Film and application of the same
A film combining thermoplastic resin, organic acid, and sugar alcohol addresses decomposition and foreign matter issues, ensuring high tensile strength and antibacterial efficacy while maintaining appearance.
Patent Information
- Application Number
- JP2023046446
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-04
AI Technical Summary
Existing antibacterial films using dehydroacetic acid or sodium dehydroacetate face issues with decomposition at high temperatures during resin molding and the generation of foreign matter affecting film appearance, which compromises their structural integrity.
A film composed of a thermoplastic resin, an organic acid, and a sugar alcohol, with a pH of 6 or less, which suppresses the generation of foreign substances and maintains excellent antibacterial properties and appearance.
The film achieves high tensile elongation at break, superior antibacterial activity, and maintains a good appearance by uniformly dispersing the antibacterial agent, addressing the limitations of previous technologies.
Smart Images

Figure 2024135653000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a film having both antibacterial properties and good appearance, and applications thereof. [Background technology]
[0002] In recent years, food waste has become a food issue. Food waste occurs when food spoils and is discarded, but it can also occur when food that has passed its expiration date or best-before date is discarded. Food waste is an issue when food that could have been eaten is discarded without being eaten, and to solve this problem, antibacterial films have been developed as a way to extend the expiration date or best-before date of food. Furthermore, with growing awareness of environmental conservation, there are also studies being conducted on making products thinner, reducing the amount of raw materials used, and improving recyclability.
[0003] For example, Patent Document 1 discloses an antibacterial sheet made of a thermoplastic resin to which 0.5 to 5.0% of dehydroacetic acid or sodium dehydroacetate has been added. Here, it has been investigated whether a sheet that exerts an antibacterial effect can be obtained by using dehydroacetic acid or sodium dehydroacetate as an antibacterial agent. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 9-267451 Summary of the Invention [Problem to be solved by the invention]
[0005] The antibacterial sheet disclosed in Patent Document 1 uses dehydroacetic acid or sodium dehydroacetate as an antibacterial agent, but when dehydroacetic acid is used, there is a problem that the antibacterial agent decomposes during resin molding because decomposition begins at 150°C or higher. In addition, when sodium dehydroacetate is used, there is a problem that if the amount of antibacterial agent used is increased to obtain the desired antibacterial properties, foreign matter is generated, which impairs the appearance of the film. If foreign matter (such as aggregates of antibacterial particles) is generated in the film, the film may break from these foreign matter, which causes problems in film formation.
[0006] In view of the above problems in the prior art, an object of the present invention is to provide a film having both excellent antibacterial properties and good appearance. [Means for solving the problem]
[0007] Examples of specific embodiments of the present invention are given below. [1] A film comprising a thermoplastic resin (A), an organic acid (B) and a sugar alcohol (C), the pH of the film surface being 6 or less. [2] The film according to [1], wherein the melting point of the thermoplastic resin (A) is 180°C or lower, or the glass transition temperature is 180°C or lower. [3] The film according to [1] or [2], wherein the thermoplastic resin (A) is a polyolefin resin. [4] The film according to [3], wherein the polyolefin resin is at least one selected from the group consisting of polyethylene, polypropylene, and ethylene-vinyl acetate copolymer. [5] The film according to any one of [1] to [4], wherein the organic acid (B) is at least one selected from the group consisting of hydroxy acids and organic acid salts of inositol phosphate. [6] The film according to any one of [1] to [5], wherein the organic acid (B) is at least one selected from the group consisting of tartaric acid and phytic acid. [7] The film according to any one of [1] to [6], wherein the content of the organic acid (B) is 0.1 to 10 mass % based on the total mass of the film. [8] The film according to any one of [1] to [7], wherein the sugar alcohol (C) is at least one selected from the group consisting of glycerin, glucitol, inositol and maltitol. [9] The film according to any one of [1] to [8], wherein the content of the sugar alcohol (C) is 0.05 to 30 mass % relative to the total mass of the film.
[10] The film according to any one of [1] to [9], which has a tensile elongation at break in at least one direction of 300% or more, as measured in accordance with JIS K7127 (1999).
[11] The film according to any one of [1] to
[10] , which has an antibacterial activity value of 2 or more as measured in accordance with JIS Z2801 (2012).
[12] The film according to any one of [1] to
[11] , which is for food packaging.
[13] A food packaging material comprising the film according to any one of [1] to
[12] . Effect of the Invention
[0008] According to the present invention, a film having both excellent antibacterial properties and good appearance can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The present invention will be described below as an example of an embodiment of the present invention. However, the scope of the present invention is not limited to the embodiment described below. In this specification, when "X to Y" (X and Y are arbitrary numbers) is expressed, unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably greater than X" or "preferably smaller than Y". In addition, when "X or more" (X is an arbitrary number) or "Y or less" (Y is an arbitrary number) is expressed, it also includes the meaning of "preferably greater than X" or "preferably less than Y". In addition, "film" and "sheet" used in the following description are not clearly distinguished from each other, and "film" includes "sheet", and "sheet" includes "film".
[0010] [Antibacterial film] The film of the present invention contains a thermoplastic resin (A), an organic acid (B), and a sugar alcohol (C). The film of the present invention (hereinafter also referred to as "the present film") contains the sugar alcohol (C) in addition to the organic acid (B), and thus can achieve both antibacterial properties and good appearance. The present film is also called an antibacterial film because it exhibits excellent antibacterial properties.
[0011] In addition, the present film has a high tensile elongation at break. If foreign matter (such as aggregates derived from acid components) occurs in the film, the foreign matter may become the starting point for the film to break, but in the present invention, by containing sugar alcohol (C) in addition to organic acid (B), the generation of foreign matter (such as aggregates derived from acid components) can be suppressed, and therefore a high tensile elongation at break can be achieved.
[0012] As described above, in the present film, an organic acid and a specific alcohol are used in combination and then composited with a thermoplastic resin, making it possible to produce an antibacterial film that combines antibacterial properties, good appearance, and high tensile elongation at break. The present invention will be described in detail below.
[0013] <Thermoplastic resin (A)> The film contains a thermoplastic resin (A). Examples of the thermoplastic resin include polyolefin resins, polyester resins, polyamide resins, polystyrene resins, acrylic resins, polyether resins, polyurethane resins, and ethylene-vinyl alcohol copolymer resins. Among them, the thermoplastic resin (A) is preferably a resin having heat sealability. In this specification, examples of the resin having heat sealability include resins having a melting point of 180° C. or less or a glass transition temperature of 180° C. or less. When the resin having heat sealability has a melting point, the melting point is more preferably 170° C. or less, even more preferably 160° C. or less, and particularly preferably 150° C. or less. When the resin having heat sealability has a glass transition temperature, the glass transition temperature is more preferably 150° C. or less, even more preferably 120° C. or less, and particularly preferably 100° C. or less. By setting the melting point or glass transition temperature within the above range, heat sealing at a lower temperature is possible, and the heat sealability is improved. By using a resin having heat sealability as the thermoplastic resin (A), the composition can be preferably used for, for example, food packaging applications.
[0014] In this embodiment, the thermoplastic resin (A) is preferably a polyolefin resin. The polyolefin resin is not particularly limited, but examples thereof include polymers containing α-olefins such as ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, or 1-decene as structural units. The polyolefin resin may be a homopolymer containing only one of the above monomers as structural units, a copolymer containing two or more of the above monomers as structural units, or a copolymer containing other copolymerizable monomers as structural units. The copolymer contains the above monomers as main structural units.
[0015] Among them, from the viewpoints of appearance, tensile elongation at break, versatility, economy, etc., the polyolefin resin is preferably a polyethylene resin containing ethylene as the main monomer component, or a polypropylene resin containing propylene as the main monomer component, and is particularly preferably a polyethylene resin. Here, the main monomer component refers to a monomer component that is a structural unit that occupies 50% by mass or more and 100% by mass or less in the polyolefin resin. In this embodiment, the polyolefin resin is preferably at least one selected from the group consisting of polyethylene, polypropylene, and an ethylene-vinyl acetate copolymer.
[0016] The content of the thermoplastic resin (A) in the film of this embodiment is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, even more preferably 75% by mass or more, and particularly preferably 80% by mass or more, based on the total mass of the film. The content of the thermoplastic resin (A) is preferably 99% by mass or less, based on the total mass of the film. By setting the content of the thermoplastic resin (A) within the above range, the generation of foreign matter (such as aggregates of antibacterial particles) can be suppressed, making it easier to obtain good appearance and high tensile elongation at break.
[0017] (Polyethylene resin) The polyethylene resin is not particularly limited as long as it is a resin containing ethylene as the main monomer component, and examples thereof include low density polyethylene, linear low density polyethylene, linear very low density polyethylene, medium density polyethylene, and high density polyethylene. The polyethylene resin may be an ethylene homopolymer, or a copolymer containing ethylene as the main monomer component and other copolymerizable monomer components. Examples of the copolymer include a copolymer or multicomponent copolymer containing ethylene as the main monomer component and one or more comonomers selected from other copolymerizable monomer components, or a mixed composition thereof. The polyethylene resin may be used alone, or two or more types of copolymerizable monomer components, which have different compositions and physical properties, may be used in combination.
[0018] Examples of other copolymerizable monomer components (comonomers) include α-olefins having 3 to 10 carbon atoms, such as propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, and 1-octene; vinyl esters, such as vinyl acetate and vinyl propionate; unsaturated carboxylic acid esters, such as methyl (meth)acrylate and ethyl (meth)acrylate, and ionomers thereof; and unsaturated compounds, such as conjugated dienes and non-conjugated dienes. The proportion of the structural unit derived from the copolymerizable monomer contained in the polyethylene resin is not particularly limited, but is usually preferably 30% by mass or less, and more preferably 15% by mass or less. The inclusion of a copolymerizable monomer component in the polyethylene resin can increase the flexibility and transparency of the film.
[0019] Among these, the polyethylene resin is preferably low-density polyethylene, linear low-density polyethylene, linear very low-density polyethylene, ethylene-vinyl acetate copolymer (EVA), ethylene-(meth)acrylic acid ester copolymer or ionomer resin, more preferably linear low-density polyethylene or ethylene-vinyl acetate copolymer (EVA), and particularly preferably linear low-density polyethylene.
[0020] The linear low density polyethylene is preferably a linear low density polyethylene containing at least one α-olefin selected from the group consisting of 1-butene, 1-hexene, and 4-methyl-1-pentene as a comonomer. The proportion of the comonomer component is not particularly limited, but is usually preferably 30% by mass or less, and more preferably 15% by mass or less. The inclusion of the comonomer component in the linear low density polyethylene can increase the flexibility and transparency of the film.
[0021] The method for producing the polyethylene resin is not particularly limited, and any known polymerization method using an olefin polymerization catalyst can be used. For example, there are a slurry polymerization method, a solution polymerization method, a bulk polymerization method, a gas phase polymerization method, etc. using a multi-site catalyst such as a Ziegler-Natta catalyst or a single-site catalyst such as a metallocene catalyst, and a bulk polymerization method using a radical initiator.
[0022] The melting point of the polyethylene resin is preferably 70 to 130° C., and more preferably 80 to 120° C. If the melting point of the polyethylene resin is within this range, the tensile strength (for example, tensile breaking strength and tensile breaking elongation) and dimensional stability of the film tend to be improved. Here, the melting point of a polyethylene-based resin is the crystalline melting peak temperature (Tm) (°C) determined from a thermogram measured using a differential scanning calorimeter (DSC) by heating approximately 10 mg of resin from -50°C to 200°C at a heating rate of 10°C / min, holding it at 200°C for 1 minute, then cooling it to -50°C at a cooling rate of 10°C / min, and again heating it to 200°C at a heating rate of 10°C / min.
[0023] The melt flow rate (MFR) of the polyethylene resin is not particularly limited, but is usually preferably 0.1 to 20 g / 10 min or more, more preferably 0.5 to 18 g / 10 min, and even more preferably 1 to 15 g / 10 min. If the MFR is 0.1 g / 10 min or more, extrusion processability is stable, and if it is 20 g / 10 min or less, stable film formation during molding is possible and thickness unevenness, reduction or variation in mechanical strength, etc. are reduced, which is preferable. Here, MFR is a value measured in accordance with JIS K7210-1 (2014), and the measurement conditions are 190°C and a load of 2.16 kg.
[0024] The density of polyethylene resin is 0.880 to 0.980 g / cm 3 It is preferable that the density is 0.890 to 0.960 g / cm 3 More preferably, it is 0.900 to 0.940 g / cm 3It is particularly preferable that the density is 0.880 to 0.980 g / cm 3 It is preferable that the density is within this range because it has an excellent balance of transparency, strength, adhesion, and flexibility. Here, the density is a value measured in accordance with JIS K6922-1 (2018).
[0025] (Polypropylene resin) The polypropylene-based resin is not particularly limited as long as it is a resin containing propylene as the main monomer component, and may be a propylene homopolymer, or a copolymer containing propylene as the main monomer component and other copolymerizable monomer components. Examples of the copolymer include a copolymer or multicomponent copolymer containing propylene as the main monomer component and one or more comonomers selected from other copolymerizable monomer components, or a mixed composition thereof. The polypropylene-based resin may be used alone, or two or more types of copolymerizable monomer components, which have different compositions and physical properties, may be used in combination.
[0026] Examples of other copolymerizable monomer components (comonomers) include α-olefins having 2 to 20 carbon atoms, such as ethylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, and 1-octene; dienes, such as divinylbenzene, 1,4-cyclohexadiene, dicyclopentadiene, cyclooctadiene, and ethylidene norbornene; vinyl acetate, (meth)acrylic acid, (meth)acrylic acid esters, (meth)acrylic acid glycidyl, vinyl alcohol, ethylene glycol, maleic anhydride, styrene, and cyclic olefins. The proportion of the structural unit derived from the copolymerizable monomer contained in the polypropylene-based resin is not particularly limited, but is usually preferably 30% by mass or less, and more preferably 15% by mass or less. The inclusion of a copolymerizable monomer component in the polypropylene-based resin can increase the flexibility and transparency of the film.
[0027] The polypropylene resin may be a block copolymer, a random copolymer, or a graft copolymer.
[0028] The method for producing the polypropylene resin is not particularly limited, and any known polymerization method using an olefin polymerization catalyst can be used. For example, there are a slurry polymerization method, a solution polymerization method, a bulk polymerization method, a gas phase polymerization method, etc. using a multi-site catalyst such as a Ziegler-Natta catalyst or a single-site catalyst such as a metallocene catalyst, and a bulk polymerization method using a radical initiator.
[0029] The melting point of the polypropylene resin is preferably 70 to 170° C., and more preferably 80 to 160° C. If the melting point of the polypropylene resin is in this range, the film will have a good balance of flexibility, strength, and heat resistance, which is preferable. Here, the melting point of a polypropylene-based resin is the crystalline melting peak temperature (Tm) (°C) determined from a thermogram measured using a differential scanning calorimeter (DSC) by heating approximately 10 mg of resin from -50°C to 200°C at a heating rate of 10°C / min, holding it at 200°C for 1 minute, then cooling it to -50°C at a cooling rate of 10°C / min, and again heating it to 200°C at a heating rate of 10°C / min.
[0030] The melt flow rate (MFR) of the polypropylene resin is not particularly limited, but is usually preferably 0.2 to 20 g / 10 min or more, more preferably 0.5 to 18 g / 10 min, and even more preferably 1 to 15 g / 10 min. If the MFR is 0.2 g / 10 min or more, the extrusion processability is stable, and if it is 20 g / 10 min or less, stable film formation during molding is possible and thickness unevenness, decrease or variation in mechanical strength, etc. are reduced, which is preferable. Here, MFR is a value measured in accordance with JIS K7210-1 (2014), and the measurement conditions are 230°C and a load of 2.16 kg.
[0031] <Organic acid (B)> This film contains an organic acid (B). In this film, the organic acid (B) has the function of lowering the pH of the film surface and imparts antibacterial properties to the film. The organic acid (B) is uniformly dispersed in the film. For example, when the film is divided into three parts in the thickness direction, the content of the organic acid (B) in each part is approximately uniform. In this specification, the phrase "the content of the organic acid (B) is approximately uniform" means that the content of the organic acid (B) in each part does not differ by 10% by mass or more.
[0032] Examples of the organic acid (B) used in the present invention include monocarboxylic acids such as acetic acid, formic acid, propionic acid, caproic acid, enanthic acid, caprylic acid, pelargonic acid, capric acid, undecanoic acid, lauric acid, myristic acid, palmitic acid, and stearic acid; dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid; hydroxy acids such as lactic acid, gluconic acid, glycolic acid, glyceric acid, malic acid, citric acid, tartaric acid, hydroxyacetic acid, hydroxybutyric acid, tartronic acid, salicylic acid, (m-, p-)hydroxybenzoic acid, 12-hydroxydodecanoic acid, 12-hydroxyisobutyric acid, (o-, m-, p-)hydroxyphenylacetic acid, 4-hydroxyphthalic acid, and 12-hydroxystearic acid; and inositol phosphates such as phytic acid. These organic acids can be used alone or in combination of two or more.
[0033] Among them, the organic acid (B) is preferably at least one selected from the group consisting of hydroxy acids and inositol phosphates, and more preferably at least one selected from tartaric acid and phytic acid. In this embodiment, in order to effectively lower the pH of the film surface, it is preferable that the organic acid is one that does not decompose during film formation (thermoforming). For this reason, it is particularly preferable that the organic acid is a heat-resistant hydroxy acid or inositol phosphate.
[0034] The organic acid (B) is preferably solid at 15° C. By using such an organic acid (B), the handleability of the organic acid (B) during film production can be improved, and the production efficiency of the film can be increased. In addition, by using a solid organic acid (B), the acid can be more uniformly dispersed in the thermoplastic resin. Examples of organic acids that are solid at 15° C. include tartaric acid, malic acid, citric acid, benzoic acid, and solid phytic acid.
[0035] The thermal decomposition temperature of the organic acid (B) is preferably 200° C. or higher. By using such an organic acid (B), a large amount of the organic acid (B) can be retained in the film, the pH of the film surface can be effectively lowered, and excellent antibacterial properties can be imparted.
[0036] The content of the organic acid (B) in the film of the present embodiment is preferably 0.1 to 10 mass % relative to the total mass of the film, more preferably 0.3 to 8 mass %, and particularly preferably 0.5 to 5 mass %. By setting the content of the organic acid (B) within the above range, it is possible to impart superior antibacterial properties to the film.
[0037] <Sugar alcohol (C)> The present film contains a sugar alcohol (C). The sugar alcohol used in the present invention exerts an effect of uniformly dispersing the antibacterial agent in the thermoplastic resin, and can improve the appearance of the film. Specific examples of sugar alcohols include chain sugar alcohols such as glycerol having three carbon atoms; sugar alcohols having four carbon atoms, such as erythritol and threitol, obtained by reducing monosaccharides; sugar alcohols having five carbon atoms, such as ribitol, arabitol, and xylitol; and sugar alcohols having six carbon atoms, such as glucitol, mannitol, iditol, talitol, and galactitol. In addition, cyclic sugar alcohols, such as cyclitols such as inositol, can be mentioned. In addition, disaccharide alcohols, such as maltitol, lactitol, and isomaltulose reduction products, obtained by reducing disaccharides, can be mentioned. In addition, when the above sugar alcohol has stereoisomers, the sugar alcohol (C) includes all of those stereoisomers. In addition, the sugar alcohol may be used alone, or two or more kinds can be used in combination.
[0038] Among these, from the viewpoints of heat resistance, availability, and economy, sugar alcohols having 3 to 12 carbon atoms are preferred, sugar alcohols having 3 to 6 carbon atoms are more preferred, and chain sugar alcohols having 3 to 6 carbon atoms are particularly preferred. Among these, these sugar alcohols (C) are preferably at least one selected from the group consisting of glycerol, glucitol, inositol, and maltitol, and more preferably at least one selected from the group consisting of glycerol, glucitol, and maltitol. The above sugar alcohols are also used in foods, and are preferably used because of their high safety.
[0039] The sugar alcohol (C) is preferably solid at 15°C. By using such a sugar alcohol (C), the handleability of the sugar alcohol (C) during film production can be improved, and the production efficiency of the film can be increased. In addition, by using a solid sugar alcohol (C), the antibacterial agent can be more uniformly dispersed in the thermoplastic resin, and the appearance of the film can be more effectively improved. Examples of sugar alcohols that are solid at 15°C include glucitol, xylitol, erythritol, mannitol, maltitol, inositol, threitol, ribitol, arabitol, iditol, talitol, galactitol, and lactitol.
[0040] The thermal decomposition temperature of the sugar alcohol (C) is preferably 200°C or higher, more preferably 220°C or higher, and particularly preferably 250°C or higher. Here, the thermal decomposition temperature refers to the temperature at which mass loss begins in thermogravimetric analysis. By setting the thermal decomposition temperature at the above level or higher, thermal decomposition of the sugar alcohol (C) during film production can be suppressed, allowing for stable film production. By suppressing the thermal decomposition of the sugar alcohol (C), film foaming due to gas generation, film coloration due to oxidative deterioration, and the generation of foreign matter (lumps) due to carbonization can be easily suppressed.
[0041] The content of the sugar alcohol (C) in the film of this embodiment is preferably 0.05 to 30% by mass, more preferably 0.1 to 20% by mass, and particularly preferably 0.5 to 15% by mass, based on the total mass of the film. By setting the content of the sugar alcohol (C) within the above range, the antibacterial agent can be more uniformly dispersed in the thermoplastic resin, so that the generation of foreign matter (lumps) caused by the antibacterial agent can be reduced, and the appearance of the film can be improved. In addition, the reduction in the generation of foreign matter (lumps) can suppress the decrease in the tensile elongation at break of the film.
[0042] <Optional ingredients> The present film may further contain optional components in addition to the above-mentioned components. An example of the optional components is an antibacterial agent. In order to enhance the antibacterial properties of the present film, the present film may contain an antibacterial agent in addition to the organic acid (B). In this case, the antibacterial agent to be combined is preferably an organic antibacterial agent.
[0043] Examples of organic antibacterial agents include monocarboxylic acids such as benzoic acid, dehydroacetic acid, sorbic acid, propionic acid, acetic acid, formic acid, caproic acid, enanthic acid, caprylic acid, pelargonic acid, capric acid, undecanoic acid, lauric acid, myristic acid, palmitic acid, and stearic acid; salts of the above monocarboxylic acids such as sodium dehydroacetate, potassium sorbate, sodium propionate, and sodium benzoate; and salts of oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, and pimelic acid. dicarboxylic acids such as carboxylic acid, suberic acid, azelaic acid, sebacic acid, and their salts; hydroxy acids such as lactic acid, gluconic acid, glycolic acid, glyceric acid, malic acid, citric acid, tartaric acid, hydroxyacetic acid, hydroxybutyric acid, tartronic acid, salicylic acid, (m-, p-)hydroxybenzoic acid, 12-hydroxydodecanoic acid, 12-hydroxyisobutyric acid, (o-, m-, p-)hydroxyphenylacetic acid, 4-hydroxyphthalic acid, 12-hydroxystearic acid, and their salts. organic acid-based antibacterial agents such as glycine; amino acid-based antibacterial agents such as hexadecylpyridinium chloride, diisobutylphenoxydimethylbenzoylammonium chloride, benzalkonium chloride, benzethonium chloride, methylbenzethonium chloride, cetylpyridinium chloride, cetrimonium, dophanium chloride, didecyldimethylammonium chloride, domiphen bromide, and other quaternary ammonium salt-based antibacterial agents; alkyldiaminoethylglycine hydrochloride, sodium alkylbenzenesulfonate, polyoxyethylene nonylphenyl ether, polyoxyethylene oleyl ether, polyoxyethylene stearylamine, lauryldimethylbenzylammonium chloride, and other surfactant-based antibacterial agents; diiodomethyl-p-trisulfone, polyvinylpyrrolidone iodide, and other halogen-based antibacterial agents; peroxide-based antibacterial agents such as peracetic acid; ester-based antibacterial agents such as glyceryl laurate and ethyl hydroxybenzoate; aldehyde-based antibacterial agents such as formaldehyde;Cresol, o-phenylphenol, 2-isopropyl-5-methylphenol, ethanol, ethyl-2,4-dihydroxy-6-methylbenzoate, methyl-2,4-dihydroxy-3,6-dimethylbenzoate, isopropyl-2,4-dihydroxy-6-methylbenzoate, 3-methoxy-5-methylphenyl-2,4-dihydroxy-6-methylbenzoate, ethyl-2,4-dihydroxy-3,6-dimethylbenzoate, ethyl-3-formyl-2,4-dihydroxy-6-methylbenzoate, iso Phenol-alcohol antibacterial agents such as propyl-3-formyl-2,4-dihydroxy-6-methylbenzoate, 3-hydroxy-5-methylphenyl-2,4-dihydroxy-6-methylbenzoate, 3-methyl-4 isopropylphenol, 3-hydroxy-5-methylphenyl-2-dihydroxy-4-methoxy-6-methylbenzoate, 3-methoxy-5-methylphenyl-2-hydroxy-4-methoxy-6-methylbenzoate, and 3-chloro-2,6-dihydroxy-4-methylbenzoate are included.
[0044] Examples of optional components include colorants, inorganic fillers, organic fillers, ultraviolet absorbers, light stabilizers, heat stabilizers, antioxidants, lubricants (slip agents), anti-blocking agents, hydrolysis inhibitors, plasticizers, flame retardants, anti-fogging agents, and adhesives. These optional components may be directly mixed with the resin constituting the film, or a master batch containing the resin and optional components may be prepared beforehand and then the film is formed. The film may contain two or more optional components in appropriate combination. The content of the optional components is preferably 10% by mass or less, more preferably 8% by mass or less, and even more preferably 5% by mass or less, based on the total mass of the film.
[0045] The film may also contain fats and oils as an optional component. Fat and oil refers to an ester compound of fatty acid and glycerin, and examples thereof include vegetable fats and oils, animal fats and oils obtained by hardening these fats and oils. Specific examples of vegetable fats and oils include rapeseed oil, soybean oil, rice oil, palm oil, palm kernel oil, coconut oil, corn oil, cottonseed oil, peanut oil, castor oil, sunflower oil, olive oil, etc. Examples of animal fats and oils include chicken oil, lard, beef tallow, milk fat, mutton tallow, horse fat, and fish oil. Examples of hardened oils and fats include hydrogenated rapeseed oil, extremely hydrogenated rapeseed oil, hydrogenated soybean oil, extremely hydrogenated soybean oil, hydrogenated rice oil, extremely hydrogenated rice oil, hydrogenated palm oil, extremely hydrogenated palm oil, hydrogenated palm kernel oil, hydrogenated coconut oil, hydrogenated corn oil, hydrogenated cottonseed oil, hydrogenated castor oil, hydrogenated sunflower oil, hydrogenated olive oil, hydrogenated chicken fat oil, extremely hydrogenated chicken fat oil, hydrogenated lard oil, extremely hydrogenated lard oil, hydrogenated beef tallow oil, extremely hydrogenated beef tallow oil, hydrogenated fish oil and extremely hydrogenated fish oil.
[0046] (Laminated film) The film may be a single layer film, or may be a laminated film with other resin layers laminated thereon. In the laminated film, when a layer containing a thermoplastic resin (A), an organic acid (B) and a sugar alcohol (C) is referred to as "Layer A" and a resin layer having another structure is referred to as "Layer B", the laminated film may have a two-layer structure of Layer A / Layer B, or a multilayer structure such as Layer A / Layer B / Layer A or Layer B / Layer A / Layer B. When the laminated film has Layer A and Layer B, and further another resin layer C (hereinafter referred to as "Layer C"), it may have a three-layer structure of Layer A / Layer B / Layer C, or a three-type five-layer structure such as Layer A / Layer B / Layer C / Layer B / Layer A. When the laminated film has Layers A to C and another resin layer D (hereinafter referred to as "Layer D"), it may have a four-layer structure of Layer A / Layer B / Layer C / Layer D, or a four-type seven-layer structure such as Layer A / Layer B / Layer C / Layer D / Layer C / Layer B / Layer A. In the laminated film, there are no limitations on the number of layers, the order of layers, or the type and number of layers other than Layer A, but it is preferable that Layer A is provided on the front and / or back surface of the film. The laminated film may have a structure in which a plurality of Layers A are laminated. When the laminated film is used for food packaging, it is preferable that Layer A containing the thermoplastic resin (A), organic acid (B) and sugar alcohol (C) is disposed on the front surface of the laminated film, as the innermost layer (the layer in contact with food).
[0047] Specific examples of the configuration of the laminate film include a laminate film having at least three layers: a layer containing a thermoplastic resin (A), an organic antibacterial agent (B) and a sugar alcohol (C), a base layer of polyester, polyamide, polypropylene, polystyrene (syndiotactic polystyrene) or the like, and a gas barrier layer having gas barrier properties of polytetrafluoroethylene, polyvinyl alcohol, ethylene-vinyl alcohol copolymer, etc. In this case, the layer containing the thermoplastic resin (A), the organic antibacterial agent (B) and the sugar alcohol (C) is preferably disposed on one surface layer (the innermost layer) of the laminate film.
[0048] When the present film is a laminated film, examples of the other resin layer include layers containing polyester, polyamide, polypropylene, polystyrene (syndiotactic polystyrene), polymethylpentene, polyimide, polytetrafluoroethylene, polyvinyl alcohol, ethylene-vinyl alcohol copolymer, polyethylene, etc. The other resin layer may be provided depending on the required function, and for example, the provision of the other resin layer can impart gas barrier properties, heat resistance, and moisture resistance. The laminated film may also have a layer containing a metal such as aluminum or iron.
[0049] When a laminated film is to be produced, it may be produced according to a conventional method, among which a method of co-extrusion using a plurality of extruders through a lamination die is preferred.
[0050] (Film manufacturing method) The present film can be produced by a known method. For example, the present film can be produced by using an inflation method, an extrusion T-die method, or the like. Specifically, the present film can be produced by melt-kneading a thermoplastic resin (A), an organic acid (B), and a sugar alcohol (C), and forming the molten resin composition into a film (sheet). The present film may be a non-stretched film or a stretched film.
[0051] When the present film is a laminated film, the laminated film can be manufactured by adopting the above-mentioned known method using the resin composition forming each layer. Alternatively, the laminated film may be manufactured by laminating previously obtained films by a lamination method or the like. Among them, it is preferable to use the co-extrusion T-die method, since the film-forming process is the same even when the number of layers of the film is large, and thickness control is relatively easy.
[0052] The manufacturing process of the present film may include a step of winding the obtained film into a roll. That is, the present embodiment may relate to a rolled body (film roll) obtained by winding the present film into a roll. When winding the film, it is preferable to wind the film around a core. It is preferable to use a core having a width equal to or greater than the width of the film.
[0053] <Film properties> The present film preferably has the following physical properties:
[0054] (Tensile breaking strength) In this film, the tensile strength at break in at least one direction measured in accordance with JIS K7127 (1999) is preferably 3 MPa or more, more preferably 5 MPa or more, even more preferably 7 MPa or more, and particularly preferably 9 MPa or more. The upper limit of the tensile strength at break is not particularly limited, but is preferably 100 MPa or less. The tensile strength at break is a value measured in accordance with JIS K7127 (1999) using a tensile tester using a test piece having a length of 50 mm in the measurement direction and a width of 10 mm under the conditions of a measurement temperature of 23±2°C, a chuck distance of 20 mm, and a test speed of 200 mm / min.
[0055] More specifically, the MD tensile breaking strength of the present film, measured in accordance with JIS K7127 (1999), is preferably 3 MPa or more, more preferably 5 MPa or more, even more preferably 7 MPa or more, and particularly preferably 9 MPa or more. The upper limit of the MD tensile breaking strength is not particularly limited, but is preferably 100 MPa or less. The TD tensile strength at break, measured in accordance with JIS K7127 (1999), is preferably 3 MPa or more, more preferably 5 MPa or more, even more preferably 7 MPa or more, and particularly preferably 9 MPa or more. The upper limit of the TD tensile strength at break is not particularly limited, but is preferably 100 MPa or less. In this embodiment, it is preferable that the tensile breaking strength in either the MD or TD is within the above range, and it is particularly preferable that the tensile breaking strength in both the MD and TD is within the above range.
[0056] (Tensile elongation at break) In this film, the tensile elongation at break in at least one direction measured in accordance with JIS K7127 (1999) is preferably 300% or more, more preferably 305% or more, and even more preferably 310% or more. The upper limit of the tensile elongation at break is not particularly limited, but is preferably 2000% or less. The tensile elongation at break is a value measured in accordance with JIS K7127 (1999) using a tensile tester using a test piece having a length of 50 mm in the measurement direction and a width of 10 mm under the conditions of a measurement temperature of 23±2°C, a chuck distance of 20 mm, and a test speed of 200 mm / min.
[0057] More specifically, the MD tensile elongation at break of the film, measured in accordance with JIS K7127 (1999), is preferably 300% or more, more preferably 305% or more, and even more preferably 310% or more. The upper limit of the MD tensile elongation at break is not particularly limited, but is preferably 2000% or less. The TD tensile elongation at break measured in accordance with JIS K7127 (1999) is preferably 300% or more, more preferably 305% or more, and even more preferably 310% or more. The upper limit of the TD tensile elongation at break is not particularly limited, but is preferably 2000% or less. In this embodiment, it is preferable that the tensile elongation at break in either the MD or TD is within the above range, but it is particularly preferable that the tensile elongation at break in both the MD and TD is within the above range.
[0058] (Total light transmittance) In this film, the antibacterial agent has high dispersibility, and the generation of foreign matter (lumps) is suppressed, so that this film has high transparency. Specifically, the total light transmittance of this film measured in accordance with JIS K7361-1 (1997) is preferably 50% or more, more preferably 65% or more, and even more preferably 75% or more. Since the higher the total light transmittance, the more preferable it is, the upper limit is not particularly limited, but it may be, for example, 100% or less, 98% or less, or 95% or less. By setting the total light transmittance within the above range, the visibility of the contents can be improved when used as a packaging film, etc. The total light transmittance was measured using a haze meter conforming to JIS K7361-1 (1997) at five measurement points (n=5), and the arithmetic average value was calculated.
[0059] (Area ratio of foreign matter (lumps)) This film has excellent appearance with little generation of foreign matter (lumps) originating from antibacterial agents, etc. The appearance of a film can be evaluated, for example, by calculating the area ratio of foreign matter (lumps) in the film. The area ratio of foreign matter (lumps) occurring in a film can be measured using a digital microscope. Specifically, the reflected field is observed with a ring light, and the brightness range of the lump is extracted from the brightness histogram of the observed image to determine the area of the lump. The area ratio of the lump is then calculated as a percentage by dividing the area of the lump by the observed area. The smaller the area ratio of foreign matter (lumps) is, the more preferable it is; it is preferably less than 0.1%, more preferably 0.09% or less, and particularly preferably 0.08% or less.
[0060] (Antibacterial performance) This film exhibits excellent antibacterial properties. For example, the antibacterial properties of the film can be evaluated by the antibacterial performance test described in JIS Z2801 (2012). Specifically, in the antibacterial performance test described in JIS Z2801 (2012), the antibacterial activity value calculated from the number of bacteria after 24 hours is preferably 2.0 or more. If the antibacterial activity value is within the above range, the film can be evaluated as having high antibacterial properties.
[0061] (Surface pH) The pH of the surface of the present film is preferably 6 or less, more preferably less than 6, and even more preferably 5.5 or less. The pH of the film surface can be measured by placing a water-soaked pH test paper in close contact with the film surface and leaving it for 3 hours, and then comparing the color of the pH test paper with a color sample.
[0062] (Thickness) The thickness of the present film is preferably 3 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more. The thickness of the present film is preferably 500 μm or less, more preferably 400 μm or less, and even more preferably 300 μm or less. By making the thickness of the present film within the above range, the processability and handling properties during film production can be more effectively improved.
[0063] (peel strength) After the film is used as a lid material and heat sealed to a base material (tray), the easy peel strength when the lid material is opened is preferably 1.0 N / mm to 20.0 N / mm when the test piece is 15 mm wide and at 23° C. By setting the easy peel strength to be equal to or higher than the above lower limit, the hermeticity of the package can be maintained. Also, by setting the easy peel strength to be equal to or lower than the above upper limit, the ease of opening can be improved.
[0064] <Application> The present film can be used for various purposes, and is preferably used for packaging food, packaging medicines such as tablets, packaging medical instruments such as syringes and needles, and packaging sanitary materials such as gauze and masks. In particular, the present film is preferably used for packaging food. This embodiment may also relate to a food packaging material. When the present film is used for packaging food, for example, the present film is formed into a bag shape, food is contained therein, and then the film is heat-sealed to obtain a package.
[0065] The present film can also be used as a lid material. In this case, for example, the present film (lid material) can be heat-sealed to a glass or resin container to seal the container and obtain a package. Examples of containers include cups and trays. EXAMPLES
[0066] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these. In the following, various measurements and evaluations of the film and its materials were performed as follows. Here, the flow direction of the film from the extruder is called the machine direction (MD), and the direction perpendicular to the machine direction is called the transverse direction or width direction (TD).
[0067] [Evaluation method] (1) Thickness According to JIS K7130 (1999), measurements were taken at 10 random points using a stand-type constant pressure thickness gauge, and the average value was taken as the film thickness.
[0068] (2) Tensile strength and tensile elongation at break The tensile strength and elongation at break in the MD and TD of the film were measured according to a method in accordance with JIS K7127 (1999). The measurement conditions were a pulling speed of 200 mm / min and an atmospheric temperature of 23°C. The measurement device used was a tensile tester (product name: Autograph AG-X, manufactured by Shimadzu Corporation). The test specimen was a rectangle cut from the film with a length of 50 mm in the measurement direction and a width of 10 mm. Both ends of the test specimen in the longitudinal direction were chucked with a chuck distance of 20 mm and pulled at a crosshead speed of 200 mm / min, and the tensile strength and elongation in the MD and TD were measured three times each, and the average values were calculated.
[0069] (3) Area ratio of the bumps The area ratio of foreign matter (lumps) occurring in the film was calculated using a digital microscope. First, the reflected field of view was observed with a ring light, and the brightness range of the foreign matter (lumps) was extracted from the brightness histogram of the observed image to determine the area of the foreign matter (lumps). The area ratio of the foreign matter (lumps) was calculated as a percentage by dividing the area of the foreign matter (lumps) by the observed area.
[0070] (4) Transparency (total light transmittance) The total light transmittance of the film was measured using a haze meter (NDH-7000II, manufactured by Nippon Denshoku Industries Co., Ltd.) according to the light transmittance measuring method described in JIS K7361-1 (1997).
[0071] (5) Antibacterial activity test Antibacterial performance was measured according to the antibacterial performance test described in JIS Z2801 (2012). Escherichia coli and Staphylococcus aureus were used as test bacteria. The antibacterial activity value was calculated from the obtained viable cell count and the viable cell count after incubation of the film without antibacterial agent using the following formula. Antibacterial activity value = log (number of viable bacteria after incubation on film without antibacterial agent) - log (number of viable bacteria after incubation on film with antibacterial agent) From the obtained antibacterial activity values, the antibacterial properties were judged to be good when the antibacterial activity value was 2 or more. The film obtained in Comparative Example 5 corresponds to the above-mentioned "film containing no antibacterial agent" and served as a control in the antibacterial performance test.
[0072] (6) pH of the film The pH of the film surface was measured as follows: After placing a water-soaked pH test paper in contact with the film surface and leaving it for 3 hours, the pH was measured by comparing the color of the pH test paper with a color sample.
[0073] [Example 1] Thermoplastic resin: Polyethylene resin (linear low-density polyethylene, ethylene / 1-butene = 93 / 7 (mass ratio), density 0.924 g / cm 3 The resin composition was mixed with 1,000g of ethyl alcohol (MFR 2.0g / 10min, melting point 123°C), tartaric acid was used as the organic acid, and glycerol was used as the sugar alcohol. They were dry blended so that the respective mass ratios were 92 mass%, 4 mass%, and 4 mass%, and melt-kneaded at a temperature of 200°C for 5 minutes using a tabletop melt-kneader. The melt-kneaded resin composition was then placed in a tabletop film-forming machine to obtain a film with a thickness of 40μm. The evaluation results of the obtained film are shown in Table 1.
[0074] [Example 2] A film having a thickness of 40 μm was produced in the same manner as in Example 1, except that the organic acid was changed to phytic acid and the mass ratios of the polyolefin resin, organic acid, and glycerol were 95 mass%, 1 mass%, and 4 mass%, respectively. The evaluation results of the obtained film are shown in Table 1.
[0075] [Example 3] A film having a thickness of 40 μm was produced in the same manner as in Example 1, except that the mass ratios of the polyolefin resin, the organic acid, and the glycerol were 88 mass%, 8 mass%, and 4 mass%, respectively. The evaluation results of the obtained film are shown in Table 1.
[0076] [Comparative Example 1] A film having a thickness of 40 μm was produced in the same manner as in Example 1, except that no sugar alcohol was used, dehydroacetic acid was used as the organic acid, and the mass ratio of the polyethylene resin to the organic acid was changed to 92 mass% and 8 mass%. The evaluation results of the obtained film are shown in Table 1.
[0077] [Comparative Example 2] A film having a thickness of 50 μm was produced in the same manner as in Comparative Example 1, except that sorbic acid was used as the organic acid. The evaluation results of the obtained film are shown in Table 1.
[0078] [Comparative Example 3] A film having a thickness of 50 μm was produced in the same manner as in Example 1, except that tartaric acid was used as the organic acid and the mass ratio of the polyethylene resin to the organic acid was changed to 99 mass% and 1 mass%, respectively. The evaluation results of the obtained film are shown in Table 1.
[0079] [Comparative Example 4] A film having a thickness of 50 μm was produced in the same manner as in Example 1, except that tartaric acid was used as the organic acid and the mass ratio of the polyethylene resin to the organic acid was changed to 96 mass% and 4 mass%, respectively. The evaluation results of the obtained film are shown in Table 1.
[0080] [Reference example 5] A film having a thickness of 40 μm was produced in the same manner as in Example 1, except that the organic acid and sugar alcohol were not used. The evaluation results of the obtained film are shown in Table 1.
[0081] [Table 1]
[0082] In the examples, the generation of foreign matter (lumps) was suppressed, and a film with excellent appearance was obtained. In the examples, the pH of the film surface was less than 6, and a film with excellent antibacterial properties was obtained. Furthermore, in the examples, the generation of foreign matter (lumps) was suppressed, and therefore the tensile elongation at break of the film was large. On the other hand, in Comparative Examples 1 and 2, the organic acid was thermally decomposed during the melt molding process, so the pH of the film surface was high at 7, and antibacterial properties were not exhibited. Also, in Comparative Examples 3 and 4, the organic acid remained, so the pH of the film surface was 6 or less, and although antibacterial properties were exhibited, foreign matter (lumps) were generated, and the foreign matter (lumps) made the film prone to breakage. [Industrial Applicability]
[0083] The thermoplastic resin film of the present invention has antibacterial properties, good appearance and high tensile elongation at break, and therefore can be suitably used for applications such as food packaging films, storage containers, building materials, miscellaneous goods and home appliances.
Claims
1. A film comprising a thermoplastic resin (A), an organic acid (B) and a sugar alcohol (C), the film having a surface pH of 6 or less.
2. The film according to claim 1, wherein the thermoplastic resin (A) has a melting point of 180°C or lower or a glass transition temperature of 180°C or lower.
3. The film according to claim 1 , wherein the thermoplastic resin (A) is a polyolefin resin.
4. 4. The film according to claim 3, wherein the polyolefin resin is at least one selected from the group consisting of polyethylene, polypropylene, and ethylene-vinyl acetate copolymer.
5. The film according to any one of claims 1 to 4, wherein the organic acid (B) is at least one selected from the group consisting of hydroxy acids and inositol phosphates.
6. The film according to any one of claims 1 to 4, wherein the organic acid (B) is at least one selected from the group consisting of tartaric acid and phytic acid.
7. The film according to any one of claims 1 to 4, wherein the content of the organic acid (B) is 0.1 to 10 mass% based on the total mass of the film.
8. The film according to any one of claims 1 to 4, wherein the sugar alcohol (C) is at least one selected from the group consisting of glycerin, glucitol, inositol and maltitol.
9. The film according to any one of claims 1 to 4, wherein the content of the sugar alcohol (C) is 0.05 to 30 mass% based on the total mass of the film.
10. The film according to any one of claims 1 to 4, which has a tensile elongation at break in at least one direction of 300% or more, as measured in accordance with JIS K7127 (1999).
11. The film according to any one of claims 1 to 4, having an antibacterial activity value of 2 or more as measured in accordance with JIS Z2801 (2012).
12. The film according to any one of claims 1 to 4, which is for food packaging.
13. A food packaging material comprising the film according to any one of claims 1 to 4.
Citation Information
Patent Citations
Antibacterial polyvinyl alcohol film, antibacterial polyvinyl alcohol composition, and preparation method of antibacterial polyvinyl alcohol film
CN109721906A
Tectosilicate-based antimicrobial agent
JP1991120204A
Laminate film for paper containers and laminated paper container
JP2022018713A
Transparent antibacterial film and method for manufacturing the same
JP2022165893A
Antibacterial film
JP2023004163A