Determination method of defect region

A non-destructive imaging method using scattered light and photoluminescence analysis effectively identifies I-rich regions on silicon substrates, enhancing defect detection accuracy and preventing defective substrates from being shipped.

JP2024140298AActive Publication Date: 2024-10-10SHIN ETSU HANDOTAI CO LTD

Patent Information

Application Number
JP2023051379
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10
Estimated Expiration
2043-03-28

AI Technical Summary

Technical Problem

Existing methods for determining defective regions on silicon single crystal substrates are destructive, fail to identify I-rich regions, and are inaccurate for defects smaller than the pixel size of two-dimensional detectors, leading to potential shipment of substrates with undesirable defects.

Method used

A non-destructive method using a two-dimensional detector to acquire images of defects through laser-irradiated scattered light and photoluminescence, analyzing the images for characteristic features like bright lines along specific crystal orientations, and calculating a defect index to determine I-rich regions based on threshold values.

Benefits of technology

Enables precise, non-destructive identification of I-rich regions, reducing the likelihood of shipping defective substrates by improving accuracy and efficiency in defect detection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

To provide a method which non-destructively and easily determines a defect region of a silicon single crystal substrate.SOLUTION: A determination method of an I-rich region of a silicon single crystal substrate includes: an image acquisition step which irradiates a surface of a silicon single crystal substrate having at least one mirror-polished (100) surface with laser light in a low-angle mode by a surface inspection device, detects scattered light and optical luminescence from a defect on the surface of the silicon single crystal substrate by a two-dimensional detector and acquires an image for the defect; an image determination step which determines whether the acquired image has features seen in the I-rich region; and a defect region determination step which calculates an index of the defect from the image when the image determination step determines that the image has the features seen in the I-rich region and determines a region whose index of the defect exceeds a predetermined threshold as the I-rich region.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for determining a defective region in a silicon single crystal substrate. [Background technology]

[0002] In recent years, with the advancement of devices, highly accurate control and evaluation of defect regions in semiconductor substrates (hereinafter, sometimes simply referred to as substrates) have become more important. If the defect regions in a substrate are different from the desired defect regions, it will cause device failure. Examples of such defect regions include regions with excess interstitial silicon (hereinafter, I-rich regions), regions where voids occur (hereinafter, V-rich regions), regions where oxygen precipitates are likely to be generated (hereinafter, OSF regions), regions with few defects (hereinafter, N regions), etc., and the types of defects present differ depending on the defect region. It is known that which defect regions are included varies depending on the manufacturing conditions of single crystals. Therefore, it is required to determine the defect regions of the substrate at the manufacturing stage of the substrate, and if undesirable crystal defects are included, to quickly feed back the information to the manufacturing process of the single crystal so that such defect regions are not generated.

[0003] As a technique for determining defect regions, for example, Patent Document 1 discloses a technique for revealing B-band regions and dislocation cluster regions of a silicon single crystal substrate by metal contamination and heat treatment.

[0004] Furthermore, Patent Document 2 discloses a technique for measuring the number and / or density of defects on the surface of a silicon single crystal substrate using a surface inspection device, and determining defective regions of the substrate from the number and / or density of defects.

[0005] Furthermore, as a method for evaluating defects, for example, Patent Document 3 discloses a technology in which multiple photodetectors installed at different angles are used to detect the intensity of scattered light caused by a defect, and the ratio of the scattered intensity is used to evaluate whether the defect is present on the surface or inside.

[0006] Moreover, Patent Document 4 discloses a technique for separately detecting adhering particles and concave defects using a surface inspection device having a dual-incident, dual-receiving light system.

[0007] Patent Document 5 discloses a technique for identifying the type of defect based on the ratio of light receiving intensities in a surface inspection device having multiple light receiving systems with different light receiving angles. By using this technique on a mirror-polished silicon single crystal substrate, defects can be classified into three groups: scratches or shallow pits, adhered particles or COP (Crystal Originated Particle), and internal defects near the surface.

[0008] Furthermore, some of the latest surface inspection equipment is equipped with a two-dimensional detector, which can capture images of scattered light and photoluminescence caused by defects, making it possible to identify scratches and stacking defects in epitaxial layers. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Patent Publication No. 2021-075403 [Patent Document 2] JP 2017-092400 A [Patent Document 3] JP 2015-070116 A [Patent Document 4] JP 2001-153635 A [Patent Document 5] WO01 / 027600 Summary of the Invention [Problem to be solved by the invention]

[0010] The method of revealing defective regions caused by etching or metal contamination, as typified by Patent Document 1, is destructive testing. Therefore, generally, a part of a substrate cut out from a crystal is sampled and inspected. However, with this method, the defective regions in most of the crystal are unknown. Therefore, if an undesirable defective region exists only in a part of the crystal, there is a problem that a substrate containing undesirable crystal defects may be shipped as a product.

[0011] Furthermore, the techniques described in Patent Documents 2 to 5 have the problem that it is difficult to determine I-rich regions.

[0012] Furthermore, it has not been confirmed whether the identification of defects using images acquired by a two-dimensional detector installed in a surface inspection device is effective for defects that depend on the defective area of ​​the substrate. In particular, there is a problem in that the shape of the defect cannot be directly identified from the image when the defect size is approximately the same as or smaller than the pixel size of the two-dimensional detector.

[0013] The present invention has been made in consideration of the above problems, and an object of the present invention is to provide a method for determining defective regions in a silicon single crystal substrate in a non-destructive and simple manner. [Means for solving the problem]

[0014] In order to solve the above problems, the method of determining an I-rich region in a silicon single crystal substrate of the present invention is a method characterized by including an image acquisition step of irradiating the surface of at least one silicon single crystal substrate having a mirror-polished (100) surface with laser light in a low-angle mode by a surface inspection device, detecting scattered light and photoluminescence from defects on the surface of the silicon single crystal substrate with a two-dimensional detector, and acquiring an image of the defects, an image judgment step of determining whether the acquired image has characteristics seen in an I-rich region, and a defect region judgment step of calculating a defect index from the image if it is judged in the image judgment step that the image has characteristics seen in an I-rich region, and judging a region in which the defect index exceeds a predetermined threshold to be an I-rich region.

[0015] In this method, the intensity distribution of scattered light and photoluminescence can be obtained by using a two-dimensional detector as the detector, and more information on scattered light and photoluminescence can be obtained than in the case of using other detectors that cannot obtain the intensity distribution, so that the defective area can be determined with high accuracy. Therefore, in this method, the defective area of ​​the substrate can be determined non-destructively and simply.

[0016] In addition, a first method for determining whether or not the image has a characteristic observed in the I-rich region in the image determination step includes: <011> It is preferable to judge that an emission line along the direction has the characteristics seen in an I-rich region.

[0017] In this way, on (100) <011> The long crystal defects are only present in the I-rich region, and the defect images show <011> If an emission line along this line is obtained, it can be easily determined that it has the characteristics seen in I-rich regions.

[0018] In the first method, it is preferable that the image of the defect is rotated so as to follow the crystal orientation of the silicon single crystal substrate before the judgment is made.

[0019] This method allows the defect image to be obtained even if the orientation of the original image does not match the crystal orientation of the substrate. <011> It is easy to determine whether the emission line is aligned along a direction.

[0020] Furthermore, when the judgment is made using the first method, it is preferable that the defect indicator is at least one of the number, density, and the proportion of defects determined to have characteristics seen in I-rich regions by the first method relative to the total number of defects determined to have characteristics seen in I-rich regions by the first method.

[0021] Such a method allows the defect index to be determined as a specific quantitative value. In particular, when density is used, it becomes possible to determine the defective area without depending on the area of ​​the range in which the determination is made. Furthermore, when the ratio of defects determined to have characteristics seen in I-rich regions to all defects is used, it becomes possible to determine the defective area without depending on the total number of defects detected by the surface inspection device. Furthermore, it is possible to combine the number of defects, density, and the ratio of defects determined to have characteristics seen in I-rich regions to all defects.

[0022] In addition, a second method for determining whether or not the defect has characteristics seen in the I-rich region in the image determination process preferably involves detecting scattered light and photoluminescence at a first low angle and a second high angle in the image acquisition process, and determining that the defect has characteristics seen in the I-rich region when an image of the defect is obtained only in the scattered light and photoluminescence at the first angle.

[0023] With this method, some of the crystal defects in the I-rich region emit almost no scattered light or photoluminescence at high angles, so if scattered light and photoluminescence are detected at a first angle, which is a low angle, but not at a second angle, which is a high angle, it can be easily determined that the region has the characteristics seen in an I-rich region.

[0024] Furthermore, when the judgment is made using the second method, it is preferable that the defect index is the proportion of defects that are judged to have characteristics seen in I-rich regions using the second method to all defects.

[0025] With this method, first, the defect index can be determined as a specific quantitative value. Furthermore, if other defects (particles or some V-rich defects) are detected only at one of the angles, it is possible to make a more accurate judgment based on the ratio of defects that are judged to have characteristics seen in the I-rich region to the total number of defects, rather than judging based on the number or density of defects.

[0026] In the image evaluation step, it is preferable that the image is subjected to at least one image processing step of trimming, pseudo-colorization, and binarization before being evaluated.

[0027] Such a method can provide effects such as reducing noise contained in the image and emphasizing specific features of the image.

[0028] In addition, it is preferable that the threshold value used to determine the I-rich region is determined in advance from the defect index of an image determined to have characteristics seen in the I-rich region by acquiring an image under the same conditions as in the image acquisition step for a silicon single crystal substrate having a mirror-polished (100) surface with known defect regions, and judging the image in the same manner as in the image judgment step.

[0029] With this method, the image is acquired and judged under the same conditions when calculating the defect index from the defect image and when determining the threshold value, so that the I-rich region can be judged with high accuracy.

[0030] The silicon single crystal substrate is preferably mirror-polished and then cleaned.

[0031] According to this method, since particles adhering to the surface of the substrate are removed by cleaning, the accuracy of determining defective areas can be improved.

[0032] In addition, in the image acquiring step, it is preferable that the acquired images are images of a plurality of defects randomly extracted from the detected defects.

[0033] With this method, even if there are a large number of defects, the image judgment can be completed in a short time.

[0034] Furthermore, it is preferable that the defect area determination step determines a defect area in a predetermined range of the silicon single crystal substrate, and that the predetermined range is an arbitrary area that contains a number of defects required for determining the defect area.

[0035] With this method, the number of defects required to determine the defective area is included in the predetermined range, so that the defective area can be determined reliably. Effect of the Invention

[0036] By using the method for determining a defective region in a substrate of the present invention, it is possible to non-destructively and simply determine whether or not a defective region in a substrate is an I-rich region. [Brief description of the drawings]

[0037] [Figure 1] 1 is a flowchart illustrating an example of the first embodiment of the present invention. [Diagram 2] 10 is a flowchart illustrating an example of a second embodiment of the present invention. [Diagram 3] 1 is a schematic diagram showing an example of a surface inspection device according to a first embodiment of the present invention. [Figure 4] FIG. 4 is a schematic diagram showing an example of a surface inspection device according to a second embodiment of the present invention. [Diagram 5] The image of the defect obtained by the two-dimensional detector of the surface inspection device <011> FIG. 13 is a diagram showing an example of an image of bright lines along the line. [Figure 6] FIG. 2 is a diagram showing an example of an image including an image of a defect acquired by a two-dimensional detector that detects scattered light and photoluminescence at a first angle, which is a low angle, of a surface inspection device. [Figure 7] FIG. 13 is a diagram showing an example of an image not including an image of a defect, acquired by a two-dimensional detector that detects scattered light and photoluminescence at a second angle, which is a high angle, of a surface inspection device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0038] The present invention will be described below with reference to the preferred embodiments, but the present invention is not limited thereto.

[0039] [First embodiment] FIG. 3 shows an example of a surface inspection apparatus for determining a defective area on a substrate according to the first embodiment of the present invention.

[0040] As shown in Figure 3, this surface inspection device 11 is equipped with a laser light irradiation means 2 that irradiates the surface of the substrate (silicon single crystal substrate) W to be evaluated with laser light having a wavelength of 266 nm in a low-angle mode, a two-dimensional detector 3 that detects scattered light and photoluminescence produced by defects D, etc. on the substrate surface from the irradiated laser light, and a moving means 4 that scans the substrate W with the laser light.

[0041] The two-dimensional detector 3 can obtain one image for each defect by detecting the scattered light and photoluminescence emitted at a specific angle. The two-dimensional detector 3 can be, for example, a CCD image sensor.

[0042] The radiation angle of the scattered light and photoluminescence detected by the two-dimensional detector 3 is preferably such that the scattered light and photoluminescence emitted at a low angle is detected, since smaller defects can be detected when the scattered light and photoluminescence are detected at a low angle.

[0043] The moving means 4 may be any means capable of scanning the substrate surface with laser light by appropriately moving the substrate W, and may be, for example, an R-θ stage, but is not particularly limited thereto.

[0044] FIG. 1 shows an example of a method for determining a defective area according to a first embodiment of the present invention.

[0045] (1st step: image acquisition step) First, a silicon single crystal substrate with a mirror-polished (100) surface for determining defect regions is prepared. The surface of the substrate is mirror-polished. After mirror-polishing the substrate, it may be cleaned. Cleaning can remove particles adhering to the substrate surface. Because particle adhesion does not depend on defect regions, removing the particles improves the accuracy of determining I-rich regions.

[0046] Next, a surface of at least one mirror-polished silicon single crystal substrate W having a (100) surface is irradiated with laser light in low-angle mode by a surface inspection device 11, and scattered light and photoluminescence from a defect D on the surface of the silicon single crystal substrate are detected by a two-dimensional detector 3 to obtain an image of the defect D. In the low-angle mode, the surface of the substrate is irradiated with laser light at a low angle θ in In this mode, the laser light is irradiated at a resolution of 1000 nm. The surface inspection device having a two-dimensional detector may be, for example, a Surfscan SP7 manufactured by KLA-Tencor. The number of pixels per image to be acquired is preferably 32×32 or more, and may be, for example, 96×96 pixels. With such a number of pixels, the entire image of the defect can be acquired even if the image of the defect is large or is offset from the center of the image.

[0047] The acquired images may be images of all detectable defects contained in the substrate, but are preferably images of a plurality of defects randomly selected from the detectable defects. The number of defects to be extracted in the case of random extraction may be, for example, 1000, but is not particularly limited as long as the number is sufficient to determine the defective area. By acquiring images of a plurality of defects randomly selected, image determination can be performed in a short time even when there are a large number of defects.

[0048] In addition, the acquired image may be subjected to image processing as necessary. It is preferable to perform at least one of image processing such as trimming, pseudo-colorization, and binarization on the image before making the judgment. With such a method, it is possible to obtain effects such as reducing noise contained in the image and emphasizing specific features of the image.

[0049] For example, by applying a pseudo-color to the image according to the intensity ratio, the difference in intensity is emphasized. Therefore, when a human judges the characteristics of an image used to judge a defective area, it is preferable to use an image that has been pseudo-colored.

[0050] Furthermore, when the moving means 4 is an R-θ stage, the substrate is rotated during measurement, so the orientation of the image changes with the rotation of the substrate, and the orientation of the original image does not match the crystal orientation of the substrate. However, in this embodiment, defect coordinates and images are acquired for each defect, so that a specific crystal orientation of the substrate can be aligned in the same direction for all images by rotating the image at an appropriate angle according to the defect coordinates. Therefore, when using such a surface inspection device, it is preferable to perform a rotation process on the acquired images. The crystal orientation to which the images are aligned can be, for example, <011> It can be said that:

[0051] (Second process: image judgment process) Next, for each image, the defect image is compared to the I-rich region as shown in Figure 5 to determine whether the image has the characteristics found in the I-rich region. <011> The determination may be made by a person or automatically by a computer, and is not particularly limited.

[0052] (Third step: Defect area determination step) Next, the image of the defect in the range to be judged is <011> The number of defects determined to be emission lines along the <011> At least one of the ratios of defects that are bright lines along the line is calculated as an indicator of the defect and compared with a predetermined threshold. If the calculation result is equal to or greater than the threshold, it is determined that the defect region in the above range of the substrate is an I-rich region. Similarly, if the calculation result is less than the threshold, it is determined that the defect region in the above range of the substrate is not an I-rich region.

[0053] The inventors investigated the defects and particles in each defect region and found that defects with the above characteristics were only found in the I-rich region. In the I-rich region, there are crystal defects such as clusters of interstitial silicon aggregates, stacking faults, and dislocations caused by these. The defects may have a shape along an energetically stable direction, and on (100), this shape is, for example, <011> The stable shape differs depending on the type of defect, and in defect regions other than the I-rich region, where there is little interstitial silicon, crystal defects with similar shapes do not form.

[0054] Therefore, the silicon single crystal substrate <011> Long, thin defects along the line that are large enough to be detected by a two-dimensional detector are only found in I-rich regions. Therefore, regions that contain defects with such characteristics can be determined to be I-rich regions.

[0055] The range in which the judgment is made (predetermined range) can be, for example, the entire surface of the substrate, or a range at a certain distance from the center of the substrate, or half the area of ​​the substrate, but is not particularly limited as long as the range contains a sufficient number of defects to judge the defective areas.

[0056] The threshold value used to determine the I-rich region is determined by acquiring an image of a given area of ​​a silicon single crystal substrate with a mirror-polished (100) surface with a known defect region under the same conditions as the substrate for which the defect region is to be determined, and <011> The defect image is then processed to determine whether the defect is a bright line along the line of the <011> The number, density, and defect images for all defects determined to be emission lines along <011> The percentage of defects that are emission lines along the

[0057] For example, for a substrate that is known to contain I-rich regions, the defect image <011> For a substrate that has a defect determined to be an emission line along the line and is known not to contain an I-rich region, the defect image <011> If there are no defects that are determined to be emission lines along the line, the threshold can be set to the number of defects. <011> Considering the possibility of defects caused by processing parallel to the direction, if the threshold is set to 2 or more, it is possible to prevent regions other than I-rich regions from being erroneously determined as I-rich regions. However, if the threshold is set too large, there is a risk that regions that should be determined as I-rich regions will not be determined as I-rich regions, so in this example, it is preferable to set the threshold to 2.

[0058] The threshold value used for the judgment is set so that the image of the defect is large enough to exclude the influence of the area of ​​the judgment range. <011> For example, the density threshold for a defect count of 2 defects over the entire surface of a 300 mm diameter substrate is 3×10 -3 pieces / cm 2 It is.

[0059] [Second embodiment] FIG. 4 shows an example of a surface inspection apparatus for determining a defective area on a substrate according to the second embodiment of the present invention.

[0060] As shown in Figure 4, this surface inspection device 12 is equipped with a laser light irradiation means 2 that irradiates the surface of the substrate W to be evaluated with laser light having a wavelength of 266 nm in a low-angle mode, a two-dimensional detector group 30 for detecting scattered light and photoluminescence produced by defects D, etc. on the substrate surface from the irradiated laser light, and a moving means 4 for scanning the substrate W with the laser light.

[0061] The two-dimensional detector group 30 detects an image at a first angle θ outL A two-dimensional detector 31 that can obtain one image per defect by detecting scattered light and photoluminescence emitted toward the defect and a second angle θ outH The two-dimensional detector group 30 includes a two-dimensional detector 32 that can obtain one image per defect by detecting scattered light and photoluminescence emitted toward the defect. The two-dimensional detector group 30 can obtain the same number of images per defect as the number of two-dimensional detectors that make up the two-dimensional detector group 30.

[0062] This allows images to be acquired from scattered light and photoluminescence scattered in different directions, increasing the amount of information available as a basis for judgment and improving the accuracy of judging defective areas.

[0063] The moving means 4 can be the same as the moving means 4 of the surface inspection device 11 used in the first embodiment.

[0064] FIG. 2 shows an example of a method for determining a defective area according to the second embodiment of the present invention.

[0065] (1st step: image acquisition step) First, a silicon single crystal substrate with a mirror-polished (100) surface for determining defect regions is prepared. The surface of the substrate is mirror-polished. After mirror-polishing the substrate, it may be cleaned. Cleaning can remove particles adhering to the substrate surface. Because particle adhesion does not depend on defect regions, removing the particles improves the accuracy of determining I-rich regions.

[0066] The substrate is then measured by a surface inspection device 12 having a two-dimensional detector group 30, and images of each defect are obtained, including defect coordinates and images at a first angle, which is a low angle, and a second angle, which is a high angle. The surface inspection device having a two-dimensional detector group may be, for example, a Surfscan SP7 manufactured by KLA-Tencor. The number of pixels per image to be obtained is preferably 32×32 or more, and may be, for example, 96×96 pixels. With such a number of pixels, the entire image of the defect can be obtained even if the image of the defect is large or is offset from the center of the image.

[0067] By separately detecting the scattered light and photoluminescence emitted at multiple angles and acquiring multiple images, it is possible to obtain the intensity distribution of the scattered light and photoluminescence emitted in different directions, thereby increasing the amount of information available as a basis for judgment and improving the accuracy of judging defective areas.

[0068] The acquired images may be images of all detectable defects contained in the substrate, but are preferably images of a plurality of defects randomly selected from the detectable defects. The number of defects to be extracted in the case of random extraction may be, for example, 1000, but is not particularly limited as long as the number is sufficient to determine the defective area. By acquiring images of a plurality of defects randomly selected, image determination can be performed in a short time even when there are a large number of defects.

[0069] In addition, the acquired image may be subjected to image processing as necessary. For example, the difference in intensity may be emphasized by pseudo-coloring according to the intensity ratio. Therefore, when the image features used to determine the defective area are determined manually, it is preferable to use the pseudo-colored image.

[0070] (Second process: image judgment process) Next, it is determined from the image of each defect whether an image of the defect as shown in Fig. 6 obtained by two-dimensional detector 31 that detects scattered light and photoluminescence radiated at a first angle, which is a low angle, cannot be obtained by two-dimensional detector 32 that detects scattered light and photoluminescence radiated at a second angle, which is a high angle, as shown in Fig. 7. The determination may be made by a person or automatically using a computer, and is not particularly limited.

[0071] (Third step: Defect area determination step) Next, the ratio of the number of defects in the range to be determined, whose images are acquired by the first 2D detector 31 at a low angle but not by the second 2D detector 32 at a high angle, to the total number of defects in the range to be determined is calculated as a defect index. If the calculation result is equal to or greater than a threshold, it is determined that the defect area in the range of the substrate is an I-rich area. Similarly, if the calculation result is less than the threshold, it is determined that the defect area in the range of the substrate is not an I-rich area.

[0072] The angular distribution of the intensity of the scattered light and photoluminescence depends on, for example, the shape of the defect. As described above, the shape of the crystal defect varies depending on the defect region, but the inventor's investigation has revealed that the I-rich region has a higher proportion of crystal defects with shapes that do not emit scattered light and photoluminescence at the second angle, which is a high angle, than other defect regions.

[0073] Therefore, defects whose images are acquired by the low-angle first-angle two-dimensional detector 31 but cannot be acquired by the high-angle second-angle two-dimensional detector 32 are detected with high frequency only in I-rich regions. Some defects and particles outside the I-rich regions also exhibit these characteristics, but their proportion is significantly lower than that of the I-rich regions, so a region where the proportion of defects having these characteristics to all defects exceeds a predetermined appropriate threshold can be determined to be an I-rich region.

[0074] The range for which the judgment is made can be, for example, the entire surface of the substrate, or a range at a certain distance from the center of the substrate, or half the area of ​​the substrate, but is not particularly limited as long as the range contains a sufficient number of defects to judge the defective areas.

[0075] The threshold value used to determine the I-rich region can be determined in advance from the ratio of the number of defects for which it is determined that the image of the defect acquired by two-dimensional detector 31 at a first angle, which is a low angle, under the same conditions as the substrate for which the defect region is to be determined, and the image of the defect acquired by two-dimensional detector 31 at a second angle, which is a high angle, under the same conditions, cannot be obtained by two-dimensional detector 32, relative to the total number of defects within the range.

[0076] For example, the threshold value can be any value between the percentage of defects for which an image of a defect acquired by two-dimensional detector 31 at a low first angle for a substrate known in advance to contain I-rich regions is determined to be incapable of being acquired by two-dimensional detector 32 at a high second angle, and the percentage of defects for which an image of a defect acquired by two-dimensional detector 31 for a substrate known in advance to not contain I-rich regions is determined to be incapable of being acquired by two-dimensional detector 32.

[0077] Furthermore, the inventors' investigation revealed that, for defects determined to be adhered particles in electron microscope images, the percentage of defects determined to be images of defects obtained by the low first angle two-dimensional detector 31 that cannot be obtained by the high second angle two-dimensional detector 32 was less than 4%. Therefore, when there is a possibility of adhered particles, the threshold value is preferably at least 4% or more, and more preferably 5% or more.

[0078] Furthermore, the present invention can be applied not only to mirror-polished silicon single crystal substrates and those that have been cleaned, but also to substrates that have been subjected to a defect area revealing process such as heat treatment or repeated cleaning and those that have been cleaned. In such cases, it is preferable that the same revealing process is performed on the substrate for determining the defect area judgment criteria and the substrate for judging the defect area. This can eliminate the influence of differences in revealing processes on the judgment of the defect area.

[0079] Although the first and second embodiments have been described above, the present invention is not limited to these embodiments. For example, the determination of an I-rich region can be performed by combining the first and second embodiments. By using a combination of multiple features, it is possible to determine a defective region with higher accuracy.

[0080] In addition, by using a two-dimensional detector as the detector, it is possible to obtain the intensity distribution of scattered light and photoluminescence, and since more information on scattered light and photoluminescence can be obtained than when a normal detector is used, it is possible to determine the defective area with high accuracy. With this method, it is possible to determine the defective area of ​​the substrate non-destructively by a process similar to the surface inspection generally performed before the shipment of the substrate.

[0081] This makes it possible to increase the number of substrates for which defect regions are to be determined, compared to when defect regions are determined by destructive testing, and greatly reduce the possibility that substrates containing undesirable crystal defects will be shipped as products. It is also possible to perform 100% substrate inspection, making it possible to prevent substrates containing undesirable crystal defects from being shipped as products.

[0082] The image used for the judgment can be one acquired from one substrate. In addition, the image can be acquired from a plurality of substrates cut from adjacent positions of a single crystal. Since substrates cut from adjacent positions of a single crystal show almost the same defect area distribution, such a method increases the number of defect images used for the judgment, and makes it possible to judge the defect areas even when the number of defects per substrate is very small.

[0083] In addition, the images used for the judgment can be acquired from the same substrate before and after cleaning. In this case, defects occurring at the same location before and after cleaning can be determined not to be due to particles. By using only images acquired from defects detected both before and after cleaning, the influence of both particles originally attached to the substrate surface and particles newly attached by cleaning can be reduced, improving the accuracy of judging the defective area.

[0084] Also, whether an image has a feature frequently found in the I-rich region can be determined by a person. Alternatively, whether an image has such a feature can be determined by a computer based on the pixel values ​​of the image. Alternatively, whether an image or a processed image has such a feature can be determined by machine learning. Such a method can reduce errors due to human intervention and can also reduce the time required for determination.

[0085] In addition, the range of the substrate for which the defect area is determined in the defect area determination step can be, for example, the entire surface of the substrate, a range with a fixed distance from the center of the substrate, or a half area of ​​the substrate, but is not particularly limited as long as the range includes a sufficient number of defects for determining the defect area. By setting the range of the substrate to the entire surface of the substrate, it is possible to determine the defect area of ​​the entire substrate. Alternatively, by setting the range of the substrate to a range with a fixed distance from the center of the substrate, it is possible to determine the defect area of ​​an appropriate range even if the defect areas are distributed concentrically from the center of the substrate. Alternatively, by setting the range of the substrate to a half area of ​​the substrate, it is possible to determine the defect area in a short time even if the number of defects present on the surface of the substrate is extremely large. EXAMPLES

[0086] The present invention will now be described more specifically with reference to examples.

[0087] [Example 1] The present invention will be further described below with reference to examples. However, these examples are given for illustrative purposes and should not be construed as limiting.

[0088] First, in order to determine the threshold value used to identify the I-rich region, a cleaned silicon single crystal substrate with a diameter of 300 mm, which was mirror-polished and had a known defect region, and which was manufactured using the Czochralski method, was prepared.

[0089] Next, the entire surface of the substrate was measured using a surface inspection device (SP7, Oblique mode (low angle mode incidence), 15 nmUp), and images were obtained for each defect by detecting the scattered light and photoluminescence emitted at low angles to the incident light. A schematic diagram of the surface inspection device is shown in Figure 3.

[0090] This image is taken from a silicon single crystal substrate. <011> The image is rotated so that the orientation is 12 o'clock, and for each image, the image of the defect is <011> We determined whether the emission lines were aligned along the direction.

[0091] Next, images of defects were taken for both the I-rich and non-I-rich regions of the substrate. <011> The number of defects, which are bright lines along the direction, was found to be 3 and 0, respectively. From this, the threshold value was determined to be a density of 3×10, which corresponds to the presence of two defects on the entire surface of a substrate with a diameter of 300 mm. -3 pieces / cm 2 and silicon <011> We decided to determine that a region where the density of defects, which are bright lines along the direction, exceeds a threshold value is an I-rich region.

[0092] Next, as samples for determining defect regions, two cleaned mirror-polished silicon single crystal substrates with a diameter of 300 mm, which had been manufactured using the Czochralski method under different conditions, were prepared and designated Substrate A and Substrate B, respectively.

[0093] These were measured in the same way as the previously described substrates with known defect areas, and images were obtained. <011> Rotate so that the direction is 12 o'clock. <011> The density of the emission lines along the directions was found to be 1.7×10 -2 pieces / cm 2 and 0 / cm 2 From this, it was determined that substrate A was an I-rich region, and substrate B was not an I-rich region.

[0094] For substrate A and substrate B, each defect was observed with a scanning electron microscope based on the defect coordinates. As a result, defects specific to I-rich regions were observed over the entire surface of substrate A, while no defects specific to I-rich regions were observed in substrate B. This confirmed that substrate A was an I-rich region over the entire surface, while substrate B did not include an I-rich region. This demonstrated that the determination of I-rich regions according to the present invention is effective.

[0095] [Example 2] First, in order to determine the threshold value used for judging the I-rich region, a substrate with a known defect region used for determining the threshold value in Example 1 was prepared.

[0096] Next, the entire surface of the substrate was measured using a surface inspection device (SP7, Oblique mode (low angle mode incidence), 15 nmUp), and for each defect, an image was obtained by detecting the scattered light and photoluminescence emitted at a first angle, which is a low angle, relative to the incident light (low angle image), and an image was obtained by detecting the scattered light and photoluminescence emitted at a second angle, which is a high angle, relative to the incident light (high angle image). A schematic diagram of the surface inspection device is shown in Figure 4.

[0097] For each defect detected, it was determined whether the low angle image yielded an image of the defect and the high angle image did not yield an image of the defect.

[0098] Next, the percentage of defects for which images were captured in low-angle images but not in high-angle images was calculated for the total number of defects in each area for both the I-rich area and other areas of the substrate, and the results were 31% and 0.04%, respectively. Based on this, the threshold was set at 10% between these two values, and an area was determined to be an I-rich area if the percentage of defects for which images could be captured by the 2D detector with the first low-angle light-receiving angle but images could not be captured by the 2D detector with the second high-angle light-receiving angle exceeded the threshold.

[0099] Next, as samples for determining defective areas, the substrates A and B used in Example 1 before observation with an electron microscope were prepared.

[0100] These were measured in the same way as the substrates with known defect areas, and low-angle and high-angle images were obtained. For each defect on each substrate, the percentage of defects for which an image of the defect was obtained in the low-angle image but not in the high-angle image was calculated, and the percentages were 35% and 0.1%, respectively. From this, it was determined that substrate A was in an I-rich region, and substrate B was not in an I-rich region.

[0101] The results of the determination were consistent with those shown in Example 1. Therefore, it was shown that the determination of the I-rich region according to the present invention was effective in Example 2 as well as in Example 1. The results of the determination of Substrate A are shown in Table 1.

[0102] [Table 1]

[0103] [Comparative Example 1] As a comparative example, an example in which an image was not acquired was examined. Substrate A and substrate B used in Example 1 before observation with an electron microscope were measured with a surface inspection device (SP7, Oblique mode, 15 nmUp), and scattered light and photoluminescence emitted at a first angle, which is a low angle, with respect to the incident light, and scattered light and photoluminescence emitted at a second angle, which is a high angle, with respect to the incident light were detected, and the number of defects, defect density, and coordinates of each defect were acquired without acquiring an image. The defective area of ​​the substrate was determined from the number of defects, defect density, and defect map. As a result, it was found that neither substrate was in the N region based on the number of defects and defect density, but further defective area determination was not possible.

[0104] The present invention includes the following aspects. [1]: A method for determining an I-rich region in a silicon single crystal substrate, comprising: an image acquisition step of irradiating the surface of at least one silicon single crystal substrate having a mirror-polished (100) surface with laser light in a low-angle mode by a surface inspection device, detecting scattered light and photoluminescence from defects on the surface of the silicon single crystal substrate by a two-dimensional detector, and acquiring an image of the defects; an image judgment step of determining whether the acquired image has characteristics seen in an I-rich region; and a defect region judgment step of calculating a defect index from the image when it is judged in the image judgment step that the image has characteristics seen in an I-rich region, and judging a region in which the defect index exceeds a predetermined threshold to be an I-rich region. [2]: A first method for determining whether or not the image of the defect has a characteristic observed in the I-rich region in the image determination step is to: <011> The method for determining an I-rich region in a silicon single crystal substrate according to the above-mentioned [1], characterized in that an emission line along a direction is determined to have characteristics seen in an I-rich region. [3]: The method for determining an I-rich region in a silicon single crystal substrate according to the above-mentioned [2], characterized in that in the first method, the image of the defect is rotated so as to follow the crystal orientation of the silicon single crystal substrate before the determination is made. [4]: The method for determining an I-rich region in a silicon single crystal substrate described in [2] or [3] above, characterized in that when the determination is made by the first method, the defect indicator is at least one of the number, density, and proportion of defects determined by the first method to have characteristics seen in I-rich regions to the total number of defects determined by the first method to have characteristics seen in I-rich regions. [5]: A second method for determining whether or not the defect has characteristics seen in the I-rich region in the image determination step is the method for determining an I-rich region in a silicon single crystal substrate described in [1] above, characterized in that in the image acquisition step, scattered light and photoluminescence are detected at a first low angle and a second high angle, and if an image of a defect is obtained only in the scattered light and photoluminescence at the first angle, it is determined that the defect has characteristics seen in an I-rich region. [6]: The method for determining an I-rich region in a silicon single crystal substrate described in [5] above, wherein, when the determination is made by the second method, the defect index is the ratio of defects determined to have characteristics observed in an I-rich region by the second method to the total number of defects. [7]: The method for determining an I-rich region in a silicon single crystal substrate according to any one of [1] to [6] above, characterized in that in the image determination step, the image is subjected to at least one image processing step of cropping, pseudocolorization, and binarization before being determined. [8]: The method for determining an I-rich region in a silicon single crystal substrate according to any one of [1] to [7] above, characterized in that the threshold value used for determining the I-rich region is determined in advance from an index of defects in an image determined to have characteristics seen in the I-rich region by acquiring an image under the same conditions as in the image acquisition step for a silicon single crystal substrate having a mirror-polished (100) surface with known defect regions, and judging the image in the same manner as in the image judgment step. [9]: The method for determining an I-rich region of a silicon single crystal substrate according to any one of [1] to [8] above, wherein the silicon single crystal substrate is mirror-polished and then cleaned.

[10] : The method for determining I-rich regions in a silicon single crystal substrate described in any one of [1] to [9] above, characterized in that in the image acquisition process, the images acquired are images of a plurality of defects randomly extracted from the detected defects.

[11] : The method for determining an I-rich region in a silicon single crystal substrate described in any one of [1] to

[10] above, characterized in that the defect region determination step determines a defect region in a predetermined range of the silicon single crystal substrate, and the predetermined range is an arbitrary region that contains the number of defects required to determine the defect region.

[0105] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and any configuration that is substantially the same as the technical idea described in the claims of the present invention and that provides similar effects is included in the technical scope of the present invention. [Explanation of symbols]

[0106] 11...surface inspection device, 2...laser light irradiation means, 3...two-dimensional detector, 4...moving means, 12...surface inspection device equipped with two two-dimensional detectors, 30...two-dimensional detector group, 31...two-dimensional detector for detecting scattered light and photoluminescence at a first angle, which is a low angle, 32...two-dimensional detector for detecting scattered light and photoluminescence at a second angle, which is a high angle. D: defect; W: substrate (single crystal silicon substrate).

Claims

1. A method for determining an I-rich region of a silicon single crystal substrate, comprising: an image acquisition step of irradiating a surface of at least one silicon single crystal substrate having a mirror-polished (100) surface with laser light in a low-angle mode by a surface inspection device, detecting scattered light and photoluminescence from defects on the surface of the silicon single crystal substrate by a two-dimensional detector, and acquiring an image of the defects; an image judgment step of judging whether the acquired image has characteristics seen in an I-rich region; and a defect region judgment step of calculating a defect index from the image when it is judged in the image judgment step that the image has characteristics seen in an I-rich region, and judging a region in which the defect index exceeds a predetermined threshold value to be an I-rich region.

2. The method for determining an I-rich region of a silicon single crystal substrate as described in claim 1, characterized in that a first method for determining whether or not the defect has characteristics seen in the I-rich region in the image determination process is to determine that the defect has characteristics seen in the I-rich region if the image of the defect acquired in the image acquisition process is an emission line along the <011> direction.

3. 3. The method for determining an I-rich region of a silicon single crystal substrate according to claim 2, wherein in the first method, the image of the defect is rotated so as to follow the crystal orientation of the silicon single crystal substrate before the determination is made.

4. The method for determining an I-rich region of a silicon single crystal substrate as described in claim 2, characterized in that, when the determination is made using the first method, the defect indicator is at least one of the number, density, and proportion of defects determined by the first method to have characteristics seen in an I-rich region to all defects, which are determined by the first method to have characteristics seen in an I-rich region.

5. A second method for determining whether or not the substrate has characteristics seen in the I-rich region in the image determination step comprises detecting scattered light and photoluminescence at a first angle, which is a low angle, and a second angle, which is a high angle, in the image acquisition step, and determining that the substrate has characteristics seen in the I-rich region when an image of the defect is obtained only in the scattered light and photoluminescence at the first angle. This is the method for determining an I-rich region in a silicon single crystal substrate as described in claim 1.

6. The method for determining an I-rich region of a silicon single crystal substrate as described in claim 5, characterized in that, when the determination is made using the second method, the defect index is the ratio of defects determined to have characteristics seen in an I-rich region by the second method to all defects.

7. 2. The method for determining an I-rich region of a silicon single crystal substrate according to claim 1, wherein in the image determination step, the image is subjected to at least one image processing step of trimming, pseudo-colorization, and binarization before the determination is made.

8. The method for determining an I-rich region of a silicon single crystal substrate, as described in claim 1, characterized in that the threshold value used for determining the I-rich region is determined in advance from an index of a defect in an image determined to have characteristics seen in the I-rich region by acquiring an image under the same conditions as in the image acquisition process for a silicon single crystal substrate having a mirror-polished (100) surface with known defect regions, and determining the image in the same manner as in the image determination process.

9. 2. The method for determining an I-rich region of a silicon single crystal substrate according to claim 1, wherein the silicon single crystal substrate is mirror-polished and then cleaned.

10. 2. The method for determining an I-rich region in a silicon single crystal substrate according to claim 1, wherein in the image acquisition step, the images acquired are images of a plurality of defects randomly extracted from the detected defects.

11. The method for determining an I-rich region of a silicon single crystal substrate according to any one of claims 1 to 10, characterized in that the defect region determination step determines a defect region in a predetermined range of the silicon single crystal substrate, and the predetermined range is any region that contains the number of defects required to determine the defect region.

Citation Information

Patent Citations

  • Silicone single crystal, its production and its evaluation

    JP1999106282A

  • Inspection device, inspection method, and manufacturing method of semiconductor device

    JP2009099820A

  • Method for determining defective region

    JP2017092400A

  • Method for determining defect region of silicon single crystal and method for manufacturing silicon single crystal

    JP2021075403A

  • Method for determining defect region

    US20180312994A1

Cited By

  • Determination method for defect region of silicon single-crystal substrate

    JP2025112209A

  • Method for determining defect regions in silicon single crystal substrates

    JP7925401B2

  • Method for determining defect region of silicon single-crystal substrate

    WO2025154521A1