Silver collection method by ferric nitrate solution
The method stabilizes silver recovery from electronic waste by using an iron nitrate solution, regenerating the solution, and removing copper ions through electrolysis, addressing safety and efficiency issues in existing methods.
Patent Information
- Application Number
- JP2023058829
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing methods for recovering silver from electronic material processing waste using iron nitrate solutions face challenges due to the accumulation of copper ions, which increases viscosity and reduces the dissolving ability of the solution, and the use of iron powder poses safety risks and disrupts ion balance.
A method involving a leaching step with an iron nitrate solution, followed by silver recovery as silver chloride, regeneration of the solution, and a decopper removal electrolysis step to separate and remove copper ions, maintaining the solution's stability and safety.
Enables safe and stable recovery of silver while maintaining the solution's effectiveness by periodically regenerating and adjusting nitrate ion concentration and removing copper ions, thereby preventing a decrease in dissolution ability.
Smart Images

Figure 2024146110000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for recovering silver using an iron nitrate solution, and more particularly to a method for recovering silver using an iron nitrate solution from a substrate coated with a coating material containing silver and copper. [Background technology]
[0002] Electronic devices such as smartphones, personal computers, and communication devices mainly use electronic materials in which the surface of an iron-nickel-cobalt alloy made of iron, nickel, and cobalt is coated with silver solder by painting or the like. This electronic material is suitable for joining metal to ceramic or glass, and is preferably used for hermetically sealing, for example, piezoelectric vibrators.
[0003] The above electronic materials are produced by punching or other processes to match the shapes of the joining surfaces when used for hermetic sealing, etc., and a large amount of processing waste is generated during the production process. This processing waste contains the precious metal silver, and the iron-nickel-cobalt alloy used as the base material also contains expensive nickel and cobalt, so it is desirable to recover the silver and iron-nickel-cobalt alloy with as high a purity as possible.
[0004] Conventionally, a method using an alkali cyanide has been known as a method for recovering silver from electronic material scraps in which the iron-based alloy substrate is coated with silver brazing while minimizing the loss of the iron-based alloy substrate. This recovery method involves immersing the iron-based alloy substrate coated with silver brazing in a cyanide stripping solution such as an aqueous solution of an alkali cyanide, and removing and recovering only the silver brazing from the surface of the iron-based alloy substrate. However, since this recovery method uses an alkali cyanide, which is a toxic substance, the recovery facility must be provided with a specific dedicated work facility, and a wastewater treatment facility must be installed to almost completely decompose the cyanide in the cleaning solution generated from the recovery facility. This has led to the problem that the recovery process requires a great deal of effort and cost.
[0005] Therefore, as a recovery method that does not use the above-mentioned alkali cyanide, Patent Document 1 proposes a technology that uses a solution containing iron nitrate. 3+ As an oxidizing agent, the method of recovery in Patent Document 1 dissolves metallic silver and metallic copper contained in the silver brazing material. Specifically, the recovery method in Patent Document 1 includes a dissolution and stripping step in which an iron nitrate-containing solution is added to scraps of electronic materials, which are made of an iron-based alloy such as an iron-nickel-cobalt alloy, coated with silver or a silver-based alloy, to dissolve the silver or silver-based alloy and thereby strip the silver or silver-based alloy from the substrate, a silver chloride generation step in which hydrochloric acid is added to the iron nitrate-containing solution in which the silver or silver-based alloy has been dissolved to generate a silver chloride precipitate, and a silver chloride precipitation step in which divalent iron ions (Fe 2+ ) to trivalent iron ions (Fe 3+ and an iron nitrate-containing solution adjustment step of adjusting the concentration of the iron nitrate-containing solution regenerated in the iron nitrate regeneration step to the concentration of the iron nitrate-containing solution to be used in the dissolution and stripping step.
[0006] In the dissolving and peeling step, Fe in the iron nitrate-containing solution after being added to the electronic material scraps is 3+ Concentration is Fe 2+ The iron nitrate-containing solution regenerated in the iron nitrate regeneration step is used in the dissolution stripping step, and the nitrate ion concentration of the iron nitrate-containing solution regenerated in the iron nitrate regeneration step is adjusted by replenishing nitric acid equivalent to the amount of nitrate ions equivalent to the amount of silver alloy components dissolved in the dissolution stripping step excluding silver. By adopting this recovery method, it is no longer necessary to use toxic alkali cyanide, and the iron nitrate solution can be reused multiple times, making it possible to recover silver and iron-based alloy substrates safely and at low cost.
[0007] When using an iron nitrate-containing solution as in the recovery method of Patent Document 1, copper, which is mainly contained in the silver-based alloy that constitutes the silver brazing material, is also dissolved. Therefore, when the iron nitrate-containing solution is repeatedly used, copper ions gradually accumulate in the iron nitrate-containing solution, the viscosity of the iron nitrate-containing solution increases, and some of the nitrate ions in the iron nitrate-containing solution are consumed to dissolve the copper. Thus, when the iron nitrate-containing solution is repeatedly used, the dissolving ability of the iron nitrate-containing solution gradually decreases, which is a problem.
[0008] To address the above problems, Patent Document 2 proposes a technique for recovering copper ions accumulated in an iron nitrate solution by utilizing a cementation reaction with iron powder. Specifically, the technique of Patent Document 2 involves adding hydrochloric acid to an iron nitrate solution containing silver ions and copper ions obtained by immersing a coated substrate containing silver and copper, separating and recovering the silver ions as silver chloride, and then adding iron powder to the separated iron nitrate solution to precipitate and recover the copper ions as copper metal. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2015-221934 A [Patent Document 2] JP 2021-116436 A Summary of the Invention [Problem to be solved by the invention]
[0010] However, iron powder is designated as a hazardous material, and ignites when heated in an oxygen-containing atmosphere. In addition, it is highly reactive with acidic liquids, so safety risks must be considered when handling it. In addition, the iron from the iron powder dissolved in the iron nitrate liquid for the cementation reaction may disrupt the balance of iron ions and nitrate ions in the iron nitrate liquid, which may cause the dissolution of silver ions and copper ions to become unstable. The present invention has been made in view of the above circumstances, and aims to provide a method for safely and stably recovering silver from a coated substrate having silver and copper by using an iron nitrate-containing solution. [Means for solving the problem]
[0011] In order to achieve the above object, the silver recovery method of the present invention comprises the steps of: a leaching step of immersing a substrate coated with a coating material containing silver and copper in an iron nitrate solution as a leaching solution to leach the coating material; a silver recovery step of adding hydrochloric acid to the iron nitrate solution containing silver ions and copper ions obtained in the leaching step to precipitate the silver ions as silver chloride, which is then separated and recovered; a regeneration step of regenerating the iron nitrate solution from which silver chloride has been separated by oxidizing it and adjusting the nitrate ion concentration, and then repeating the regeneration as the leachate; and a copper removal electrolysis step of extracting a portion of the iron nitrate solution before or after the regeneration and performing electrowinning to separate and remove the copper ions as copper metal, and then discharging the solution as a waste liquid or repeating at least a portion of the solution as the leachate. Effect of the Invention
[0012] According to the present invention, it becomes possible to recover silver safely and stably. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a block flow diagram of an embodiment of a silver recovery process according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, an embodiment of the silver recovery method according to the present invention will be described in detail with reference to the drawings. As shown in FIG. 1, the silver recovery method according to the embodiment of the present invention includes a leaching step S1 in which a coated substrate coated with a coating material containing silver and copper to be treated is immersed in an iron nitrate solution as a leaching solution to leach only the coating material without leaching the substrate portion; a silver recovery step S2 in which hydrochloric acid is added to the Ag-containing, Cu-containing iron nitrate solution containing silver ions and copper ions obtained in the leaching step S1 to precipitate the silver ions as silver chloride, and the precipitated silver chloride is separated and recovered by solid-liquid separation; a regeneration step S3 in which the Ag-depleted, Cu-containing iron nitrate solution after the silver chloride has been separated and recovered in the silver recovery step S2 is regenerated by acidifying it and adjusting the nitrate ion concentration so that it can be reused as a leachate by repeating the leaching step S1; and a copper removal electrolysis step S4 in which a part of the Ag-depleted, Cu-containing iron nitrate solution before or after the regeneration is extracted and subjected to electrowinning to separate and remove the copper ions as copper metal, and the Ag-depleted, Cu-depleted iron nitrate solution obtained is discharged as a waste liquid or is repeated as the leachate.
[0015] More specifically, the substrate coated with a coating material containing silver and copper to be treated by the silver recovery method according to the embodiment of the present invention may be, for example, a substrate made of an iron-based alloy metal such as an iron-nickel-cobalt alloy, coated on one or both sides with an alloy containing silver and copper. An example of the alloy containing silver and copper is silver brazing. As specified in JIS Z 3261 1998, this silver brazing is an alloy mainly composed of silver and copper, to which elements such as zinc, tin, cadmium, nickel, and lithium are further added depending on the application, and generally contains 15 to 45% copper.
[0016] The above-mentioned coated substrate is mainly processing waste or out-of-spec products generated during punching or the like in the manufacturing stage of electronic materials, but is not limited to these as long as the coating material contains at least silver and copper. This coated substrate may be treated as is in the above-mentioned leaching step S1, but in order to more efficiently leach the coating material from the substrate, it is preferable to increase the surface area per unit volume by cutting, shredding, crushing, etc. before the leaching treatment. In addition, if impurities such as oils and fats, contaminants, etc. are attached to or mixed with the coated substrate, it is preferable to perform pretreatment such as washing and classification. Next, each step constituting the silver recovery method of the embodiment of the present invention described above will be described.
[0017] (1) Leaching process S1 In the leaching step S1, the coated substrate is immersed in an iron nitrate solution as a leaching liquid, whereby silver and copper contained in the coating material are oxidized by the iron nitrate acting as an oxidizing agent according to the following reactions 1 and 2, and are leached into the iron nitrate solution as silver ions and copper ions, respectively.
[0018] [Reaction Scheme 1] Fe(NO3)3+Ag→Fe(NO3)2+Ag(NO3) [Reaction Scheme 2] 2Fe(NO3)3+Cu→2Fe(NO3)2+Cu(NO3)2
[0019] The iron nitrate solution used in the leaching treatment of the coated substrate is an aqueous iron nitrate solution containing iron nitrate (III) at a concentration of preferably 35 to 40 mass%. The temperature of the iron nitrate solution during the leaching treatment is not particularly limited, but it is preferable to use a temperature of about 30 to 35°C because it can increase the reaction rate. After the leaching treatment, the Ag-containing Cu-containing iron nitrate solution containing silver ions and copper ions is recovered, and the residue consisting of the substrate from which the coating material has been almost completely removed by dissolution with the leaching solution is taken out. The removed residue can be reused as a raw material for the substrate after removing the iron nitrate solution by washing with water or the like as necessary. Meanwhile, the recovered Ag-containing Cu-containing iron nitrate solution is treated in the next silver recovery step S2.
[0020] (2) Silver recovery process S2 In the silver recovery step S2, a predetermined equivalent amount of hydrochloric acid is added to the Ag-containing Cu-containing iron nitrate solution containing silver ions and copper ions recovered in the previous leaching step S1, thereby causing a reaction between silver ions and chloride ions as shown in the following reaction formula 3. As a result, almost all of the silver ions contained in the iron nitrate solution are precipitated as silver chloride. The precipitated silver chloride is recovered by solid-liquid separation means such as filtration. The recovered silver chloride can be dehydrated and reduced separately by a known method to produce metallic silver.
[0021] [Reaction Scheme 3] Ag(NO3)+HCl→AgCl↓+HNO3
[0022] (3) Regeneration process S3 The Ag-free iron nitrate solution containing Cu after the silver chloride is separated and collected is treated with the Fe 2+ Since the Ag-depleted iron nitrate solution containing Cu is reused as a leaching solution in the above-mentioned leaching step S1, the solution is subjected to an oxidation treatment in the regeneration step S3. 2+ Fe 3+ Since the Ag-depleted Cu-containing iron nitrate solution is oxidized to the Ag-depleted Cu-containing iron nitrate solution, it can be regenerated as an oxidizing agent. There is no particular limitation on the method of this oxidation treatment, and examples include a method of introducing an oxidizing agent such as air, oxygen-enriched air, oxygen, ozone, hydrogen peroxide, etc. into the Ag-depleted Cu-containing iron nitrate solution. Among these, the aeration method in which the Ag-depleted Cu-containing iron nitrate solution is charged into a vessel equipped with a stirrer and air is blown in while stirring, is more preferable because it allows efficient oxidation treatment at low cost.
[0023] The Ag-free Cu-containing iron nitrate solution oxidized as described above is further adjusted in the regeneration step S3 so that the nitrate ion concentration falls within a predetermined concentration range. That is, in the leaching step S1, nitrate ions are consumed in the leaching of metals other than silver, and part of the iron nitrate solution is lost along with the solids separated and recovered in the leaching step S1 and the silver recovery step S2. For this reason, the nitrate ion concentration gradually decreases during the repeated circulation cycle of the iron nitrate solution in the system in which a series of processes including the leaching step S1, the silver recovery step S2, and the regeneration step S3 are repeatedly performed, and there is a risk that the dissolving ability of the iron nitrate solution for silver in the coating material will decrease accordingly. Therefore, the nitrate ion concentration of the iron nitrate solution is measured periodically or as needed, and nitric acid or iron nitrate is added based on the measurement results. The regenerated iron nitrate solution regenerated by the oxidation treatment and concentration adjustment as described above is repeatedly reused as a leachate in the leaching step S1.
[0024] (4) Copper removal electrolysis process S4 As described above, in the leaching step S1, not only the silver but also the copper contained in the coating material is leached into the iron nitrate solution, so that copper ions gradually accumulate in the system as the circulation cycle of the iron nitrate solution is repeated in the system. If this state is left as it is, the dissolving ability of the iron nitrate solution for silver decreases, and the silver recovery efficiency decreases.
[0025] Therefore, the silver recovery method according to the embodiment of the present invention has a copper removal electrolysis step S4 in which a part of the iron nitrate solution before or after regeneration in the regeneration step S3 is extracted and subjected to electrolytic extraction to separate and remove the copper ions as copper metal. In the electrolytic extraction, an insoluble anode and a cathode are immersed in the iron sulfate solution to be electrolytically treated in a state where they face each other, and an electric current is passed between them to deposit the copper ions, which are the target metal in the iron nitrate solution, on the cathode as electrolytic copper. Note that FIG. 1 shows an example in which a part of the Ag-free Cu-containing iron nitrate solution before being regenerated in the regeneration step S3 is treated in the copper removal electrolysis step S4. The Ag-free Cu-free iron nitrate solution after the copper ions are separated and removed by the electrolytic extraction is discharged as waste liquid as shown by the solid line in FIG. 1, or at least a part of it is returned to the system as shown by the dotted line and reused as leachate together with the remaining Ag-free Cu-containing iron nitrate solution.
[0026] In the above-mentioned silver recovery step S2 and regeneration step S3, chemicals such as hydrochloric acid and nitric acid are added, and at that time, water for diluting the chemicals may also be introduced into the system at the same time. In this case, the total amount of the iron nitrate solution circulating in the system (also called hold-up) gradually increases, so it is desirable to appropriately withdraw a part of the circulating iron nitrate solution from the system so that the circulation amount of the iron nitrate solution does not exceed the capacity of the device. Therefore, in the silver recovery method of the embodiment of the present invention, the amount of withdrawal required to maintain the water balance in the system within a predetermined range is calculated, and a part of the iron nitrate solution extracted from the iron nitrate solution circulating in the system with the calculated amount is electrolytically extracted in the above-mentioned copper removal electrolysis step S4. In this case, the iron nitrate solution after the copper ions are separated and removed by electrolytic extraction is discharged as waste liquid, making it possible to stabilize the water balance in the system.
[0027] By determining the amount of extraction by the above method, the water balance in the system can be stabilized, but on the other hand, the copper ions introduced into the system can vary depending on various conditions such as the copper content contained in the coated substrate treated in the leaching step S1, so that with the amount of extraction determined based on the water balance in the system as described above, copper ions will gradually accumulate in the iron nitrate solution circulating in the system, and the copper ion concentration of the iron nitrate solution may eventually exceed its allowable level. Therefore, the copper ion concentration of the iron nitrate solution circulating in the system is measured periodically or as needed, and if the copper ion concentration of the iron nitrate solution circulating in the system gradually increases with the amount of extraction determined based on the water balance, the amount of extraction is determined based on the copper ion balance instead of the water balance. In this case, the iron nitrate solution after separating and removing the copper ions by electrowinning is used as the leachate in its entirety for reuse, or a portion of it is discharged as waste liquid to maintain the water balance in the system, and the remainder is returned to the system to be used as the leachate for reuse. This makes it possible to suppress the fluctuation of the hold-up of the iron nitrate solution in the system within an allowable range while maintaining the copper ion balance in the system.
[0028] As described above, the embodiment of the silver recovery method according to the present invention makes it possible to recover silver safely and stably from the iron nitrate solution obtained by leaching the coated substrate. In addition, since the copper ion balance in the iron nitrate solution in the system can be maintained, the problem of the copper ion concentration in the iron nitrate solution increasing and the dissolving ability decreasing during repeated use of the iron nitrate solution can be prevented. Furthermore, copper can be removed more economically than the conventional copper removal method by cementation. That is, since the copper removal electrolysis step is a batch process independent of the other steps, the preparation thereof and the electrolytic copper recovery work are required separately, but the copper removal electrolysis can be performed every day to several days, so there is no excessive work burden, and the recovered electrolytic copper has a high purity and can be sold at a high price. Next, the silver recovery method of the present invention will be described with examples, but the present invention is not limited to the following examples. EXAMPLES
[0029] [Example 1] The scraps of electronic materials containing silver and copper were treated by a silver recovery method according to the block flow shown in Figure 1. Specifically, first, in the leaching step S1, the scraps were immersed in an iron nitrate solution to perform leaching, and then the iron nitrate solution and the scraps were separated by filtration. In the silver recovery step S2, hydrochloric acid was added to the iron nitrate solution from which the scraps were separated, in an amount equivalent to the silver ions contained in the iron nitrate solution, to precipitate silver chloride, which was then separated and recovered by filtration. The recovered silver chloride was dehydrated. Next, in the regeneration step S3, the iron nitrate solution on the filtrate side obtained in the silver recovery step S2 was charged into a reaction tank equipped with a stirrer, and air was blown into it to perform aeration, thereby performing an oxidation treatment, and then iron nitrate and nitric acid were replenished. The iron nitrate solution thus regenerated was used in the leaching step S1 of the next batch.
[0030] The silver recovery process consisting of the above-mentioned leaching step S1, silver recovery step S2, and regeneration step S3 was repeated 60 batches. In this case, 4 L of water was added per batch in the silver recovery step S2 and regeneration step S3, so in order to maintain the water balance in the system in which the above-mentioned leaching step S1, silver recovery step S2, and regeneration step S3 are performed, a total of 240 L was extracted from the iron nitrate solution before treatment in the regeneration step S3 in several batches, and copper removal electrolysis was performed by electrowinning in each batch to recover the copper ions contained in the iron nitrate solution as electrolytic copper.
[0031] The electrolytic cell used for the electrolytic extraction was equipped with a SUS anode electrode plate and a SUS cathode electrode plate, and a rectifier with a maximum current of 250-500A was used to perform the electrolytic extraction at a current value of about 350A. The iron nitrate solution after the copper ions were removed by the electrolytic extraction was not returned to the system but was disposed of as waste liquid. The above 60 batches of silver recovery were carried out over a period of one month, and it was possible to efficiently process 110-150 kg of processing waste per batch and recover silver at the desired recovery rate. In addition, 50 kg of electrolytic copper was recovered from a total of 240 L of iron nitrate solution extracted from the system.
[0032] [Example 2] Using the same equipment as in Example 1, different lots of processing waste were treated in the same manner as in Example 1. Since the copper ion concentration in the iron nitrate solution circulating in the system gradually increased, the total amount of iron nitrate solution for electrowinning was changed from 240L to 600L, and this was withdrawn in several batches. As a result, the copper ion balance in the system was stabilized, and 110 to 150 kg of processing waste per batch was efficiently treated in the same manner as in Example 1, and silver was recovered at the desired recovery rate. In addition, 100 kg of electrolytic copper was recovered from a total of 600 L of iron nitrate solution in electrowinning. In this Example 2, 360 L of the iron nitrate solution, which is the increase from Example 1, was returned to the system after the copper ions were removed by electrowinning, and the remaining 240 L was disposed of as waste liquid.
Claims
1. A method for recovering silver, comprising the steps of: a leaching step of immersing a substrate coated with a coating material containing silver and copper in an iron nitrate solution as a leaching solution to leach the coating material; a silver recovery step of adding hydrochloric acid to the iron nitrate solution containing silver ions and copper ions obtained in the leaching step to precipitate the silver ions as silver chloride, thereby separating and recovering the silver ions; a regeneration step of regenerating the iron nitrate solution from which the silver chloride has been separated by oxidizing it and adjusting the nitrate ion concentration, and then repeating the process as the leachate; and a copper removal electrolysis step of extracting a portion of the iron nitrate solution before or after the regeneration and performing electrolytic winning to separate and remove the copper ions as copper metal, and then discharging the solution as a waste liquid or repeating at least a portion of the solution as the leachate.
2. 2. The method for recovering silver according to claim 1, wherein the amount of the part of the iron nitrate solution to be withdrawn is determined based on the water balance in the system in which the leaching step, the silver recovery step and the regeneration step are carried out, and the entire amount of the iron nitrate solution after the electrolytic recovery is used as the waste liquid.
3. 2. The method for recovering silver according to claim 1, characterized in that the amount of the part of the iron nitrate solution to be withdrawn is determined based on the copper ion balance in the system in which the leaching step, the silver recovery step and the regeneration step are carried out, and the iron nitrate solution after the electrolytic extraction is either entirely used as the leaching solution and then reused, or a part of the solution is used as the waste liquid in order to maintain the water balance in the system, and the remainder is used as the leaching solution and then reused.
Citation Information
Patent Citations
Silver recovery method
JP2015221934A
Recovery method of silver
JP2021116436A