Protective film-forming film, protective film-forming composite sheet, and method for producing chip with protective film

The use of an energy ray-curable protective film with high image clarity and low curing rate addresses the issue of opaque films deteriorating during reflow, ensuring clear markings and effective chip inspection.

JP2024143056APending Publication Date: 2024-10-11LINTEC CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023055535
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-30
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Conventional energy-beam-curable protective films for semiconductor wafers are opaque and deteriorate during the reflow process, affecting the visibility of laser markings on the back surface of the wafer.

Method used

An energy ray-curable protective film with high image clarity and low curing rate is applied to the back surface of semiconductor wafers, allowing for clear laser markings and improved visibility, and a method for manufacturing chips with a protective film that includes pasting, curing, and dividing the film.

Benefits of technology

The solution provides a protective film with excellent print visibility and stability under fluorescent lighting, enabling clear reading of markings and inspection of semiconductor chips, while maintaining the integrity of the film during the reflow process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024143056000001_ABST
    Figure 2024143056000001_ABST
Patent Text Reader

Abstract

To provide an energy ray-curable protective film-forming film that is applicable for bonding onto the rear face of a wafer to protect the marking face, while exhibiting superior print visibility, and a protective film-forming composite sheet including the same, and a method for producing a chip with a protective film.SOLUTION: An energy ray-curable protective film-forming film 13 has an image clarity of 110 or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a protective film-forming film, a composite sheet for forming a protective film, and a method for producing a chip with a protective film. [Background technology]

[0002] Some wafers, such as semiconductor wafers and insulator wafers, have circuits formed on one surface (circuit surface) and further have protruding electrodes such as bumps on that surface (circuit surface). Such wafers are divided into chips, and are mounted on a circuit board by connecting the protruding electrodes to connection pads on the circuit board using the so-called face-down method. In such wafers and chips, the surface opposite the circuit surface (back surface) may be protected with a protective film in order to prevent damage such as cracks.

[0003] In order to form such a protective film, a protective film-forming film for forming the protective film is attached to the back surface of the wafer. The protective film-forming film may be laminated on a support sheet for supporting it, and may be used in the form of a composite sheet for forming a protective film, or may be used without being laminated on a support sheet. After laser marking on the protective film-forming film, the semiconductor wafer is divided into chips by dicing and picked up after being cured by heat or energy rays as necessary to enhance the protective performance of the protective film-forming layer. Alternatively, the protective film-forming film is cured by heat or energy rays to form a protective film, and the semiconductor wafer is divided into chips by dicing and picked up. Next, the semiconductor chip with the protective film that has been picked up is flip-chip connected to a connection pad on a circuit board such as a motherboard, and the circuit board is heated to melt the protruding electrodes on the protective film-forming chip (hereinafter referred to as a reflow process), and the electrical connection between the protruding electrodes and the connection pads on the circuit board is strengthened, and the semiconductor chip is mounted on the circuit board.

[0004] The protective film-forming film includes a non-curable type that does not have curability and functions as a protective film as it is. When a non-curable protective film-forming film is used, a curing process is not required, so a chip with a protective film can be manufactured at low cost by a simplified method. On the other hand, when a curable protective film-forming film is used, the cured product is used as a protective film, so that the protective film has an advantage of high wafer protection ability. A thermosetting protective film-forming film that is cured by heating requires a relatively long heating time during curing, but an energy ray-curable protective film-forming film that is cured by irradiation with energy rays has an advantage of requiring only a short energy ray irradiation time during curing. Therefore, various developments of energy ray-curable protective film-forming films have been promoted (see Patent Documents 1 to 3). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2010-031183 A [Patent Document 2] International Publication No. 2017 / 188197 [Patent Document 3] International Publication No. 2019 / 082977 Summary of the Invention [Problem to be solved by the invention]

[0006] In a conventional method for manufacturing a semiconductor chip with a protective film using a protective film-forming film or a composite sheet for forming a protective film, the protective film-forming film is laser-marked, and there is a risk that the laser marking will deteriorate during the curing process of the protective film-forming film or the reflow process when mounting a semiconductor package on a substrate. In response to this, a method of laser marking the back surface of a semiconductor wafer can be considered in which the laser marking is not deteriorated during the curing process or reflow process of the protective film-forming film.

[0007] However, conventional energy ray-curable protective film-forming films are black and opaque so that printing processing can be performed by irradiation with laser light, and are not suitable for applications in which laser marking is performed directly on the back surface of a semiconductor wafer because the printing is hidden.

[0008] The present invention has been made in consideration of the above circumstances, and provides an energy ray-curable protective film-forming film that can be attached to the back surface of a wafer to protect a marking surface (i.e., the back surface of a laser-marked wafer, or the back surface of a laser-marked chip obtained by dividing the wafer) and has excellent printing visibility, as well as a composite sheet for forming a protective film comprising the same, and a method for manufacturing a chip with a protective film. [Means for solving the problem]

[0009] The present invention has the following aspects. [1] An energy ray-curable protective film-forming film, The protective film-forming film has an image clarity of 110 or more. [2] Contains an energy ray-curable component (a) having a group containing an energy ray-curable C=C double bond, The protective film-forming film according to [1] has a cure rate of 16% or less after exposure to a circular daylight fluorescent lamp having a rated lamp power of 28 W at a distance of 1 m for 168 hours. [3] A composite sheet for forming a protective film comprising a support sheet and the protective film-forming film according to [1] or [2] provided on one surface of the support sheet. [4] A method for manufacturing a chip with a protective film, comprising: a chip and a protective film provided on the back surface of the chip, the method including a bonding step of bonding the protective film-forming film described in [1] or [2] to the back surface of a wafer; a curing step of curing the protective film-forming film with energy rays to form the protective film; and a division step of dividing the wafer and cutting the protective film to produce a plurality of chips with the protective film. [5] A method for manufacturing a chip with a protective film, comprising a chip and a protective film provided on the back surface of the chip, the method including a bonding step of bonding the protective film-forming film described in [1] or [2] to the back surface of a wafer, a curing step of curing the protective film-forming film with energy rays to form the protective film, a dividing step of dividing the wafer and cutting the protective film to produce a plurality of chips with the protective film, and a laser marking step of irradiating the back surface of the wafer with a laser. Effect of the Invention

[0010] According to the present invention, there is provided an energy ray curable protective film forming film which can be attached to the back surface of a wafer to protect the marking surface and has excellent print visibility, a composite sheet for forming a protective film comprising the same, and a method for manufacturing a chip with a protective film. [Brief description of the drawings]

[0011] [Figure 1] 1 is a cross-sectional view showing a schematic example of a protective film-forming film according to an embodiment of the present invention. [Diagram 2] 1 is a cross-sectional view showing a schematic example of a composite sheet for forming a protective film according to an embodiment of the present invention. [Diagram 3] FIG. 2 is a cross-sectional view showing a schematic diagram of another example of a composite sheet for forming a protective film according to an embodiment of the present invention. [Figure 4] FIG. 2 is a cross-sectional view showing a schematic diagram of still another example of the composite sheet for forming a protective film according to one embodiment of the present invention. [Diagram 5] FIG. 2 is a cross-sectional view showing a schematic diagram of still another example of the composite sheet for forming a protective film according to one embodiment of the present invention. [Figure 6] 1A to 1C are cross-sectional views for illustrating an example of a method for manufacturing a chip with a protective film according to an embodiment of the present invention. [Figure 7] 10A to 10C are cross-sectional views for illustrating a schematic example of a method for manufacturing a chip with a protective film according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] ◇Protective film A protective film-forming film according to one embodiment of the present invention is an energy ray-curable protective film-forming film, and the image clarity of the protective film-forming film is not less than 110. The image clarity of the protective film-forming film refers to the total value of evaluation values ​​measured using five types of slits (slit widths: 0.125 mm, 0.25 mm, 0.5 mm, 1 mm, and 2 mm) in accordance with JIS K 7374:2007.

[0013] The image clarity of the protective film-forming film of this embodiment is 110 or more, preferably 150 or more, more preferably 200 or more, even more preferably 300 or more, and particularly preferably 350 or more. Since the image clarity of the protective film-forming film of the present invention is equal to or more than the lower limit, the image clarity of the protective film formed by attaching the protective film-forming film to the back surface of the semiconductor wafer is also good. The image clarity of the protective film-forming film may be 500 or less, 450 or less, or 400 or less.

[0014] The protective film-forming film of this embodiment is used, for example, to provide a protective film on the back surface of a semiconductor chip to protect the semiconductor chip. Since the protective film-forming film of this embodiment has good image clarity, the semiconductor wafer or the semiconductor chip can be inspected through the protective film formed by attaching the protective film-forming film to the back surface of the semiconductor wafer or the back surface of the semiconductor chip obtained by dividing the semiconductor wafer. More specifically, the printing such as characters, symbols, patterns, etc. laser-marked on the semiconductor wafer or the semiconductor chip can be read through the protective film formed by attaching the protective film-forming film to the back surface of the semiconductor wafer or the back surface of the semiconductor chip obtained by dividing the semiconductor wafer, and the presence or absence of the printing, grinding marks on the back surface of the semiconductor wafer or the semiconductor chip, or foreign matter between the semiconductor wafer or the semiconductor chip and the protective film can be inspected. In addition, if there is a foreign matter, the state of the foreign matter can be inspected.

[0015] The image clarity of the protective film-forming film can be adjusted by the components contained in the protective film-forming composition described below, and in particular, fine adjustments can be made by selecting the type and size of the filler and the type and content of the colorant.

[0016] The light transmittance of the protective film-forming film at a wavelength of 550 nm is preferably 30% or more, more preferably 40% or more, and particularly preferably 45% or more. When the light transmittance of the protective film-forming film at a wavelength of 550 nm is the lower limit or more, it becomes possible to read the laser-printed characters, symbols, patterns, and other printed characters more clearly. The light transmittance of the protective film-forming film at a wavelength of 550 nm may be 99.5% or less, or may be 99.0% or less. The light transmittance of the protective film-forming film at a wavelength of 550 nm can be adjusted by the components contained in the protective film-forming composition described later, particularly the type and content of the thermosetting component, filler, and / or colorant.

[0017] By using the protective film-forming film of this embodiment, or a composite sheet for forming a protective film comprising the same, a chip with a protective film can be manufactured, comprising a chip and a protective film provided on the back surface of the chip. The chip with a protective film can be manufactured, for example, by attaching a protective film-forming film to the back surface of a wafer, forming a protective film by hardening the protective film-forming film, dividing the wafer into chips, and cutting the protective film along the outer periphery of the chip.

[0018] In this specification, the term "wafer" refers to semiconductor wafers made of elemental semiconductors such as silicon, germanium, and selenium, and compound semiconductors such as GaAs, GaP, InP, CdTe, ZnSe, and SiC; and insulating wafers made of insulators such as sapphire, glass, lithium niobate, and lithium tantalate. A circuit is formed on one surface of each of these wafers, and in this specification, the surface of the wafer on which the circuit is formed is referred to as the "circuit surface," and the surface of the wafer opposite to the circuit surface is referred to as the "back surface." The wafer is divided into chips by dicing or other means. In this specification, as in the case of the wafer, the surface of the chip on which the circuit is formed is referred to as the "circuit surface," and the surface of the chip opposite the circuit surface is referred to as the "back surface." Both the circuit surface of the wafer and the circuit surface of the chip are provided with protruding electrodes such as bumps, pillars, etc. The protruding electrodes are preferably made of solder.

[0019] Furthermore, by using the chip with the protective film, a substrate device can be manufactured. In this specification, the term "substrate device" refers to a device in which a chip with a protective film is flip-chip connected to a connection pad on a circuit board at a protruding electrode on the circuit surface of the chip. For example, when a semiconductor wafer is used as the wafer, a semiconductor device is an example of the substrate device.

[0020] The protective film-forming film of the present embodiment is energy ray curable.

[0021] In this specification, the term "energy rays" refers to electromagnetic waves or charged particle beams that have an energy quantum. Examples of energy rays include ultraviolet rays, radiation, and electron beams. Ultraviolet rays can be irradiated by using, for example, a high-pressure mercury lamp, a fusion lamp, a xenon lamp, a black light, or an LED lamp as an ultraviolet ray source. Electron beams can be irradiated by generating them using an electron beam accelerator or the like. In this specification, "energy ray curable" means a property that is cured by irradiation with energy rays, and "non-energy ray curable" means a property that is not cured even when irradiated with energy rays. Moreover, the term "non-curable" means a property that does not cure by any means such as heating or irradiation with energy rays.

[0022] The curing conditions when the protective film-forming film is cured with energy rays to form a protective film are not particularly limited as long as the protective film is cured to a degree that allows it to fully perform its function, and may be appropriately selected depending on the type of protective film-forming film. For example, the illuminance of the energy rays during energy ray curing of the energy ray curable protective film-forming film is 60 to 320 mW / cm 2 The amount of energy rays during the curing is preferably 100 to 1000 mJ / cm. 2 It is preferable that:

[0023] The protective film-forming film may, for example, contain an energy ray-curable component (a) and a polymer (b) having no energy ray-curable group. The components contained in the protective film-forming film will be described in detail later.

[0024] The protective film-forming film may be made of one layer (single layer) or may be made of two or more layers. When the protective film-forming film is made of multiple layers, these multiple layers may be the same or different from each other, and the combination of these multiple layers is not particularly limited.

[0025] In this specification, not only in the case of protective film-forming films, "multiple layers may be the same or different from each other" means "all layers may be the same, all layers may be different, or only some layers may be the same", and further, "multiple layers are different from each other" means "at least one of the constituent materials and thicknesses of each layer is different from each other".

[0026] The thickness of the protective film-forming film is preferably 1 to 100 μm, more preferably 3 to 80 μm, and particularly preferably 3 to 60 μm. When the thickness of the protective film-forming film is equal to or greater than the lower limit, a protective film having higher protective ability can be formed. When the thickness of the protective film-forming film is equal to or less than the upper limit, the thickness of the chip with the protective film can be prevented from becoming excessive, which is suitable for miniaturizing and thinning the semiconductor device. Here, "thickness of the protective film-forming film" means the thickness of the entire protective film-forming film, for example, the thickness of a protective film-forming film consisting of multiple layers means the total thickness of all layers that constitute the protective film-forming film. In this specification, the "thickness" can be determined by the method specified in JIS K 7130:1999 (ISO 4593:1993).

[0027] <<Composition for forming protective film>> The protective film-forming film can be formed using an energy ray curable composition for forming a protective film (sometimes simply referred to as a "composition for forming a protective film" in this specification) containing its constituent materials. For example, the protective film-forming film can be formed by applying the composition for forming a protective film to the surface to be formed and drying it as necessary. The ratio of the contents of the components that do not vaporize at room temperature in the composition for forming a protective film is usually the same as the ratio of the contents of the components in the protective film-forming film. In this specification, "room temperature" means a temperature that is not particularly cooled or heated, that is, a normal temperature, and examples thereof include a temperature of 18 to 28°C.

[0028] The protective film-forming composition may be applied by a known method, such as a method using various coaters such as an air knife coater, a blade coater, a bar coater, a gravure coater, a roll coater, a roll knife coater, a curtain coater, a die coater, a knife coater, a screen coater, a Mayer bar coater, or a kiss coater.

[0029] The drying conditions of the composition for forming a protective film are not particularly limited. However, when the composition for forming a protective film contains a solvent described later, it is preferable to heat-dry it. And, the composition for forming a protective film containing a solvent is preferably heat-dried under conditions of, for example, 70 to 130°C for 10 seconds to 5 minutes.

[0030] <Energy ray-curable protective film-forming composition (IV)> A preferred example of a composition for forming a protective film includes an energy ray-curable composition for forming a protective film (IV) (sometimes simply referred to as "composition (IV)" in this specification) containing the energy ray-curable component (a), the polymer (b) having no energy ray-curable group, and the inorganic filler (d).

[0031] [Energy ray curable component (a)] The energy ray curable component (a) is a component that is cured by irradiation with energy rays, and imparts film-forming properties, flexibility, etc. to the protective film-forming film, and is also a component for forming a hard protective film after curing. The protective film-forming film forms a protective film with good properties by containing the energy ray curable component (a). In the protective film-forming film, the energy ray-curable component (a) is preferably uncured and has adhesive properties, and more preferably is uncured and has adhesive properties.

[0032] The composition (IV) and the protective film-forming film preferably contain an energy ray-curable component (a) having a group containing an energy ray-curable C=C double bond. In addition, the energy ray-curable protective film-forming film preferably has a cure rate of 16% or less, more preferably 12% or less, and even more preferably 8% or less after being exposed to a circular daylight fluorescent lamp having a rated lamp power of 28 W at a distance of 1 m for 168 hours. In the conventional energy ray curable protective film-forming film, after storage under fluorescent light, the group containing the C=C double bond may undergo a curing reaction, and the tackiness may be lost before use. Since the curing rate is small, the protective film-forming film has excellent stability under fluorescent light during storage.

[0033] Examples of the energy ray curable component (a) include a polymer (a1) having an energy ray curable group and a weight average molecular weight of 7000 to 100000, and a compound (a2) having an energy ray curable group and a molecular weight of 100 to 7000. The polymer (a1) may be at least partially crosslinked with a crosslinking agent, or may not be crosslinked.

[0034] (Polymer (a1) having an energy ray-curable group and a weight average molecular weight of 7,000 to 100,000) An example of the polymer (a1) having an energy ray-curable group and a weight average molecular weight of 7,000 to 100,000 includes an acrylic resin (a1-1) obtained by reacting an acrylic polymer (a11) having a functional group capable of reacting with a group possessed by another compound with an energy ray-curable compound (a12) having a group reactive with the functional group and an energy ray-curable group such as a C=C double bond.

[0035] Examples of the functional group capable of reacting with a group possessed by another compound include a hydroxyl group, a carboxy group, an amino group, a substituted amino group (a group having a structure in which one or two hydrogen atoms of an amino group are substituted with a group other than a hydrogen atom), an epoxy group, etc. However, from the viewpoint of preventing corrosion of circuits of a wafer, a chip, etc., it is preferable that the functional group is a group other than a carboxy group. Of these, the functional group is preferably a hydroxyl group.

[0036] In the composition (IV) and the protective film-forming film, the content ratio of the polymer (a1) having an energy ray-curable group and having a weight average molecular weight of 7,000 to 100,000 relative to the total content of the energy ray-curable component (a) having a group containing an energy ray-curable C=C double bond is preferably 80 to 100%, more preferably 90 to 100%, and even more preferably 95 to 100%.

[0037] Acrylic polymers having functional groups (a11) The acrylic polymer (a11) having a functional group may be, for example, a polymer obtained by copolymerizing an acrylic monomer having the functional group with an acrylic monomer not having the functional group. In addition to these monomers, a monomer other than the acrylic monomer (non-acrylic monomer) may also be copolymerized. The acrylic polymer (a11) may be a random copolymer or a block copolymer, and the polymerization method may be a known method.

[0038] Examples of the acrylic monomer having a functional group include a hydroxyl group-containing monomer, a carboxyl group-containing monomer, an amino group-containing monomer, a substituted amino group-containing monomer, and an epoxy group-containing monomer.

[0039] Examples of the hydroxyl group-containing monomer include hydroxyalkyl (meth)acrylates such as hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; and non-(meth)acrylic unsaturated alcohols (unsaturated alcohols not having a (meth)acryloyl skeleton) such as vinyl alcohol and allyl alcohol.

[0040] Examples of the carboxy group-containing monomer include ethylenically unsaturated monocarboxylic acids (monocarboxylic acids having an ethylenically unsaturated bond) such as (meth)acrylic acid and crotonic acid; ethylenically unsaturated dicarboxylic acids (dicarboxylic acids having an ethylenically unsaturated bond) such as fumaric acid, itaconic acid, maleic acid and citraconic acid; anhydrides of the ethylenically unsaturated dicarboxylic acids; and (meth)acrylic acid carboxyalkyl esters such as 2-carboxyethyl methacrylate.

[0041] The acrylic monomer having a functional group is preferably a hydroxyl group-containing monomer.

[0042] In this specification, the term "(meth)acrylic acid" is a concept that includes both "acrylic acid" and "methacrylic acid". The same applies to terms similar to (meth)acrylic acid. For example, "(meth)acrylate" is a concept that includes both "acrylate" and "methacrylate", and "(meth)acryloyl group" is a concept that includes both "acryloyl group" and "methacryloyl group".

[0043] In this specification, when a structure in which one or more hydrogen atoms in a certain specific compound are replaced with a group other than a hydrogen atom is assumed, the compound having such a replaced structure is referred to as a "derivative" of the above-mentioned specific compound. In this specification, the term "group" includes not only an atomic group formed by bonding a plurality of atoms, but also a single atom.

[0044] The acrylic monomer having a functional group constituting the acrylic polymer (a11) may be of only one kind, or of two or more kinds. When there are two or more kinds, the combination and ratio thereof can be selected arbitrarily.

[0045] Examples of the acrylic monomer not having a functional group include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, ethyl ... Examples of (meth)acrylic acid alkyl esters include those in which the alkyl group constituting the alkyl ester has a chain structure having 1 to 18 carbon atoms, such as sononyl, decyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate (lauryl (meth)acrylate), tridecyl (meth)acrylate, tetradecyl (meth)acrylate (myristyl (meth)acrylate), pentadecyl (meth)acrylate, hexadecyl (meth)acrylate (palmityl (meth)acrylate), heptadecyl (meth)acrylate, and octadecyl (meth)acrylate (stearyl (meth)acrylate).

[0046] Examples of the acrylic monomer not having a functional group include alkoxyalkyl group-containing (meth)acrylic acid esters such as methoxymethyl (meth)acrylate, methoxyethyl (meth)acrylate, ethoxymethyl (meth)acrylate, and ethoxyethyl (meth)acrylate; (meth)acrylic acid esters having an aromatic group, including (meth)acrylic acid aryl esters such as phenyl (meth)acrylate; non-crosslinkable (meth)acrylamide and derivatives thereof; and (meth)acrylic acid esters having a non-crosslinkable tertiary amino group, such as N,N-dimethylaminoethyl (meth)acrylate and N,N-dimethylaminopropyl (meth)acrylate.

[0047] The acrylic monomer not having a functional group constituting the acrylic polymer (a11) may be of only one kind or of two or more kinds, and when it is of two or more kinds, the combination and ratio thereof can be arbitrarily selected.

[0048] Examples of the non-acrylic monomer include olefins such as ethylene and norbornene; vinyl acetate; and styrene. The non-acrylic monomer constituting the acrylic polymer (a11) may be of only one kind, or may be of two or more kinds. When it is of two or more kinds, the combination and ratio thereof can be selected arbitrarily.

[0049] In the acrylic polymer (a11), the ratio (content) of the amount of the structural unit derived from the acrylic monomer having the functional group to the total amount of the structural units constituting the acrylic polymer (a11) is preferably 0.1 to 50 mass%, more preferably 1 to 40 mass%, and particularly preferably 3 to 30 mass%. When the ratio is in such a range, the content of the energy ray curable group in the acrylic resin (a1-1) obtained by copolymerization of the acrylic polymer (a11) and the energy ray curable compound (a12) makes it possible to adjust the degree of curing of the protective film within a preferred range.

[0050] The acrylic polymer (a11) constituting the acrylic resin (a1-1) may be of only one kind, or may be of two or more kinds. When there are two or more kinds, the combination and ratio thereof can be selected arbitrarily.

[0051] The content ratio of the acrylic resin (a1-1) in the protective film-forming film relative to the total mass of the protective film-forming film is preferably 1 to 70 mass%, more preferably 5 to 60 mass%, and particularly preferably 10 to 50 mass%.

[0052] Energy ray curable compounds (a12) The energy ray curable compound (a12) preferably has one or more groups selected from the group consisting of an isocyanate group, an epoxy group, and a carboxy group as a group capable of reacting with the functional group of the acrylic polymer (a11), and more preferably has an isocyanate group as the group. For example, when the energy ray curable compound (a12) has an isocyanate group as the group, the isocyanate group easily reacts with the hydroxyl group of the acrylic polymer (a11) having a hydroxyl group as the functional group.

[0053] The number of the energy ray-curable groups that the energy ray-curable compound (a12) has in one molecule is not particularly limited, and can be appropriately selected in consideration of the physical properties, such as the shrinkage rate, required for the intended protective film, for example. For example, the energy ray-curable compound (a12) preferably has 1 to 5, and more preferably 1 to 3, energy ray-curable groups in one molecule.

[0054] Examples of the energy ray-curable compound (a12) include 2-methacryloyloxyethyl isocyanate, meta-isopropenyl-α,α-dimethylbenzyl isocyanate, methacryloyl isocyanate, allyl isocyanate, and 1,1-(bisacryloyloxymethyl)ethyl isocyanate; an acryloyl monoisocyanate compound obtained by reacting a diisocyanate compound or a polyisocyanate compound with hydroxyethyl (meth)acrylate; Examples of the isocyanate include an acryloyl monoisocyanate compound obtained by reacting a diisocyanate compound or a polyisocyanate compound with a polyol compound and hydroxyethyl (meth)acrylate. Among these, the energy ray-curable compound (a12) is preferably 2-methacryloyloxyethyl isocyanate.

[0055] The energy ray-curable compound (a12) constituting the acrylic resin (a1-1) may be of only one type, or of two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0056] In the acrylic resin (a1-1), the content ratio of the energy ray curable group derived from the energy ray curable compound (a12) to the content of the functional group derived from the acrylic polymer (a11) is preferably 20 to 120 mol%, more preferably 35 to 100 mol%, and particularly preferably 50 to 100 mol%. When the content ratio is in such a range, the adhesive strength of the cured product of the protective film-forming film becomes higher. Note that, when the energy ray curable compound (a12) is a monofunctional compound (having one of the groups in one molecule), the upper limit of the content ratio is 100 mol%, but when the energy ray curable compound (a12) is a polyfunctional compound (having two or more of the groups in one molecule), the upper limit of the content ratio may exceed 100 mol%.

[0057] The weight average molecular weight (Mw) of the polymer (a1) is preferably from 7,000 to 100,000, and more preferably from 8,000 to 20,000.

[0058] In this specification, unless otherwise specified, the "weight average molecular weight" is a polystyrene equivalent value measured by gel permeation chromatography (GPC).

[0059] The polymer (a1) contained in the composition (IV) and the protective film-forming film may be one type or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0060] (Compound (a2) having an energy ray-curable group and a molecular weight of 100 to 7000) The energy ray-curable group in the compound (a2) having an energy ray-curable group and a molecular weight of 100 to 7000 includes a group containing an energy ray-curable C=C double bond, and preferred examples thereof include a (meth)acryloyl group and a vinyl group.

[0061] The compound (a2) is not particularly limited as long as it satisfies the above conditions, and examples of the compound (a2) include a low molecular weight compound having an energy ray-curable group, an epoxy resin having an energy ray-curable group, and a phenol resin having an energy ray-curable group.

[0062] Among the compounds (a2), examples of the low molecular weight compound having an energy ray-curable group include polyfunctional monomers or oligomers, and acrylate compounds having a (meth)acryloyl group are preferred.

[0063] The acrylate-based compound may, for example, be a polyfunctional monomer or oligomer, and is preferably a polyfunctional acrylate-based compound having two or more (meth)acryloyl groups in one molecule. Examples of the polyfunctional acrylate compounds include 2-hydroxy-3-(meth)acryloyloxypropyl methacrylate, polyethylene glycol di(meth)acrylate, propoxylated ethoxylated bisphenol A di(meth)acrylate, 2,2-bis[4-((meth)acryloxypolyethoxy)phenyl]propane, ethoxylated bisphenol A di(meth)acrylate, 2,2-bis[4-((meth)acryloxydiethoxy)phenyl]propane, 9,9-bis[4-(2-(meth)acryloyloxyethoxy)phenyl]fluorene, 2,2-bis[4-((meth)acryloxypolypropoxy)phenyl]propane, tricyclodecane dimethanol di(meth)acrylate (also known as tricyclodecane dimethylol di(meth)acrylate), 1,10-decane diol di(meth)acrylate, 1, Bifunctional (meth)acrylates such as 6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, 2,2-bis[4-((meth)acryloxyethoxy)phenyl]propane, neopentyl glycol di(meth)acrylate, ethoxylated polypropylene glycol di(meth)acrylate, and 2-hydroxy-1,3-di(meth)acryloxypropane ((meth)acrylates having two (meth)acryloyl groups in one molecule); Polyfunctional (meth)acrylates ((meth)acrylates having three or more (meth)acryloyl groups in one molecule) such as tris(2-(meth)acryloxyethyl)isocyanurate, ε-caprolactone-modified tris-(2-(meth)acryloxyethyl)isocyanurate, ethoxylated glycerin tri(meth)acrylate, pentaerythritol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol poly(meth)acrylate, and dipentaerythritol hexa(meth)acrylate; Examples of the polyfunctional (meth)acrylate oligomer include a polyfunctional urethane (meth)acrylate oligomer (a (meth)acrylate oligomer having two or more (meth)acryloyl groups in one molecule).

[0064] Among the compounds (a2), examples of the epoxy resin having an energy ray curable group and the phenolic resin having an energy ray curable group that can be used include those described in paragraph 0043 of JP 2013-194102 A. Although such resins also fall under the category of resins constituting the thermosetting component described below, they are treated as the compound (a2) in the composition (IV).

[0065] The weight average molecular weight of the compound (a2) is preferably 100 to 7,000, and more preferably 200 to 5,000.

[0066] The compound (a2) contained in the composition (IV) and the protective film-forming film may be one type or two or more types, and when there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0067] The protective film-forming film preferably contains the compound (a2) as the energy ray curable component (a), more preferably contains a polyfunctional acrylate compound having two or more (meth)acryloyl groups in one molecule, and further preferably contains a polyfunctional urethane (meth)acrylate oligomer. The cured product (protective film) of the protective film-forming film containing such energy ray curable component (a) by energy ray irradiation has good protective ability and flexibility, and has particularly excellent properties.

[0068] When the composition (IV) and the protective film-forming film contain the energy ray-curable component (a), the content of the energy ray-curable component (a) in the composition (IV) and the protective film-forming film is preferably 60 to 200 parts by mass, more preferably 70 to 140 parts by mass, relative to 100 parts by mass of the content of the polymer (b) not having an energy ray-curable group, and may be, for example, 75 to 120 parts by mass or 210 to 280 parts by mass.

[0069] In the composition (IV), the content ratio of the energy ray curable component (a) relative to the total content of all components other than the solvent (i.e., the content ratio of the energy ray curable component (a) in the protective film-forming film relative to the total mass of the protective film-forming film) is preferably 12 to 31 mass%, more preferably 14 to 28 mass%, and more preferably 16 to 25 mass%. When the content ratio of the energy ray curable component (a) (i.e., the content ratio of the energy ray curable component (a)) is equal to or more than the lower limit, the energy ray curability of the protective film-forming film becomes better. When the content ratio of the energy ray curable component (a) (i.e., the content ratio of the energy ray curable component (a)) is equal to or less than the upper limit, it is easy to prepare a desired protective film-forming film.

[0070] [Polymer (b) having no energy ray-curable group] The composition (IV) and the energy ray-curable protective film-forming film preferably contain, in addition to the energy ray-curable component (a), a polymer (b) having no energy ray-curable group. The polymer (b) may be at least partially crosslinked with a crosslinking agent, or may not be crosslinked.

[0071] Examples of the polymer (b) having no energy ray-curable group include acrylic resins, phenoxy resins, urethane resins, polyesters, rubber-based resins, and acrylic urethane resins. Among these, the polymer (b) is preferably an acrylic resin (hereinafter sometimes abbreviated as "acrylic resin (b-1)").

[0072] The acrylic resin (b-1) may be a known one, and may be, for example, a homopolymer of one kind of acrylic monomer, a copolymer of two or more kinds of acrylic monomers, or a copolymer of one or more kinds of acrylic monomers and one or more kinds of monomers other than the acrylic monomers (non-acrylic monomers).

[0073] Examples of the acrylic monomer constituting the acrylic resin (b-1) include (meth)acrylic acid alkyl esters, (meth)acrylic acid esters having a cyclic skeleton, glycidyl group-containing (meth)acrylic acid esters, hydroxyl group-containing (meth)acrylic acid esters, substituted amino group-containing (meth)acrylic acid esters, etc. Here, the "substituted amino group" is as explained above.

[0074] Examples of the (meth)acrylic acid alkyl ester include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, and (meth)acrylic acid. Examples of (meth)acrylic acid alkyl esters in which the alkyl group constituting the alkyl ester has a chain structure having 1 to 18 carbon atoms include isononyl, decyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate (lauryl (meth)acrylate), tridecyl (meth)acrylate, tetradecyl (meth)acrylate (myristyl (meth)acrylate), pentadecyl (meth)acrylate, hexadecyl (meth)acrylate (palmityl (meth)acrylate), heptadecyl (meth)acrylate, and octadecyl (meth)acrylate (stearyl (meth)acrylate).

[0075] Examples of the (meth)acrylic acid ester having a cyclic skeleton include cycloalkyl (meth)acrylic acid esters such as isobornyl (meth)acrylate and dicyclopentanyl (meth)acrylate; (Meth)acrylic acid aralkyl esters such as benzyl (meth)acrylate; (Meth)acrylic acid cycloalkenyl esters such as (meth)acrylic acid dicyclopentenyl ester; (Meth)acrylic acid cycloalkenyloxyalkyl esters such as (meth)acrylic acid dicyclopentenyloxyethyl ester are included.

[0076] The glycidyl group-containing (meth)acrylic acid ester may, for example, be glycidyl (meth)acrylate. Examples of the hydroxyl group-containing (meth)acrylic acid ester include hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. The substituted amino group-containing (meth)acrylic acid ester may, for example, be N-methylaminoethyl (meth)acrylate.

[0077] Examples of the non-acrylic monomer constituting the acrylic resin (b-1) include olefins such as ethylene and norbornene; vinyl acetate; and styrene.

[0078] The polymer (b) having no energy ray-curable group and at least a portion of which is crosslinked with a crosslinking agent may be, for example, a polymer in which a reactive functional group in the polymer (b) has reacted with a crosslinking agent. The reactive functional group may be appropriately selected according to the type of crosslinking agent, and is not particularly limited. For example, when the crosslinking agent is a polyisocyanate compound, the reactive functional group may be a hydroxyl group, a carboxyl group, an amino group, etc., and among these, a hydroxyl group having high reactivity with an isocyanate group is preferred. When the crosslinking agent is an epoxy compound, the reactive functional group may be a carboxyl group, an amino group, an amide group, etc., and among these, a carboxyl group having high reactivity with an epoxy group is preferred. However, from the viewpoint of preventing corrosion of the circuits of a semiconductor wafer or a semiconductor chip, the reactive functional group is preferably a group other than a carboxyl group.

[0079] The polymer (b) having the reactive functional group and not having the energy ray curable group may be, for example, one obtained by polymerizing at least a monomer having the reactive functional group. In the case of the acrylic resin (b-1), one or both of the acrylic monomers and non-acrylic monomers listed as the monomers constituting the acrylic resin may be one having the reactive functional group. For example, the polymer (b) having a hydroxyl group as a reactive functional group may be one obtained by polymerizing a hydroxyl group-containing (meth)acrylic acid ester, and other examples include one obtained by polymerizing a monomer in which one or more hydrogen atoms in the acrylic monomers or non-acrylic monomers listed above are substituted with the reactive functional group.

[0080] In the polymer (b) having a reactive functional group, the ratio (content) of the amount of the structural unit derived from the monomer having a reactive functional group to the total amount of the structural units constituting the polymer (b) is preferably 1% by mass or more and 20% by mass or less, more preferably 2% by mass or more and 10% by mass or less. When the ratio is in such a range, the degree of crosslinking in the polymer (b) becomes a more preferable range.

[0081] The weight average molecular weight (Mw) of the polymer (b) having no energy ray-curable group is preferably from 10,000 to 2,000,000, more preferably from 100,000 to 1,500,000, in order to improve the film-forming property of the composition (IV). Here, the "weight average molecular weight" is as explained above.

[0082] The polymer (b) not having an energy ray-curable group contained in the composition (IV) and the energy ray-curable protective film-forming film may be one type or two or more types, and when there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0083] The composition (IV) may contain either one or both of the polymer (a1) and the compound (a2). When the composition (IV) contains the compound (a2), it is preferable that the composition (IV) further contains the polymer (b) having no energy ray curable group, and in this case, it is also preferable that the composition (IV) further contains the (a1). The composition (IV) may not contain the compound (a2), and may contain both the polymer (a1) and the polymer (b) having no energy ray curable group.

[0084] When the composition (IV) contains the polymer (a1), the compound (a2), and the polymer (b) having no energy ray-curable group, the content of the compound (a2) in the composition (IV) is preferably 10 parts by mass or more and 400 parts by mass or less, and more preferably 30 parts by mass or more and 350 parts by mass or less, relative to 100 parts by mass of the total content of the polymer (a1) and the polymer (b) having no energy ray-curable group.

[0085] In the composition (IV), the ratio of the total content of the energy ray curable component (a) and the polymer (b) having no energy ray curable group to the total content of components other than the solvent (i.e., the total content of the energy ray curable component (a) and the polymer (b) having no energy ray curable group in the protective film-forming film) is preferably 5% by mass or more and 90% by mass or less, more preferably 10% by mass or more and 80% by mass or less, and particularly preferably 20% by mass or more and 70% by mass or less. When the ratio of the content of the energy ray curable component is in such a range, the energy ray curability of the protective film-forming film becomes better.

[0086] [Other ingredients] The composition (IV) and the protective film-forming film may contain other components that do not fall under either the energy ray curable component (a) or the acrylic resin (b-1), as long as the effects of the present invention are not impaired. Examples of the other components include photopolymerization initiators (c); inorganic fillers (d); coupling agents (e); crosslinking agents (f); colorants (g); thermosetting components (h); ultraviolet absorbers (m); and general-purpose additives (z).

[0087] (Photopolymerization initiator (c)) When the composition (IV) and the protective film-forming film contain a photopolymerization initiator (c), the polymerization (curing) reaction of the energy ray-curable component (a) can be efficiently promoted.

[0088] Examples of the photopolymerization initiator include benzoin compounds such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, benzoin benzoic acid, benzoin methyl benzoate, and benzoin dimethyl ketal; acetophenone compounds such as acetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 2,2-dimethoxy-1,2-diphenylethane-1-one, 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methylpropan-1-one, and 2-(dimethylamino)-1-(4-morpholinophenyl)-2-benzyl-1-butanone; and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide. Examples of suitable compounds include acylphosphine oxide compounds such as 2,4,6-trimethylbenzoyldiphenylphosphine oxide; sulfide compounds such as benzyl phenyl sulfide and tetramethylthiuram monosulfide; α-ketol compounds such as 1-hydroxycyclohexyl phenyl ketone; azo compounds such as azobisisobutyronitrile; titanocene compounds such as titanocene; thioxanthone compounds such as thioxanthone; peroxide compounds; diketone compounds such as diacetyl; benzyl; dibenzyl; benzophenone; 2,4-diethylthioxanthone; 1,2-diphenylmethane; 2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propanone; and quinone compounds such as 1-chloroanthraquinone and 2-chloroanthraquinone. Examples of the photopolymerization initiator include photosensitizers such as amines.

[0089] The photopolymerization initiator (c) contained in the composition (IV) and the protective film-forming film may be one type or two or more types, and when two or more types are used, the combination and ratio thereof can be selected arbitrarily. For example, a photopolymerization initiator that is liquid at room temperature and highly reactive, such as 2-hydroxy-2-methyl-1-phenylpropan-1-one, can be used alone to efficiently crosslink the protective film-forming film, thereby increasing the gel fraction. A photopolymerization initiator with low reactivity, such as 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methylpropan-1-one or 1-hydroxycyclohexyl-phenyl ketone, can be used in combination with a photopolymerization initiator with high reactivity, such as 2-(dimethylamino)-1-(4-morpholinophenyl)-2-benzyl-1-butanone, to efficiently crosslink the protective film-forming film, thereby increasing the gel fraction.

[0090] When a photopolymerization initiator (c) is used, the content of the photopolymerization initiator (c) in the composition (IV) is preferably 0.1 to 20 parts by mass, more preferably 1 to 10 parts by mass, and particularly preferably 2 to 5 parts by mass, per 100 parts by mass of the energy ray-curable component (a).

[0091] (Inorganic filler (d)) When the composition (IV) and the protective film-forming film contain an inorganic filler (d), the thermal expansion coefficient of the cured product of the protective film-forming film (e.g., a protective film) can be more easily adjusted by adjusting the amount of the inorganic filler (d) in the composition (IV) and the protective film-forming film. For example, the reliability of the package obtained by using the protective film-forming film is further improved by optimizing the thermal expansion coefficient of the protective film for the object on which the protective film is formed. In addition, by using a protective film-forming film containing an inorganic filler (d), it is also possible to reduce the moisture absorption rate of the cured product of the protective film-forming film (e.g., a protective film) and improve the heat dissipation property.

[0092] Examples of the inorganic filler (d) include powders of inorganic materials such as silica, alumina, talc, calcium carbonate, titanium white, red iron oxide, silicon carbide, and boron nitride; beads made by shaping these inorganic materials; surface-modified products of these inorganic materials; single crystal fibers of these inorganic materials; and glass fibers. Among these, the inorganic filler (d) is preferably silica or alumina.

[0093] The inorganic filler (d) contained in the composition (IV) and the protective film-forming film may be one type or two or more types, and when there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0094] The average particle size of the inorganic filler (d) is preferably 15 μm or less, more preferably 12 μm or less, and even more preferably 10 μm or less. The average particle size of the inorganic filler (d) may be 0.1 μm or more, 0.2 μm or more, or 0.4 μm or more.

[0095] In the composition (IV), the ratio of the content of the inorganic filler (d) to the total content of all components other than the solvent (i.e., the ratio of the content of the inorganic filler (d) to the total mass of the protective film-forming film in the protective film-forming film) is preferably 35 to 75 mass%, and may be, for example, any of 45 to 70 mass% and 50 to 65 mass%. By having the ratio in such a range, the effect of using the inorganic filler (d) is enhanced without impairing the properties of the protective film-forming film.

[0096] (Coupling Agent (e)) When the composition (IV) and the protective film-forming film contain a coupling agent (e) having a functional group capable of reacting with an inorganic compound or an organic compound, the adhesiveness and adhesion of the protective film-forming film to an adherend are improved. In addition, the cured product of the protective film-forming film (e.g., a protective film) is improved in water resistance without impairing heat resistance.

[0097] The coupling agent (e) is preferably a compound having a functional group capable of reacting with a functional group possessed by the acrylic resin (b-1), the energy ray-curable component (a), etc., and is more preferably a silane coupling agent. Preferred examples of the silane coupling agent include 3-glycidyloxypropyltrimethoxysilane, 3-glycidyloxypropylmethyldiethoxysilane, 3-glycidyloxypropyltriethoxysilane, 3-glycidyloxymethyldiethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-methacryloyloxypropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-(2-aminoethylamino)propyltrimethoxysilane, 3-(2- Examples of the silane include bis(3-(aminoethylamino)propylmethyldiethoxysilane, 3-(phenylamino)propyltrimethoxysilane, 3-anilinopropyltrimethoxysilane, 3-ureidopropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, bis(3-triethoxysilylpropyl)tetrasulfane, methyltrimethoxysilane, methyltriethoxysilane, vinyltrimethoxysilane, vinyltriacetoxysilane, and imidazole silane.

[0098] The coupling agent (e) contained in the composition (IV) and the protective film-forming film may be one type or two or more types, and when there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0099] When the coupling agent (e) is used, the content of the coupling agent (e) in the composition (IV) and the protective film-forming film is preferably 0.03 to 20 parts by mass relative to 100 parts by mass of the total content of the energy ray curable component (a) and the acrylic resin (b-1). When the content of the coupling agent (e) is equal to or more than the lower limit, the effects of using the coupling agent (e), such as improved dispersibility of the inorganic filler (d) in the resin and improved adhesion of the protective film-forming film to the adherend, are more significantly obtained. When the content of the coupling agent (e) is equal to or less than the upper limit, the generation of outgassing is more suppressed.

[0100] (Crosslinking agent (f)) When the acrylic resin (b-1) has a functional group such as a vinyl group, a (meth)acryloyl group, an amino group, a hydroxyl group, a carboxyl group, or an isocyanate group that can be bonded to other compounds, the composition (IV) and the protective film-forming film may contain a crosslinking agent (f). The crosslinking agent (f) is a component for bonding the functional group in the acrylic resin (b-1) to other compounds to crosslink the functional group, and by crosslinking in this way, the initial adhesive strength and cohesive strength of the protective film-forming film can be adjusted.

[0101] Examples of the crosslinking agent (f) include organic polyvalent isocyanate compounds, organic polyvalent imine compounds, metal chelate crosslinking agents (crosslinking agents having a metal chelate structure), and aziridine crosslinking agents (crosslinking agents having an aziridinyl group).

[0102] Examples of the organic polyisocyanate compound include aromatic polyisocyanate compounds, aliphatic polyisocyanate compounds, and alicyclic polyisocyanate compounds (hereinafter, these compounds may be collectively referred to as "aromatic polyisocyanate compounds, etc."); trimers, isocyanurates, and adducts of the aromatic polyisocyanate compounds, etc.; and terminal isocyanate urethane prepolymers obtained by reacting the aromatic polyisocyanate compounds, etc. with polyol compounds. The "adduct" refers to a reaction product of the aromatic polyisocyanate compound, aliphatic polyisocyanate compound, or alicyclic polyisocyanate compound with a low molecular weight active hydrogen-containing compound such as ethylene glycol, propylene glycol, neopentyl glycol, trimethylolpropane, or castor oil. Examples of the adduct include a xylylene diisocyanate adduct of trimethylolpropane, as described below. Moreover, the term "isocyanate-terminated urethane prepolymer" refers to a prepolymer having a urethane bond and an isocyanate group at the terminal of the molecule.

[0103] More specific examples of the organic polyisocyanate compound include 2,4-tolylene diisocyanate; 2,6-tolylene diisocyanate; 1,3-xylylene diisocyanate; 1,4-xylylene diisocyanate; diphenylmethane-4,4'-diisocyanate; diphenylmethane-2,4'-diisocyanate; 3-methyldiphenylmethane diisocyanate; hexamethylene diisocyanate; isophorone diisocyanate; dicyclohexylmethane-4,4'-diisocyanate; dicyclohexylmethane-2,4'-diisocyanate; a compound in which one or more of tolylene diisocyanate, hexamethylene diisocyanate, and xylylene diisocyanate are added to all or a portion of the hydroxyl groups of a polyol such as trimethylolpropane; lysine diisocyanate, and the like.

[0104] Examples of the organic polyvalent imine compound include N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxamide), trimethylolpropane-tri-β-aziridinylpropionate, tetramethylolmethane-tri-β-aziridinylpropionate, N,N'-toluene-2,4-bis(1-aziridinecarboxamide)triethylenemelamine, and the like.

[0105] When an organic polyisocyanate compound is used as the crosslinking agent (f), it is preferable to use a hydroxyl group-containing polymer as the acrylic resin (b-1). When the crosslinking agent (f) has an isocyanate group and the acrylic resin (b-1) has a hydroxyl group, a crosslinked structure can be easily introduced into the protective film-forming film by the reaction between the crosslinking agent (f) and the acrylic resin (b-1).

[0106] The crosslinking agent (f) contained in the composition (IV) and the protective film-forming film may be one type or two or more types, and when there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0107] When the crosslinking agent (f) is used, the content of the crosslinking agent (f) in the composition (IV) is preferably 0.01 to 20 parts by mass per 100 parts by mass of the acrylic resin (b-1). When the content of the crosslinking agent (f) is equal to or more than the lower limit, the effect of using the crosslinking agent (f) is more remarkable. When the content of the crosslinking agent (f) is equal to or less than the upper limit, the excessive use of the crosslinking agent (f) is suppressed.

[0108] (Colorant (g)) When a colorant (g) is used, the colorant (g) is preferably an inorganic pigment, such as carbon black, cobalt-based pigments, iron-based pigments, chromium-based pigments, titanium-based pigments, vanadium-based pigments, zirconium-based pigments, molybdenum-based pigments, ruthenium-based pigments, platinum-based pigments, ITO (indium tin oxide)-based pigments, and ATO (antimony tin oxide)-based pigments, with carbon black being preferred.

[0109] The content of the colorant (g) in the composition (IV) and the protective film-forming film may be appropriately adjusted. For example, in the composition (IV), the content ratio of the colorant (g) to the total content of all components other than the solvent (i.e., the content ratio of the colorant (g) to the total mass of the protective film-forming film in the protective film-forming film) is preferably 0.05% by mass or more and less than 1% by mass, more preferably 0.05 to 0.8% by mass, and particularly preferably 0.1 to 0.5% by mass. When the ratio is equal to or more than the lower limit, the effect of using the colorant (g) is more prominent. When the ratio is equal to or less than the upper limit, poor curing caused by energy rays is suppressed.

[0110] The colorant (g) may contain, in addition to inorganic pigments, known substances such as organic pigments and organic dyes.

[0111] The colorant (g) contained in the composition (IV) and the protective film-forming film may be one type or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0112] (Thermosetting component (h)) When the composition (IV) and the protective film-forming film contain an energy ray-curable component (a) and a thermosetting component (h), the adhesive strength of the protective film-forming film to an adherend is improved by heating, and the strength of the cured product of the protective film-forming film (e.g., a protective film) is also improved.

[0113] Examples of the thermosetting component (h) include epoxy-based thermosetting resins, polyimide resins, and unsaturated polyester resins, with epoxy-based thermosetting resins being preferred.

[0114] The epoxy thermosetting resin is composed of an epoxy resin (h1) and a thermosetting agent (h2). The epoxy-based thermosetting resin contained in the composition (IV) and the protective film-forming film may be one type or two or more types, and when there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0115] (Ultraviolet absorber (m)) The composition (IV) and the protective film-forming film preferably contain an ultraviolet absorber. By using the composition (IV) containing an ultraviolet absorber, the protective film-forming film formed has excellent stability under fluorescent light. Examples of the ultraviolet absorber include 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-tert-amyl-5'-isobutylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-isobutyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-isobutyl-5'-methylphenyl)-5-chlorobenzotriazole, and 2-(2'-hydroxy-3'-isobutyl-5'-propylphenyl)-5-chlorobenzotriazole. 2'-hydroxyphenyl-5-chlorobenzotriazole-based ultraviolet absorbers such as 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)benzotriazole and 2-(2'-hydroxy-5'-methylphenyl)benzotriazole; 2,2'-dihydroxy-4-methoxybenzophenone, 2,2'-dihydroxy-4,4'-dimethoxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, etc. ,2'-Dihydroxybenzophenone-based UV absorbers; 2-hydroxybenzophenone-based UV absorbers such as 2-hydroxy-4-methoxybenzophenone and 2,4-dihydroxybenzophenone; salicylic acid ester-based UV absorbers such as phenyl salicylate and 4-tert-butyl-phenyl-salicylate; cyanoacrylate-based UV absorbers such as 2-ethyl-hexyl-2-cyano-3,3-diphenylacrylate, ethyl-2-cyano-3,3-diphenylacrylate, and octyl-2-cyano-3,3-diphenylacrylate; 2-( Examples of such ultraviolet absorbents include triazine-based ultraviolet absorbents such as 4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl)-5-hydroxyphenyl, 2-(2,4-dihydroxyphenyl)-4,6-bis-(2,4-dimethylphenyl)-1,3-5-triazine, 2,4-bis[2-hydroxy-4-butoxyphenyl]-6-(2,4-dibutoxyphenyl)-1,3,5-triazine, and tris(hydroxyphenyl)triazine; and reactive ultraviolet absorbents in which an acryloyl group or a methacryloyl group is introduced into a benzotriazole skeleton.

[0116] In composition (IV), the ratio of the content of the ultraviolet absorber to the total content of all components other than the solvent (i.e., the ratio of the content of the ultraviolet absorber in the protective film-forming film to the total mass of the protective film-forming film) is preferably 0.1 to 5.0 mass%, more preferably 0.2 to 4.5 mass%, and even more preferably 0.4 to 4.0 mass%. When the ratio is equal to or greater than the lower limit, the effect of using the ultraviolet absorber is more pronounced. When the ratio is equal to or less than the upper limit, excessive use of the ultraviolet absorber is suppressed.

[0117] (General purpose additives (z)) The general-purpose additive (z) may be a known one and may be selected according to the purpose without any particular limitation. Preferable general-purpose additive (z) includes, for example, a plasticizer, an antistatic agent, an antioxidant, a gettering agent, etc.

[0118] The general-purpose additive (z) contained in the composition (IV) and the protective film-forming film may be one type or two or more types, and when there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0119] When the general-purpose additive (z) is used, the content of the general-purpose additive (z) in the composition (IV) and the protective film-forming film is not particularly limited and may be appropriately selected depending on the purpose.

[0120] <<Method of manufacturing a composition for forming an energy ray-curable protective film>> The energy ray-curable protective film-forming composition such as composition (IV) can be obtained by blending the respective components constituting the composition. The order of addition of the components when blending is not particularly limited, and two or more components may be added simultaneously. When a solvent is used, the solvent may be used by mixing it with any of the other ingredients to pre-dilute the ingredients, or the solvent may be used by mixing it with any of the other ingredients without pre-diluting the ingredients. The method for mixing the components during blending is not particularly limited, and may be appropriately selected from known methods such as a method of mixing by rotating a stirrer or stirring blades, a method of mixing using a mixer, a method of mixing by adding ultrasound, etc. The temperature and time during addition and mixing of each component are not particularly limited as long as the components do not deteriorate, and may be adjusted appropriately, but the temperature is preferably 15°C or higher and 30°C or lower.

[0121] [solvent] Composition (IV) preferably further contains a solvent. Composition (IV) containing a solvent has good handleability. The solvent is not particularly limited, but preferred examples include hydrocarbons such as toluene and xylene; alcohols such as methanol, ethanol, 2-propanol, isobutyl alcohol (2-methylpropan-1-ol), and 1-butanol; esters such as ethyl acetate; ketones such as acetone and methyl ethyl ketone; ethers such as tetrahydrofuran; and amides (compounds having an amide bond) such as dimethylformamide and N-methylpyrrolidone. The solvent contained in the composition (IV) may be only one type, or may be two or more types. When two or more types are contained, the combination and ratio thereof can be selected arbitrarily.

[0122] A more preferred example of the solvent contained in composition (IV) is methyl ethyl ketone, etc., which allows the components contained in composition (IV) to be mixed more uniformly.

[0123] The content of the solvent in the composition (IV) is not particularly limited, and may be appropriately selected depending on, for example, the types of components other than the solvent.

[0124] <<Method of manufacturing the composition for forming the protective film>> The energy ray-curable protective film-forming composition such as composition (IV) can be obtained by blending the respective components constituting the composition. The order of addition of the components when blending is not particularly limited, and two or more components may be added simultaneously. The method for mixing the components during blending is not particularly limited, and may be appropriately selected from known methods such as a method of mixing by rotating a stirrer or stirring blades, a method of mixing using a mixer, a method of mixing by adding ultrasound, etc. The temperature and time during addition and mixing of each component are not particularly limited as long as the components do not deteriorate, and may be adjusted appropriately. A temperature of 15 to 30°C is preferred.

[0125] Fig. 1 is a cross-sectional view showing an example of the protective film-forming film of the present embodiment. In addition, the drawings used in the following description may show the main parts in an enlarged manner for the sake of convenience in order to make the features of the present invention easier to understand, and the dimensional ratios of each component may not necessarily be the same as the actual ones.

[0126] The protective film-forming film 13 shown here has a first release film 151 on one of its surfaces (sometimes referred to as the "first surface" in this specification) 13a, and a second release film 152 on the other surface (sometimes referred to as the "second surface" in this specification) 13b opposite the first surface 13a. Such a protective film-forming film 13 is suitable for storage, for example, in a roll form.

[0127] The protective film-forming film 13 has the above-mentioned characteristics. The protective film-forming film 13 can be formed using the above-mentioned protective film-forming composition.

[0128] The first release film 151 and the second release film 152 may both be known films. The first release film 151 and the second release film 152 may be the same as each other, or may be different from each other, for example, in that the peeling forces required to peel them from the protective film-forming film 13 are different from each other.

[0129] 1, one of the first release film 151 and the second release film 152 is removed, and the resulting exposed surface becomes a surface to be attached to the back surface of a wafer (not shown). Then, the remaining other of the first release film 151 and the second release film 152 is removed, and the resulting exposed surface becomes a surface to be attached to a support sheet or a dicing sheet, which will be described later.

[0130] Figure 1 shows an example in which a release film is provided on both sides (first side 13a and second side 13b) of the protective film-forming film 13, but the release film may be provided on only one side of the protective film-forming film 13, i.e., only the first side 13a or only the second side 13b.

[0131] The protective film-forming film of this embodiment can be attached to the back surface of the wafer without using a support sheet described later. In that case, a release film may be provided on the surface of the protective film-forming film opposite to the surface attached to the wafer, and this release film may be removed at an appropriate time.

[0132] On the other hand, the protective film-forming film of the present embodiment can be used in combination with a support sheet described later to form a composite sheet for forming a protective film, which can perform both the formation of a protective film and dicing. Hereinafter, such a composite sheet for forming a protective film will be described.

[0133] ◇Composite sheet for forming protective film A composite sheet for forming a protective film according to one embodiment of the present invention comprises a support sheet and the protective film-forming film according to one embodiment of the present invention provided on one surface of the support sheet.

[0134] In this specification, as long as the laminated structure of the support sheet and the cured product of the protective film-forming film is maintained even after the protective film-forming film has hardened, this laminated structure is referred to as a "composite sheet for forming a protective film."

[0135] Each layer constituting the composite sheet for forming a protective film will be described in detail below.

[0136] ◎ Support sheet The support sheet may be one layer (single layer) or two or more layers. When the support sheet is made of multiple layers, the constituent materials and thicknesses of the multiple layers may be the same or different, and the combination of the multiple layers is not particularly limited as long as it does not impair the effects of the present invention.

[0137] The support sheet is preferably transparent, and may be colored depending on the purpose. In the present embodiment in which the protective film-forming film has energy ray curing properties, the support sheet is preferably one that transmits energy rays.

[0138] Examples of the support sheet include a sheet having a substrate and a pressure-sensitive adhesive layer provided on one surface of the substrate, a sheet consisting of only a substrate, etc. When the support sheet has a pressure-sensitive adhesive layer, the pressure-sensitive adhesive layer is disposed between the substrate and the protective film-forming film in the composite sheet for forming a protective film.

[0139] When a support sheet having a substrate and a pressure-sensitive adhesive layer is used, the adhesion and peelability between the support sheet and the protective film-forming film in the composite sheet for forming a protective film can be easily adjusted. When a support sheet consisting of only a substrate is used, the composite sheet for forming a protective film can be produced at low cost.

[0140] Examples of the composite sheet for forming a protective film according to this embodiment will be described below for each type of support sheet with reference to the drawings.

[0141] FIG. 2 is a cross-sectional view that illustrates an example of the composite sheet for forming a protective film according to the present embodiment. In FIG. 2 and subsequent figures, the same components as those shown in the figures already described are given the same reference numerals as in the figures already described, and detailed description thereof will be omitted.

[0142] The composite sheet 101 for forming a protective film shown here is composed of a support sheet 10 and a protective film forming film 13 provided on one side 10a (sometimes referred to as the "first side" in this specification) of the support sheet 10. The support sheet 10 is configured to include a base material 11 and an adhesive layer 12 provided on one surface (first surface) 11a of the base material 11. In the composite sheet 101 for forming a protective film, the adhesive layer 12 is disposed between the base material 11 and a protective film-forming film 13. That is, the composite sheet 101 for forming a protective film is configured by laminating a substrate 11, a pressure-sensitive adhesive layer 12, and a protective film-forming film 13 in this order in the thickness direction. The first surface 10a of the support sheet 10 is the same as the surface 12a of the pressure-sensitive adhesive layer 12 opposite the substrate 11 side (sometimes referred to as the "first surface" in this specification).

[0143] The composite sheet 101 for forming a protective film further includes a jig adhesive layer 16 and a release film 15 on the protective film-forming film 13 . In the composite sheet 101 for forming a protective film, the protective film-forming film 13 is laminated on the entire or almost entire surface of the first surface 12a of the adhesive layer 12, and the jig adhesive layer 16 is laminated on a part of the surface 13a of the protective film-forming film 13 opposite the adhesive layer 12 side (sometimes referred to as the "first surface" in this specification), i.e., on a region near the peripheral portion. Furthermore, a release film 15 is laminated on the region of the first surface 13a of the protective film-forming film 13 where the jig adhesive layer 16 is not laminated, and on the surface 16a of the jig adhesive layer 16 opposite the protective film-forming film 13 side (sometimes referred to as the "first surface" in this specification). A support sheet 10 is provided on the surface 13b of the protective film-forming film 13 opposite the first surface 13a (sometimes referred to as the "second surface" in this specification).

[0144] Not only in the case of the composite sheet 101 for forming a protective film, but in the composite sheet for forming a protective film of this embodiment, the release film (for example, release film 15 shown in Figure 2) has an optional configuration, and the composite sheet for forming a protective film of this embodiment may or may not have a release film.

[0145] The jig adhesive layer 16 is used to fix the composite sheet for forming a protective film 101 to a jig such as a ring frame. The jig adhesive layer 16 may have, for example, a single-layer structure containing an adhesive component, or may have a multi-layer structure including a core sheet and layers containing an adhesive component provided on both sides of the core sheet.

[0146] The composite sheet 101 for forming a protective film is used by attaching the back surface of a wafer to the first surface 13a of the protective film forming film 13 with the release film 15 removed, and further attaching the first surface 16a of the jig adhesive layer 16 to a jig such as a ring frame.

[0147] Fig. 3 is a cross-sectional view showing a schematic diagram of another example of the composite sheet for forming a protective film according to the present embodiment. The composite sheet for forming a protective film 102 shown here is the same as the composite sheet for forming a protective film 101 shown in Fig. 2, except that the shape and size of the protective film-forming film are different, and the jig adhesive layer is laminated on the first surface of the pressure-sensitive adhesive layer, not on the first surface of the protective film-forming film.

[0148] More specifically, in the composite sheet 102 for forming a protective film, the protective film-forming film 23 is laminated in a part of the region of the first surface 12a of the adhesive layer 12, that is, in the central region in the width direction (left and right direction in FIG. 3) of the adhesive layer 12. Furthermore, in the region of the first surface 12a of the adhesive layer 12 where the protective film-forming film 23 is not laminated, the jig adhesive layer 16 is laminated so as to surround the protective film-forming film 23 from the outside in the width direction without contact. A release film 15 is laminated on the surface (sometimes referred to as the "first surface" in this specification) 23a of the protective film-forming film 23 opposite the adhesive layer 12 side and the first surface 16a of the jig adhesive layer 16. A support sheet 10 is provided on the surface (sometimes referred to as the "second surface" in this specification) 23b of the protective film-forming film 23 opposite the first surface 23a.

[0149] FIG. 4 is a cross-sectional view that illustrates a schematic diagram of still another example of the composite sheet for forming a protective film according to the present embodiment. The composite sheet 103 for forming a protective film shown here is the same as the composite sheet 102 for forming a protective film shown in FIG.

[0150] FIG. 5 is a cross-sectional view that illustrates a schematic diagram of still another example of the composite sheet for forming a protective film according to the present embodiment. The composite sheet 104 for forming a protective film shown here is the same as the composite sheet 101 for forming a protective film shown in FIG.

[0151] The support sheet 20 is composed of only a substrate 11 . That is, the protective film-forming composite sheet 104 is configured by laminating the base material 11 and the protective film-forming film 13 in the thickness direction. The surface (first surface) 20 a of the support sheet 20 on the protective film-forming film 13 side is the same as the first surface 11 a of the base material 11 . The substrate 11 has adhesiveness at least on its first surface 11a.

[0152] The composite sheet for forming a protective film of this embodiment is not limited to that shown in Figures 2 to 5, and may be one in which some of the configurations shown in Figures 2 to 5 have been changed or removed, or other configurations may be added to those described above, within the scope that does not impair the effects of the present invention.

[0153] Next, each layer constituting the support sheet will be described in more detail.

[0154] ○Base material The substrate is in the form of a sheet or film, and examples of the constituent materials thereof include various resins. Examples of the resin include polyethylenes such as low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), and high-density polyethylene (HDPE); polyolefins other than polyethylene such as polypropylene, polybutene, polybutadiene, polymethylpentene, and norbornene resin; ethylene-based copolymers (copolymers obtained by using ethylene as a monomer) such as ethylene-vinyl acetate copolymer, ethylene-(meth)acrylic acid copolymer, ethylene-(meth)acrylic acid ester copolymer, and ethylene-norbornene copolymer; vinyl chloride-based resins (copolymers obtained by using vinyl chloride as a monomer) such as polyvinyl chloride and vinyl chloride copolymer. resins having aromatic ring groups); polystyrene; polycycloolefins; polyesters such as polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, polyethylene isophthalate, polyethylene-2,6-naphthalenedicarboxylate, and wholly aromatic polyesters in which all constituent units have aromatic cyclic groups; copolymers of two or more of the above polyesters; poly(meth)acrylic acid esters; polyurethanes; polyurethane acrylates; polyimides; polyamides; polycarbonates; fluororesins; polyacetals; modified polyphenylene oxides; polyphenylene sulfides; polysulfones; and polyether ketones. The resin may also be a polymer alloy such as a mixture of the polyester and another resin. The polymer alloy of the polyester and another resin is preferably one in which the amount of the resin other than the polyester is relatively small. Examples of the resin include crosslinked resins in which one or more of the resins exemplified above are crosslinked; and modified resins such as ionomers using one or more of the resins exemplified above.

[0155] The resin constituting the substrate may be of only one type, or of two or more types. When two or more types are used, the combination and ratio thereof can be selected arbitrarily.

[0156] The substrate may consist of one layer (single layer), or may consist of two or more layers. When the substrate consists of multiple layers, the multiple layers may be the same or different, and the combination of the multiple layers is not particularly limited.

[0157] The thickness of the substrate is preferably 50 to 300 μm, and more preferably 60 to 100 μm. When the thickness of the substrate is within such a range, the flexibility of the composite sheet for forming a protective film and the suitability for attachment to a wafer are further improved. Here, the "thickness of the substrate" means the thickness of the entire substrate. For example, the thickness of a substrate consisting of multiple layers means the total thickness of all layers constituting the substrate.

[0158] The substrate may contain, in addition to the main constituent materials such as the resin, various known additives such as fillers, colorants, antioxidants, organic lubricants, catalysts, softeners (plasticizers), and the like.

[0159] The substrate is preferably transparent, and may be colored according to the purpose, or other layers may be vapor-deposited thereon. In the present embodiment in which the protective film-forming film has energy ray curing properties, the substrate is preferably one that transmits energy rays.

[0160] In order to adjust the adhesiveness with a layer (for example, a pressure-sensitive adhesive layer, a protective film-forming film, or the other layer) provided thereon, the surface of the substrate may be subjected to roughening treatment such as sandblasting or solvent treatment, oxidation treatment such as corona discharge treatment, electron beam irradiation treatment, plasma treatment, ozone / ultraviolet radiation treatment, flame treatment, chromic acid treatment, or hot air treatment, lipophilic treatment, hydrophilic treatment, etc. The surface of the substrate may be treated with a primer.

[0161] The substrate may have adhesiveness on at least one surface thereof by containing a specific range of components (for example, a resin, etc.).

[0162] The substrate can be produced by a known method. For example, a substrate containing a resin can be produced by molding a resin composition containing the resin.

[0163] Adhesive layer The pressure-sensitive adhesive layer is in the form of a sheet or film and contains a pressure-sensitive adhesive. Examples of the adhesive include adhesive resins such as acrylic resins, urethane resins, rubber-based resins, silicone resins, epoxy-based resins, polyvinyl ethers, polycarbonates, and ester-based resins.

[0164] In this specification, the term "adhesive resin" includes both a resin having adhesiveness and a resin having adhesiveness. For example, the adhesive resin includes not only resins that are adhesive by themselves, but also resins that exhibit adhesiveness when used in combination with other components such as additives, and resins that exhibit adhesiveness in the presence of a trigger such as heat or water.

[0165] The adhesive layer may consist of one layer (single layer), or may consist of two or more layers. If it consists of multiple layers, these multiple layers may be the same or different, and the combination of these multiple layers is not particularly limited.

[0166] The thickness of the pressure-sensitive adhesive layer is not particularly limited, but is preferably from 1 to 100 μm, more preferably from 1 to 60 μm, and particularly preferably from 1 to 30 μm. Here, "the thickness of the adhesive layer" means the thickness of the entire adhesive layer. For example, the thickness of an adhesive layer consisting of multiple layers means the total thickness of all layers that make up the adhesive layer.

[0167] The pressure-sensitive adhesive layer is preferably transparent, and may be colored depending on the purpose. In the present embodiment in which the protective film-forming film has energy ray curing properties, the pressure-sensitive adhesive layer is preferably one that transmits energy rays.

[0168] The adhesive layer may be either energy ray curable or non-energy ray curable. The physical properties of the energy ray curable adhesive layer can be adjusted before and after curing. For example, before picking up the chip with the protective film described below, the chip with the protective film can be picked up more easily by curing the energy ray curable adhesive layer. When the adhesive layer is non-energy ray curable, it has high light stability and excellent storage stability.

[0169] The adhesive layer can be formed using an adhesive composition containing an adhesive. For example, the adhesive composition is applied to the surface on which the adhesive layer is to be formed, and then dried as necessary to form the adhesive layer at the desired location. The ratio of the contents of the components that do not vaporize at room temperature in the adhesive composition is usually the same as the ratio of the contents of the components in the adhesive layer.

[0170] The pressure-sensitive adhesive composition can be applied and dried, for example, by the same method as in the application and drying of the above-mentioned composition for forming a protective film.

[0171] When the adhesive layer is provided on the substrate, for example, the adhesive composition may be applied to the substrate and dried as necessary. Alternatively, for example, the adhesive composition may be applied to a release film and dried as necessary to form an adhesive layer on the release film, and the exposed surface of the adhesive layer may be attached to one surface of the substrate to laminate the adhesive layer on the substrate. In this case, the release film may be removed at any timing during the manufacturing process or the use process of the composite sheet for forming a protective film.

[0172] When the adhesive layer is energy ray curable, examples of the energy ray curable adhesive composition include an adhesive composition (I-1) containing a non-energy ray curable adhesive resin (I-1a) (hereinafter may be abbreviated as "adhesive resin (I-1a)") and an energy ray curable compound; an adhesive composition (I-2) containing an energy ray curable adhesive resin (I-2a) (hereinafter may be abbreviated as "adhesive resin (I-2a)") in which an unsaturated group has been introduced into the side chain of the non-energy ray curable adhesive resin (I-1a); an adhesive composition (I-3) containing the adhesive resin (I-2a) and an energy ray curable compound, and the like.

[0173] When the adhesive layer is non-energy ray curable, examples of the non-energy ray curable adhesive composition include an adhesive composition (I-4) containing the non-energy ray curable adhesive resin (I-1a).

[0174] [Non-energy ray curable adhesive resin (I-1a)] The adhesive resin (I-1a) is preferably an acrylic resin.

[0175] The acrylic resin may, for example, be an acrylic polymer having at least a structural unit derived from an alkyl (meth)acrylate ester. The (meth)acrylic acid alkyl ester may, for example, be one in which the alkyl group constituting the alkyl ester has 1 to 20 carbon atoms, and the alkyl group is preferably linear or branched.

[0176] The acrylic polymer preferably further contains a constituent unit derived from a functional group-containing monomer in addition to the constituent unit derived from an alkyl (meth)acrylate ester. Examples of the functional group-containing monomer include those in which the functional group reacts with a crosslinking agent described below to become a crosslinking starting point, and those in which the functional group reacts with a functional group such as an isocyanate group or a glycidyl group in an unsaturated group-containing compound described below to enable the introduction of an unsaturated group into a side chain of an acrylic polymer.

[0177] Examples of the functional group-containing monomer include a hydroxyl group-containing monomer, a carboxyl group-containing monomer, an amino group-containing monomer, and an epoxy group-containing monomer.

[0178] The acrylic polymer may further contain a constituent unit derived from another monomer, in addition to the constituent unit derived from the (meth)acrylic acid alkyl ester and the constituent unit derived from the functional group-containing monomer. The other monomer is not particularly limited as long as it is copolymerizable with the (meth)acrylic acid alkyl ester and the like. Examples of the other monomers include styrene, α-methylstyrene, vinyl toluene, vinyl formate, vinyl acetate, acrylonitrile, and acrylamide.

[0179] In the pressure-sensitive adhesive composition (I-1), pressure-sensitive adhesive composition (I-2), pressure-sensitive adhesive composition (I-3) and pressure-sensitive adhesive composition (I-4) (hereinafter, these pressure-sensitive adhesive compositions are collectively abbreviated as "pressure-sensitive adhesive compositions (I-1) to (I-4)"), the structural unit possessed by the acrylic resin such as the acrylic polymer may be of only one type or of two or more types, and when there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0180] In the acrylic polymer, the proportion of the amount of the structural units derived from functional group-containing monomers relative to the total amount of the structural units is preferably 1 to 35% by mass.

[0181] The adhesive resin (I-1a) contained in the adhesive composition (I-1) or the adhesive composition (I-4) may be one type or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0182] In the pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition (I-1) or the pressure-sensitive adhesive composition (I-4), the content of the pressure-sensitive adhesive resin (I-1a) relative to the total mass of the pressure-sensitive adhesive layer is preferably 5 to 99 mass%, and may be, for example, any one of 25 to 95 mass%, 45 to 95 mass%, and 65 to 95 mass%.

[0183] [Energy ray curable adhesive resin (I-2a)] The adhesive resin (I-2a) can be obtained, for example, by reacting a functional group in the adhesive resin (I-1a) with an unsaturated group-containing compound having an energy ray-polymerizable unsaturated group.

[0184] The unsaturated group-containing compound is a compound that, in addition to the energy ray-polymerizable unsaturated group, further has a group that can bond to the adhesive resin (I-1a) by reacting with a functional group in the adhesive resin (I-1a). Examples of the energy ray-polymerizable unsaturated group include a (meth)acryloyl group, a vinyl group (ethenyl group), and an allyl group (2-propenyl group), and the like, with a (meth)acryloyl group being preferred. Examples of groups capable of bonding to functional groups in the adhesive resin (I-1a) include isocyanate groups and glycidyl groups capable of bonding to hydroxyl groups or amino groups, and hydroxyl groups and amino groups capable of bonding to carboxy groups or epoxy groups.

[0185] Examples of the unsaturated group-containing compound include (meth)acryloyloxyethyl isocyanate, (meth)acryloyl isocyanate, and glycidyl (meth)acrylate.

[0186] The adhesive resin (I-2a) contained in the adhesive composition (I-2) or (I-3) may be one type or two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0187] In the pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition (I-2) or (I-3), the content of the pressure-sensitive adhesive resin (I-2a) relative to the total mass of the pressure-sensitive adhesive layer is preferably 5 to 99 mass %.

[0188] [Energy ray curable compounds] The energy ray-curable compound contained in the pressure-sensitive adhesive composition (I-1) or (I-3) includes a monomer or oligomer having an energy ray-polymerizable unsaturated group and capable of being cured by irradiation with energy rays.

[0189] Among the energy ray-curable compounds, examples of the monomer include polyvalent (meth)acrylates such as trimethylolpropane tri(meth)acrylate, pentaerythritol (meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,4-butylene glycol di(meth)acrylate, and 1,6-hexanediol (meth)acrylate; urethane (meth)acrylate; polyester (meth)acrylate; polyether (meth)acrylate; and epoxy (meth)acrylate. Among the energy ray-curable compounds, examples of the oligomer include oligomers which are polymers of the monomers exemplified above.

[0190] The pressure-sensitive adhesive composition (I-1) or (I-3) may contain only one type of energy ray-curable compound, or two or more types. When two or more types are contained, the combination and ratio thereof can be selected arbitrarily.

[0191] In the pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition (I-1) or (I-3), the content of the energy ray-curable compound relative to the total mass of the pressure-sensitive adhesive layer is preferably 1 to 95 mass %.

[0192] [Crosslinking agent] When the adhesive resin (I-1a) is an acrylic polymer having, in addition to a structural unit derived from a (meth)acrylic acid alkyl ester, a structural unit derived from a functional group-containing monomer, the adhesive composition (I-1) or (I-4) preferably further contains a crosslinking agent. In addition, when the adhesive resin (I-2a) is, for example, an acrylic polymer having a structural unit derived from a functional group-containing monomer similar to that in the adhesive resin (I-1a), the adhesive composition (I-2) or (I-3) may further contain a crosslinking agent.

[0193] The crosslinking agent, for example, reacts with the functional group to crosslink the adhesive resins (I-1a) together or the adhesive resins (I-2a) together. Examples of the crosslinking agent include isocyanate-based crosslinking agents (crosslinking agents having an isocyanate group) such as tolylene diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, and adducts of these diisocyanates; epoxy-based crosslinking agents (crosslinking agents having a glycidyl group) such as ethylene glycol glycidyl ether; aziridine-based crosslinking agents (crosslinking agents having an aziridinyl group) such as hexa[1-(2-methyl)-aziridinyl]triphosphatriazine; metal chelate-based crosslinking agents (crosslinking agents having a metal chelate structure) such as aluminum chelate; and isocyanurate-based crosslinking agents (crosslinking agents having an isocyanuric acid skeleton).

[0194] The crosslinking agent contained in the pressure-sensitive adhesive compositions (I-1) to (I-4) may be one type, or two or more types. When two or more types are contained, the combination and ratio thereof can be selected arbitrarily.

[0195] In the pressure-sensitive adhesive composition (I-1) or (I-4), the content of the crosslinking agent is preferably 0.01 to 50 parts by mass relative to 100 parts by mass of the pressure-sensitive adhesive resin (I-1a), and may be, for example, any one of 1 to 40 parts by mass, 5 to 35 parts by mass, and 10 to 30 parts by mass. In the pressure-sensitive adhesive composition (I-2) or (I-3), the content of the crosslinking agent is preferably 0.01 to 50 parts by mass per 100 parts by mass of the pressure-sensitive adhesive resin (I-2a).

[0196] [Photopolymerization initiator] The pressure-sensitive adhesive compositions (I-1), (I-2) and (I-3) (hereinafter collectively referred to as "pressure-sensitive adhesive compositions (I-1) to (I-3)") may further contain a photopolymerization initiator. The pressure-sensitive adhesive compositions (I-1) to (I-3) containing a photopolymerization initiator sufficiently undergo a curing reaction even when irradiated with relatively low-energy energy rays such as ultraviolet rays.

[0197] The photopolymerization initiator may be, for example, the same as the above-mentioned photopolymerization initiator (c).

[0198] The photopolymerization initiator contained in the pressure-sensitive adhesive compositions (I-1) to (I-3) may be only one type, or may be two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0199] In the pressure-sensitive adhesive composition (I-1), the content of the photopolymerization initiator is preferably 0.01 to 20 parts by mass relative to 100 parts by mass of the energy ray-curable compound.In the pressure-sensitive adhesive composition (I-2), the content of the photopolymerization initiator is preferably 0.01 to 20 parts by mass relative to 100 parts by mass of the pressure-sensitive adhesive resin (I-2a). In the pressure-sensitive adhesive composition (I-3), the content of the photopolymerization initiator is preferably 0.01 to 20 parts by mass per 100 parts by mass of the total content of the pressure-sensitive adhesive resin (I-2a) and the energy ray-curable compound.

[0200] [Other additives] The pressure-sensitive adhesive compositions (I-1) to (I-4) may contain other additives that do not fall into any of the above-mentioned components, as long as the effects of the present invention are not impaired. Examples of the other additives include known additives such as antistatic agents, antioxidants, softeners (plasticizers), fillers, rust inhibitors, colorants (pigments, dyes), sensitizers, tackifiers, reaction retarders, and crosslinking accelerators (catalysts). The reaction retarder is, for example, a component that suppresses the progress of unintended crosslinking reactions in the pressure-sensitive adhesive compositions (I-1) to (I-4) during storage due to the action of a catalyst mixed in the pressure-sensitive adhesive compositions (I-1) to (I-4). Examples of the reaction retarder include those that form a chelate complex by chelating with the catalyst, and more specifically, those that have two or more carbonyl groups (-C(=O)-) in one molecule.

[0201] The other additives contained in the pressure-sensitive adhesive compositions (I-1) to (I-4) may be of only one type, or of two or more types. When there are two or more types, the combination and ratio thereof can be selected arbitrarily.

[0202] The content of other additives in the pressure-sensitive adhesive compositions (I-1) to (I-4) is not particularly limited and may be appropriately selected depending on the type of additive.

[0203] [solvent] The pressure-sensitive adhesive compositions (I-1) to (I-4) may contain a solvent. By containing a solvent, the pressure-sensitive adhesive compositions (I-1) to (I-4) have improved suitability for application to a surface to be coated.

[0204] The solvent is preferably an organic solvent, and examples of the organic solvent include ketones such as methyl ethyl ketone and acetone; esters (carboxylates) such as ethyl acetate; ethers such as tetrahydrofuran and dioxane; aliphatic hydrocarbons such as cyclohexane and n-hexane; aromatic hydrocarbons such as toluene and xylene; and alcohols such as 1-propanol and 2-propanol.

[0205] The pressure-sensitive adhesive compositions (I-1) to (I-4) may contain only one type of solvent, or two or more types. When two or more types are contained, the combination and ratio thereof can be selected arbitrarily.

[0206] The content of the solvent in each of the pressure-sensitive adhesive compositions (I-1) to (I-4) is not particularly limited and may be appropriately adjusted.

[0207] Method for producing pressure-sensitive adhesive composition The pressure-sensitive adhesive compositions such as the pressure-sensitive adhesive compositions (I-1) to (I-4) can be obtained by blending the pressure-sensitive adhesive and, if necessary, components other than the pressure-sensitive adhesive, for constituting the pressure-sensitive adhesive composition. The pressure-sensitive adhesive composition can be produced in the same manner as in the case of the composition for forming a protective film described above, except that the types of ingredients used are different.

[0208] ◇Manufacturing method of composite sheet for forming protective film The composite sheet for forming a protective film can be produced by laminating the above-mentioned layers so as to have a corresponding positional relationship, and adjusting the shape of some or all of the layers as necessary. The method for forming each layer is as described above.

[0209] For example, when a pressure-sensitive adhesive layer is laminated on a substrate during the production of a support sheet, the pressure-sensitive adhesive composition may be applied onto the substrate and dried as necessary. Alternatively, the pressure-sensitive adhesive layer can be laminated on the substrate by coating the pressure-sensitive adhesive composition on a release film, drying it as necessary to form a pressure-sensitive adhesive layer on the release film, and then laminating the exposed surface of the pressure-sensitive adhesive layer to one surface of the substrate. In this case, the pressure-sensitive adhesive composition is preferably coated on the release-treated surface of the release film. Up to this point, the case where a pressure-sensitive adhesive layer is laminated on a substrate has been taken as an example, but the above-mentioned method can also be applied to, for example, the case where a layer other than the pressure-sensitive adhesive layer is laminated on a substrate.

[0210] On the other hand, for example, when a protective film-forming film is laminated on an adhesive layer already laminated on a substrate, a protective film-forming composition can be applied on the adhesive layer to directly form a protective film-forming film. A layer other than the protective film-forming film can also be laminated on the adhesive layer in a similar manner using a composition for forming this layer. In this way, when a new layer (hereinafter abbreviated as "second layer") is formed on any layer (hereinafter abbreviated as "first layer") already laminated on a substrate to form a continuous two-layer laminate structure (in other words, a laminate structure of the first layer and the second layer), a method of applying a composition for forming the second layer on the first layer and drying as necessary can be applied. However, it is preferable to form the second layer in advance on a release film using a composition for forming the second layer, and then bond the exposed surface of the second layer opposite to the side in contact with the release film to the exposed surface of the first layer to form a continuous two-layer laminate structure. In this case, it is preferable to coat the composition on the release-treated surface of the release film. The release film can be removed as necessary after the laminate structure is formed. Here, we have given an example of laminating a protective film-forming film onto an adhesive layer, but the target laminate structure can be selected arbitrarily, for example, when laminating a layer (film) other than the protective film-forming film onto the adhesive layer.

[0211] In this way, all layers other than the substrate that make up the composite sheet for forming a protective film can be formed in advance on a release film and then laminated by bonding it to the surface of the desired layer, so the composite sheet for forming a protective film can be manufactured by appropriately selecting the layers that will undergo such a process as necessary.

[0212] The composite sheet for forming a protective film is usually stored in a state where a release film is attached to the surface of the outermost layer (for example, the protective film-forming film) on the opposite side to the support sheet. Therefore, a composition for forming a layer constituting the outermost layer, such as a composition for forming a protective film, is applied to this release film (preferably its release-treated surface), and dried as necessary to form a layer constituting the outermost layer on the release film, and the remaining layers are laminated on the exposed surface opposite to the side in contact with the release film by any of the above-mentioned methods, and the release film is not removed and the laminated state is left as it is, thereby obtaining a composite sheet for forming a protective film with a release film.

[0213] The composite sheet for forming a protective film may be in the form of a sheet, and is preferably in the form of a roll.

[0214] ◇Manufacturing method of chips with protective film (method of using protective film forming film and composite sheet for protective film forming) The protective film-forming film and the composite sheet for forming a protective film can be used for producing the chip with the protective film. The manufacturing method of a chip with a protective film according to this embodiment is a manufacturing method of a chip with a protective film comprising a chip and a protective film provided on the back surface of the chip, and includes a bonding step of bonding a protective film forming film according to one embodiment of the present invention described above to the back surface of a wafer, a curing step of curing the protective film forming film with energy rays to form the protective film, and a division step of dividing the wafer and cutting the protective film to produce a plurality of chips with the protective film. The method for producing a chip with a protective film according to this embodiment preferably includes a laser marking step of irradiating a laser onto the back surface of the wafer.

[0215] A method for producing a chip with a protective film in the case where a protective film-forming film that does not constitute a composite sheet for forming a protective film is attached to the rear surface of a wafer (sometimes referred to as "production method 1" in this specification) is a method for producing a chip with a protective film, which includes a chip and a protective film provided on the rear surface of the chip, and includes a bonding step of producing a first laminated film in which the protective film-forming film and the wafer are laminated in their thickness direction by bonding the protective film-forming film according to one embodiment of the present invention to the rear surface of the wafer, and a bonding step of bonding the protective film-forming film in the first laminated film or the first laminated composite sheet. The method may include a curing step of forming the protective film by energy ray curing a wafer to produce a second laminate film in which the protective film and the wafer are laminated in their thickness direction; a dividing step of dividing the wafer in the second laminate film and cutting the protective film with a dicing sheet provided on the protective film side of the second laminate film to produce a third laminate film in which a plurality of chips with the protective film are fixed on the dicing sheet; and a back-up step of separating the chips with the protective film in the third laminate film from the dicing sheet.

[0216] A manufacturing method for a chip with a protective film in the case where a protective film-forming film in a composite sheet for forming a protective film is attached to the back surface of a wafer (sometimes referred to as "manufacturing method 2" in this specification) is a manufacturing method for a chip with a protective film comprising a chip and a protective film provided on the back surface of the chip, and may include a bonding step of bonding the protective film-forming film in the composite sheet for forming a protective film according to one embodiment of the present invention to the back surface of the wafer to produce a first laminated composite sheet in which the support sheet, the protective film-forming film and the wafer are stacked in this order in their thickness direction, a curing step of producing a second laminated composite sheet in which the support sheet, the protective film and the wafer are stacked in this order in their thickness direction, a dividing step of dividing the wafer in the second laminated composite sheet and cutting the protective film to produce a third laminated composite sheet in which a plurality of the protective film-attached chips are fixed on the support sheet, and a picking up step of the protective film-attached chips in the third laminated composite sheet by separating them from the support sheet.

[0217] Hereinafter, the manufacturing method 1 and the manufacturing method 2 will be described in order with reference to the drawings.

[0218] <<Manufacturing method 1>> 6 is a cross-sectional view for typically explaining the manufacturing method 1. Here, the manufacturing method 1 will be explained by taking as an example the case where the protective film-forming film 13 shown in FIG. In the bonding step of manufacturing method 1, as shown in Fig. 6(a), the above-mentioned protective film-forming film 13 is bonded to the back surface 9b of the wafer 9 to produce a first laminated film 601 in which the protective film-forming film 13 and the wafer 9 are laminated in their thickness direction. A first surface 13a of the protective film-forming film 13 is bonded to the back surface 9b of the wafer 9. A second release film 152 is provided on the second surface 13b of the protective film-forming film 13. Here, the case is shown in which the first peel-off film 151 is removed from the protective film-forming film 13 shown in Figure 1 and the first surface 13a of the protective film-forming film 13 is attached to the back surface 9b of the wafer 9, but the second peel-off film 152 may be removed from the protective film-forming film 13 shown in Figure 1 and the second surface 13b of the protective film-forming film 13 may be attached to the back surface 9b of the wafer 9.

[0219] The protective film-forming film 13 can be attached to the wafer 9 by a known method. For example, the protective film-forming film 13 may be attached to the wafer 9 while being heated.

[0220] Next, in the curing step of the manufacturing method 1, the protective film-forming film 13 in the first laminated film 601 is cured with energy rays to form a protective film 13', thereby producing a second laminated film 602 in which the protective film 13' and the wafer 9 are laminated in their thickness direction, as shown in Fig. 6(b). Reference numeral 13a' denotes the surface of the protective film 13' that was the first surface 13a of the protective film-forming film 13 (sometimes referred to as the "first surface" in this specification). Reference numeral 13b' denotes the surface of the protective film 13' that was the second surface 13b of the protective film-forming film 13 (sometimes referred to as the "second surface" in this specification).

[0221] In the curing process, the protective film 13' is formed by irradiating the protective film-forming film 13 with energy rays from the outside of the protective film-forming film 13 side of the first laminate film 601 through the second peelable film 152 (by transmitting through the second peelable film 152). In the curing process, the second release film 152 may be removed from the protective film-forming film 13 in the first laminate film 601 to expose the second surface 13b of the protective film-forming film 13, and then the protective film-forming film 13 may be irradiated with energy rays to form the protective film 13'.

[0222] The conditions for the energy ray irradiation in the curing step are as described above.

[0223] The rear surface 9b of the wafer 9 in FIG. 6(a) may be laser-marked by laser irradiation. Laser marking may be performed by irradiating a laser onto the back surface 9b of the wafer 9 shown in Figure 6(a) through the second release film 152 and the protective film forming film 13 (passing through the second release film 152 and the protective film forming film 13), or laser marking may be performed by irradiating a laser onto the back surface 9b of the wafer 9 shown in Figure 6(b) through the second release film 152 and the protective film 13' (passing through the second release film 152 and the protective film 13').

[0224] Next, in the dividing step of manufacturing method 1, first, the second release film 152 is removed from the protective film 13' in the second laminate film 602. Then, one surface 8a (sometimes referred to as the "first surface" in this specification) of the dicing sheet 8 is attached to the second surface 13b' of the protective film 13' newly exposed as a result, as shown in FIG. 6(c). The dicing sheet 8 shown here is configured to include a base material 81 and an adhesive layer 82 provided on one surface 81a of the base material 81, and the adhesive layer 82 in the dicing sheet 8 is attached to the protective film 13'. A surface 82a of the adhesive layer 82 facing the protective film 13' (sometimes referred to as the "first surface" in this specification) is the same as the first surface 8a of the dicing sheet 8.

[0225] The dicing sheet 8 may be a known one. For example, the base material 81 may be the same as the base material in the composite sheet for forming a protective film described above, and the adhesive layer 82 may be the same as the adhesive layer in the composite sheet for forming a protective film described above. That is, the dicing sheet 8 can be replaced with the support sheet 10.

[0226] Here, a dicing sheet 8 having a base material 81 and an adhesive layer 82 is used as the support sheet 10, but in the division process, something other than this may be used as the support sheet 10, for example, a support sheet consisting of only a base material.

[0227] Next, in the dividing step, as shown in Fig. 6(d), with the dicing sheet 8 provided on the protective film 13' side of the second laminate film 602, the wafer 9 in the second laminate film 602 is divided and the protective film 13' is cut. The wafer 9 is divided into individual pieces into a plurality of chips 90.

[0228] The division of the wafer 9 and the cutting of the protective film 13′ may be performed by a known method. For example, the division of the wafer 9 and the cutting of the protective film 13′ can be performed successively by dicing such as blade dicing, laser dicing using laser irradiation, or water dicing using water containing an abrasive. The protective film 13' is cut along the outer periphery of the chip 90, regardless of the cutting method.

[0229] In this manner, by dividing the wafer 9 and cutting the protective film 13', a plurality of chips 901 with protective film are obtained, each chip 90 including a protective film (sometimes simply referred to as "protective film" in this specification) 130' after cutting provided on the back surface 90b of the chip 90. Reference numeral 130b' denotes a surface of the protective film 130' after cutting that was the second surface 13b' of the protective film 13' (sometimes referred to as "second surface" in this specification).

[0230] In the dividing step of manufacturing method 1, the third laminated film 603 is produced in which the plurality of protective film-coated chips 901 are fixed on the dicing sheet 8 as described above.

[0231] Next, in the pick-up step of manufacturing method 1, as shown in FIG. 6(e), protective film-equipped chip 901 in third laminate film 603 is picked up by being pulled away from dicing sheet 8. In the pick-up step, peeling occurs between the second surface 130b' of the protective film 130' in the protective film-coated chip 901 and the first surface 82a of the adhesive layer 82 in the dicing sheet 8.

[0232] Here, a case is shown in which a separating means 7 such as a vacuum collet is used to separate the protective film-coated chip 901 in the direction of arrow P. Note that a cross-sectional view of the separating means 7 is omitted here. The chip 901 with the protective film can be picked up by a known method.

[0233] When the adhesive layer 82 is energy ray curable, in the pick-up step, it is preferable to irradiate the adhesive layer 82 with energy rays to cure the adhesive layer 82 and form a cured product (not shown), and then separate the protective film-equipped chip 901 from the dicing sheet 8. In this case, in the pick-up step, peeling occurs between the protective film 130' in the protective film-equipped chip 901 and the cured product of the adhesive layer 82 in the dicing sheet 8. In this case, the cured product of the adhesive layer 82 becomes less likely to deform than before curing, so that the protective film-attached chip 901 can be picked up more easily.

[0234] The conditions for irradiating the pressure-sensitive adhesive layer 82 with energy rays in the pick-up step may be the same as the conditions for irradiating the protective film-forming film 13 with energy rays in the curing step, for example.

[0235] In this specification, even after the energy ray-curable pressure-sensitive adhesive layer is cured with energy rays, as long as the laminated structure of the substrate and the cured product of the energy ray-curable pressure-sensitive adhesive layer is maintained, this laminated structure is referred to as a "dicing sheet."

[0236] On the other hand, if the adhesive layer 82 is non-energy ray curable, the protective film-equipped chip 901 can be simply pulled away from the adhesive layer 82, and since there is no need to harden the adhesive layer 82, the protective film-equipped chip 901 can be picked up in a simplified process. Even if the adhesive layer 82 is energy ray curable, by picking up the protective film-attached chip 901 without curing the adhesive layer 82, the protective film-attached chip 901 can be picked up in a simplified process.

[0237] In the pick-up step, such pick-up of protective film-coated chips 901 is performed for all of the desired protective film-coated chips 901 .

[0238] In the manufacturing method 1, the intended chip 901 with a protective film is obtained by carrying out the steps up to the pick-up step.

[0239] In the manufacturing method 1, since the protective film-forming film according to the embodiment of the present invention described above is used, even if the rear surface 9b of the wafer 9 is laser marked, the print visibility is excellent.

[0240] <<Manufacturing method 2>> FIG. 7 is a cross-sectional view for explaining the manufacturing method 2. Here, the manufacturing method 2 will be explained by taking the case where the composite sheet 101 for forming a protective film shown in FIG. 2 is used as an example. In the pasting step of the manufacturing method 2, as shown in FIG. 7(a), the protective film-forming film 13 in the composite sheet 101 for forming a protective film is pasted to the back surface 9b of the wafer 9 to produce a first laminated composite sheet 501 in which the support sheet 10, the protective film-forming film 13, and the wafer 9 are laminated in this order in the thickness direction. In this case, as in the case of the manufacturing method 1, the first surface 13a of the protective film-forming film 13 in the composite sheet 101 for forming a protective film is pasted to the back surface 9b of the wafer 9.

[0241] The protective film-forming film 13 in the composite sheet for forming a protective film 101 can be attached to the wafer 9 by a known method. For example, the protective film-forming film 13 may be attached to the wafer 9 while being heated.

[0242] Next, in the curing step of manufacturing method 2, the protective film-forming film 13 in the first laminated composite sheet 501 is cured with energy rays to form a protective film 13', thereby producing a second laminated composite sheet 502 in which the support sheet 10, the protective film 13' and the wafer 9 are laminated in this order in the thickness direction, as shown in Figure 7(b).

[0243] In the curing process, the protective film 13' is formed by irradiating the protective film-forming film 13 with energy rays from the outside of the support sheet 10 side of the first laminated composite sheet 501 through the support sheet 10 (by transmitting through the support sheet 10).

[0244] The curing step can be carried out in the same manner as the curing step in the manufacturing method 1, except that the first laminated composite sheet 501 is used instead of the first laminated film 601.

[0245] The rear surface 9b of the wafer 9 in FIG. 7(a) may be laser-marked by laser irradiation. Laser marking may be performed by irradiating the back surface 9b of the wafer 9 shown in Figure 7(a) with a laser through the support sheet 10 and the protective film forming film 13 (through the support sheet 10 and the protective film forming film 13), or by irradiating the back surface 9b of the wafer 9 shown in Figure 7(b) with a laser through the support sheet 10 and the protective film 13' (through the support sheet 10 and the protective film 13').

[0246] The second laminated composite sheet 502 obtained in the curing step has the same structure as the laminate of the second laminate film 602 and the dicing sheet 8 in the dividing step in the manufacturing method 1. When the dicing sheet 8 is the same as the support sheet 10, the second laminated composite sheet 502 is the same as the laminate.

[0247] 7(c), the wafer 9 in the second laminated composite sheet 502 is divided and the protective film 13′ is cut. The wafer 9 is divided into individual pieces into a plurality of chips 90.

[0248] The dividing step can be carried out in the same manner as the dividing step in manufacturing method 1, except that a second laminated composite sheet 502 is used instead of the laminate of the second laminated film 602 and the dicing sheet 8. In the manufacturing method 2, the protective film 13' is also cut along the outer periphery of the chip 90, regardless of the cutting method used.

[0249] In this manner, by dividing the wafer 9 and cutting the protective film 13', a plurality of chips 901 with protective film are obtained, each chip 90 having a protective film 130' after cutting provided on the back surface 90b of the chip 90. These protective film-attached chips 901 obtained in the dividing step in manufacturing method 2 are the same as the protective film-attached chips 901 obtained in the dividing step in manufacturing method 1.

[0250] In the dividing step of manufacturing method 2, third laminated composite sheet 503 is produced in which a plurality of chips 901 with protective film are fixed on support sheet 10 as described above. The third laminated composite sheet 503 has the same structure as the third laminated film 603 obtained in the dividing step in the manufacturing method 1. When the dicing sheet 8 is the same as the support sheet 10, the third laminated composite sheet 503 is the same as the third laminated film 603.

[0251] Next, in the pick-up step of manufacturing method 2, as shown in FIG. 7(d), chip 901 with protective film in third laminated composite sheet 503 is picked up by being pulled away from support sheet 10. In the pick-up step, peeling occurs between second surface 130b' of protective film 130' in protective film-attached chip 901 and first surface 12a of adhesive layer 12 in support sheet 10.

[0252] The pick-up step can be performed in the same manner as the pick-up step in manufacturing method 1, except that the third laminated composite sheet 503 is used instead of the third laminated film 603.

[0253] For example, when the adhesive layer 12 is energy ray curable, in the pick-up step, it is preferable to irradiate the adhesive layer 12 with energy rays to cure the adhesive layer 12 and form a cured product (not shown), and then separate the protective film-equipped chip 901 from the support sheet 10. In this case, in the pick-up step, peeling occurs between the protective film 130′ in the protective film-equipped chip 901 and the cured product of the adhesive layer 12 in the support sheet 10. In this case, the cured product of the adhesive layer 12 becomes less likely to deform than before curing, so that the protective film-attached chip 901 can be picked up more easily.

[0254] On the other hand, if the adhesive layer 12 is non-energy ray curable, the protective film-attached chip 901 can be simply pulled away from the adhesive layer 12, and since there is no need to harden the adhesive layer 12, the protective film-attached chip 901 can be picked up in a simplified process. Even if the adhesive layer 12 is energy ray curable, by picking up the protective film-attached chip 901 without curing the adhesive layer 12, the protective film-attached chip 901 can be picked up in a simplified process.

[0255] In manufacturing method 2, by performing the steps up to the pick-up step, the desired chip with protective film 901 is obtained. The chip with protective film 901 obtained by manufacturing method 2 is the same as the chip with protective film 901 obtained by manufacturing method 1.

[0256] In manufacturing method 2, the above-mentioned composite sheet for forming a protective film is used, which has the protective film forming film of one embodiment of the present invention described above, so that the printing visibility is excellent even when laser marking is performed on the back surface 9b of the wafer 9.

[0257] So far, manufacturing method 2 has been described in the case where the composite sheet for forming a protective film 101 shown in Figure 2 is used. However, in manufacturing method 2, a composite sheet for forming a protective film of this embodiment other than the composite sheet for forming a protective film 101 may also be used, such as the composite sheet for forming a protective film 102, the composite sheet for forming a protective film 103 or the composite sheet for forming a protective film 104 shown in Figures 3 to 5. EXAMPLES

[0258] The present invention will be described in more detail below with reference to specific examples, although the present invention is not limited to the following examples.

[0259] <Raw materials for resin production> The full names of the raw materials for producing the resins, which are abbreviated in the present examples and comparative examples, are shown below. BA: n-butyl acrylate MA: Methyl acrylate ACrMO: 4-Acryloylmorpholine HEA: 2-hydroxyethyl acrylate MMA: Methyl methacrylate GMA: glycidyl methacrylate

[0260] <Raw materials for producing the protective film-forming composition> The raw materials used in the production of the composition for forming a protective film are shown below. [Energy ray curable component (a)] (a)-1: Urethane acrylate (KJ Chemicals' "Quick cure 8100EA70") (a)-2: ε-caprolactone-modified tris-(2-acryloxyethyl)isocyanurate ("A-9300-1CL" manufactured by Shin-Nakamura Chemical Co., Ltd., a trifunctional ultraviolet-curable compound)

[0261] [Polymer (b) having no energy ray-curable group] (b)-1: Acrylic resin which is a copolymer of MA (85 parts by mass) and HEA (15 parts by mass) (weight average molecular weight: 370,000, glass transition temperature: 5°C) (b)-2: Acrylic resin (weight average molecular weight: 700,000, glass transition temperature: 2° C.) which is a copolymer of BA (33 parts by mass), MA (27 parts by mass), ACrMO (25 parts by mass), and HEA (15 parts by mass) (b)-3: Acrylic resin which is a copolymer of BA (13 parts by mass), MA (70 parts by mass), GMA (5 parts by mass) and HEA (12 parts by mass) (weight average molecular weight (420,000), glass transition temperature: -2°C)

[0262] [Thermosetting component (B1)] Thermosetting component (B1)-1: Bisphenol A type epoxy resin (JER828 manufactured by Mitsubishi Chemical, epoxy equivalent 184-194g / eq) Thermosetting component (B1)-2: Bisphenol A type epoxy resin (Mitsubishi Chemical JER1055, epoxy equivalent 800-900g / eq) Thermosetting component (B1)-3: Dicyclopentadiene type epoxy resin (DIC Corporation, Epicron HP-7200HH, epoxy equivalent 255-260g / eq) Thermosetting component (B2)-1: Thermoactive latent epoxy resin curing agent (dicyandiamide (ADEKA Hardener EH-3636AS, active hydrogen amount 21g / eq))

[0263] [Photopolymerization initiator (c)] (c)-1: 2-hydroxy-1-(4-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methylpropan-1-one (BASF "Omnirad (registered trademark) 127D") (c)-2: 2-Dimethylamino-2-(4-methylbenzyl)-1-(4-morpholin-4-yl-phenyl)-butan-1-one (BASF "Omnirad (registered trademark) 379")

[0264] [Inorganic filler (d)] (d)-1: Silica filler (fused quartz filler, average particle size 8 μm, manufactured by Tatsumori Co., Ltd., "SV-10") (d)-2: Silica filler (average particle size 0.5 μm, product name "SC2050MA", manufactured by Admatechs Co., Ltd.)

[0265] [Colorant (g)] (g)-1: Organic black pigment (6377 Black, manufactured by Dainichiseika Color & Chemicals Co., Ltd.)

[0266] [Ultraviolet absorber (m)] (m)-1: Hydroxyphenyltriazine-based ultraviolet absorber "Tinuvin (registered trademark) 479, manufactured by BASF"

[0267] [Coupling agent (E)] Coupling agent (E)-1: Silane coupling agent (A-1110 made by Nippon Unicar)

[0268] <<Protective Film Forming Film Manufacturing>> [Example 1] <Production of protective film-forming composition (IV)-1> Energy ray curable component (a)-1 (17.5 parts by mass), polymer (b)-1 (22.7 parts by mass) not having energy ray curable group, photopolymerization initiator (c)-1 (0.6 parts by mass), inorganic filler (d)-1 (58.4 parts by mass) and ultraviolet absorber (m)-1 (0.8 parts by mass) were dissolved or dispersed in methyl ethyl ketone and stirred at 23 ° C. to obtain an energy ray curable protective film forming composition (IV)-1 having a total concentration of 55 mass% of all components other than the solvent. Note that the blending amounts of all components other than the solvent shown here are blending amounts of the target material not including the solvent, and are the same in the following protective film forming compositions.

[0269] <Production of protective film-forming film> A release film (second release film, "SP-PET382150" manufactured by Lintec Corporation, thickness 38 μm) made of polyethylene terephthalate film, one side of which had been treated for release by silicone treatment, was used, and the protective film-forming composition (IV)-1 obtained above was applied to the release-treated surface, followed by drying at 100°C for 2 minutes to produce an energy ray-curable protective film-forming film having a thickness of 25 μm.

[0270] Furthermore, a release-treated surface of a release film (first release film, "SP-PET381031" manufactured by Lintec Corporation, thickness 38 μm) was bonded to the exposed surface of the obtained protective film-forming film that did not have the second release film, thereby obtaining a protective film-forming film with a release film, which is composed of a protective film-forming film, a first release film provided on one surface of the protective film-forming film, and a second release film provided on the other surface of the protective film-forming film.

[0271] [Examples 2 to 4, Comparative Examples 1 to 3] According to the blending ratios (solid content) in Tables 1 and 2, a composition for forming a protective film was obtained in the same manner as in Example 1. Using each composition for forming a protective film, protective film-forming films of Examples 2 to 4 and Comparative Examples 1 to 3 were produced in the same manner as in Example 1.

[0272] <<Evaluation of protective film formation film>> <Evaluation of image clarity> Using an image clarity measuring instrument "ICM-10P" manufactured by Suga Test Instruments Co., Ltd., the total value of five types of slits (slit widths: 0.125 mm, 0.25 mm, 0.5 mm, 1 mm and 2 mm) was measured as the image clarity of the protective film-forming film (1) in accordance with JIS K 7374:2007. The measurement results are shown in Table 1.

[0273] (Light transmittance of protective film with wavelength of 550 nm) The light transmittance of the protective film-forming film at a wavelength of 550 nm was measured using a spectrophotometer (UV-VIS-NIR SPECTROPHOTOMETER UV-3600, manufactured by SHIMADZU CORPORATION). The measurement results are shown in Table 1.

[0274] <Measurement of the cure rate of protective film exposed to fluorescent light> For the protective film-forming films of Examples 1 to 4 and Comparative Examples 1 to 2 obtained above, samples were prepared by exposing the films to a circular daylight fluorescent lamp (manufactured by Panasonic Corporation, 30 type, FCL30ECW / 28X) with a rated lamp power of 28 W at a distance of 1 m directly below the lamp for 168 hours, as well as samples before exposure. Using a Fourier transform infrared / near-far infrared spectrometer (PerkinElmer's "Spectrum100"), FT-IR measurements were performed on one side of the protective film (the side exposed to the fluorescent light) before and after exposure to the fluorescent light, at an incident angle of 45°, using the diamond ATR method. Wavenumber: 790-791 cm -1 After normalizing the peak intensity of the peak to 1.5 Abs and correcting the spectral deviation, the wavenumber of 807 cm for the protective film before and after exposure to fluorescent light was -1 The change in peak intensity of the peak in the vicinity was calculated by the following formula (A), and this was taken as the cure rate [%] of the protective film-forming film upon exposure to the fluorescent lamp. More specifically, in the chart before and after standardization, the wave number is 798 cm -1 , 818cm -1 Draw a line (L1) connecting these points, and the wave number is 807 cm -1 A vertical line (L2) was drawn from the straight line (L1) in the image. Then, the length from the intersection of the vertical line (L2) and the peak top to the straight line (L1) was measured, and this was taken as the peak intensity before and after exposure to the fluorescent lamp.

[0275] In addition, 790~791cm -1 The peak is due to (d)-1. Also, 807cm -1 The peaks are derived from the vinyl groups of the energy ray curable components (a)-1 and (a)-2, and the higher the peak intensity, the more unreacted vinyl groups remain, meaning that the protective film-forming film is not cured.

[0276] Cure rate [%] = {(Peak intensity before exposure to fluorescent light - Peak intensity after exposure to fluorescent light) / Peak intensity before exposure to fluorescent light} × 100 (A) The measurement results of the curing rate of the protective film-forming film exposed to a fluorescent lamp are shown in Tables 1 and 2.

[0277] <Evaluation of print visibility> An 8-inch semiconductor wafer was printed using an EO Technics CSM300M laser printer, and a protective film (1) was attached to the surface. The size of the laser printed characters was 0.3 mm x 0.2 mm. The laser-printed characters were visually observed through the protective film-forming film (1), and it was judged whether the characters were visible or not. The evaluation results are shown in Table 1. A: It looks clear B: Slightly blurred but still visible C: Not visible

[0278] [Table 1]

[0279] [Table 2]

[0280] As is clear from the above results, the protective film-forming films of Examples 1 to 4 have a low cure rate when exposed to fluorescent light. That is, even when exposed to fluorescent light, the effect of the protective film-forming film does not progress and the performance can be maintained.

[0281] In Comparative Example 1, the degree of cure under exposure to fluorescent light was greater than that of the Examples, and it is understood that the curing reaction proceeds under exposure to fluorescent light. In Comparative Example 2, the degree of cure under exposure to fluorescent light was low and curing did not progress, but the image clarity and transmittance at 550 nm were low, making it impossible to visually recognize the print.

[0282] The thermosetting protective film-forming film of Comparative Example 3 requires a curing time of several hours, whereas the energy ray-curable protective film-forming film cures in a short time (several minutes). [Industrial Applicability]

[0283] The present invention can be used in the manufacture of semiconductor devices, such as chips with protective films, and various substrate devices. [Explanation of symbols]

[0284] 10, 20... Support sheet; 10a, 20a... One side (first side) of the support sheet; 11... Base material; 12... Pressure-sensitive adhesive layer; 13, 23... Energy ray curable protective film-forming film; 101, 102, 103, 104... Composite sheet for forming protective film; 501...first laminated composite sheet, 502...second laminated composite sheet, 503...third laminated composite sheet, 601...first laminate film, 602...second laminate film, 603...third laminate film, 8...Dicing sheet, 9...wafer, 9b...backside of wafer, 90...chip, 90b...backside of chip, 901...chip with protective film

Claims

1. An energy ray-curable protective film-forming film, The protective film-forming film has an image clarity of 110 or more.

2. Contains an energy ray-curable component (a) having a group containing an energy ray-curable C═C double bond, 2. The protective film according to claim 1, which has a cure rate of 16% or less after being exposed to a circular daylight fluorescent lamp having a rated lamp power of 28 W at a distance of 1 m for 168 hours.

3. A composite sheet for forming a protective film, comprising: a support sheet; and the protective film-forming film according to claim 1 or 2 provided on one surface of the support sheet.

4. A method for manufacturing a chip with a protective film, comprising a chip and a protective film provided on the back surface of the chip, the method comprising the steps of: attaching the protective film-forming film described in claim 1 or 2 to the back surface of a wafer; curing the protective film-forming film with energy rays to form the protective film; and dividing the wafer and cutting the protective film to produce a plurality of chips with the protective film.

5. A method for manufacturing a chip with a protective film, comprising a chip and a protective film provided on the back surface of the chip, the method comprising: a bonding step of bonding the protective film-forming film described in claim 1 or 2 to the back surface of a wafer; a curing step of curing the protective film-forming film with energy rays to form the protective film; a dividing step of dividing the wafer and cutting the protective film to produce a plurality of chips with the protective film; and a laser marking step of irradiating the back surface of the wafer with a laser.

Citation Information

Patent Citations

  • Energy ray hardening type chip protecting film

    JP2010031183A

  • Composite sheet for forming protective film, method for producing semiconductor chip equipped with protective film, and method for producing semiconductor device

    WO2017188197A1

  • Film for forming protective coating, composite sheet for forming protective coating, and method for manufacturing semiconductor chip

    WO2019082977A1