Steel material

A steel material with controlled segregation and specific composition addresses the issues of wire drawability and loosening resistance in bolts by positioning the maximum segregation area optimally, enhancing both properties.

JP2024148436APending Publication Date: 2024-10-18NIPPON STEEL CORPORATION
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023061558
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-05
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

Existing steel materials for bolts lack excellent wire drawability and effective loosening resistance, particularly when subjected to vibrations, as they do not consider the chemical composition and segregation distribution during manufacturing.

Method used

A steel material with a specific chemical composition and controlled segregation distribution is developed, where the cross section perpendicular to the axial direction has a diameter D, with elements like C, Si, Mn, and Cr, and a segregation degree Stot and Sctr within defined ranges, ensuring the maximum segregation area is positioned appropriately to enhance both wire drawability and loosening resistance.

Benefits of technology

The steel material achieves improved wire drawability and enhanced loosening resistance in bolts, preventing loosening under vibration, by optimizing the segregation pattern and element distribution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024148436000001_ABST
    Figure 2024148436000001_ABST
Patent Text Reader

Abstract

To provide a steel material which can obtain excellent wire drawing workability and looseness resistance.SOLUTION: A steel material contains, by mass%, 0.15 to 0.55% C, 0.01 to 0.40% Si, 0.20 to 1.80% Mn, 0.01 to 1.80% Cr, 0.005 to 0.100% Al, and 0.001 to 0.020% N, wherein when specific element concentration X is represented by expression (1A), specific element concentration X in the whole cross section is represented by Xave, specific element concentration X of a maximum segregation part is represented by Xmax, and specific element concentration X of a central part of a cross section is represented by Xctr, a whole segregation degree Stot of expression (2) is 0.02 to 0.30, a center segregation degree Sctr of expression (3) is 0.02 to 0.30, and a shortest distance between the surface of the steel material and the maximum segregation part is 0.30D to 0.48D. Expression (1A): X=C+Si / 20+Mn / 5+Cr / 5. Expression (2): Stot=(Xmax-Xave) / Xave. Expression (3): Sctr=(Xmax-Xctr) / Xctr.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to steel materials, and more particularly to steel materials suitable for use as bolt materials. [Background technology]

[0002] Bolts are used in mechanical structures such as automobiles and industrial machines, and civil engineering buildings such as bridges. The steel material used to make bolts is manufactured in the following manufacturing process. Molten steel with adjusted composition is poured into a circular or square mold to produce a slab. The slab is hot processed to produce a steel material (steel bar or wire rod) with a circular cross section perpendicular to the axial direction. Bolts made from steel are manufactured in the following manufacturing process. The steel material is subjected to wire drawing (cold drawing). The steel material after wire drawing is subjected to hot forging or cold forging to form a base material including the bolt head. The base material is subjected to thread processing (cutting or rolling) to form the threaded portion of the bolt. Bolts are manufactured through the above manufacturing process. For bolts that require particularly high strength, heat treatment such as quenching and tempering is performed after thread processing.

[0003] Steel materials suitable for use as bolt materials have been studied for some time now. Steel materials suitable for use as bolt materials have been proposed in, for example, JP-A-11-012689 (Patent Document 1) and JP-A-2000-204433 (Patent Document 2).

[0004] The steel material disclosed in Patent Document 1 contains 0.20 to 0.40 weight% C, 0.05 to 3.2 weight% Mn, and 0.001 to 0.15 weight% Si, and has a ferrite fraction of not more than (1-[C%] / 0.4) x 100. The steel material in Patent Document 1 increases the strength of the bolt by adjusting the ferrite fraction according to the C content.

[0005] The steel material disclosed in Patent Document 2 contains C: 0.002 to 0.85%, sol. Al: 0.1% or less, N: 0.015% or less, and further contains one or more selected from the group consisting of Cr: 2% or less, Ti: 0.2% or less, B: 0.01% or less, Nb: 0.1% or less, V: 0.2% or less, Zr: 0.1% or less, and Mo: 0.3% or less, and has a carbon peak height of 2.0 × 10 in an internal friction test. -4 and the nitrogen peak height is 1.7 x 10 -4 The steel material of Patent Document 2 has the above-mentioned configuration, and thereby improves cold workability.

[0006] Incidentally, bolts fastened to mechanical structures, civil engineering buildings, etc. are subject to vibrations and the like after fastening. Continuous exposure to vibrations and the like can cause the fastened bolt to loosen and the fastening axial force to decrease. Recently, there has been a trend toward lighter mechanical structures and civil engineering buildings. To suppress the loss of rigidity that accompanies weight reduction, there is a demand for bolts that are more resistant to loosening. In the following explanation, the property of a bolt that is less likely to loosen is referred to as "loosening resistance."

[0007] A technique for improving the loosening resistance of bolts is proposed in International Publication No. 2010 / 092817 (Patent Document 3). In Patent Document 3, the loosening resistance is improved by adjusting the shape of the threaded portion of the bolt. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Japanese Patent Application Publication No. 11-012689 [Patent Document 2] JP 2000-204433 A [Patent Document 3] International Publication No. 2010 / 092817 Summary of the Invention [Problem to be solved by the invention]

[0009] As described above, wire drawing is performed on steel materials used as bolt materials. Therefore, excellent wire drawing workability is required for the steel materials used as bolt materials. Patent Document 1 and Patent Document 2 do not consider wire drawing workability. Also, Patent Document 3 improves the loosening resistance of the bolt by adjusting the shape of the threaded portion of the bolt. However, no consideration is given to improving the loosening resistance of the bolt at the stage of the steel materials used as bolt materials.

[0010] An object of the present disclosure is to provide a steel material which has excellent wiredrawability and which, when manufactured as a raw material for a bolt, has excellent resistance to loosening. [Means for solving the problem]

[0011] The steel material according to the present disclosure is A steel material having a cross section perpendicular to the axial direction that is circular with a diameter D, Chemical composition, in mass%, C: 0.15-0.55%, Si: 0.01 to 0.40%, Mn: 0.20-1.80%, P: 0.030% or less, S: 0.040% or less, Cr: 0.01 to 1.80%, Al: 0.005 to 0.100%, and N: 0.001 to 0.020%, The balance is Fe and impurities. The specific element concentration X is expressed by the formula (1A), The specific element concentration X in the entire cross section is designated as Xave, The specific element concentration X of the maximum segregation portion of the cross section is defined as Xmax, When the specific element concentration X at the center of the cross section is Xctr, The total segregation degree Stot defined by the formula (2) is 0.02 to 0.30, The center segregation ratio Sctr defined by the formula (3) is 0.02 to 0.30, In the cross section, the shortest radial distance from the surface of the steel material to the maximum segregation portion is 0.30D to 0.48D. X=C+Si / 20+Mn / 5+Cr / 5 (1A) Stot=(Xmax-Xave) / Xave (2) Sctr = (Xmax - Xctr) / Xctr (3) Here, each element symbol in formula (1A) is substituted with the content of the corresponding element in mass %.

[0012] The steel material according to the present disclosure is A steel material having a cross section perpendicular to the axial direction that is circular with a diameter D, Chemical composition, in mass%, C: 0.15-0.55%, Si: 0.01 to 0.40%, Mn: 0.20-1.80%, P:0.030% or less, S: 0.040% or less, Cr: 0.01 to 1.80%, Al: 0.005 to 0.100%, and N: 0.001 to 0.020%, Further, it contains one or more selected from the group consisting of Groups 1 to 3, The balance is Fe and impurities. The specific element concentration X is expressed by the formula (1), The specific element concentration X in the entire cross section is designated as Xave, The specific element concentration X of the maximum segregation portion of the cross section is defined as Xmax, When the specific element concentration X at the center of the cross section is Xctr, The total segregation degree Stot defined by the formula (2) is 0.02 to 0.30, The center segregation ratio Sctr defined by the formula (3) is 0.02 to 0.30, In the cross section, the shortest radial distance from the surface of the steel material to the maximum segregation portion is 0.30D to 0.48D. [Group 1] Cu: 0.40% or less, Ni: 0.40% or less, Mo: 0.80% or less V: 0.80% or less, and B: 0.0100% or less, one or more selected from the group consisting of [Group 2] Ti: 0.100% or less, and Nb: 0.100% or less, one or more selected from the group consisting of [Group 3] Ca: 0.010% or less, Bi: 0.300% or less, Te: 0.300% or less, Zr: 0.300% or less, and Pb: 0.090% or less, one or more selected from the group consisting of X=C+Si / 20+Mn / 5+Cr / 5+Mo / 5 (1) Stot=(Xmax-Xave) / Xave (2) Sctr = (Xmax - Xctr) / Xctr (3) Here, the content of the corresponding element in mass% is substituted for each element symbol in formula (1). When the corresponding element is not contained, "0" is substituted for the corresponding element symbol. Effect of the Invention

[0013] The steel material according to the present disclosure has excellent wiredrawability, and bolts manufactured using the steel material have excellent resistance to loosening. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a cross-sectional view perpendicular to the axial direction of a steel material. [Diagram 2] FIG. 2 is a side view of a bolt manufactured in the loosening resistance evaluation test in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The inventor first investigated steel materials that could be used as bolt materials from the viewpoint of chemical composition. As a result, the inventor concluded that any steel material that has a chemical composition that satisfies the following characteristic 1 could be used as a bolt material. (Feature 1) Chemical composition, by mass%, is C: 0.15-0.55%, Si: 0.01-0.40%, Mn: 0.20-1.80%, P: 0.030% or less, S: 0.040% or less, Cr: 0.01-1.80%, Al: 0.005-0.100%, N: 0.001-0.020%, Cu: 0-0.40%, Ni: 0-0.40%. %, Mo: 0-0.80%, V: 0-0.80%, B: 0-0.0100%, Ti: 0-0.100%, Nb: 0-0.100%, Ca: 0-0.010%, Bi: 0-0.300%, Te: 0-0.300%, Zr: 0-0.300%, and Pb: 0-0.090%, and the balance is Fe and impurities.

[0016] Therefore, further investigation was carried out into means for obtaining excellent wire drawability in a steel material satisfying the characteristic 1. As a result, the present inventors obtained the following findings.

[0017] In a cross section perpendicular to the axial direction of a steel material, a segregation portion exists. The segregation portion occurs due to the following mechanism. When a slab is produced in a casting process during the steel manufacturing process, the molten steel gradually solidifies from the outside to the inside, and the center of the slab is the last to complete solidification. In the final solidification portion, the components become more concentrated than the average solute concentration of the entire steel material, and positive segregation occurs. The portion where this positive segregation occurs is called the maximum segregation portion. Generally, the maximum segregation portion exists in the center of the slab. When a slab having a maximum segregation portion in the center is hot worked to produce a steel material such as a steel bar or wire rod, the maximum segregation portion remains in the center of the produced steel material. If the component concentration of this maximum segregation portion is higher than that of other portions of the steel material, a hard structure is generated in the maximum segregation portion. If a hard structure is generated locally in this way, the toughness of the steel material decreases, and the wiredrawability of the steel material decreases.

[0018] Based on the above findings, the inventors of the present invention considered that if the generation of hard structures in the maximum segregation parts can be suppressed, the wiredrawability of the steel material will be improved. Among the elements in the chemical composition of Feature 1, C, Si, Mn, Cr, and Mo are likely to concentrate in the maximum segregation parts, and if these elements concentrate in the maximum segregation parts, hard structures are likely to be generated in the maximum segregation parts. Therefore, the inventors of the present invention considered that if the concentration of these elements in the maximum segregation parts can be suppressed, the wiredrawability of the steel material will be improved.

[0019] The present inventor further investigated means for obtaining excellent resistance to loosening in a bolt manufactured as a material. In conventional investigations, as disclosed in the above-mentioned Patent Document 3, attempts have been made to improve resistance to loosening by adjusting the shape of the threaded portion of the bolt. However, unlike the conventional approach, the present inventor investigated means for improving the resistance to loosening of a bolt at the stage of the steel material from which the bolt is manufactured, rather than the shape of the manufactured bolt. As a result, the present inventor obtained the following findings.

[0020] The maximum segregation area of ​​the steel remains in the bolt manufactured using the steel as the material. The degree of elastic deformation differs between the maximum segregation area and the area other than the maximum segregation area. In conventional steel, the maximum segregation area is located in the center. Therefore, even in bolts manufactured using steel as the material, the maximum segregation area is located in the center of the bolt (the area including the central axis of the bolt). In this case, the elastic deformation that occurs in the bolt when fastened occurs equally and symmetrically about the axis. As a result, the frictional force at the interface between the male thread of the bolt and the female thread of the fastened material is difficult to maintain, and there are cases in which sufficient loosening resistance cannot be obtained.

[0021] On the other hand, if the maximum segregation area is located away from the center of the steel material, there will be a slight bias in the elastic deformation that occurs during fastening. In this case, there will be a bias in the stress of the threaded portion. This will cause a local increase in the friction force at the interface between the male thread of the bolt and the female thread of the fastened material. As a result, the bolt's resistance to loosening will increase.

[0022] Based on the above findings, the inventors considered that excellent wiredrawability could be obtained in a steel material and excellent loosening resistance could be obtained in a bolt by (1) setting the degree of segregation in the maximum segregation part within an appropriate range, and (2) shifting the maximum segregation part to an appropriate range from the center in a cross section perpendicular to the axial direction of the steel material. As a result of further investigation, the inventors found that, in a steel material satisfying characteristic 1, if the following characteristics 2 and 3 are also satisfied, excellent wiredrawability can be obtained, and further, a bolt manufactured using the steel material as a raw material can have excellent loosening resistance. (Feature 2) When the specific element concentration X is defined as formula (1), the specific element concentration X in the entire cross section perpendicular to the axial direction of the steel material is defined as Xave, the specific element concentration X in the maximum segregation part of the cross section is defined as Xmax, and the specific element concentration X in the center part of the cross section is defined as Xctr, the total segregation degree Stot defined by formula (2) is 0.02 to 0.30, and the central segregation degree Sctr defined by formula (3) is 0.02 to 0.30. X=C+Si / 20+Mn / 5+Cr / 5+Mo / 5 (1) Stot=(Xmax-Xave) / Xave (2) Sctr = (Xmax - Xctr) / Xctr (3) Here, the content of the corresponding element in mass% is substituted for each element symbol in formula (1). When the corresponding element is not contained, "0" is substituted for the corresponding element symbol. Specifically, when the chemical composition does not contain the optional element Mo, the specific element concentration X is expressed by the following formula (1A). X=C+Si / 20+Mn / 5+Cr / 5 (1A) (Feature 3) When the diameter of the cross section is D (mm), the shortest radial distance from the surface of the steel material to the maximum segregation portion in the cross section is 0.30D to 0.48D.

[0023] The steel material of this embodiment has been completed based on the above-mentioned technical concept, and has the following configuration.

[0024] [1] A steel material having a cross section perpendicular to the axial direction that is circular with a diameter D, Chemical composition, in mass%, C: 0.15-0.55%, Si: 0.01 to 0.40%, Mn: 0.20-1.80%, P:0.030% or less, S: 0.040% or less, Cr: 0.01 to 1.80%, Al: 0.005 to 0.100%, and N: 0.001 to 0.020%, The balance is Fe and impurities. The specific element concentration X is expressed by the formula (1A), The specific element concentration X in the entire cross section is designated as Xave, The specific element concentration X of the maximum segregation portion of the cross section is defined as Xmax, When the specific element concentration X at the center of the cross section is Xctr, The total segregation degree Stot defined by the formula (2) is 0.02 to 0.30, The center segregation ratio Sctr defined by the formula (3) is 0.02 to 0.30, In the cross section, the shortest radial distance from the surface of the steel material to the maximum segregation portion is 0.30D to 0.48D. Steel material. X=C+Si / 20+Mn / 5+Cr / 5 (1A) Stot=(Xmax-Xave) / Xave (2) Sctr = (Xmax - Xctr) / Xctr (3) Here, each element symbol in formula (1A) is substituted with the content of the corresponding element in mass %.

[0025] [2] A steel material having a cross section perpendicular to the axial direction that is circular with a diameter D, Chemical composition, in mass%, C: 0.15-0.55%, Si: 0.01 to 0.40%, Mn: 0.20-1.80%, P: 0.030% or less, S: 0.040% or less, Cr: 0.01 to 1.80%, Al: 0.005 to 0.100%, and N: 0.001 to 0.020%, Further, it contains one or more selected from the group consisting of Groups 1 to 3, The balance is Fe and impurities. The specific element concentration X is expressed by the formula (1), The specific element concentration X in the entire cross section is designated as Xave, The specific element concentration X of the maximum segregation portion of the cross section is defined as Xmax, When the specific element concentration X at the center of the cross section is Xctr, The total segregation degree Stot defined by the formula (2) is 0.02 to 0.30, The center segregation ratio Sctr defined by the formula (3) is 0.02 to 0.30, In the cross section, the shortest radial distance from the surface of the steel material to the maximum segregation portion is 0.30D to 0.48D. Steel material. [Group 1] Cu: 0.40% or less, Ni: 0.40% or less, Mo: 0.80% or less V: 0.80% or less, and B: 0.0100% or less, one or more selected from the group consisting of [Group 2] Ti: 0.100% or less, and Nb: 0.100% or less, one or more selected from the group consisting of [Group 3] Ca: 0.010% or less, Bi: 0.300% or less, Te: 0.300% or less, Zr: 0.300% or less, and Pb: 0.090% or less, one or more selected from the group consisting of X=C+Si / 20+Mn / 5+Cr / 5+Mo / 5 (1) Stot=(Xmax-Xave) / Xave (2) Sctr = (Xmax - Xctr) / Xctr (3) Here, the content of the corresponding element in mass% is substituted for each element symbol in formula (1). When the corresponding element is not contained, "0" is substituted for the corresponding element symbol.

[0026] [3] [2] The steel material according to the present invention, The chemical composition contains the first group, Steel material.

[0027] [4] The steel material according to [2] or [3], The chemical composition contains the second group, Steel material.

[0028] [5] The steel material according to any one of [2] to [4], The chemical composition contains the third group, Steel material.

[0029] The steel material according to this embodiment will be described in detail below. "%" for elements means mass % unless otherwise specified.

[0030] [Features of the steel material of this embodiment] The steel material of this embodiment is a steel material whose cross section perpendicular to the axial direction is circular and has a diameter D (mm), and satisfies the following characteristics 1 to 3. (Feature 1) The chemical composition, in mass%, is C: 0.15-0.55%, Si: 0.01-0.40%, Mn: 0.20-1.80%, P: 0.030% or less, S: 0.040% or less, Cr: 0.01-1.80%, Al: 0.005-0.100%, N: 0.001-0.020%, Cu: 0-0.40%, Ni: 0-0.4 0%, Mo: 0-0.80%, V: 0-0.80%, B: 0-0.0100%, Ti: 0-0.100%, Nb: 0-0.100%, Ca: 0-0.010%, Bi: 0-0.300%, Te: 0-0.300%, Zr: 0-0.300%, Pb: 0-0.090%, and the balance is Fe and impurities. (Feature 2) The specific element concentration X is expressed by the formula (1), The concentration of a specific element in the entire cross section perpendicular to the axial direction of the steel material is designated as Xave. The specific element concentration X in the maximum segregation portion of the cross section is defined as Xmax. When the concentration of a specific element at the center of the above cross section is Xctr, The total segregation degree Stot defined by the formula (2) is 0.02 to 0.30, The center segregation ratio Sctr defined by formula (3) is 0.02 to 0.30. X=C+Si / 20+Mn / 5+Cr / 5+Mo / 5 (1) Stot=(Xmax-Xave) / Xave (2) Sctr = (Xmax - Xctr) / Xctr (3) Here, the content of the corresponding element in mass% is substituted for each element symbol in formula (1). When the corresponding element is not contained, "0" is substituted for the corresponding element symbol. Specifically, when the chemical composition does not contain the optional element Mo, the specific element concentration X is expressed by the following formula (1A). X=C+Si / 20+Mn / 5+Cr / 5 (1A) (Feature 3) When the diameter of the cross section is D (mm), the shortest radial distance from the surface of the steel material to the maximum segregation portion in the cross section is 0.30D to 0.48D. Features 1 to 3 will be explained below.

[0031] [(Feature 1) Chemical composition] The chemical composition of the steel material according to this embodiment contains the following elements.

[0032] C: 0.15-0.55% Carbon (C) increases the strength of steel. If the C content is less than 0.15%, the above effect cannot be sufficiently obtained. On the other hand, if the C content exceeds 0.55%, it segregates in the final solidified part of the steel. In this case, the wire drawability of the steel decreases. Therefore, the C content is 0.15 to 0.55%. The lower limit of the C content is preferably 0.16%, more preferably 0.17%, and further preferably 0.18%. The upper limit of the C content is preferably 0.53%, more preferably 0.51%, and further preferably 0.50%.

[0033] Silicon: 0.01 to 0.40% Silicon (Si) deoxidizes steel. Si also increases the strength of steel. If the Si content is less than 0.01%, the above effects are not sufficiently obtained. On the other hand, if the Si content exceeds 0.40%, it segregates in the final solidification part of the steel. In this case, the wire drawability of the steel decreases. Therefore, the Si content is 0.01 to 0.40%. The lower limit of the Si content is preferably 0.02%, more preferably 0.03%, and further preferably 0.04%. The upper limit of the Si content is preferably 0.38%, more preferably 0.36%, and further preferably 0.35%.

[0034] Mn: 0.20 to 1.80% Manganese (Mn) deoxidizes steel. Mn also increases the strength of steel. If the Mn content is less than 0.20%, the above effects are not fully achieved. On the other hand, if the Mn content exceeds 1.80%, it segregates in the final solidification part of the steel. In this case, the drawability of the steel decreases. Therefore, the Mn content is 0.20 to 1.80%. The lower limit of the Mn content is preferably 0.21%, more preferably 0.22%, and further preferably 0.23%. The upper limit of the Mn content is preferably 1.70%, more preferably 1.60%, and further preferably 1.50%.

[0035] P:0.030% or less Phosphorus (P) is an impurity. P segregates at the grain boundaries of steel and reduces grain boundary strength. If the P content exceeds 0.030%, the grain boundary strength decreases, resulting in a decrease in the hydrogen embrittlement resistance of the steel. Therefore, the P content is 0.030% or less. The P content is preferably as low as possible. However, excessive reduction in the P content reduces productivity and increases production costs. Therefore, in consideration of normal industrial production, the lower limit of the P content is preferably more than 0%, more preferably 0.001%, more preferably 0.002%, and even more preferably 0.003%. The upper limit of the P content is preferably 0.028%, more preferably 0.026%, and further preferably 0.025%.

[0036] S: 0.040% or less Sulfur (S) is an impurity. S segregates at the grain boundaries of steel and reduces grain boundary strength. If the S content exceeds 0.040%, the grain boundary strength decreases, resulting in a decrease in the hydrogen embrittlement resistance of the steel. Therefore, the S content is 0.040% or less. The S content is preferably as low as possible. However, excessive reduction in the S content reduces productivity and increases manufacturing costs. Therefore, in consideration of normal industrial production, the preferred lower limit of the S content is more than 0%, more preferably 0.001%, more preferably 0.002%, and even more preferably 0.003%. The upper limit of the S content is preferably 0.038%, more preferably 0.036%, and further preferably 0.035%.

[0037] Cr: 0.01~1.80% Chromium (Cr) increases the strength of steel. If the Cr content is less than 0.01%, the above effect cannot be sufficiently obtained. On the other hand, if the Cr content exceeds 1.80%, it segregates in the final solidification part of the steel. In this case, the wire drawability of the steel decreases. Therefore, the Cr content is 0.01 to 1.80%. The lower limit of the Cr content is preferably 0.02%, more preferably 0.03%, and further preferably 0.04%. The upper limit of the Cr content is preferably 1.60%, more preferably 1.50%, and further preferably 1.40%.

[0038] Al: 0.005 to 0.100% Aluminum (Al) deoxidizes steel. Furthermore, Al bonds with N to form Al nitrides. Al nitrides suppress the coarsening of crystal grains through a pinning effect. As a result, the hydrogen embrittlement resistance of the steel material is improved. If the Al content is less than 0.005%, the above effect cannot be sufficiently obtained. On the other hand, if the Al content exceeds 0.100%, coarse Al nitrides are formed. Coarse Al nitrides cause defects during hot rolling. Therefore, the Al content is 0.005 to 0.100%. The lower limit of the Al content is preferably 0.006%, more preferably 0.007%, and further preferably 0.008%. The upper limit of the Al content is preferably 0.080%, more preferably 0.060%, and further preferably 0.040%. In the chemical composition of the steel material of this embodiment, the Al content means the total Al (Total-Al) content.

[0039] N: 0.001 to 0.020% Nitrogen (N) combines with Al to form nitrides. Al nitrides suppress the coarsening of crystal grains through a pinning effect. As a result, hydrogen embrittlement resistance of the steel is improved. If the N content is less than 0.001%, the above effect cannot be sufficiently obtained. On the other hand, if the N content exceeds 0.020%, coarse Al nitrides that cause defects during hot rolling are generated. Therefore, the N content is 0.001 to 0.020%. The lower limit of the N content is preferably 0.002%, more preferably 0.003%, and further preferably 0.004%. The upper limit of the N content is preferably 0.019%, more preferably 0.018%, and further preferably 0.017%.

[0040] The balance of the chemical composition of the steel material of the present embodiment is composed of Fe and impurities. Here, the term "impurities" refers to substances that are mixed in from raw materials such as ores and scraps or from the manufacturing environment during industrial production of the steel material, but are not intentionally contained and are permissible within a range that does not adversely affect the steel material of the present embodiment.

[0041] [About optional elements] The chemical composition of the steel material of this embodiment may further contain one or more elements selected from the group consisting of first to third groups. [Group 1] Cu: 0.40% or less, Ni: 0.40% or less, Mo: 0.80% or less V: 0.80% or less, and B: 0.0100% or less, one or more selected from the group consisting of [Group 2] Ti: 0.100% or less, and Nb: 0.100% or less, one or more selected from the group consisting of [Group 3] Ca: 0.010% or less, Bi: 0.300% or less, Te: 0.300% or less, Zr: 0.300% or less, and Pb: 0.090% or less, one or more selected from the group consisting of The first to third groups will be explained below.

[0042] [Group 1 (Cu, Ni, Mo, V and B)] The chemical composition of the steel material of this embodiment may further contain, instead of a part of Fe, one or more elements selected from the group consisting of Cu, Ni, Mo, V, and B. All of these elements are optional elements and may not be contained. When contained, Cu, Ni, Mo, V, and B increase the strength of the steel material. Each element will be described below.

[0043] Cu: 0.40% or less Copper (Cu) is an optional element and may not be contained. In other words, the Cu content may be 0%. When it is contained, that is, when the Cu content is more than 0%, it increases the strength of the steel material. Even if even a small amount of Cu is contained, the above effect can be obtained to a certain extent. However, when the Cu content exceeds 0.40%, the effect is saturated. Therefore, the Cu content is 0 to 0.40%, and when it is contained, the Cu content is 0.40% or less. The lower limit of the Cu content is preferably 0.01%, more preferably 0.02%, and further preferably 0.03%. The upper limit of the Cu content is preferably 0.35%, more preferably 0.30%, and further preferably 0.25%.

[0044] Ni: 0.40% or less Nickel (Ni) is an optional element and may not be contained. In other words, the Ni content may be 0%. When it is contained, that is, when the Ni content is more than 0%, it increases the strength of the steel material. Even if even a small amount of Ni is contained, the above effect can be obtained to a certain extent. However, when the Ni content exceeds 0.40%, the effect is saturated. Therefore, the Ni content is 0 to 0.40%, and when it is contained, the Ni content is 0.40% or less. The lower limit of the Ni content is preferably 0.01%, more preferably 0.02%, and further preferably 0.03%. The upper limit of the Ni content is preferably 0.35%, more preferably 0.30%, and further preferably 0.25%.

[0045] Mo: 0.80% or less Molybdenum (Mo) is an optional element and may not be contained. In other words, the Mo content may be 0%. When contained, that is, when the Mo content is more than 0%, it increases the strength of the steel material. Even if even a small amount of Mo is contained, the above effects can be obtained to a certain extent. However, when the Mo content exceeds 0.80%, the effect is saturated. Therefore, the Mo content is 0 to 0.80%, and when contained, the Mo content is 0.80% or less. The lower limit of the Mo content is preferably 0.01%, more preferably 0.02%, and further preferably 0.03%. The upper limit of the Mo content is preferably 0.75%, more preferably 0.70%, and further preferably 0.65%.

[0046] V:0.80% or less Vanadium (V) is an optional element and may not be contained. In other words, the V content may be 0%. When it is contained, that is, when the V content is more than 0%, it increases the strength of the steel material. Even if even a small amount of V is contained, the above effect can be obtained to a certain extent. However, when the V content exceeds 0.80%, the effect is saturated. Therefore, the V content is 0 to 0.80%, and when it is contained, the V content is 0.80% or less. The lower limit of the V content is preferably 0.01%, more preferably 0.02%, and further preferably 0.03%. The upper limit of the V content is preferably 0.75%, more preferably 0.70%, and further preferably 0.65%.

[0047] B: 0.0100% or less Boron (B) is an optional element and may not be contained. In other words, the B content may be 0%. When it is contained, that is, when the B content is more than 0%, it increases the strength of the steel material. Even if even a small amount of B is contained, the above effect can be obtained to a certain degree. However, when the B content exceeds 0.0100%, the effect is saturated. Therefore, the B content is 0 to 0.0100%, and when it is contained, the B content is 0.0100% or less. The lower limit of the B content is preferably 0.0002%, more preferably 0.0004%, and further preferably 0.0005%. The upper limit of the B content is preferably 0.0080%, more preferably 0.0060%, and further preferably 0.0040%.

[0048] [Group 2 (Ti and Nb)] The chemical composition of the steel material of this embodiment may further contain one or more elements selected from the group consisting of Ti and Nb, instead of a portion of Fe. All of these elements are optional elements and may not be contained. When contained, Ti and Nb combine with C and N to form carbonitrides. These carbonitrides suppress the coarsening of crystal grains by a pinning effect. As a result, the hydrogen embrittlement resistance of the steel material is improved. Each element will be described below.

[0049] Ti:0.100% or less Titanium (Ti) is an optional element and may not be contained. In other words, the Ti content may be 0%. When titanium is contained, that is, when the Ti content is more than 0%, Ti combines with C and N to form carbonitrides and suppress the coarsening of crystal grains. As a result, the hydrogen embrittlement resistance of the steel material is improved. If even a small amount of Ti is contained, the above effect can be obtained to some extent. However, if the Ti content exceeds 0.100%, coarse carbonitrides are formed, which causes defects during hot rolling. Therefore, the Ti content is 0 to 0.100%, and when contained, the Ti content is 0.100% or less. The lower limit of the Ti content is preferably 0.002%, more preferably 0.004%, and further preferably 0.006%. The upper limit of the Ti content is preferably 0.080%, more preferably 0.060%, and further preferably 0.050%.

[0050] Nb: 0.100% or less Niobium (Nb) is an optional element and may not be contained. In other words, the Nb content may be 0%. When it is contained, that is, when the Nb content is more than 0%, Nb bonds with C and N to form carbonitrides and suppresses the coarsening of crystal grains. As a result, the hydrogen embrittlement resistance of the steel material is improved. If even a small amount of Nb is contained, the above effect can be obtained to some extent. However, if the Nb content exceeds 0.100%, coarse carbonitrides are formed, which causes defects during hot rolling. Therefore, the Nb content is 0 to 0.100%, and when it is contained, the Nb content is 0.100% or less. The lower limit of the Nb content is preferably 0.002%, more preferably 0.004%, and further preferably 0.006%. The upper limit of the Nb content is preferably 0.080%, more preferably 0.060%, and further preferably 0.050%.

[0051] [Group 3 (Ca, Bi, Te, Zr and Pb)] The chemical composition of the steel material of this embodiment may further contain Ca, Bi, Te, Zr and Pb instead of a part of Fe. All of these elements are optional elements and may not be contained. When contained, Ca, Bi, Te, Zr and Pb all improve the machinability of the steel material. Each element will be described below.

[0052] Ca: 0.010% or less Calcium (Ca) is an optional element and may not be contained. In other words, the Ca content may be 0%. When contained, Ca improves the machinability of the steel material. Even if even a small amount of Ca is contained, the above effect can be obtained to a certain degree. However, if the Ca content exceeds 0.010%, the hot ductility of the steel material decreases. Therefore, the Ca content is 0 to 0.010%, and when contained, the Ca content is 0.010% or less. The lower limit of the Ca content is preferably 0.001%, more preferably 0.002%, and further preferably 0.003%. The upper limit of the Ca content is preferably 0.080%, more preferably 0.060%, and further preferably 0.040%.

[0053] Bi:0.300% or less Bismuth (Bi) is an optional element and may not be contained. In other words, the Bi content may be 0%. When contained, Bi improves the machinability of the steel material. Even if even a small amount of Bi is contained, the above effect can be obtained to a certain degree. However, if the Bi content exceeds 0.300%, the hot ductility of the steel material decreases. Therefore, the Bi content is 0 to 0.300%, and when contained, the Bi content is 0.300% or less. The lower limit of the Bi content is preferably 0.001%, more preferably 0.002%, and further preferably 0.003%. The upper limit of the Bi content is preferably 0.280%, more preferably 0.260%, and further preferably 0.240%.

[0054] Te: 0.300% or less Tellurium (Te) is an optional element and may not be contained. In other words, the Te content may be 0%. When contained, Te improves the machinability of the steel. Even if even a small amount of Te is contained, the above effect can be obtained to a certain degree. However, if the Te content exceeds 0.300%, the hot ductility of the steel decreases. Therefore, the Te content is 0 to 0.300%, and when contained, the Te content is 0.300% or less. The lower limit of the Te content is preferably 0.001%, more preferably 0.002%, and further preferably 0.003%. The upper limit of the Te content is preferably 0.280%, more preferably 0.260%, and further preferably 0.240%.

[0055] Zr: 0.300% or less Zirconium (Zr) is an optional element and may not be contained. In other words, the Zr content may be 0%. When contained, Zr improves the machinability of the steel material. Even if even a small amount of Zr is contained, the above effect can be obtained to some extent. However, if the Zr content exceeds 0.300%, the hot ductility of the steel material decreases. Therefore, the Zr content is 0 to 0.300%, and when contained, the Zr content is 0.300% or less. The lower limit of the Zr content is preferably 0.001%, more preferably 0.002%, and further preferably 0.003%. The upper limit of the Zr content is preferably 0.280%, more preferably 0.260%, and further preferably 0.240%.

[0056] Pb:0.090% or less Lead (Pb) is an optional element and may not be contained. In other words, the Pb content may be 0%. When contained, Pb improves the machinability of the steel. Even if even a small amount of Pb is contained, the above effect can be obtained to some extent. However, if the Pb content exceeds 0.090%, the hot ductility of the steel decreases. Therefore, the Pb content is 0 to 0.090%, and when contained, the Pb content is 0.090% or less. The lower limit of the Pb content is preferably 0.001%, more preferably 0.002%, and further preferably 0.003%. The upper limit of the Pb content is preferably 0.089%, more preferably 0.088%, and further preferably 0.087%.

[0057] [(Feature 2) Segregation of specific elements] In the steel material of this embodiment, the segregation degree of elements that are prone to segregation, C, Si, Mn, Cr, and Mo, in the chemical composition that satisfies the characteristic 1, is set to an appropriate range. Specifically, the specific element concentration X is defined by the formula (1). X=C+Si / 20+Mn / 5+Cr / 5+Mo / 5 (1) Here, the content of the corresponding element in mass% is substituted for each element symbol in formula (1). When the corresponding element is not contained, "0" is substituted for the corresponding element symbol. Specifically, when the chemical composition does not contain the optional element Mo, the specific element concentration X is expressed by the following formula (1A). X=C+Si / 20+Mn / 5+Cr / 5 (1A)

[0058] Here, the specific element concentration X in the entire cross section perpendicular to the axial direction of the steel material is designated as Xave. In other words, Xave means the average value of the specific element concentration X in the cross section. Furthermore, the specific element concentration X in the maximum segregation part of the cross section is designated as Xmax, and the specific element concentration X in the center part of the cross section is designated as Xctr. In this case, the total segregation degree Stot defined by formula (2) is set to 0.02 to 0.30, and the center segregation degree Sctr defined by formula (3) is set to 0.02 to 0.30. Stot=(Xmax-Xave) / Xave (2) Sctr = (Xmax - Xctr) / Xctr (3) If the overall segregation degree Stot is 0.02 to 0.30 and the center segregation degree Sctr is 0.02 to 0.30, the segregation degree distribution in the steel material is appropriate. In this case, excellent wiredrawability is obtained, and further, excellent loosening resistance is obtained in the bolt. Formulas (1) to (3) will be explained below.

[0059] [Regarding the specific element concentration X defined in formula (1)] Of the chemical compositions that satisfy characteristic 1, C, Si, Mn, Cr, and Mo are all elements that tend to concentrate in the final solidified portion during the casting process. If these elements concentrate, localized hard structures are formed after solidification. The specific element concentration X defined in formula (1) is an index of the concentration of elements that tend to concentrate in the final solidified portion. If the specific element concentration X is high, it means that these elements tend to concentrate in the final solidified portion. The coefficient of each element in formula (1) indicates the degree of influence of each element on segregation.

[0060] [Regarding the total segregation degree Stot defined by formula (2)] The total segregation degree Stot defined by formula (2) indicates the degree of segregation between the specific element concentration Xave throughout the entire cross section perpendicular to the axial direction of the steel material and the specific element concentration Xmax at the maximum segregation portion of the cross section.

[0061] If the overall segregation degree Stot is less than 0.02, the segregation degree in the cross section of the steel material is too low. In this case, the loosening resistance of a bolt manufactured using the steel material as a raw material decreases. In other words, the fastened bolt is more likely to loosen. On the other hand, if the overall segregation degree Stot exceeds 0.30, the segregation degree is too high. In this case, the wiredrawability of the steel material decreases. In other words, when the steel material is used as a raw material for wiredrawing, the steel material is more likely to break. Therefore, the overall segregation degree Stot is 0.02 to 0.30.

[0062] The lower limit of the total segregation degree Stot is preferably 0.03, more preferably 0.04, and even more preferably 0.05. The upper limit of the total segregation degree Stot is preferably 0.29, more preferably 0.28, and even more preferably 0.27.

[0063] [Regarding the central segregation ratio Sctr defined by formula (3)] The central segregation ratio Sctr defined by formula (3) is the ratio of the specific element concentration Xmax at the maximum segregation portion to the specific element concentration Xctr at the center in a cross section perpendicular to the axial direction of the steel material.

[0064] The central segregation degree Sctr indicates the degree of segregation between the specific element concentration Xctr at the center of a cross section perpendicular to the axial direction of the steel material and the specific element concentration Xmax at the maximum segregation portion of the cross section. If the central segregation ratio Sctr is less than 0.02, the difference in specific element concentration between the cross-section center and the maximum segregation part is too small. Or, the maximum segregation part is close to the cross-section center. In this case, the loosening resistance of a bolt manufactured using the steel material as a material is reduced. On the other hand, if the central segregation ratio Sctr exceeds 0.30, the segregation ratio between the cross-section center and the maximum segregation part is too high. In this case, the wiredrawability of the steel material is reduced. Therefore, the central segregation ratio Sctr is 0.02 to 0.30.

[0065] The lower limit of the central segregation ratio Sctr is preferably 0.03, more preferably 0.04, and even more preferably 0.05. The upper limit of the central segregation ratio Sctr is preferably 0.29, more preferably 0.28, and even more preferably 0.27.

[0066] [(Feature 3) Position of maximum segregation in cross section] As described above, in a steel material having a circular cross section perpendicular to the axial direction, the maximum segregation portion is usually located at the center of the cross section. However, in the steel material of the present embodiment, the maximum segregation portion is intentionally shifted from the center of the cross section to a predetermined range. This ensures sufficient wiredrawability while suppressing loosening during fastening of a bolt manufactured using the steel material as a material.

[0067] Fig. 1 is a cross-sectional view perpendicular to the axial direction of a steel material. Referring to Fig. 1, when the diameter of the cross-section perpendicular to the axial direction of the steel material is defined as D (mm), the shortest radial distance Lmin from the surface of the steel material to the maximum segregation part 10 in the cross-section perpendicular to the axial direction of the steel material is set to 0.30D to 0.48D.

[0068] If the minimum radial distance Lmin from the surface of the steel material to the maximum segregation part is less than 0.30D, the maximum segregation part is too far from the center of the cross section. In this case, when the steel material is used as a material for wire drawing, non-uniform deformation occurs and processing strain is locally concentrated. Therefore, the wire drawing workability of the steel material is reduced. On the other hand, if the minimum radial distance Lmin from the surface of the steel material to the maximum segregation part exceeds 0.48D, the maximum segregation part is too close to the center of the cross section. In this case, the stress when the bolt manufactured using the steel material as a material is fastened is distributed evenly symmetrically along the axis. Therefore, the friction force at the interface between the male thread of the bolt and the female thread of the fastened material cannot be sufficiently secured, and the loosening resistance of the bolt is reduced. Therefore, in a cross section perpendicular to the axial direction of the steel material, the minimum radial distance Lmin from the surface of the steel material to the maximum segregation part is 0.30D to 0.48D.

[0069] The lower limit of the minimum distance Lmin is preferably 0.33D, more preferably 0.35D, more preferably 0.37D, more preferably 0.40D, and even more preferably 0.41D. A preferred upper limit of the minimum distance Lmin is 0.47D, more preferably 0.46D, and even more preferably 0.45D.

[0070] [Method of measuring the chemical composition of steel] The chemical composition of the steel material of this embodiment can be measured by a known compositional analysis method. Specifically, chips are collected from the entire cross section perpendicular to the longitudinal direction of the steel material by milling or the like, evenly in the longitudinal direction. The collected chips are dissolved in acid to obtain a solution. An elemental analysis of the chemical composition is performed on the solution by ICP-AES (Inductively Coupled Plasma Atomic Emission Spectrometry). The C content and S content are determined by a known high-frequency combustion method (combustion-infrared absorption method). The N content is determined by a known inert gas fusion-thermal conductivity method.

[0071] [How to determine specific element concentration Xave] The specific element concentration Xave is calculated by substituting the C content, Si content, Mn content, Cr content, and Mo content in mass% obtained in the above-mentioned [Method of measuring the chemical composition of steel material] into formula (1) or formula (1A).

[0072] [Method of measuring the shortest distance Lmin, specific element concentration Xmax and Xctr] The shortest distance Lmin, specific element concentrations Xmax and Xctr are calculated as follows. A cross section perpendicular to the axial direction of the steel material is cut, and this cross section is used as the investigation surface. The diameter of the investigation surface is measured at six points (0°, 60°, 120°, 180°, 240°, 300°) at 60° intervals from an arbitrary measurement start position. The diameter is measured using a measuring microscope or an image dimension measuring device. If each of the six diameters obtained on the investigation surface is within ±3% of the arithmetic mean of the six diameters, the investigation surface is considered to be circular. If any of the diameters on the investigation surface exceeds ±3% of the arithmetic mean of the six diameters, a cross section perpendicular to the axial direction is cut at a different position in the axial direction of the steel material, and the diameter is measured again using this cross section as the investigation surface. For measuring the specific element concentrations Xmax and Xctr, an investigation surface is used in which each of the six diameters is within ±3% of the arithmetic mean value of the six diameters. Preferably, each of the six diameters on the investigation surface is within ±2% of the arithmetic mean value of the six diameters, and more preferably within ±1%.

[0073] The investigation surface is mirror-polished. After mirror polishing, the investigation surface is etched by hydrochloric acid according to JIS G 0553:2012 to reveal macro-corrosion on the investigation surface. The maximum segregation area on the investigation surface after macro-corrosion is identified. On the investigation surface after macro-corrosion, a person skilled in the art can easily identify the maximum segregation area based on the contrast by visually inspecting the appearance or observing with a magnifying glass.

[0074] After identifying the maximum segregation area, the shortest radial distance Lmin from the surface to the maximum segregation area is measured on the investigation surface using a measuring microscope or image dimension measuring device. Furthermore, the diameter D on the same line as the shortest distance Lmin is obtained. Based on the obtained diameter D and shortest distance Lmin, the ratio of the shortest distance Lmin to the diameter D (=Lmin / D) is obtained. The obtained ratio is multiplied by the diameter D to convert the shortest distance Lmin into D. The shortest distance Lmin is obtained by the above method.

[0075] Next, a mark such as an indentation is made around the identified maximum segregation area. After making the mark, the investigation surface is mirror-polished again. The mark remains on the investigation surface after mirror polishing. The maximum segregation area is identified based on the mark on the investigation surface after mirror polishing. An elemental analysis is performed on the identified maximum segregation area using an electron probe micro analyzer (EPMA). With the EPMA, an accelerating voltage of 15 kV and a probe current of 5×10 -7 A and a beam diameter of 1 μm are used to obtain the element contents of C, Si, Mn, Cr, and Mo in the maximum segregation area. The obtained element contents are substituted into formula (1) to obtain the specific element concentration Xmax in the maximum segregation area.

[0076] In addition, when there are multiple segregation parts on the macro-exposed investigation surface, the above-mentioned EPMA is performed on all the segregation parts to obtain the specific element concentration of each segregation part. Then, the segregation part with the maximum specific element concentration among the obtained specific element concentrations is recognized as the maximum segregation part. The specific element concentration of the segregation part recognized as the maximum segregation part is designated as the specific element concentration Xmax of the maximum segregation part.

[0077] In addition, the above-mentioned elemental analysis is performed by EPMA at the center position of any of the six diameters of the investigation surface to obtain the elemental contents of C, Si, Mn, Cr, and Mo. The obtained elemental contents are substituted into formula (1) to obtain the specific element concentration Xctr at the center.

[0078] Based on the obtained characteristic element concentrations Xave, Xmax, and Xctr, the total segregation degree Stot and the center segregation degree Sctr are calculated using equations (2) and (3).

[0079] [Regarding the form and applicable uses of the steel material of this embodiment] The steel material of this embodiment may be a steel bar or a wire rod. The steel material of this embodiment satisfies Features 1 to 3. Therefore, the steel material of this embodiment has excellent wiredrawability. Furthermore, the steel material has improved resistance to loosening of a bolt manufactured using the steel material as a material, and can sufficiently suppress loosening during fastening. Therefore, the steel material is suitable as a material for steel parts that are subjected to wiredrawing, and is suitable as a material for bolts used in mechanical structures, civil engineering, and the like.

[0080] [Steel manufacturing method] An example of a method for manufacturing a steel material according to this embodiment will be described. The method for manufacturing a steel material described below is one example for manufacturing a steel material according to this embodiment. Therefore, a steel material having the above-mentioned configuration may be manufactured by a manufacturing method other than the manufacturing method described below. However, the manufacturing method described below is a preferred example of a method for manufacturing a steel material according to this embodiment.

[0081] [Manufacturing method] An example of a method for manufacturing the above-mentioned steel material will now be described. The example of the manufacturing method includes the following steps. (Process 1) Casting process (Process 2) Hot processing process Each step will be described below.

[0082] [(Process 1) Casting process] Molten steel having a chemical composition that satisfies Feature 1 is produced by a known method. The produced molten steel is used to produce a cast piece (slab or bloom) by a continuous casting method.

[0083] In a typical continuous casting process, the slab is cooled from the outside. Therefore, the poured molten steel gradually solidifies from the outside to the inside in a cross section perpendicular to the axial direction of the slab, with the center part completing solidification last. In the center part, which is the last part to solidify in a casting, the components become more concentrated than the average solute concentration, resulting in positive segregation. This segregation part usually exists in the center part of the slab, and is called central segregation. Central segregation remains in the center part of the cross section perpendicular to the axial direction even after the slab is hot worked into steel material.

[0084] [Manufacturing conditions in the continuous casting process] In the manufacturing method of this embodiment, the maximum segregation part is shifted from the center of the cross section perpendicular to the axial direction. Specifically, the maximum segregation part is shifted from the center by utilizing the gravity acting on the slab during solidification of the slab in continuous casting. During continuous casting, casting is started in a state where the axial direction of the slab is parallel to the direction of gravity (vertical direction), and before solidification of the center is completed, the axial direction of the slab is tilted in a direction perpendicular to the direction of gravity (horizontal direction). In this case, the final solidification part can be shifted from the center, and as a result, the maximum segregation part is shifted from the center. If the timing of tilting the axial direction of the slab in the horizontal direction during continuous casting is delayed, the maximum segregation part in the steel material will be too close to the center, and the shortest distance Lmin will be too long. On the other hand, if the timing of tilting the axial direction of the slab in the horizontal direction during continuous casting is too early, the maximum segregation part will be too far from the center, and the shortest distance Lmin will be too short. In consideration of the above matters, the continuous casting process is carried out so as to satisfy the following conditions 1 to 3.

[0085] (Condition 1) The continuous casting machine used is a curved type that has a small bending load.

[0086] (Condition 2) The radius of curvature of the curved casting of the continuous casting machine is R (m), the casting speed in the continuous casting process is Vc (m / min), and the temperature difference between the liquidus temperature at the start of steel casting and the solidus temperature is the degree of superheat ΔT (℃). In this case, the solidification index G defined by the following formula is set to 200 to 800. Coagulation index G=15R / Vc-ΔT

[0087] When the solidification index G is less than 200, the timing of tilting the axial direction of the slab from the vertical to the horizontal during continuous casting is too early. In this case, in the produced steel, the maximum segregation part is too far from the center, and the shortest distance Lmin is too short. On the other hand, when the solidification index exceeds 800, the timing of tilting the axial direction of the slab from the vertical to the horizontal during continuous casting is too late. In this case, in the produced steel, the maximum segregation part is too close to the center, and the shortest distance Lmin is too long. When the solidification index G is 200 to 800, in the produced steel, the maximum segregation part is located at an appropriate position from the center, and the shortest distance Lmin is 0.30D to 0.48D.

[0088] The shape and size of the cross section (transverse section) perpendicular to the axial direction of the slab are not particularly limited. The transverse section of the slab is, for example, rectangular, with a side length of, for example, 200 to 600 mm. The radius of curvature R is, for example, 10 to 25 m, and the casting speed Vc is, for example, 0.1 to 1.0 m / min. The degree of superheat ΔT is 10 to 80°C.

[0089] (Condition 3) The electromagnetic stirring device installed in the continuous casting machine is used to perform electromagnetic stirring on the undissolved molten steel inside the slab. The electromagnetic stirring is adjusted so that the stirring index H, defined by the following formula, is 5 to 50. H = (I × F) / (50 + α) Here, α is the position of the electromagnetic stirring device of the continuous casting machine, and is the angle (°) when the casting start position is set to 0 (°) and the center point of the curvature radius R is used as the fulcrum. I is the current (A) during electromagnetic stirring, and F is the frequency (Hz) during electromagnetic stirring.

[0090] If the stirring index H is less than 5, the molten steel in the slab is not stirred sufficiently or stirring is started too late. As a result, the resulting steel will have excessive segregation. On the other hand, if the stirring index H exceeds 50, the molten steel in the slab is stirred excessively or stirring is started too early. As a result, the resulting steel will have insufficient segregation. If the stirring index H is 5 to 50, the resulting steel will have a total segregation degree Stot of 0.02 to 0.30 and a center segregation degree Sctr of 0.02 to 0.30.

[0091] In the electromagnetic stirring, the angle α is, for example, 0 to 80°, but is not particularly limited thereto. The current I is, for example, 200 to 800 A. The frequency F is, for example, 0.5 to 4.0 Hz. The electromagnetic stirring device may be disposed in the mold (i.e., α=0°) or downstream of the mold (i.e., α>0°).

[0092] [(Process 2) Hot processing process] In the hot working process, hot working is performed on the slab produced in the casting process to produce a steel material having a circular cross section perpendicular to the axial direction. The steel material is, for example, a steel bar or a wire rod. The hot working process includes, for example, a rough rolling process and a finish rolling process.

[0093] In the rough rolling process, the slab is hot rolled to produce a billet. For example, a blooming mill is used in the rough rolling process. The slab is bloomed by the blooming mill to produce a billet. If a continuous rolling mill is installed downstream of the blooming mill, the billet after blooming may be further hot rolled by the continuous rolling mill to produce a billet of a smaller size. The heating temperature in the heating furnace in the rough rolling process is not particularly limited, but is, for example, 1000 to 1300°C.

[0094] In the finish rolling process, a billet is first heated using a heating furnace. The heated billet is then hot-rolled using a continuous rolling mill to produce a steel material (steel bar or wire rod). The heating temperature in the heating furnace in the finish rolling process is not particularly limited, but is, for example, 1000 to 1300°C. The area reduction rate in the continuous rolling mill is preferably 70% or more. Here, the area reduction rate is defined by the following formula. Reduction rate = (cross-sectional area of ​​billet before finish rolling - cross-sectional area of ​​steel after finish rolling) / cross-sectional area of ​​billet before finish rolling x 100

[0095] Through the above manufacturing process, the steel material according to this embodiment is manufactured.

[0096] [Bolt manufacturing method] The method for manufacturing a bolt using the steel material of this embodiment is a well-known manufacturing method. An example of the method for manufacturing a bolt includes the following steps. ·Wire drawing process Bolt forming process Each step will be described below.

[0097] [Wire drawing process] In the wire drawing process, the steel material is subjected to cold wire drawing (cold drawing) for dimensional adjustment. The wire drawing process includes a pickling process, a lubricating coating formation process, and a cold drawing process. Annealing may be performed by a known method for the purpose of softening the steel material prior to the wire drawing process.

[0098] [Pickling process and lubricating film formation process] In the pickling process, the steel material is immersed in an acid to perform descaling. The conditions for the pickling may be well-known. The pickling bath is, for example, hydrochloric acid or sulfuric acid. In the lubricating film forming process, a well-known lubricant is applied to the surface of the steel material after the pickling process to form a lubricating film. The type of lubricant (lubricating film) and the lubrication conditions are not particularly limited. Examples of the lubricant include zinc phosphate, lime soap, metal soap, and lubricants containing inorganic salts without phosphorus and lubricants. In the lubricating film forming process, the steel material is immersed in a lubricating bath containing a lubricant to form a lubricating film on the surface of the steel material.

[0099] [Cold drawing process] In the cold drawing process, the steel material on which the lubricating film has been formed is subjected to a known cold drawing process. The shape of the die and the area reduction rate in the cold drawing process are not particularly limited. The opening angle on the entry side of the die is, for example, 10 to 25°. The area reduction rate in the cold drawing process is, for example, 1 to 50%, and the wire drawing speed is, for example, 0.1 to 10.0 m / sec.

[0100] [Bolt forming process] In the bolt forming process, hot or cold forging is performed to form the steel material after the wire drawing process into a bolt. Instead of hot or cold forging, or after hot or cold forging, cutting may be performed. In addition, quenching and tempering may be performed by a known method as necessary to increase strength.

[0101] Through the above manufacturing process, the bolt made of the steel material of this embodiment is manufactured.

[0102] [Bolt tightening method] An example of a method for tightening a bolt manufactured using the steel material of this embodiment as a material will be described. The bolt tightening method uses, for example, the well-known torque method. For the purpose of precise management of axial force, a rotation angle method or a torque gradient method may also be used. Below, as an example, a method for tightening a bolt using the torque method will be described.

[0103] [Torque method] The tightening torque is calculated using the following formula: T=kdF Here, T is the tightening torque (N m), F is the tightening axial force (N), d is the nominal diameter of the bolt thread (m), and k is the torque coefficient (-).

[0104] The tightening axial force F is, for example, 40 to 70% of the yield stress of the bolt. The torque coefficient k is, for example, 0.1 to 0.3. The nominal diameter d of the screw is, for example, 1.0 to 50.0 mm. The tightening torque that obtains the target tightening axial force F is calculated using the above formula, and the bolt is tightened using a torque wrench until the calculated torque value is reached. The bolt may be tightened by an embedded bolt that does not use a nut, or by nut tightening. The material to be fastened is not particularly limited, and may be any metal member such as aluminum, steel, stainless steel, or cast iron. If the strength of the material to be fastened is low, a washer may be used to prevent the seat from collapsing.

[0105] Bolts used in mechanical structures, civil engineering, and construction may loosen due to unavoidable vibrations after fastening. In this case, the fastening axial force may decrease. If the maximum segregation part of the steel material from which the bolt is made is located at the center of the cross section perpendicular to the axial direction of the bolt, the stress in the bolt's threads will be equally symmetrical to the axis when the bolt is fastened. Therefore, it is difficult to obtain sufficient friction at the interface between the male thread of the bolt and the female thread of the fastened material. In this case, the fastened bolt will be prone to loosening.

[0106] On the other hand, if the segregation level of the steel material from which the bolt is made is too high or if the maximum segregation point is too far from the center, the wiredrawability of the steel material is reduced, and in this case, the steel material may break during the wiredrawing process.

[0107] The steel material of this embodiment satisfies the above-mentioned features 1 to 3. Therefore, the degree of segregation in the steel material is set within an appropriate range, and further, the shortest distance Lmin between the maximum segregation part and the center part is set within an appropriate range. Therefore, excellent wiredrawability is obtained, and loosening can be sufficiently suppressed when a bolt manufactured using the steel material as a material is fastened. EXAMPLES

[0108] The effect of one aspect of the steel material of this embodiment will be described more specifically with reference to an example. The conditions in the following example are an example of conditions adopted to confirm the feasibility and effect of the steel material of this embodiment. Therefore, the steel material of this embodiment is not limited to this example of conditions.

[0109] Steel materials having the chemical compositions shown in Tables 1A and 1B were produced.

[0110] [Table 1A]

[0111] [Table 1B]

[0112] Specifically, a casting process was carried out using the molten steel of each test number. In the casting process, a curved continuous casting machine with a curvature radius R (m) of 15 m was used. A bloom with a rectangular cross section perpendicular to the axial direction and a rectangular size of 300 mm x 400 mm was produced by the casting process. In the casting process, electromagnetic stirring was carried out using an electromagnetic stirring device with an angle α of 0° (i.e., inside the mold). The solidification index G and the stirring index H were adjusted with a casting speed Vc of 0.1 to 1.0 m / min, ΔT of 10 to 80° C., current I of 200 to 800 A, and frequency F of 0.5 to 4.0 Hz. The solidification index G and the stirring index H are shown in Table 2.

[0113] [Table 2]

[0114] The blooms produced in the casting process were subjected to hot working processes (rough rolling process and finish rolling process). Specifically, in the rough rolling process, the blooms were heated to 1200°C, and then hot rolling was performed to produce billets having a cross-sectional shape of 160 mm x 160 mm. In the finish rolling process, the billets were heated to 1200°C, and then hot rolling was performed to produce wire rods (steel materials) with a diameter of 15 mm, which were then allowed to cool. The steel materials of each test number were produced by the above production processes.

[0115] [Evaluation test] The following evaluation tests were carried out on the steel materials with each test number. (Test 1) Measurement test of chemical composition of steel (Test 2) Determination test of minimum distance Lmin, total segregation degree Stot and center segregation degree Sctr (Test 3) Steel wire drawing test (Test 4) Loosening resistance evaluation test Tests 1 to 4 will be described below.

[0116] [(Test 1) Measurement of chemical composition of steel] The chemical composition of the steel material of each test number was analyzed according to the above-mentioned [Method of measuring the chemical composition of steel material]. The analysis results are shown in Tables 1A and 1B. The specific element concentration Xave of each test number was calculated using the C content, Si content, Mn content, Cr content, and Mo content (mass%) in the obtained chemical composition.

[0117] [(Test 2) Determination test of shortest distance Lmin, total segregation degree Stot, and center segregation degree Sctr] According to the above-mentioned [Measuring method of shortest distance Lmin, specific element concentration Xmax and Xctr], the shortest distance Lmin, specific element concentration Xmax and Xctr of each test number were obtained. In addition, in the investigation surface, each of the six diameters was within ±3% of the arithmetic mean value of the six diameters. Based on the obtained specific element concentrations Xave, Xmax, and Xctr, the total segregation degree Stot and the center segregation degree Sctr were calculated using formulas (2) and (3). The obtained total segregation degree Stot, center segregation degree Sctr, and Lmin / D are shown in Table 2.

[0118] [(Test 3) Steel wire drawing test] The steel material (wire material) of each test number was subjected to wire drawing to evaluate the wire drawability of the steel material. Specifically, the steel material of each test number was immersed in a pickling tank of a hydrochloric acid bath to perform pickling treatment and remove the surface scale. The descaled steel material was subjected to a lubricating film forming process to form a phosphate film as a lubricating film on the steel material surface. The steel material on which the lubricating film was formed was subjected to cold drawing. In the cold drawing, the opening angle on the entry side of the die was set to 14°, and the wire drawing speed was set to 5 m / sec. By the cold drawing, 5 m of wire drawing was performed from a diameter of 15 mm to a diameter of 12.5 mm (reduction in area rate of 30.6%). The steel material (steel wire) after wire drawing was evaluated for the presence or absence of breakage. The steel material of each test number was subjected to wire drawing 10 times, and the probability of breakage during the 10 times was evaluated as follows. Rating A: Probability of breakage 0% (0 / 10) Rating B: Probability of breakage 10% (1 / 10) Rating C: Probability of breakage 20% (2 / 10) Rating D: Probability of breakage 30% (3 / 10) Rating ×: Probability of breakage is 40% or more (4 / 10 or more) When the evaluation result was within the range of A to D, that is, when the fracture probability was 30% or less, it was evaluated that excellent wiredrawability was obtained.

[0119] [(Test 4) Loosening resistance evaluation test] The following evaluation test was carried out using bolts manufactured from the steel material having each test number, to evaluate the loosening resistance. Cold forging was performed under the same conditions for each test number of steel material to manufacture fully threaded hexagonal bolts with the shape shown in Figure 2. The hexagonal bolts conformed to JIS B 1180:2014, with a nominal thread diameter d of M12 and a neck length L of 100 mm. Hexagonal nuts conforming to JIS B 1180:2014 were also prepared. The hexagonal nuts had a chemical composition equivalent to S20C as specified in JIS G 4051:2018.

[0120] The loosening resistance evaluation test was performed using an impact vibration type screw loosening test (vibration frequency 30Hz, amplitude 11.43mmp-p, impact stroke 19mm) in accordance with the US aviation standard NAS3350. In the screw loosening test, the bolts were tightened using the torque method with a torque coefficient of 0.15, so that the axial force was 40% of the bolt's yield strength. The bolts were then evaluated for possible falling off after 30,000 vibrations. The screw loosening test was performed 20 times using bolts manufactured from the steel material with each test number. The probability of falling off during the 20 times was evaluated as follows: Rating A: Probability of breakage 0% (0 / 20) Rating B: Probability of breakage 5-10% (1-2 / 20) Rating C: Probability of breakage 15-20% (3-4 / 20) Rating D: Probability of breakage 25-30% (5-6 / 20) Rating ×: Probability of breakage is 35% or more (7 / 20 or more) When the evaluation result was within the range of A to D, that is, when the fracture probability was 30% or less, it was evaluated that excellent loosening resistance was obtained.

[0121] [Evaluation Results] The evaluation results are shown in Table 2. Referring to Table 2, the steel materials of test numbers 1 to 47 satisfied characteristics 1 to 3. Therefore, the steel materials had excellent wiredrawability, and the bolts manufactured using the steel materials had excellent resistance to loosening.

[0122] On the other hand, in test number 48, the C content was too high, and therefore sufficient wire drawability was not obtained.

[0123] In test number 49, the Si content was too high, and therefore sufficient wire drawability was not obtained.

[0124] In test number 50, the Mn content was too high, and therefore sufficient wire drawability was not obtained.

[0125] In test number 51, the Cr content was too high, and therefore sufficient wire drawability was not obtained.

[0126] In test numbers 52 to 54, the solidification index G was too high. Therefore, the shortest distance Lmin exceeded 0.48D. As a result, the bolts manufactured using the steel material did not have sufficient loosening resistance.

[0127] In test numbers 55 to 57, the solidification index G was too low, and therefore the shortest distance Lmin was less than 0.30D, resulting in insufficient wire drawability.

[0128] In test numbers 58 to 60, the stirring index H was too low, and therefore the overall segregation degree Stot and the center segregation degree Sctr were too high, resulting in insufficient wiredrawability.

[0129] In test numbers 61 to 63, the stirring index H was too high, and therefore the overall segregation degree Stot and the center segregation degree Sctr were too low, resulting in insufficient loosening resistance.

[0130] The embodiments of the present disclosure have been described above. However, the above-described embodiments are merely examples for implementing the present disclosure. Therefore, the present disclosure is not limited to the above-described embodiments, and can be implemented by appropriately modifying the above-described embodiments without departing from the spirit of the present disclosure.

Claims

1. A steel material having a cross section perpendicular to the axial direction that is circular with a diameter D, The chemical composition, in mass%, is C: 0.15-0.55%, Si: 0.01-0.40%, Mn: 0.20-1.80%, P: 0.030% or less, S: 0.040% or less, Cr: 0.01-1.80%, Al: 0.005 to 0.100%, and N: 0.001 to 0.020%; The balance is Fe and impurities. The specific element concentration X is expressed by the formula (1A), The specific element concentration X in the entire cross section is Xave, The specific element concentration X of the maximum segregation portion of the cross section is defined as Xmax, When the specific element concentration X at the center of the cross section is Xctr, The total segregation degree Stot defined by the formula (2) is 0.02 to 0.30, The center segregation ratio Sctr defined by the formula (3) is 0.02 to 0.30, In the cross section, the shortest radial distance from the surface of the steel material to the maximum segregation portion is 0.30D to 0.48D; Steel material. X=C+Si / 20+Mn / 5+Cr / 5 (1A) Stot=(Xmax-Xave) / Xave (2) Sctr=(Xmax-Xctr) / Xctr (3) Here, each element symbol in formula (1A) is substituted with the content of the corresponding element in mass %.

2. A steel material having a cross section perpendicular to the axial direction that is circular with a diameter D, The chemical composition, in mass%, is C: 0.15-0.55%, Si: 0.01-0.40%, Mn: 0.20-1.80%, P: 0.030% or less, S: 0.040% or less, Cr: 0.01-1.80%, Al: 0.005 to 0.100%, and N: 0.001 to 0.020%; Further, the composition contains one or more selected from the group consisting of Groups 1 to 3, The balance is Fe and impurities. The specific element concentration X is expressed by the formula (1), The specific element concentration X in the entire cross section is Xave, The specific element concentration X of the maximum segregation portion of the cross section is defined as Xmax, When the specific element concentration X at the center of the cross section is Xctr, The total segregation degree Stot defined by the formula (2) is 0.02 to 0.30, The center segregation ratio Sctr defined by the formula (3) is 0.02 to 0.30, In the cross section, the shortest radial distance from the surface of the steel material to the maximum segregation portion is 0.30D to 0.48D; Steel material. [Group 1] Cu: 0.40% or less, Ni: 0.40% or less, Mo: 0.80% or less, V: 0.80% or less, and B: 0.0100% or less, one or more selected from the group consisting of [Group 2] Ti: 0.100% or less, and Nb: 0.100% or less, one or more selected from the group consisting of [Group 3] Ca: 0.010% or less, Bi: 0.300% or less, Te: 0.300% or less, Zr: 0.300% or less; and Pb: 0.090% or less, one or more selected from the group consisting of X=C+Si / 20+Mn / 5+Cr / 5+Mo / 5 (1) Stot=(Xmax-Xave) / Xave (2) Sctr=(Xmax-Xctr) / Xctr (3) Here, the content of the corresponding element in mass% is substituted for each element symbol in formula (1). When the corresponding element is not contained, "0" is substituted for the corresponding element symbol.

3. The steel material according to claim 2, The chemical composition contains the first group, Steel material.

4. The steel material according to claim 2, The chemical composition contains the second group, Steel material.

5. The steel material according to claim 2, The chemical composition contains the third group, Steel material.

Citation Information

Patent Citations

  • Steel for non-heattreated bolt

    JP1999012689A

  • Steel excellent in cold workability and machine parts

    JP2000204433A

  • Fastener and fastening structure

    WO2010092817A1