles to improve the density of the positive electrode active material.
[0038] However, as the primary particles become larger, the lithium ion diffusion distance increases, which can cause overpotential due to concentration polarization of lithium ions during charging and discharging. As a result, the kinetics decreases, and the capacity of the positive electrode active material may decrease. However, by forming the ion-conductive coating layer, the kinetics of lithium ions increases, which increases the capacity and reduces the overpotential.
[0039] The secondary particles of the positive electrode active material according to the embodiment of the present invention may have an average particle size of 2 μm to 20 μm.
[0040] The average particle size of the present invention can be defined as a particle size that corresponds to 50% of the cumulative volume in a particle size distribution curve of the particles. The average particle size can be measured, for example, by a laser diffraction method.
[0041] In the positive electrode active material according to the embodiment of the present invention, the size of the primary particles in the positive electrode active material stage is larger than the size of the primary particles in the precursor stage under the manufacturing process conditions according to the following embodiment. Also, under the manufacturing process conditions according to the following embodiment, the ratio of (the size of the primary particles of the positive electrode active material to which a dopant acting as a flux is added) / (the size of the primary particles of the positive electrode active material to which a dopant acting as a flux is not added) is 1 or more, more preferably 30 or more, and most preferably 50 or more.
[0042] The M1 in Formula 1 is a dopant that acts as a flux to grow the primary particles, and can be doped into the lattice structure. As an example, the size of the primary particles can be controlled to increase by adding and mixing the flux dopant in the firing step with a lithium compound and then heat treating the mixture. Acting as a flux means that it can act as a dopant that increases the size of the primary particles by the growth between the primary particles.
[0043] In the positive electrode active material according to the embodiment of the present invention, the more the portion corresponding to the single crystal structure, that is, the fewer the number of primary particles, the more the problem of voltage drop represented by polycrystals can be improved.
[0044] When performing XRD analysis of the positive electrode active material according to the embodiment of the present invention, the half-value width (FWHM (deg.)) at I(104) can be 0.1 (deg.) to 0.25 (deg.), but the value can vary depending on the manganese content. Therefore, by adjusting the reduction rate of the half-value width through the addition and content adjustment of the dopant M1, the problems of lifespan and voltage drop can be solved.
[0045] In the present invention, by adjusting to increase the size of the primary particles with a lithium-excess layered oxide, when fired under the same conditions, in XRD analysis, the half-value width (FWHM (deg.)) at I(104) can be adjusted to decrease by 5% to 50%, 5% to 40%, 5% to 30%, 5% to 20%, 10% to 25%, or 10% to 20% when M1 is included compared to the comparative example without M1.
[0046] The positive electrode active material according to the embodiment of the present invention can contain a substance represented by the following Chemical Formula 3. The substance represented by the following Chemical Formula 3 can be a substance generated by the reaction of a dopant that acts as a flux for inducing growth between primary particles with lithium. [Chemical Formula 3]Li a M3O b (where 0 < a ≤ 8, 0 < b ≤ 15, and M3 is at least one selected from Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Mg, Gd, Sm, Ca, Ce, Fe, Al, Ta, Mo, Sc, V, Zn, Cu, In, S, B, Ge, Si, and Bi.)
[0047] The M1 in the formula 1 may be included in an amount of 0.001 mol% to 10 mol%, 0.01 mol% to 5.0 mol%, 0.01 mol% to 3.0 mol%, 0.1 mol% to 2.0 mol%, or 0.1 mol% to 1.0 mol% based on the total number of moles of metals constituting the positive electrode active material. If the dopant M1 included as a flux for inducing the growth of primary particles exceeds the above range, an excessive amount of lithium composite oxide is formed, which may cause a decrease in capacity and efficiency, whereas if the dopant M1 is less than the above range, the effect of growing the primary particles may be insignificant.
[0048] In addition, the energy density per volume (Wh / L) of the positive electrode active material according to the embodiment of the present invention may be 2.7 (Wh / L) to 4.0 (Wh / L).
[0049] In addition, the energy density per volume (Wh / L) of the positive electrode active material according to the embodiment of the present invention may be increased by 5% to 30% compared to a material not containing M1. The positive electrode active material according to the present invention may be adjusted to increase the size of the primary particles in the lithium-excess layered oxide, so that the energy density per volume (Wh / L) may be increased by 5% to 25%, 5% to 20%, 10% to 25%, or 10% to 20% when M1 is contained compared to a comparative example not containing M1.
[0050] In addition, the packing density (g / cc) of the positive electrode active material, which is adjusted by adding and adjusting the content of the dopant M1, may be 2.0 (g / cc) to 4.0 (g / cc).
[0051] In addition, the specific surface area (BET, m 2 / g) is 0.1(BET,m 2 / g) ~ 1.5 (BET, m 2 / g).
[0052] In the positive electrode active material according to the present invention, the specific surface area (BET, m 2 / g) can be adjusted to be reduced by 20% to 80% when M1 is included, compared to a comparative example not including M1.
[0053] The present invention increases the energy density per volume by inducing the growth of the primary particles and controls the portion corresponding to the single crystal structure of the positive active material, and reduces the specific surface area to reduce the surface area of the positive active material, thereby resolving problems of lifespan and voltage drop. In the present invention, inducing the growth of the primary particles includes all of the concepts of nucleation, ostwald ripening, and particle aggregation.
[0054] A method for producing a positive electrode active material according to an embodiment of the present invention includes a first step of producing a positive electrode active material precursor, such as a carbonate or a hydroxide.
[0055] The precursor particles may have an average particle size of 2 μm to 20 μm.
[0056] The precursor may be prepared by co-precipitation, spray-drying, solid phase method, wet grinding, fluidized bed drying, or vibration drying, but is not limited thereto.
[0057] In the method for preparing a positive electrode active material according to an embodiment of the present invention, after the first step and before the second step, a step of roasting the prepared precursor at 300° C. to 600° C. or 500° C. to 600° C. may be further included.
[0058] In the method for preparing a positive electrode active material according to an embodiment of the present invention, after the first step and before the second step, the step of washing and drying the calcined material may be further included.
[0059] Next, the method includes a second step of mixing the positive electrode active material precursor with a lithium compound and baking the mixture to form a lithium composite oxide.
[0060] In the second step, a compound containing M1 of Formula 1 may be further mixed and fired. M1 may be mixed in an amount of 0.1 mol % to 1.0 mol %, or 0.3 mol % to 0.8 mol % relative to the particles of the lithium-excess layered oxide.
[0061] To solve the above problems, the temperature of the firing step may be 750°C to 950°C, or 850°C to 950°C.
[0062] In the method for preparing a positive electrode active material according to an embodiment of the present invention, after the second step and before the third step, the step of washing and drying the calcined material may be further included.
[0063] Then, the method includes a third step of mixing the lithium composite oxide formed in the second step with a coating precursor to form an ion-conductive coating layer.
[0064] The present invention can uniformly coat an ion-conductive coating layer on the surface of a lithium-excess layered oxide through the following steps.
[0065] In a third step, the coating precursor may be subjected to a dry blending process.
[0066] In addition, in the third step, a wet mixing process may be performed on the coating precursor. For example, the coating precursor may be dispersed or dissolved in water, alcohol, or a dispersion solution, and then mixed with the material formed in the second step.
[0067] The third step may include mixing the material formed in the second step with a coating precursor, maintaining the mixture at 400°C to 800°C or 600°C to 800°C for 7 hours to 12 hours, and then cooling the mixture in a furnace.
[0068] For example, when the ion conductive coating layer contains at least one selected from Ti, Al, and Zr, the coating precursor may be at least one selected from TiO2, Al2O3, Al(OH)3, ZrO2, and Zr(OH)4, but is not particularly limited thereto.
[0069] A secondary battery according to an embodiment of the present invention includes the positive electrode active material.
[0070] The positive electrode active material is as described above, and the binder, conductive material, and solvent are not particularly limited as long as they can be used on a positive electrode current collector of a secondary battery.
[0071] Specifically, the lithium secondary battery may include a positive electrode, a negative electrode facing the positive electrode, and an electrolyte between the positive electrode and the negative electrode, but is not particularly limited thereto as long as it can be used as a secondary battery. Effect of the Invention
[0072] The present invention provides a lithium-excess layered oxide that improves lithium ion conductivity and reduces resistance, thereby reducing overvoltage that occurs during charging and discharging and improving rate characteristics.
[0073] In addition, it suppresses the dissolution of Mn from the Mn-rich positive electrode active material and the lattice change from the spinel phase to the rock-salt phase that occurs from the surface during cycling, thereby suppressing the decrease in discharge capacity and voltage drop and improving the lifespan. [Brief description of the drawings]
[0074] [Figure 1] FIG. 1 is a diagram showing the results of EDS measurement according to an embodiment of the present invention. [Diagram 2] FIG. 1 is a diagram showing the results of EDS measurement according to an embodiment of the present invention. [Diagram 3] FIG. 1 is a diagram showing SEM measurement results according to an embodiment of the present invention and a comparative example. [Figure 4]FIG. 2 is a diagram showing the results of XRD analysis according to examples and comparative examples of the present invention. [Diagram 5] FIG. 2 is a diagram showing the results of XRD analysis according to examples and comparative examples of the present invention. [Figure 6] 4 is a graph showing charge and discharge characteristics according to an embodiment of the present invention and a comparative example. [Figure 7] 1 is a graph showing overvoltage curves according to an embodiment of the present invention and a comparative example. [Figure 8] 1 is a graph showing rate characteristics according to an embodiment of the present invention and a comparative example. [Figure 9] 1 is a graph showing life characteristics according to an embodiment of the present invention and a comparative example. [Figure 10] 1 is a graph showing life characteristics according to an embodiment of the present invention and a comparative example. [Figure 11] 4 is a voltage characteristic graph according to an example and a comparative example of the present invention. [Figure 12] 4 is a voltage characteristic graph according to an example and a comparative example of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0075] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples.
[0076] As used herein, expressions such as "comprises" should be understood as open-ended terms that encompass the possibility of including other components.
[0077] As used herein, "preferred" and "preferably" refer to embodiments of the invention that may provide certain benefits, under certain circumstances, and are not intended to exclude other embodiments from the scope of the invention.
[0078] <Example 1> Preparation of positive electrode active material
[0079] synthesis Using the co-precipitation method, spherical Ni0.2 Co 0.1 Mn 0.7 The CO3 precursor was synthesized. In a 90L reactor, 25wt% NaCO3 and 28wt% NH4OH were added to a 2.5M composite transition metal sulfate aqueous solution, which was a mixture of NiSO4·6H2O, CoSO4·7H2O, and MnSO4·H2O in a molar ratio of 20:10:70. The pH in the reactor was maintained at 10.0-12.0, and the temperature was maintained at 45℃-50℃. In addition, N2, an inert gas, was added to the reactor to prevent the precursor from being oxidized.
[0080] After the synthesis and mixing were completed, washing and dehydration were carried out using a filter press (F / P) equipment. Finally, the dehydrated product was dried at 120°C for 2 days and filtered through a 75μm (200mesh) sieve to remove 18μm and 4μm Ni particles. 0.2 O 0.1 Mn 0.7 The CO3 precursor was obtained.
[0081] Roasting The prepared precursor was maintained in an O2 or air (50 L / min) atmosphere in a box furnace, heated at 2°C per minute, maintained at 550°C for 1 to 6 hours, and then cooled in the furnace.
[0082] Firing LiOH or Li2CO3 was weighed out so that the Li / (Ni+Co+Mn) ratio was 1.45 for the roasted precursor, and 0.6 mol% of Nb2O5 was weighed out as a flux dopant, and these were mixed using a manual mixer (MM).
[0083] The mixture was maintained in an O2 or air (50 L / min) atmosphere in a box furnace, the temperature was increased by 2°C per minute, and the firing temperature was maintained at 900°C for 7 to 12 hours, and then the furnace was cooled to produce lithium composite oxide particles.
[0084] coating As a surface treatment dopant, 1.0 mol % of TiO2 was weighed out and mixed using a mixer (Manual mixer, MM).
[0085] The mixture was maintained in an O2 or air (50 L / min) atmosphere in a box firing furnace, the temperature was increased by 4.4°C per minute, and the firing temperature was maintained at 700°C for 7 to 12 hours, followed by furnace cooling to produce a positive electrode active material.
[0086] <Example 2> Preparation of positive electrode active material A positive active material was prepared in the same manner as in Example 1, except that in the coating step, 1.0 mol % of Al2O3 was mixed as a surface treatment dopant.
[0087] <Example 3> Preparation of positive electrode active material A positive electrode active material was prepared in the same manner as in Example 1, except that in the coating step, 1.0 mol % of n-ZrO2 was mixed as a surface treatment dopant.
[0088] <Example 4> Preparation of positive electrode active material A positive electrode active material was prepared in the same manner as in Example 1, except that in the coating step of Example 1, 0.19 mol % of TiO2, 0.77 mol % of Al2O3, and 0.04 mol % of n-ZrO2 were mixed as the surface treatment dopant.
[0089] <Comparative Example 1> Preparation of Positive Electrode Active Material A positive active material was prepared in the same manner as in Example 1, except that no flux dopant was mixed and no coating step was performed.
[0090] <Comparative Example 2> Preparation of Positive Electrode Active Material A positive electrode active material was prepared in the same manner as in Example 1, except that the coating step was not performed.
[0091] <Manufacturing example> Manufacturing of lithium secondary batteries 90 wt% of the positive electrode active material according to the examples and comparative examples, 5.5 wt% of carbon black, and 4.5 wt% of PVDF binder were dispersed in 30 g of N-methyl-2-pyrrolidone (NMP) to prepare a positive electrode slurry. The positive electrode slurry was applied to a 15 μm-thick aluminum (Al) thin film as a positive electrode current collector, dried, and roll-pressed to prepare a positive electrode. The loading level of the positive electrode was 5.5 mg / cm. 2 and the electrode density is 2.3 g / cm 3 It was.
[0092] Metallic lithium was used as a counter electrode for the positive electrode, and 1M LiPF6, EC / DMC=1 / 1 (v / v) was used as the electrolyte.
[0093] A separator made of a porous polyethylene (PE) film was interposed between the positive electrode and the negative electrode to form a battery assembly, and the electrolyte was injected to manufacture a lithium secondary battery (coin cell).
[0094] <Experimental Example> Referring to FIG. 1, it can be seen that the Ti, Al and Zr coating layers are uniformly distributed on the surfaces of the positive electrode active materials according to Examples 1 to 3.
[0095] Referring to FIG. 2, it can be seen that the Ti, Al and Zr coating layers are uniformly distributed on the surface of the positive active material according to Example 4.
[0096] Referring to FIG. 3, it can be seen that primary particles are grown by the flux dopant Nb, and Ti, Al and Zr coating layers are formed on the grown primary particles.
[0097] XRD analysis of Figures 4 and 5 was performed using CuK α radiation at a wavelength of 1.5406 Å. Referring to Figures 4 and 5, it can be seen that the surface treatment dopant is partially doped into the surface of the particles. It can also be seen that the interslab expansion effect caused by the partial doping facilitates the diffusion of lithium ions.
[0098] 6, in the case of Comparative Example 2, as the primary particles become larger, the lithium ion diffusion distance increases, which causes a problem of a decrease in kinetics and a small decrease in capacity, but in the case of the embodiment in which an ion conductive coating layer is formed, it can be seen that the capacity increases because the ionic conductivity increases and the kinetics of the lithium ions increases.
[0099] 7, in the case of Comparative Example 2, as the primary particles become larger, the lithium ion diffusion distance increases, which causes a problem of overpotential due to the concentration polarization of lithium ions, but in the case of the embodiment in which an ion conductive coating layer is formed, it can be seen that the overpotential is reduced because the kinetics of lithium ions increases.
[0100] 8, it can be seen that the rate characteristics of the example are improved by about 10% or more compared to Comparative Example 2. This is because the resistance is reduced by the ion conductive coating layer.
[0101] 9 and 10, it can be seen that the life characteristics of the example are improved and the capacity retention rate is 80% or more compared to Comparative Example 2. This is because the ion conductive coating layer reduces resistance, suppresses Mn elution, and suppresses the phase change from the spinel phase to the rock salt phase that starts from the surface during cycling.
[0102] 11 and 12, it can be seen that the voltage retention rate of the example is improved and the problem of voltage drop is resolved compared to Comparative Example 2. This is because the ion conductive coating layer suppresses the phase change of the lithium-excess layered oxide that occurs during cycling.
[0103] The results of the above experiments are shown in Table 1 below. [Table 1]
Claims
1. A lithium-rich layered oxide represented by the following chemical formula 1; and an ion-conductive coating layer formed on the surface of the lithium-excess layered oxide represented by Chemical Formula 1; Primary particles having a size of more than 500 nm and not larger than 10 μm are present in an amount of 50 vol % to 100 vol % of the primary particles constituting the secondary particles, The ion-conductive coating layer includes a material represented by the following Chemical Formula 2: The positive electrode active material for a secondary battery, wherein the primary particles are aggregated to form the secondary particles. [Chemical Formula 1] rLi 2 MnO 3 ・(1 - r)Li a Ni x Co y Mn z M1 1-(x+y+z) O 2 (In the above Chemical Formula 1, 0<r≦0.6, 0<a≦1, 0≦x≦1, 0≦y<1, 0≦z<1, and 0<x+y+z≦1, and M1 is at least one selected from Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Mg, Gd, Sm, Ca, Ce, Fe, Al, Ta, Mo, Sc, V, Zn, Cu, In, S, B, Ge, Si, and Bi.) [Chemical 2] Li a M2 b O c (0<a≦4, 0<b≦5, and 0<c≦12, and M2 is at least one selected from Ti, Al, and Zr.)
2. 2. The positive electrode active material for a secondary battery according to claim 1, wherein the ion conductive coating layer is included in an amount of 0.05 mol % to 5.0 mol % based on the lithium-excess layered oxide.
3. 2. The positive electrode active material for a secondary battery according to claim 1, wherein the ion-conductive coating layer has a thickness of 1 nm to 100 nm.
4. 2. The positive electrode active material for a secondary battery according to claim 1, wherein the positive electrode active material is adjusted such that primary particles having a size of 300 nm to 10 μm are contained in the primary particles constituting the secondary particles at a ratio of 50 vol % to 100 vol %.
5. 2 . The positive electrode active material for a secondary battery according to claim 1 , wherein M1 in Formula 1 is a dopant acting as a flux for growing the primary particles.
6. 2 . The positive electrode active material for a secondary battery according to claim 1 , wherein M1 in Formula 1 is at least one selected from the group consisting of Ba, Sr, B, P, Y, Zr, Nb, Mo, Ta, and W.
7. 2. The positive electrode active material for a secondary battery according to claim 1, wherein M1 in Formula 1 is included in an amount of 0.001 mol % to 10 mol % based on the total moles of metal in the lithium-excess layered oxide.
8. 2. The positive electrode active material for a secondary battery according to claim 1, wherein the ratio of the moles of lithium to the moles of all metals, Ni, Co, or Mn, contained in the lithium-excess layered oxide represented by Chemical Formula 1 (Li / Ni+Co+Mn) is 1.1 to 1.
6.
9. 2. The positive electrode active material for a secondary battery according to claim 1, wherein in the lithium-excess layered oxide represented by Chemical Formula 1, a ratio of the number of moles of Mn to the number of moles of total Ni (Mn / Ni) is 1 to 4.
5.
10. The method for producing a positive electrode active material for a secondary battery according to claim 1, A first step of producing a positive electrode active material precursor; A second step of mixing the positive electrode active material precursor with a lithium compound and calcining the mixture to form a lithium composite oxide; and a third step of mixing the lithium composite oxide formed in the second step with a coating precursor to form an ion-conductive coating layer.
11. The method of claim 10, wherein the second step further comprises mixing and firing a compound including M1 of Formula 1.
12. The coating precursor is TiO 2 , Al 2 O 3 , Al(OH) 3 , ZrO 2 , and Zr(OH) 4 The method for producing a positive electrode active material for a secondary battery according to claim 10, wherein the positive electrode active material is at least one selected from the following:
13. A secondary battery comprising the positive electrode active material of claim 1.
Citation Information
Patent Citations
Lithium nickel composite oxide, manufacture thereof, and positive electrode active substance for secondary battery
JP1998069910A
Positive electrode active material for use in non-aqueous lithium secondary battery and method of fabricating it
JP2001155728A
Cathode active material containing solid-solution active material, cathode containing cathode active material, and nonaqueous electrolyte secondary battery employing cathode
JP2014222607A
Metal oxide powder, method for preparing same, and lithium secondary battery comprising same