Substrate with beta-type gallium oxide film and method for producing same

By using oxygen and ozone plasma treatment technology on Si or GaN single crystal substrates, the β-type gallium oxide film is grown at low temperature, solving the growth problems on heterogeneous materials, and achieving high-quality and fast-growing β-type gallium oxide films , suitable for industrial applications.

CN118922920APending Publication Date: 2024-11-08NAT UNIV CORP TOKAI NAT HIGHER EDUCATION & RES SYST

Patent Information

Application Number
CN202380029909.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-28
Filing Date
2023-03-20
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The prior art is difficult to grow high-quality β-type gallium oxide films on single crystal substrates of heterogeneous materials, especially due to the problems of high growth temperature, slow speed, insufficient crystallinity and flatness.

Method used

By using a mixed gas plasma treatment containing oxygen and ozone on a Si single crystal substrate or a gallium nitride single crystal substrate, oxygen-constituting particles are formed, and β-type gallium oxide film is epitaxially grown under conditions below 600°C, single-type gallium oxide film is used Axial orientation growth technology avoids the use of buffer layers of heterogeneous materials.

Benefits of technology

The growth of high-quality, uniaxially oriented β-type gallium oxide film on a single crystal substrate of heterogeneous materials is achieved, which reduces the growth temperature, increases the growth rate, and obtains good crystallinity and flatness, which is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118922920A_ABST
    Figure CN118922920A_ABST
Patent Text Reader

Abstract

The present invention pertains to a substrate with a beta-type gallium oxide film, the substrate having a Si single crystal substrate and a beta-type gallium oxide film provided on the Si single crystal substrate, the beta-type gallium oxide film being uniaxially oriented.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a substrate with a β-type gallium oxide film, and more particularly to a substrate with a β-type gallium oxide film, wherein the β-type gallium oxide film is provided on a Si single crystal substrate or a gallium nitride single crystal substrate. In addition, the present invention also relates to a method for manufacturing a substrate with a β-type gallium oxide film, wherein the β-type gallium oxide film is provided on a single crystal substrate. Background Art

[0002] Gallium oxide (Ga2O3) has various crystal structures such as α-type, β-type, γ-type, δ-type, and ε-type. Among them, β-type gallium oxide (β-type Ga2O3) is a stable phase at low temperature and normal pressure. It is known that the crystal system of β-type gallium oxide is monoclinic, and the lattice constants are as follows: the a-axis, i.e., the

[100] axis, is The b axis, i.e. the

[010] axis, is The c-axis, i.e. the

[001] axis, is The angle (β) between the a-axis and the c-axis is 103.83°. The band gap of β-type gallium oxide is about 4.5eV to 4.9eV, which is larger than the band gap of 4H-SiC substrate 3.26eV and the band gap of GaN 3.39eV. Therefore, β-type gallium oxide is expected to be a semiconductor material with high dielectric breakdown strength.

[0003] For example, Patent Document 1 discloses a technique in which a gallium element is supplied from a first cell 13a inside a vacuum chamber 10 to a β-type gallium oxide substrate 2, and oxygen gas containing ozone is supplied to the β-type gallium oxide substrate 2, thereby growing a β-type gallium oxide single crystal film. In addition, Non-Patent Document 1 discloses a technique in which a molecular beam epitaxy (MBE) apparatus is used to grow β-type gallium oxide, and oxygen gas is treated by rf-plasma.

[0004] Although for other semiconductor materials, technologies for heteroepitaxially growing necessary semiconductor materials on Si substrates have also been developed. For example, for GaN, non-patent document 2 has developed a technology for epitaxially growing GaN on a Si (111) substrate through an AlN buffer layer by methods such as organic metal chemical vapor deposition (MOCVD), and has also been applied in industry.

[0005] In contrast, it is difficult to grow gallium oxide on a heterogeneous substrate. For example, Non-Patent Document 3 studies the growth of gallium oxide on a Si substrate by inserting a SiC buffer layer between the Si substrate and the gallium oxide, and Non-Patent Document 4 studies the growth of gallium oxide on a Si substrate by inserting an Al2O3 buffer layer between the Si substrate and the gallium oxide. In addition, Non-Patent Document 5, which grows gallium oxide without inserting a buffer layer, forms an amorphous layer of gallium oxide.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2013-56802

[0009] Non-patent literature

[0010] Non-patent document 1: Rf-plasma-assisted molecular-beam epitaxy of β-Ga2O3, EG Villora, et al., Appl. Phys. Lett. 88, 031105 (2006)

[0011] Non-patent document 2: III-Nitride Based Lighting Emitting Diodes and Applications; Ch.3LEDs Based on Heteroepitaxial GaN on Si Substrates, T.Egawaand O.Oda, Springer Verlag, p.27-58 (2013))

[0012] Non-patent document 3: Study of the Anisotropic Elastoplastic Properties ofβ-Ga2O3 Films Synthesized on SiC / Si Substrates, ASGrashchenko et al., Phys.Solid State, 60, 852-857 (2018))

[0013] Non-patent document 4: β-Ga2O3 on Si(001) grown by plasma-assisted MBE with γ-Al2O3(111) buffer layer: Structural characterization, T.Hadamek et al., AIPAdvances, 11, 045209 (2021))

[0014] Non-patent literature 5: β-Ga2O3 MOSFETs on the Si substrate fabricated by the ion-cutting process, YB Wang et al., Sci. China: Phys., Mech. Astron., 63, 277311 (2020) Summary of the invention

[0015] In contrast, the gallium oxide film manufactured using the manufacturing device described in Patent Document 1 is not a heterogeneous material but is formed on a gallium oxide substrate. Although large-aperture gallium oxide has recently been able to be manufactured at low cost through the EFG (Edge-defined Film-fed Growth) method, the maximum aperture is still only 4 inches. In addition, although the cost is lower than before, the gallium oxide substrate is quite expensive compared to other semiconductor substrates. Furthermore, the growth temperature of the gallium oxide film is as high as 700°C or more, and the growth rate is also slow to about 0.1μm / h.

[0016] For these reasons, it is difficult to manufacture industrially viable devices as long as a gallium oxide substrate is used for forming a gallium oxide film. In addition, the gallium oxide manufactured by the above method has poor crystallinity and has problems with the flatness of gallium oxide.

[0017] As shown in Non-Patent Document 2, for semiconductor materials other than gallium oxide, technologies related to heteroepitaxial growth have been developed. On the other hand, for gallium oxide, the growth technology of semiconductor materials is not yet mature, and no good growth technology has been found. That is, the technology of heteroepitaxially growing gallium oxide on a single crystal substrate composed of a different material is under development.

[0018] For example, in the technologies disclosed in the above-mentioned non-patent documents 3 and 4, gallium oxide is grown via a buffer layer, and it is not possible to grow gallium oxide on a Si substrate without a buffer layer. In addition, the growth temperature of the gallium oxide film is as high as 600° C. or more, and the growth rate is also slow. Furthermore, the obtained gallium oxide film is not flat, has a domain structure, and has low orientation.

[0019] In addition, the gallium oxide film obtained by the method disclosed in the above-mentioned Non-Patent Document 5 is an amorphous layer, and no crystalline layer is obtained.

[0020] As shown above, heteroepitaxial growth of gallium oxide on a single crystal substrate composed of a different material is extremely difficult and technically challenging.

[0021] Therefore, an object of the present invention is to provide a substrate with a β-type gallium oxide film, in which a β-type gallium oxide film having an orientation is provided on a Si single crystal substrate or a gallium nitride single crystal substrate. In addition, an object of the present invention is also to provide a novel manufacturing method for obtaining a substrate with a β-type gallium oxide film, in which a β-type gallium oxide film having an orientation is provided on a single crystal substrate.

[0022] The present inventors have conducted intensive studies on the above-mentioned problems and have found a method for forming an oriented β-type gallium oxide film on a single crystal substrate composed of a different material other than gallium oxide, thereby completing the present invention.

[0023] That is, the gist of the present invention is as follows.

[0024] [1] A substrate with a β-type gallium oxide film, comprising a Si single crystal substrate and a β-type gallium oxide film disposed on the Si single crystal substrate, wherein the β-type gallium oxide film is uniaxially oriented.

[0025] [2] The substrate with a β-type gallium oxide film according to [1] above, wherein the β-type gallium oxide film is a single crystal.

[0026] [3] The substrate with a β-type gallium oxide film according to [1] or [2] above, wherein a peak of β-type gallium oxide attributed to the (100) plane is observed by symmetric X-ray diffraction.

[0027] [4] The substrate with a β-type gallium oxide film according to [1] or [2] above, wherein the β-type gallium oxide film with a (100) plane orientation is provided on the Si single crystal substrate with a (100) plane orientation.

[0028] [5] The substrate with a β-type gallium oxide film according to [1] or [2] above, wherein the

[001] direction of the Si single crystal substrate coincides with the [0-11] direction of the β-type gallium oxide film.

[0029] [6] The substrate with a β-type gallium oxide film according to [1] or [2] above, wherein the Si single crystal substrate is in direct contact with the β-type gallium oxide film.

[0030] [7] The substrate with a β-type gallium oxide film according to [1] or [2] above, wherein the β-type gallium oxide film is provided on the Si single crystal substrate via at least one of a nucleation layer and a surface modification layer.

[0031] [8] The substrate with a β-type gallium oxide film according to [1] or [2] above, wherein the thickness of the β-type gallium oxide film is 0.1 μm to 50 μm.

[0032] [9] A substrate with a β-type gallium oxide film, comprising a gallium nitride single crystal substrate and a β-type gallium oxide film disposed on the gallium nitride single crystal substrate, wherein the β-type gallium oxide film is uniaxially oriented.

[0033]

[10] The substrate with a β-type gallium oxide film according to [9] above, wherein the β-type gallium oxide film is a single crystal.

[0034]

[11] The substrate with a β-type gallium oxide film according to [9] or

[10] above, wherein a peak of β-type gallium oxide attributed to the (100) plane is observed by symmetric X-ray diffraction.

[0035]

[12] A substrate with a β-type gallium oxide film according to [9] or

[10] above, wherein the β-type gallium oxide film with a (100) plane orientation is provided on the gallium nitride single crystal substrate with a (0001) plane orientation.

[0036]

[13] The substrate with a β-type gallium oxide film according to [9] or

[10] above, wherein the gallium nitride single crystal substrate is in direct contact with the β-type gallium oxide film.

[0037]

[14] A substrate with a β-type gallium oxide film according to [9] or

[10] above, wherein the β-type gallium oxide film is provided on the gallium nitride single crystal substrate via at least one of a nucleation layer and a surface modification layer.

[0038]

[15] The substrate with a β-type gallium oxide film according to [9] or

[10] above, wherein the thickness of the β-type gallium oxide film is 0.1 μm to 50 μm.

[0039]

[16] A method for manufacturing a substrate with a β-type gallium oxide film, comprising the following steps: placing a single crystal substrate inside a reaction chamber, plasmatizing a mixed gas containing oxygen and ozone to dissociate the ozone into oxygen-constituting particles, and supplying the mixed gas to the reaction chamber under reduced pressure, and supplying gallium elements to the reaction chamber to epitaxially grow β-type gallium oxide on the single crystal substrate.

[0040]

[17] A method for manufacturing a substrate with a β-type gallium oxide film according to

[16] above, wherein the ratio of lattice constant mismatch between the single crystal substrate and the epitaxially grown β-type gallium oxide film is less than 15%.

[0041]

[18] A method for manufacturing a substrate with a β-type gallium oxide film according to

[16] or

[17] above, wherein a Si single crystal substrate, a gallium nitride single crystal substrate or a sapphire single crystal substrate is used as the single crystal substrate.

[0042]

[19] A method for manufacturing a substrate with a β-type gallium oxide film according to

[16] or

[17] above, wherein the surface of the single crystal substrate is treated with oxygen plasma and then the β-type gallium oxide is epitaxially grown.

[0043]

[20] A method for manufacturing a substrate with a β-type gallium oxide film according to

[16] or

[17] above, wherein the epitaxial growth of the β-type gallium oxide is performed at a film formation temperature of 600° C. or less.

[0044]

[21] A method for manufacturing a substrate with a β-type gallium oxide film according to

[16] or

[17] above, wherein the concentration of the ozone in the mixed gas relative to the total of the oxygen and the ozone is greater than 10% by volume.

[0045] The present invention provides for the first time a substrate with a β-type gallium oxide film uniaxially oriented on a single crystal substrate of a heterogeneous material. In addition, the substrate with the β-type gallium oxide film does not require a buffer layer composed of a heterogeneous material. In addition, the substrate with the β-type gallium oxide film not only has orientation, but also can make the crystallinity and flatness of the film good.

[0046] In addition, the method for manufacturing a substrate with a β-type gallium oxide film of the present invention can not only obtain a β-type gallium oxide film having the above characteristics, but also the heteroepitaxial growth rate of β-type gallium oxide is fast and a low growth temperature can be used. Therefore, it is expected to be industrialized at a lower cost than before. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 It is a schematic cross-sectional view showing the structure of a substrate with a β-type gallium oxide film according to the present embodiment.

[0048] Figure 2 This is a schematic structural diagram of a manufacturing apparatus used for manufacturing a substrate with a β-type gallium oxide film according to the present embodiment.

[0049] Figure 3 This is a scanning electron microscope photograph of the surface of the Si single crystal substrate with the obtained β-type gallium oxide film. Figure 3 (a) is a photo with a magnification of 5000 times. Figure 3 (b) is a photograph at a magnification of 100,000 times.

[0050] Figure 4 This is a scanning electron microscope photograph of a cross section of a Si single crystal substrate with a β-type gallium oxide film. Figure 4 (a) is a photo with a magnification of 10,000 times. Figure 4 (b) is a photograph at a magnification of 20,000 times.

[0051] Figure 5 : is the symmetrical X-ray diffraction pattern of the obtained Si single crystal substrate with β-type gallium oxide film.

[0052] Figure 6 This is an in-plane X-ray diffraction pattern of the obtained Si single crystal substrate with a β-type gallium oxide film.

[0053] Figure 7 This is an atomic force microscope (AFM) image of the surface of the Si single crystal substrate obtained. Figure 7 (a) is an AFM image of a Si single crystal substrate before oxygen plasma treatment. Figure 7 (b) is an AFM image of a Si single crystal substrate after being treated with oxygen plasma for 15 minutes. DETAILED DESCRIPTION

[0054] Hereinafter, the present invention will be described in detail, but the present invention is not limited to the following embodiments and can be implemented with arbitrary modifications within the scope not departing from the gist of the present invention.

[0055] In this specification, a single crystal substrate refers to a substrate in which the entire substrate is a single crystal.

[0056] In this specification, uniaxial orientation means that there are crystal grains in which at least one of the multiple crystal axes is oriented in the same direction, and there are multiple crystal grains rotating around the single axis. The uniaxial orientation of the β-type gallium oxide film can be confirmed by, for example, symmetric X-ray diffraction (symmetric XRD).

[0057] In the present specification, oxygen-constituting particles refer to particles containing oxygen atoms including singlet oxygen atoms and triplet oxygen atoms, oxygen molecules, ozone, or excited states thereof.

[0058] In the present specification, “to” indicating a numerical range is used to mean that the numerical values ​​described before and after it are included as the lower limit and the upper limit.

[0059] <Substrate with β-type gallium oxide film>

[0060] like Figure 1 As shown, the substrate 100 with a β-type gallium oxide film according to the present embodiment includes a single crystal substrate 110 and a β-type gallium oxide film 120 provided on the single crystal substrate 110 , and the β-type gallium oxide film 120 is uniaxially oriented.

[0061] The β-type gallium oxide film 120 may be provided on at least one of the principal surfaces, that is, the first principal surface 110a, of the single crystal substrate 110. However, from the perspective of epitaxial growth of the β-type gallium oxide film 120, the β-type gallium oxide film 120 is preferably provided only on the first principal surface 110a.

[0062] The cases where a Si single crystal substrate and a gallium nitride single crystal substrate are used as the single crystal substrate will be described respectively.

[0063] (Si single crystal substrate with β-type gallium oxide film)

[0064] The Si single crystal substrate with a β-type gallium oxide film according to the present embodiment includes a Si single crystal substrate and a β-type gallium oxide film provided on the Si single crystal substrate, wherein the β-type gallium oxide film is uniaxially oriented.

[0065] As the Si single crystal substrate, a conventionally known substrate can be used, and for example, a substrate obtained by crystal growth by a Czochralski method or an FZ (Floating Zone) method, and then cut and polished can be used.

[0066] The Si single crystal substrate is preferably a substrate with a (100) plane orientation, and the β-type gallium oxide film is preferably provided thereon with the principal surface on the (100) plane orientation side as the first principal surface.

[0067] The β-type gallium oxide film is a film epitaxially grown on a Si single crystal substrate, preferably on the (100) plane of the Si single crystal substrate, and may be uniaxially oriented.

[0068] The β-type gallium oxide film may be a single crystal or a polycrystalline film, but from the viewpoint of the yield and characteristics of the semiconductor device, a single crystal or a crystal close to a single crystal is preferred, and a single crystal is more preferred.

[0069] Furthermore, when an n-type or p-type gallium oxide semiconductor is grown by mixing a small amount of impurities, the β-type gallium oxide film may also contain these impurities.

[0070] In this specification, whether the β-type gallium oxide film is a single crystal film can be determined by, for example, a crystal X-ray diffraction (XRD) device using CuKα rays as a radiation source. If it is a single crystal, an XRD pattern unique to a single crystal can be obtained.

[0071] When the β-type gallium oxide film is single crystal, the β-type gallium oxide film is preferably a film with a (100) plane orientation, for example. More preferably, the β-type gallium oxide film with a (100) plane orientation is provided on a Si single crystal substrate with a (100) plane orientation.

[0072] For the Si single crystal substrate with a β-type gallium oxide film of this embodiment, the presence or absence of a peak of β-type gallium oxide attributable to the (100) plane by symmetric X-ray diffraction can be cited as an indicator of the crystallinity of the single crystal film of β-type gallium oxide. By observing this peak, it can be confirmed that heteroepitaxial growth is being performed. For example, the peak of β-type gallium oxide attributable to the (100) plane can include peaks of the (400) plane, the (600) plane, the (800) plane, etc.

[0073] Symmetrical X-ray diffraction measurement uses, for example, CuKα rays as a radiation source, irradiates the surface of the Si single crystal substrate with an incident angle of the X-ray at a Bragg diffraction angle θ, and rotates the diffracted X-rays in the detector at θ-2θ for measurement. In the symmetric X-ray diffraction pattern obtained by this measurement, the Ga2O3 (400) plane obtains a diffraction peak at a Bragg diffraction angle of 2θ = 30.07°, and the Ga2O3 (600) plane obtains a diffraction peak at a Bragg diffraction angle of 2θ = 44.7°. Therefore, if a diffraction peak is obtained at the above-mentioned Bragg diffraction angle, it can be attributed to the peak of the (100) plane of β-type gallium oxide.

[0074] As for the relationship between the crystal orientations of the Si single crystal substrate and the β-type gallium oxide film, from the viewpoint of epitaxial relationship, it is preferred that the

[001] direction of the Si single crystal substrate and the [0-11] direction of the β-type gallium oxide film coincide with each other.

[0075] The orientation of the Si single crystal substrate and the β-type gallium oxide film can be understood by in-plane X-ray diffraction.

[0076] The

[001] direction of the Si single crystal substrate and the [0-11] direction of the β-gallium oxide film do not need to be completely consistent, as long as they are substantially consistent. That is, according to the results of in-plane X-ray diffraction, if the angle formed by the

[001] direction of the Si single crystal substrate and the

[001] direction of the β-gallium oxide film is about 23 to 28 degrees, it can be said that the

[001] direction of the Si single crystal substrate and the [0-11] direction of the β-gallium oxide film are substantially consistent.

[0077] It should be noted that the ratio of lattice constant mismatch, which is called lattice mismatch, can also be quantified by the above-mentioned in-plane X-ray diffraction.

[0078] The Si single crystal substrate with a β-type gallium oxide film of this embodiment can be provided with a β-type gallium oxide film on the Si single crystal substrate without a buffer layer. The buffer layer refers to a layer inserted mainly to alleviate the lattice constant mismatch, and generally has a thickness of 20 nm or more. However, the Si single crystal substrate with a β-type gallium oxide film of this embodiment does not exclude any method including a buffer layer.

[0079] The Si single crystal substrate with a β-type gallium oxide film of the present embodiment does not require a buffer layer, and a preferred embodiment is a Si single crystal substrate with a β-type gallium oxide film in which the Si single crystal substrate and the β-type gallium oxide film are in direct contact with each other.

[0080] Furthermore, it is also preferable that a β-type gallium oxide film is provided on the Si single crystal substrate via at least one of a nucleation layer and a surface modification layer.

[0081] The nucleation layer or the surface modification layer is a layer provided to promote the crystallization of β-type gallium oxide, and is different from the buffer layer from the viewpoint of crystallinity.

[0082] The buffer layer refers to, for example, a single crystal film of the material of a predetermined thickness, a layer formed by gradually changing the composition of a mixed crystal of the material and a different material, or a layer formed by growing a superlattice structure of the material and a different material.

[0083] On the other hand, the nucleation layer is a layer inserted to promote the crystallization of β-gallium oxide, and refers to an adsorption layer or a thin film having a lattice constant different from that of the material. The thickness of the nucleation layer is, for example, less than 20 nm, preferably less than 10 nm, and more preferably less than 5 nm.

[0084] The nucleation layer can be a continuous layer or a discontinuous layer. The existence of the nucleation layer can be determined based on the similarities and differences in the atomic arrangement observed by cross-sectional TEM (transmission electron microscope). When no change in the atomic arrangement is observed, it can be determined that the Si single crystal substrate is in direct contact with the β-type gallium oxide film.

[0085] Examples of the nucleation layer include a layer containing an element different from that of the substrate, or a surface modification layer formed by modifying the substrate surface, etc. That is, the surface modification layer is a layer formed by modifying the surface of a substrate such as a single crystal substrate, and has a lattice constant different from that of the material.

[0086] The thickness of the β-gallium oxide film is preferably 0.1 to 50 μm, more preferably 0.5 to 50 μm, further preferably 0.8 to 30 μm, and particularly preferably 1 to 20 μm. Here, from the viewpoint of application to power devices, etc., the thickness of the β-gallium oxide film is preferably 0.1 μm or more, more preferably 0.5 μm or more, further preferably 0.8 μm or more, and particularly preferably 1 μm or more. In addition, the upper limit is not particularly limited, but from the viewpoint of film formation speed and film quality, the thickness of the β-gallium oxide film is preferably 50 μm or less, more preferably 30 μm or less, and further preferably 20 μm or less. It should be noted that the above thickness can be measured by using a scanning electron microscope or the like on a cross section of a Si single crystal substrate with a β-gallium oxide film.

[0087] The lattice constant mismatch ratio between the Si single crystal substrate and the β-type gallium oxide film is preferably 15% or less, more preferably 12% or less, and further preferably 8% or less. The lower the ratio, the better, but it is usually more than 0%.

[0088] The ratio of lattice constant mismatch is obtained by analyzing the epitaxial relationship of the β-type gallium oxide film on the Si single crystal substrate based on the results of symmetric X-ray diffraction measurement and in-plane X-ray diffraction measurement. It should be noted that the lattice constant mismatch refers to the ratio of the lattice constant difference of the β-type gallium oxide film in the same orientation to the lattice constant of the Si single crystal substrate, and as described later, it can be calculated, for example, based on the ratio of the lattice constant of the Si single crystal substrate and the lattice constant of the β-type gallium oxide single crystal film projected in a certain direction of the Si single crystal substrate.

[0089] (GaN single crystal substrate with β-type gallium oxide film)

[0090] The gallium nitride single crystal substrate with a β-type gallium oxide film according to the present embodiment includes a gallium nitride single crystal substrate and a β-type gallium oxide film provided on the gallium nitride single crystal substrate, wherein the β-type gallium oxide film is uniaxially oriented.

[0091] The gallium nitride single crystal substrate can use a conventionally known substrate, for example, a substrate obtained by crystal growth through hydride vapor phase epitaxy (Halide vapor phase epitaxy, HVPE) method, supercritical acidic ammonia technology (SCAAT method), low-pressure acidic ammonothermal (LPAAT method), Na flux method, etc., and a substrate obtained by cutting and polishing, or a substrate obtained by heteroepitaxially growing gallium nitride on a sapphire single crystal substrate or a Si single crystal substrate.

[0092] The gallium nitride single crystal substrate is preferably a substrate having a (0001) plane orientation, and the β-type gallium oxide film is preferably provided thereon with the principal surface on the (0001) plane orientation side as the first principal surface.

[0093] The β-type gallium oxide film is a film epitaxially grown on a gallium nitride single crystal substrate, preferably on the (0001) plane of the gallium nitride single crystal substrate, and may be uniaxially oriented.

[0094] The β-type gallium oxide film may be a single crystal or a polycrystalline film, but from the viewpoint of semiconductor applications, a single crystal or a crystal close to a single crystal is preferred, and a single crystal is more preferred.

[0095] Furthermore, when an n-type or p-type gallium oxide semiconductor is grown by mixing a small amount of impurities, the β-type gallium oxide film may also contain these impurities.

[0096] When the β-type gallium oxide film is single crystal, the β-type gallium oxide film is preferably a film with a (100) plane orientation, for example. More preferably, the β-type gallium oxide film with a (100) plane orientation is provided on a gallium nitride single crystal substrate with a (0001) plane orientation.

[0097] For the gallium nitride single crystal substrate with a β-type gallium oxide film of this embodiment, the presence or absence of a peak of β-type gallium oxide attributed to the (100) plane by symmetric X-ray diffraction can be cited as an indicator of the crystallinity of the single crystal film of β-type gallium oxide. By observing this peak, it can be confirmed that heteroepitaxial growth is being performed. For example, the peak of β-type gallium oxide attributed to the (100) plane can include peaks of the (400) plane, the (600) plane, the (800) plane, etc.

[0098] The peak of β-type gallium oxide attributable to the (100) plane by symmetric X-ray diffraction is the same as the peak described above in (Si single crystal substrate with β-type gallium oxide film).

[0099] The gallium nitride single crystal substrate with a β-type gallium oxide film of this embodiment can be provided with a β-type gallium oxide film on the gallium nitride single crystal substrate without a buffer layer. However, the gallium nitride single crystal substrate with a β-type gallium oxide film of this embodiment does not exclude any mode including a buffer layer. In addition, the buffer layer is the same as the buffer layer in the above-mentioned Si single crystal substrate with a β-type gallium oxide film.

[0100] The gallium nitride single crystal substrate with a β-type gallium oxide film of the present embodiment does not require a buffer layer, and a preferred embodiment is a gallium nitride single crystal substrate with a β-type gallium oxide film in which the gallium nitride single crystal substrate and the β-type gallium oxide film are in direct contact with each other.

[0101] Furthermore, it is also preferable that a β-type gallium oxide film is provided on the gallium nitride single crystal substrate via at least one of a nucleation layer and a surface modification layer.

[0102] The nucleation layer and the surface modification layer are respectively the same as the nucleation layer and the surface modification layer in the above-mentioned Si single crystal substrate with a β-type gallium oxide film, and the preferred aspects are also the same.

[0103] The thickness of the β-type gallium oxide film is preferably 0.1 to 50 μm, more preferably 0.5 to 50 μm, further preferably 0.8 to 30 μm, and particularly preferably 1 to 20 μm. Here, from the perspective of withstand voltage applied to power devices, etc., the thickness of the β-type gallium oxide film is preferably 0.1 μm or more, more preferably 0.5 μm or more, further preferably 0.8 μm or more, and particularly preferably 1 μm or more. In addition, the upper limit is not particularly limited, but from the perspective of film formation speed and film quality, the thickness of the β-type gallium oxide film is preferably 50 μm or less, more preferably 30 μm or less, and further preferably 20 μm or less.

[0104] The lattice constant mismatch ratio between the gallium nitride single crystal substrate and the β-type gallium oxide film is preferably 15% or less, more preferably 10% or less. The lower the ratio, the better, but it is usually more than 0%.

[0105] <Method for producing substrate with β-type gallium oxide film>

[0106] The method for producing a substrate with a β-type gallium oxide film according to the present embodiment includes the following steps 1 to 4.

[0107] Step 1: Step of placing a single crystal substrate inside a reaction chamber

[0108] Step 2: A step of converting a mixed gas containing oxygen and ozone into plasma to dissociate ozone into oxygen-forming particles and supplying the particles to the above reaction chamber under reduced pressure.

[0109] Step 3: A step of supplying gallium element to the reaction chamber together with step 2

[0110] Step 4: Step of epitaxially growing β-type gallium oxide on the single crystal substrate

[0111] Before explaining each process, refer to Figure 2 An embodiment of a production apparatus used will be described. It should be noted that the production apparatus used in the production method of this embodiment is not limited to the following.

[0112] (Manufacturing equipment)

[0113] The manufacturing method of this embodiment can be used, for example, Figure 2 A manufacturing device 1000 is shown in a schematic structural diagram.

[0114] The manufacturing apparatus 1000 includes a reaction chamber 1100 , a substrate placement unit 1200 , a gallium element supply device 1300 , an oxygen element supply device 1400 , and a heating device 1220 .

[0115] The reaction chamber 1100 is a place where a β-type gallium oxide film is epitaxially grown on a single crystal substrate 110 . A substrate placement unit 1200 and a susceptor 1210 are provided inside the reaction chamber 1100 . The single crystal substrate 110 is placed in the substrate placement unit 1200 and supported by the susceptor 1210 .

[0116] The substrate arrangement part 1200 in the reaction chamber 1100 can be heated by the heating device 1220, and the single crystal substrate 110 can be set to a desired temperature. Preferably, the temperature of the substrate arrangement part 1200 can be set to 0°C or above, or above room temperature, by using the heating device. In addition, the upper limit of the heating temperature is not particularly limited, and for example, it is sufficient as long as it can be heated to 700°C.

[0117] Gallium (Ga) is supplied to the arranged single crystal substrate 110 by a gallium supply device 1300. The gallium supply device 1300 is not particularly limited as long as it can supply gallium, and an example thereof is a Knudsen cell.

[0118] In the case of the Knudsen container, the gallium element supplier 1300 has a baffle 1310, thereby connecting or blocking the gallium element supplier 1300 and the reaction chamber 1100. The gallium element supplier 1300 may also have a heating device and a cooling device.

[0119] In addition, oxygen constituting particles are supplied to the arranged single crystal substrate 110 by an oxygen element supply device 1400. The oxygen element supply device 1400 has a plasma generating portion 1450 and further has a baffle 1410 as required. The oxygen element supply device 1400 is connected to or blocked from the reaction chamber 1100 by the baffle 1410. The oxygen element supply device 1400 may also have a heating device and a cooling device.

[0120] The oxygen particles supplied to the single crystal substrate 110 by the oxygen element supply device 1400 are obtained by plasma-forming a mixed gas containing oxygen and ozone by the plasma generation unit 1450 and dissociating ozone.

[0121] Specifically, oxygen is supplied to the oxygen element supply device 1400 by the oxygen supply unit 1500. The oxygen passes through the oxygen supply pipe 1810 and flows into the ozone generator 1700 while the flow rate is adjusted by the mass flow controller 1820.

[0122] A part of the oxygen gas flowing into the ozone generator 1700 is ozonized to form a mixed gas containing oxygen and ozone. As such an ozone generator 1700, for example, a first plasma generating device that converts oxygen gas into plasma is exemplified.

[0123] The ozone generator 1700 preferably has a capability of making the concentration of ozone relative to the total of oxygen and ozone 10% by volume or more, more preferably 20% by volume or more, and even more preferably 25% by volume or more.

[0124] The mixed gas containing oxygen and ozone generated by the ozone generator 1700 flows into the oxygen element supply device 1400 through the ozone-oxygen mixed gas supply pipe 1830 while the flow rate is adjusted by the mass flow controller 1840 .

[0125] It should be noted that the ozone generator 1700 may be directly connected to the oxygen element supply device 1400. In this case, the ozone-oxygen mixed gas supply pipe 1830 and the mass flow controller 1840 are not required.

[0126] In addition to the mixed gas containing oxygen and ozone, an inert gas is also supplied from the inert gas supply unit 1600 to the oxygen element supply device 1400. Examples of the inert gas include rare gases such as Ar gas and He gas. However, as long as there is a mixed gas containing oxygen and ozone, plasma formation described later can be performed even without the inert gas, so the supply of the inert gas is arbitrary.

[0127] The inert gas flows from the inert gas supply unit 1600 through the inert gas supply pipe 1850 and into the oxygen supply device 1400 while the flow rate is adjusted by the mass flow controller 1860 .

[0128] The mixed gas containing oxygen and ozone and the inert gas can be flowed into the oxygen element supply device 1400 separately, but can also be as follows Figure 2As shown, the two gases flow into the mixed gas supply pipe 1870 and are supplied to the oxygen element supply device 1400 in a mixed state. That is, the mixed gas supply pipe 1870 is a pipe for supplying a gas obtained by mixing a mixed gas containing oxygen and ozone with an inert gas for generating plasma to the oxygen element supply device 1400.

[0129] It should be noted that, when the mixed gas for generating plasma does not contain an inert gas, the inert gas supply unit 1600 , the inert gas supply pipe 1850 , and the mass flow controller 1860 are not necessary.

[0130] The manufacturing apparatus 1000 may further include an impurity element supplier (not shown) for supplying impurities in addition to the above. The impurity element supplier supplies the impurity element to grow n-type gallium oxide or p-type gallium oxide.

[0131] (Process 1)

[0132] In step 1, the single crystal substrate 110 is placed inside the reaction chamber 1100. That is, the single crystal substrate 110 is placed on the substrate placement part 1200 and supported by the susceptor 1210. Then, the substrate placement part 1200 is heated using the heating device 1220 to heat the single crystal substrate 110 to a desired temperature, and the reaction chamber 1100 is depressurized in preparation for the subsequent step 2.

[0133] It should be noted that the internal pressure of the reaction chamber 1100 and the temperature of the substrate placement portion 1200 , that is, the temperature of the single crystal substrate 110 are preferably the internal pressure and temperature described in (Step 4) described later.

[0134] The single crystal substrate 110 is preferably a Si single crystal substrate, a gallium nitride single crystal substrate or a sapphire single crystal substrate. In addition, single crystal substrates of various oxides and SiC single crystal substrates may also be used. Examples of oxides include MgO, MgAl2O4, SrTiO3, and ZrO2.

[0135] Before the single crystal substrate 110 is subjected to the subsequent step 2 , a nucleation layer or a surface modification layer may be formed on the surface of the single crystal substrate 110 , or a β-type gallium oxide film may be directly formed on the surface of the single crystal substrate 110 .

[0136] By forming the nucleation layer and the surface modification layer, the β-type gallium oxide film can be easily grown.

[0137] When forming the surface modification layer, for example, a method of performing oxygen plasma treatment on the surface of the single crystal substrate 110 can be mentioned. Oxygen plasma treatment is a surface treatment in which a mixed gas containing oxygen and ozone is converted into plasma and the ozone is dissociated into oxygen particles.

[0138] In addition, a nucleation layer made of a different material may be formed on the surface of the single crystal substrate 110. Examples of the different material include SiO2, Si3N4, Al2O3, In2O3, AlN, GaN, and InN.

[0139] (Process 2)

[0140] In step 2, a mixed gas containing oxygen and ozone is converted into plasma, ozone is dissociated into oxygen constituent particles, and the particles are supplied to the reaction chamber 1100 under reduced pressure.

[0141] Specifically, as described above, part of the oxygen supplied from the oxygen supply unit 1500 to the ozone generator 1700 is plasma-treated by the first plasma generated by the ozone generator 1700 to form ozone, thereby obtaining a mixed gas containing oxygen and ozone. The mixed gas is supplied to the oxygen element supply device 1400 via the mixed gas supply pipe 1870.

[0142] The ozone generator 1700 preferably has an ozone concentration of 10% by volume or more relative to the total of oxygen and ozone, more preferably 20% by volume or more, and even more preferably 25% by volume or more. The upper limit of the volume is not particularly limited, but is usually 50% by volume or less.

[0143] In addition, as needed, an inert gas such as Ar gas is supplied from the inert gas supply unit 1600 to the oxygen element supply device 1400 via the mixed gas supply pipe 1870. In this case, the mixed gas containing oxygen and ozone is mixed with the inert gas inside the mixed gas supply pipe 1870 to form a mixed gas containing oxygen, ozone and inert gas.

[0144] When the mixed gas containing oxygen and ozone is set to 100 parts by volume, the proportion of the inert gas is preferably 230 to 1900 parts by volume, more preferably 230 to 1500 parts by volume, further preferably 350 to 1000 parts by volume, and further preferably 350 to 460 parts by volume. Here, from the viewpoint of plasma ignition, the proportion of the inert gas is preferably 230 parts by volume or more, more preferably 350 parts by volume or more. In addition, from the viewpoint of the density of oxygen free radicals, the proportion of the inert gas is preferably 1900 parts by volume or less, more preferably 1500 parts by volume or less, further preferably 1000 parts by volume or less, and further preferably 460 parts by volume or less.

[0145] It is believed that the mixed gas supplied to the oxygen supply device 1400 via the mixed gas supply pipe 1870 is mainly decomposed by the second plasma generated by the plasma generating unit 1450 in the oxygen supply device 1400 to generate oxygen molecules and a large number of singlet oxygen atoms O( 1 D) of strong oxidizing oxygen free radicals. The above oxygen free radicals include singlet oxygen atoms O( 1 D) and triplet oxygen atoms O( 3 P). Singlet oxygen atom O( 1 D) transitions to triplet oxygen atoms O( 3 P).

[0146] Thus, the substances obtained by dissociating ozone into oxygen molecules and oxygen radicals are called oxygen constituent particles, and are supplied to the reduced pressure reaction chamber 1100. It should be noted that it is not excluded that not only oxygen constituent particles but also a mixed gas containing oxygen and ozone that is not plasmatized is supplied to the reduced pressure reaction chamber 1100.

[0147] (Process 3)

[0148] In step 3, together with step 2, gallium element is supplied to the reaction chamber 1100 under reduced pressure.

[0149] That is, gallium (Ga) is supplied from gallium supply device 1300 to reaction chamber 1100 under reduced pressure. As a result, the supplied Ga reacts with oxygen radicals supplied in step 2 on the surface of single crystal substrate 110, thereby forming a flat β-type gallium oxide film on the surface of single crystal substrate 110.

[0150] Specifically, near the surface of the single crystal substrate 110, Ga and singlet oxygen atoms or singlet oxygen atoms O ( 1 D) triplet oxygen atom O( 3 P) reaction, β-type gallium oxide film growth. If a large number of singlet oxygen atoms or singlet oxygen atoms O( 1 D) triplet oxygen atom O( 3 P) reaches the surface of the single crystal substrate 110, a β-type gallium oxide film with excellent crystallinity and good flatness grows. The film formation rate of this β-type gallium oxide film is faster than the film formation rate of the β-type gallium oxide film when using a conventional manufacturing apparatus.

[0151] The pressure of the gas supplied from the oxygen element supply device 1400 containing oxygen-forming particles in step 2 is preferably 1.0×10 -5 ~1.0×10 -1 Pa, more preferably 1.0×10 -4 ~1.0×10 -1 Pa, more preferably 1.0×10 -3~1.0×10 - 2 Here, from the viewpoint of supplying sufficient oxygen radicals, the gas pressure is preferably 1.0×10 -5 Pa or more, more preferably 1.0×10 -4 Pa or more, more preferably 1.0×10 -3 In addition, from the viewpoint of generating sufficient oxygen free radicals, the gas pressure supplied from the oxygen element supply device 1400 containing oxygen constituent particles in step 2 is preferably 1.0×10 -1 Pa or less, more preferably 1.0×10 -2 Below Pa.

[0152] The gas pressure supplied from the gallium element supply device 1300 in step 3 is preferably 1.0×10 -5 ~1.0×10 -2 Pa, more preferably 5.0×10 -5 ~1.0×10 -2 Pa, more preferably 1.0×10 -4 ~1.0×10 -3 Here, from the viewpoint of supplying sufficient Ga element, the above-mentioned gas pressure is preferably 1.0×10 -5 Pa or more, more preferably 5.0×10 -5 Pa or more, more preferably 1.0×10 -4 In addition, from the viewpoint of supplying sufficient Ga element, the gas pressure supplied from the gallium element supply device 1300 in step 3 is preferably 1.0×10 -2 Pa or less, more preferably 1.0×10 -3 Below Pa.

[0153] (Process 4)

[0154] Step 4 is a step of epitaxially growing β-type gallium oxide on the single crystal substrate 110 through the above-mentioned steps 2 and 3.

[0155] The internal pressure of the reaction chamber 1100 is preferably 0.001 to 0.01 Pa, and more preferably 0.006 to 0.009 Pa. Here, from the viewpoint of the exhaust capacity of the device, the internal pressure is preferably 0.001 Pa or more, and more preferably 0.006 Pa or more. In addition, from the viewpoint of the mean free path of oxygen radicals and gallium, the internal pressure is preferably 0.01 Pa or less, and more preferably 0.009 Pa or less.

[0156] The temperature of the single crystal substrate 110, that is, the film forming temperature for epitaxial growth of β-type gallium oxide, is preferably 0 to 600° C., more preferably 0 to 500° C., further preferably 0 to 400° C., and may be 10 to 350° C., or 20 to 300° C. Here, from the viewpoint of crystal growth, the film forming temperature is preferably 0° C. or higher, and may be 10° C. or higher, or above room temperature, that is, 20° C. or higher. In addition, from the viewpoint of growth rate, the film forming temperature is preferably 600° C. or lower, more preferably 500° C. or lower, further preferably 400° C. or lower, further preferably 350° C. or lower, and particularly preferably 300° C. or lower.

[0157] The lattice constant mismatch ratio between the obtained β-type gallium oxide film and the single crystal substrate is preferably 15% or less, more preferably 12% or less, and further preferably 8% or less. The lower the ratio, the better, but it is usually more than 0%.

[0158] The ratio of lattice constant mismatch has a physically optimum epitaxial relationship with respect to the single crystal substrate according to the bonding energy between the single crystal constituent elements and the constituent elements of β-type gallium oxide, and is uniquely determined from this epitaxial relationship.

[0159] The thickness of the β-type gallium oxide film is preferably 0.5 to 50 μm, more preferably 0.8 to 30 μm, and even more preferably 1 to 20 μm. Here, from the perspective of withstand voltage applied to power devices, etc., the thickness is preferably 0.5 μm or more, more preferably 0.8 μm or more, and even more preferably 1 μm or more. In addition, the upper limit is not particularly limited, but from the perspective of film formation speed and film quality, the thickness of the β-type gallium oxide film is preferably 50 μm or less, more preferably 30 μm or less, and even more preferably 20 μm or less.

[0160] As mentioned above, the substrate with a β-type gallium oxide film and the manufacturing method thereof according to the present embodiment have been described in detail. However, another aspect of the present embodiment is as follows.

[0161] [1] A substrate with a β-type gallium oxide film comprises a Si single crystal substrate and a β-type gallium oxide film disposed on the Si single crystal substrate, wherein the β-type gallium oxide film is uniaxially oriented.

[0162] [2] The substrate with a β-type gallium oxide film according to [1], wherein the β-type gallium oxide film is a single crystal.

[0163] [3] The substrate with a β-type gallium oxide film according to [1]' or [2]' above, wherein a peak of β-type gallium oxide attributed to the (100) plane is observed by symmetric X-ray diffraction.

[0164] [4] The substrate with a β-type gallium oxide film according to any one of [1]' to [3]' above, wherein the β-type gallium oxide film having a (100) plane orientation is provided on the Si single crystal substrate having a (100) plane orientation.

[0165] [5] The substrate with a β-type gallium oxide film according to any one of [1]' to [4]' above, wherein a

[001] direction of the Si single crystal substrate coincides with a [0-11] direction of the β-type gallium oxide film.

[0166] [6] The substrate with a β-type gallium oxide film according to any one of [1]' to [5]' above, wherein the Si single crystal substrate is in direct contact with the β-type gallium oxide film.

[0167] [7] The substrate with a β-type gallium oxide film according to any one of [1]' to [6]', wherein the β-type gallium oxide film is provided on the Si single crystal substrate via at least one of a nucleation layer and a surface modification layer.

[0168] [8] The substrate with a β-type gallium oxide film according to any one of [1]' to [7]' above, wherein the β-type gallium oxide film has a thickness of 0.1 μm to 50 μm.

[0169] [9] A substrate with a β-type gallium oxide film comprises a gallium nitride single crystal substrate and a β-type gallium oxide film disposed on the gallium nitride single crystal substrate, wherein the β-type gallium oxide film is uniaxially oriented.

[0170]

[10] The substrate with a β-type gallium oxide film according to the above [9], wherein the β-type gallium oxide film is a single crystal.

[0171]

[11] The substrate with a β-type gallium oxide film according to [9]' or

[10] ' above, wherein a peak of β-type gallium oxide attributed to the (100) plane is observed by symmetric X-ray diffraction.

[0172]

[12] The substrate with a β-type gallium oxide film according to any one of [9]' to

[11] ', wherein the β-type gallium oxide film having a (100) plane orientation is provided on the gallium nitride single crystal substrate having a (0001) plane orientation.

[0173]

[13] The substrate with a β-type gallium oxide film according to any one of [9]' to

[12] ' above, wherein the gallium nitride single crystal substrate is in direct contact with the β-type gallium oxide film.

[0174]

[14] The substrate with a β-type gallium oxide film according to any one of [9]' to

[13] ', wherein the β-type gallium oxide film is provided on the gallium nitride single crystal substrate via at least one of a nucleation layer and a surface modification layer.

[0175]

[15] The substrate with a β-type gallium oxide film according to any one of [9]' to

[14] ' above, wherein the thickness of the β-type gallium oxide film is 0.1 μm to 50 μm.

[0176]

[16] A method for manufacturing a substrate with a β-type gallium oxide film, comprising the following steps: placing a single crystal substrate inside a reaction chamber, plasmatizing a mixed gas containing oxygen and ozone to dissociate the ozone into oxygen-constituting particles, and supplying the mixed gas to the reaction chamber under reduced pressure, and supplying gallium element to the reaction chamber to epitaxially grow β-type gallium oxide on the single crystal substrate.

[0177]

[17] The method for manufacturing a substrate with a β-type gallium oxide film according to

[16] , wherein the lattice constant mismatch ratio between the single crystal substrate and the epitaxially grown β-type gallium oxide film is 15% or less.

[0178]

[18] The method for manufacturing a substrate with a β-type gallium oxide film according to

[16] or

[17] , wherein a Si single crystal substrate, a gallium nitride single crystal substrate or a sapphire single crystal substrate is used as the single crystal substrate.

[0179]

[19] The method for manufacturing a substrate with a β-type gallium oxide film according to any one of

[16] ' to

[18] ', wherein the surface of the single crystal substrate is subjected to oxygen plasma treatment, and then the β-type gallium oxide is epitaxially grown.

[0180]

[20] The method for producing a substrate with a β-type gallium oxide film according to any one of

[16] ' to

[19] ' above, wherein the epitaxial growth of the β-type gallium oxide is performed at a film formation temperature of 600° C. or less.

[0181]

[21] The method for producing a substrate with a β-type gallium oxide film according to any one of

[16] ' to

[20] ', wherein the concentration of the ozone in the mixed gas is 10% by volume or more relative to the total of the oxygen and the ozone.

[0182] Example

[0183] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples.

[0184] (Manufacturing of a substrate with a β-type gallium oxide film)

[0185] use Figure 2 The manufacturing apparatus 1000 shown in the figure epitaxially grows a β-type gallium oxide film on a Si single crystal substrate according to the following steps to obtain a substrate with a β-type gallium oxide film.

[0186] Specifically, the Si single crystal substrate is first cleaned with an organic solvent, then cleaned with an acid and dried. Next, the Si single crystal substrate is placed on the substrate placement unit 1200 with the (100) plane facing the surface, and supported by the susceptor 1210 .

[0187] The temperature of the Si single crystal substrate was heated to 300°C, and the pressure in the reaction chamber 1100 was reduced to 8.0×10 -3 Pa.

[0188] On the other hand, the concentration of ozone relative to the total of oxygen and ozone supplied from the oxygen supply unit was made 28% by volume using an ozone generator 1700, and a mixed gas containing oxygen and ozone was supplied to the oxygen element supply device 1400. At the same time, Ar gas was also supplied from the inert gas supply unit 1600 to the oxygen element supply device 1400. The ratio of the mixed gas containing oxygen and ozone to the Ar gas was 1:4.

[0189] Then, O2 and O3 were set to a flow rate of 8sccmO2+O3 and supplied from the oxygen element supply device 1400 to the reaction chamber 1100 under the reduced pressure, and the Si single crystal substrate was treated with oxygen plasma for 15 minutes at a plasma output of 1000W to form a surface modification layer. Then, Ga was further set to a pressure of 1.13×10 -4 Pa is supplied from the gallium element supply device 1300 to the reaction chamber 1100 to grow the β-type gallium oxide film for 60 minutes. Through the above steps, a Si single crystal substrate with a gallium oxide film is obtained.

[0190] The scanning electron microscope photograph of the surface of the Si single crystal substrate with the gallium oxide film obtained above is shown in Figure 3 . Figure 3 (a) is a magnification of 5000 times. Figure 3 (b) is a magnification of 100,000 times, and both confirm that the surface of the grown gallium oxide film is very clean and has high flatness.

[0191] A scanning electron microscope photograph of a cross section of the Si single crystal substrate with a gallium oxide film obtained above is shown in Figure 4 . Figure 4 (a) is a magnification of 10,000 times. Figure 4 (b) is a magnification of 20,000 times. From these results, it can be seen that the thickness of the grown gallium oxide film is measured to be 1.05 μm, and the film formation rate is 1.05 μm / hour, that is, 17.5 nm / min.

[0192] Symmetric X-ray diffraction measurement was performed on the obtained Si single crystal substrate with gallium oxide film. The radiation source used CuKα radiation, and the incident angle of the X-ray was irradiated at a Bragg diffraction angle θ relative to the Si surface. The diffracted X-ray was rotated in the detector at θ-2θ to measure the diffraction angle.

[0193] The obtained pattern is shown in Figure 5 , the horizontal axis is 2θ-θ°, and the vertical axis is intensity. In addition to the peak of the Si (200) plane and the Si (400) plane, the peak of the β-type gallium oxide (400) plane was observed at 2θ=30.07°, and the peak of the β-type gallium oxide (600) plane was observed at 2θ=44.7°. Thus, it is clear that the gallium oxide film in the obtained Si single crystal substrate with gallium oxide film is a single crystal film of β-type gallium oxide.

[0194] The in-plane X-ray diffraction measurement was performed on the Si single crystal substrate with a gallium oxide film. The radiation source used CuKα radiation, and the X-ray incident angle was a small angle of 0.3° relative to the Si surface. The X-ray diffracted in the direction perpendicular to the normal direction of the Si single crystal substrate was rotated in the detector at θ-2θ to measure the diffraction angle.

[0195] The obtained pattern is shown in Figure 6 , the horizontal axis is 2θ-θ°, and the vertical axis is intensity. When the direction of θ=0° is rotated clockwise about 26° from the

[010] direction of Si, the peak of the β-type gallium oxide (00-3) surface is observed at 2θ=48.05°. This further confirmed that a single crystal film of β-type gallium oxide can be formed as a gallium oxide film, and also clarified that there is an epitaxial relationship between the Si single crystal substrate and the β-type gallium oxide film.

[0196] Based on the above X-ray diffraction measurement results, the epitaxial relationship between the (100)-oriented Si single crystal substrate and the β-type gallium oxide single crystal thin film epitaxially grown on the surface is estimated as follows.

[0197] Si(100) / / β-Ga2O3(100)

[0198] Si

[001] / / β-Ga2O3[0-11]

[0199] There has been no reported case of growth of a β-type gallium oxide single crystal film on a (100)-oriented Si single crystal substrate in such an epitaxial relationship in the past, and this is the first time that it has been achieved.

[0200] The present invention was completed based on a new finding that the β-type gallium oxide single crystal is a monoclinic single crystal with a lattice constant of The angles between the lattices are also α = γ = 90° and β = 103.83°, and each orientation has a different lattice constant, and has a crystal structure in which the a-axis is tilted relative to the c-axis. Due to this unique crystal structure, the β-type gallium oxide single crystal grows epitaxially on the Si single crystal substrate in a direction with the smallest lattice mismatch rate possible, compared to Si with a simple diamond crystal structure.

[0201] Based on the epitaxial relationship obtained from the results of the above-mentioned symmetric X-ray diffraction measurement and in-plane X-ray diffraction measurement, the lattice mismatch between the (100)-oriented Si single crystal substrate and the β-type gallium oxide single crystal film is calculated. The lattice mismatch can be calculated, for example, based on the ratio of the lattice constant of the Si single crystal substrate to the lattice constant of the β-type gallium oxide single crystal film projected in a certain direction of the Si single crystal substrate.

[0202] Specifically, the lattice constant of the β-type gallium oxide single crystal film in the

[001] direction is projected onto the

[001] direction of the Si single crystal substrate, and the difference is divided by the lattice constant of the Si single crystal substrate in the

[001] direction. Similarly, twice the lattice constant of the β-type gallium oxide single crystal film in the

[010] direction is projected onto the

[010] direction of the Si single crystal substrate, and the difference is divided by the lattice constant of the Si single crystal substrate in the

[010] direction.

[0203] Assuming that the

[001] direction of the Si single crystal substrate is completely parallel to the [0-11] direction of the β-gallium oxide single crystal film, the lattice mismatch in the

[001] direction of the Si single crystal substrate obtained above is estimated to be 5.4%, and the lattice mismatch in the

[010] direction of the Si single crystal substrate is estimated to be 0.9%. Due to the arrangement of Si atoms and β-gallium oxide atoms, the

[001] direction of the Si single crystal substrate and the [0-11] direction of the β-gallium oxide single crystal film may also be slightly offset, but from this result, it can be seen that the lattice mismatch is very small, and the reason why a high-quality β-gallium oxide single crystal film can be grown on a (100)-oriented Si single crystal substrate is scientifically explained.

[0204] Next, when manufacturing a Si single crystal substrate with a β-type gallium oxide film, AFM images of the surface of the Si single crystal substrate were observed before and after the Si single crystal substrate was subjected to oxygen plasma treatment for 15 minutes.

[0205] The results are shown in Figure 7 , Figure 7 (a) is an AFM image of a Si single crystal substrate before oxygen plasma treatment. Figure 7 (b) is an AFM image of a Si single crystal substrate after being treated with oxygen plasma for 15 minutes.

[0206] The surface roughness before the oxygen plasma treatment was 0.152 nm, and the surface roughness after the treatment was 0.131 nm. This confirmed that the surface of the Si single crystal substrate became flatter by the oxygen plasma treatment.

[0207] As described above, the manufacturing method of this embodiment can manufacture a β-gallium oxide film on a Si single crystal substrate without a buffer layer. More specifically, a (100)-oriented β-gallium oxide single crystal film can be epitaxially grown on a (100)-oriented Si single crystal substrate.

[0208] The growth temperature of the β-type gallium oxide film is 300°C, which is very low, so the film formation speed is very fast and the film thickness can be increased. Furthermore, the surface of the β-type gallium oxide film is very smooth and has good flatness. In addition, it is a single crystal film and has good crystallinity.

[0209] There have been no reported examples of growing a β-type gallium oxide film on a (100)-oriented Si single crystal substrate without a buffer layer, not to mention the surprisingly fast growth rate, low film formation temperature, and good flatness and crystallinity as in the present embodiment. The effect of the present invention is obvious.

[0210] In addition, a gallium nitride single crystal substrate was used instead of a Si single crystal substrate, and a gallium oxide film was formed on its surface in the same manner as described above. Symmetrical X-ray diffraction measurement was also performed on the obtained gallium nitride single crystal substrate with a gallium oxide film, and diffraction peaks of the Ga2O3 (400) plane with a Bragg diffraction angle of 2θ = 30.07° and the Ga2O3 (600) plane with a Bragg diffraction angle of 2θ = 44.7° were obtained, confirming that the gallium oxide film was a single crystal film of β-type gallium oxide. Specifically, a single crystal film of β-type gallium oxide was formed in a (100) plane orientation on a gallium nitride single crystal substrate with a (0001) plane orientation. In addition, the flatness of the surface of the β-type gallium oxide single crystal film was confirmed by scanning electron microscopy, and the thickness of the β-type gallium oxide film was confirmed to be 0.9 to 1.0 μm by cross-sectional observation.

[0211] The present invention is described in detail and with reference to specific embodiments, but it is obvious to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on Japanese patent applications (Special Application No. 2022-050538) filed on March 25, 2022 and Japanese patent applications (Special Application No. 2022-075480) filed on April 28, 2022, the contents of which are incorporated herein by reference.

[0212] Industrial Applicability

[0213] The present invention can use low-cost Si single crystal substrates or other single crystal substrates to replace conventional gallium oxide single crystal substrates and manufacture a β-type gallium oxide single crystal film thereon. In addition, a β-type gallium oxide single crystal film can be obtained with any film thickness, at a low temperature and at a fast film forming speed, and the obtained β-type gallium oxide film has good surface flatness and crystallinity. Therefore, the industrial applicability is very high.

[0214] Explanation of symbols

[0215] 100Substrate with β-type gallium oxide film

[0216] 110 single crystal substrate

[0217] 110a first main surface

[0218] 120β-type gallium oxide film

[0219] 1000 Manufacturing Devices

[0220] 1100 Reaction Room

[0221] 1200 substrate configuration department

[0222] 1210 base

[0223] 1220 Heating device

[0224] 1300 Gallium element supply device

[0225] 1310, 1410 baffle

[0226] 1400 Oxygen supply device

[0227] 1450 Plasma generation unit

[0228] 1500 Oxygen Supply Department

[0229] 1600 Inert gas supply unit

[0230] 1700 Ozone Generator

[0231] 1810 oxygen supply tube

[0232] 1820, 1840, 1860 Mass Flow Controllers

[0233] 1830 Ozone-oxygen mixed gas supply pipe

[0234] 1850 Inert gas supply pipe

[0235] 1870 Mixed gas supply pipe

Claims

1. A substrate with a β-type gallium oxide film, comprising a Si single crystal substrate and a β-type gallium oxide film provided on the Si single crystal substrate, The β-type gallium oxide film is uniaxially oriented.

2. The substrate with a β-type gallium oxide film according to claim 1, wherein: The β-type gallium oxide film is single crystal.

3. The substrate with a β-type gallium oxide film according to claim 1 or 2, wherein: A peak of β-type gallium oxide attributed to the (100) plane was observed by symmetric X-ray diffraction.

4. The substrate with a β-type gallium oxide film according to claim 1 or 2, wherein: The β-type gallium oxide film having a (100) plane orientation is provided on the Si single crystal substrate having a (100) plane orientation.

5. The substrate with a β-type gallium oxide film according to claim 1 or 2, wherein: The [001] direction of the Si single crystal substrate is consistent with the [0-11] direction of the β-type gallium oxide film.

6. The substrate with a β-type gallium oxide film according to claim 1 or 2, wherein: The Si single crystal substrate is in direct contact with the β-type gallium oxide film.

7. The substrate with a β-type gallium oxide film according to claim 1 or 2, wherein: The β-type gallium oxide film is provided on the Si single crystal substrate via at least one of a nucleation layer and a surface modification layer.

8. The substrate with a β-type gallium oxide film according to claim 1 or 2, wherein: The thickness of the β-type gallium oxide film is 0.1 μm to 50 μm.

9. A substrate with a β-type gallium oxide film, comprising a gallium nitride single crystal substrate and a β-type gallium oxide film disposed on the gallium nitride single crystal substrate, The β-type gallium oxide film is uniaxially oriented.

10. The substrate with a β-type gallium oxide film according to claim 9, wherein: The β-type gallium oxide film is single crystal.

11. The substrate with a β-type gallium oxide film according to claim 9 or 10, wherein: A peak of β-type gallium oxide attributed to the (100) plane was observed by symmetric X-ray diffraction.

12. The substrate with a β-type gallium oxide film according to claim 9 or 10, wherein: The β-type gallium oxide film having a (100) plane orientation is provided on the gallium nitride single crystal substrate having a (0001) plane orientation.

13. The substrate with a β-type gallium oxide film according to claim 9 or 10, wherein: The gallium nitride single crystal substrate is in direct contact with the β-type gallium oxide film.

14. The substrate with a β-type gallium oxide film according to claim 9 or 10, wherein: The β-type gallium oxide film is provided on the gallium nitride single crystal substrate via at least one of a nucleation layer and a surface modification layer.

15. The substrate with a β-type gallium oxide film according to claim 9 or 10, wherein: The thickness of the β-type gallium oxide film is 0.1 μm to 50 μm.

16. A method for manufacturing a substrate with a β-type gallium oxide film, comprising the following steps: A single crystal substrate is placed inside the reaction chamber. A mixed gas containing oxygen and ozone is converted into plasma to dissociate the ozone into oxygen-constituting particles, and the mixed gas is supplied to the reaction chamber under reduced pressure, and supplying gallium element to the reaction chamber, β-type gallium oxide is epitaxially grown on the single crystal substrate.

17. The method for manufacturing a substrate with a β-type gallium oxide film according to claim 16, wherein: The ratio of lattice constant mismatch between the single crystal substrate and the epitaxially grown β-type gallium oxide film is 15% or less.

18. The method for manufacturing a substrate with a β-type gallium oxide film according to claim 16 or 17, wherein: As the single crystal substrate, a Si single crystal substrate, a gallium nitride single crystal substrate, or a sapphire single crystal substrate is used.

19. The method for manufacturing a substrate with a β-type gallium oxide film according to claim 16 or 17, wherein: The surface of the single crystal substrate is subjected to oxygen plasma treatment, and then the β-type gallium oxide is epitaxially grown.

20. The method for manufacturing a substrate with a β-type gallium oxide film according to claim 16 or 17, wherein: The epitaxial growth of the β-type gallium oxide is performed at a film formation temperature of 600° C. or less.

21. The method for manufacturing a substrate with a β-type gallium oxide film according to claim 16 or 17, wherein: The concentration of the ozone in the mixed gas relative to the total of the oxygen and the ozone is set to 10% by volume or more.

Citation Information

Patent Citations

  • METHOD FOR PRODUCING -Ga2O3 SINGLE CRYSTAL FILM AND LAMINATED CRYSTAL STRUCTURE

    JP2013056802A

Cited By

  • Epitaxial growth method of gallium oxide material, gallium oxide epitaxial structure and ultraviolet detector

    CN120174475A