Amorphous carbon film and method of vapor deposition for the same
By doping amorphous carbon films with oxygen and nitrogen, the method addresses the challenge of high compressive stress in semiconductor manufacturing, ensuring high selectivity and low stress for effective hard mask performance in vertical NAND structures.
Patent Information
- Application Number
- JP2024065518
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-13
- Filing Date
- 2024-04-15
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-04-15
AI Technical Summary
Existing amorphous carbon films used as hard masks in semiconductor manufacturing, particularly for vertical NAND structures, face a challenge in achieving high selectivity while maintaining low compressive stress, which can lead to wafer chucking issues and decreased device yield.
A method involving the deposition of an amorphous carbon film doped with oxygen and nitrogen using a precursor containing carbon, oxygen, and nitrogen, under specific PECVD conditions, to achieve a compressive stress of 200 MPa or less and a modulus of 40 MPa or more, while maintaining high selectivity.
The resulting amorphous carbon film exhibits high selectivity and low compressive stress, preventing wafer fixation defects and enabling efficient fabrication of vertical NAND devices without increasing film thickness.
Smart Images

Figure 2024152724000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a deposition technique for an amorphous carbon film that is mainly used as a hard mask in a semiconductor manufacturing process, and more particularly, to an amorphous carbon film having a high selectivity and a relatively low compressive stress, and a deposition method thereof. [Background technology]
[0002] In recent years, NAND device structures that are being applied in semiconductor manufacturing processes include horizontal NAND structures and vertical NAND structures. Due to the demand for finer patterns, much research has been conducted recently on vertical NAND structures (VNAND).
[0003] To achieve a vertical NAND structure, a hard mask process that requires high selectivity is necessary. To meet this requirement, amorphous carbon film (ACL) has been used as a typical hard mask. An amorphous carbon film is deposited as a hard mask on a multi-layer insulating film in which tens to hundreds of layers of silicon oxide and silicon nitride films are alternately stacked vertically using a PECVD (Plasma Enhanced Chemical Vapor Deposition) process, and then an etching process is used to form a long and narrow hole that vertically penetrates the multi-layer insulating film.
[0004] Considering the high number of multi-layer insulating films in vertical NAND devices, the selectivity of the amorphous carbon film needs to be high in order for the amorphous carbon film to function properly as a hard mask.
[0005] Various methods have been proposed for increasing the selectivity of an amorphous carbon film. For example, Korean Patent Publication No. 10-2017-0093003 (August 14, 2017) discloses a method for depositing an amorphous carbon film having a multilayer structure in which boron-doped carbon films and non-boron-doped carbon films are alternately stacked by repeating a step of depositing a carbon film not doped with a dopant using a hydrocarbon precursor and a step of depositing a carbon film doped with a dopant using a hydrocarbon precursor and a boron precursor.
[0006] On the other hand, as the selectivity of the amorphous carbon film increases, the compressive stress also tends to increase, but if the compressive stress increases too much, problems may occur in wafer chucking, resulting in a decrease in device yield. Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a method for depositing an amorphous carbon film having a relatively low compressive stress while having a high selectivity by controlling a PECVD process.
[0008] Another problem to be solved by the present invention is to provide an amorphous carbon film having a high selectivity and a relatively low compressive stress. [Means for solving the problem]
[0009] In order to solve the above problems, a method for depositing an amorphous carbon film according to an embodiment of the present invention includes the steps of: (a) loading a substrate into a chamber; and (b) discharging a carbon-containing precursor, an oxygen-containing precursor, and a nitrogen-containing precursor to deposit an oxygen- and nitrogen-doped amorphous carbon film on the substrate.
[0010] The carbon-containing precursor may be a carbon compound in a gaseous state.
[0011] The oxygen-containing precursor may be oxygen gas, and the oxygen gas may be supplied into the chamber at a flow rate of 80 to 500 sccm.
[0012] The nitrogen-containing precursor may include nitrogen gas, and the nitrogen gas may be supplied into the chamber at a flow rate of 100 to 1000 sccm.
[0013] The above step (b) can be performed under the conditions of a process pressure of 3 to 8 Torr, a plasma power of 1000 to 3000 W, and a substrate temperature of 400 to 650°C.
[0014] The carbon-containing precursor may be supplied with Ar or He.
[0015] In order to solve the above problems, an amorphous carbon film according to one embodiment of the present invention has a carbon matrix doped with oxygen and nitrogen, and is characterized by having a compressive stress of 200 MPa or less and a modulus of 40 MPa or more.
[0016] The amorphous carbon film can exhibit a Vickers hardness of 5.0 GPa or more. Effect of the Invention
[0017] According to the method for depositing an amorphous carbon film according to the present invention, an amorphous carbon film doped with oxygen and nitrogen can be deposited by using a precursor containing carbon, an oxygen-containing precursor, and a nitrogen-containing precursor.
[0018] The amorphous carbon film doped with oxygen and nitrogen according to the present invention has a high selectivity and low compressive stress, and therefore can suppress wafer fixing failure that may occur due to excessively high compressive stress.
[0019] In addition, the oxygen and nitrogen doped amorphous carbon film according to the present invention may have a high modulus while having a low compressive stress, and may be used as a hard mask for manufacturing a vertical NAND device, for example, without increasing the thickness of the amorphous carbon film.
[0020] The effects of the present invention are not limited to those mentioned above, and other effects not mentioned above will be clearly understood by those skilled in the art from the detailed description below. [Brief description of the drawings]
[0021] [Figure 1] 1 is a schematic diagram illustrating a method for depositing an amorphous carbon film according to the present invention; [Diagram 2] FIG. 1 is a schematic diagram illustrating an example of a PECVD apparatus used in the method for depositing an amorphous carbon film according to the present invention. [Diagram 3] FIG. 1 is a diagram showing the stress and hardness of amorphous carbon films deposited according to the examples and comparative examples. [Figure 4] FIG. 1 is a diagram showing the stress and modulus of amorphous carbon films deposited according to the examples and comparative examples. [Diagram 5] FIG. 1 is a diagram showing the hardness and modulus of amorphous carbon films deposited according to the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] The advantages and features of the present invention, as well as the methods for achieving them, will become clear from the following detailed description of the embodiments in conjunction with the accompanying drawings. However, the present invention is not limited to the embodiments disclosed below, and may be embodied in various different forms. However, the embodiments are provided to complete the disclosure of the present invention and fully inform those skilled in the art of the scope of the invention, and the present invention is defined only by the scope of the claims.
[0023] References to an element or layer being "on" or "under" another element or layer include not only directly on or directly under the other element or layer, but also when there are other layers or elements between. Also, when an element is described as being "coupled," "bonded," or "connected" to another element, it should be understood that the elements may be directly coupled or connected to each other, but also that there may be other elements "intervening" between each element, or each element may be "coupled," "bonded," or "connected" through other elements.
[0024] The terms used in the present specification are for the purpose of describing the embodiments and are not intended to limit the present invention. In the present specification, the singular form includes the plural form unless otherwise stated in the text. When used in the specification, "comprises" and / or "includes" refers to a recited element, element, step and / or operation, and does not exclude the presence or addition of one or more other elements, elements, steps and / or operations.
[0025] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, an amorphous carbon film and a deposition method thereof according to a preferred embodiment of the present invention will be described in detail with reference to the accompanying drawings.
[0026] In general, an amorphous carbon film refers to a film in which carbon is arranged in an amorphous state, unlike graphite in which carbon is regularly arranged. The amorphous carbon film has a high etching selectivity and high rigidity, and is suitable for use as a hard mask in semiconductor manufacturing processes, particularly in processes that require deep vertical etching.
[0027] However, when the thickness of the material to be etched increases, such as the multi-layer insulating film of a vertical NAND device, the thickness of the amorphous carbon film must also increase in order to function as a hard mask until the end of etching. Increasing the thickness of the amorphous carbon film can cause problems such as a decrease in productivity and a decrease in CD (Critical Dimension) characteristics. For this reason, an amorphous carbon film having a high modulus as well as a high selectivity is required, which can be achieved by an amorphous carbon film having compressive stress. However, if the compressive stress is too high, problems such as poor wafer fixing can occur. Therefore, an amorphous carbon film having a high selectivity and a relatively low compressive stress is required. After a long period of research, the inventors of the present invention have found that when depositing an amorphous carbon film using a PECVD (Plasma Enhanced Chemical Vapor Deposition) process, by doping both oxygen (O2) and nitrogen (N2), an amorphous carbon film having a high selectivity and a relatively low compressive stress can be deposited.
[0028] This is because dissociated species of oxygen and nitrogen generated by the plasma process can react with hydrogen dissociated from hydrocarbons, such as C3H6, reducing the hydrogen content, which can increase the proportion of carbon films formed with sp3 structure rather than sp2 structure.
[0029] As a result, an amorphous carbon film having a relatively higher stiffness and excellent selectivity due to the increased sp3 structure even if it has a similar compressive stress can be deposited. Similarly, an amorphous carbon film having a similar selectivity but a lower compressive stress can be deposited.
[0030] FIG. 1 is a schematic diagram showing a method for depositing an amorphous carbon film according to the present invention.
[0031] Referring to FIG. 1, the method for depositing an amorphous carbon film includes a substrate loading step (S110) and an Oxygen-doped and Nitrogen-doped Amorphous Carbon Layer (ONACL) deposition step (S120).
[0032] The method for depositing the amorphous carbon film shown in FIG. 1 can use, for example, a PECVD apparatus shown in FIG.
[0033] Referring to FIG. 2, the illustrated PECVD apparatus 1 includes a gas supply line (S), a chamber 2 , a showerhead 3 , a susceptor 4 , an RF power supply 5 , and a first electrode 6 .
[0034] The gas supply line (S) serves to supply reactive gas, inert gas, etc., from outside the chamber 2 to the inside of the chamber 2. In FIG. 2, only one gas supply line (S) connected to the chamber 2 is shown. In this case, multiple gas supply lines may be connected to one gas supply line connected to the chamber 2. In another example, each gas supply line may be connected to the chamber 2.
[0035] For example, when the carbon-containing precursor is a hydrocarbon gas and the oxygen-containing precursor is an oxygen gas, they are more likely to react with each other, and therefore it is preferable that they are supplied separately to the chamber and then contact each other in the chamber 2. It is more preferable that the hydrocarbon gas and the oxygen gas contact each other between the showerhead 3 and the susceptor 4.
[0036] The gases supplied to the interior of the chamber through one or more gas supply lines can be a carbon-containing precursor, an oxygen-containing precursor, a nitrogen-containing precursor, an inert gas, etc. The carbon-containing precursor may be supplied independently to the interior of the chamber without a carrier gas, or may be supplied together with an inert gas as a carrier gas. Similarly, the oxygen-containing precursor or the nitrogen-containing precursor may be supplied independently to the interior of the chamber, or may be supplied together with an inert gas.
[0037] On the other hand, when the carbon-containing precursor is in a liquid state, it may be vaporized via a vaporizer and supplied to the inside of the chamber.
[0038] The inert gas may be supplied into the chamber along with the other precursors or may be supplied into the chamber through a separate gas supply line.
[0039] The shower head 3 is provided at an upper portion inside the chamber 2 and sprays gases injected through a gas supply line (S) into the chamber.
[0040] A susceptor 4 is provided at the bottom inside the chamber 2 on which a substrate (W) such as a wafer is loaded (supported). The susceptor 4 may be provided with a temperature control means for heating / cooling the substrate. The susceptor 4 may also function as a ground electrode as in the example shown in FIG. 1. A separate ground line 8 may be provided to further improve the grounding property. Although not shown, the susceptor 4 itself may be connected to a high frequency power source or a DC power source to form a second electrode (bias electrode).
[0041] The first electrode 6 is electrically connected to the RF power source 5 and is used as an electrode for plasma discharge in the chamber 2. In the example shown in FIG. 1, the showerhead 3 is electrically connected (3a) to the first electrode 6, so that the first electrode 6 and the showerhead 3 function together as a single electrode. Thus, RF power generated by the RF power source 5 is applied to the inside of the process chamber 2 through the first electrode 6 and the showerhead 3. The RF filter 7 serves to remove signal interference generated around the process chamber 2.
[0042] In the method for depositing an amorphous carbon film according to the present invention, in addition to using the PECVD apparatus exemplified in FIG. 2, various known PECVD apparatuses can be used.
[0043] 1, in a substrate loading step (S110), a substrate (W) is loaded onto a susceptor 4 in the chamber, after which the inside of the process chamber 2 is evacuated using an external vacuum system (not shown).
[0044] In the ONACL deposition step (S120), a carbon-containing precursor, an oxygen-containing precursor, and a nitrogen-containing precursor are discharged to deposit an oxygen- and nitrogen-doped amorphous carbon film on the substrate. That is, while starting to supply the carbon-containing precursor, the inert gas, the oxygen-containing precursor, and the nitrogen-containing precursor, an RF power of about 1000 to 3000 W is applied from the RF power source 5 to discharge the carbon compound gas between the shower head 3 and the susceptor 4, thereby depositing an amorphous carbon film on the substrate.
[0045] The carbon-containing precursor, the oxygen-containing precursor, and the nitrogen-containing precursor may be discharged inside chamber 2 of the PECVD apparatus shown in Fig. 2. In another example, at least some of the carbon-containing precursor, the oxygen-containing precursor, and the nitrogen-containing precursor may be discharged in a remote plasma system (RPS) outside the chamber and supplied to the inside of the chamber.
[0046] The carbon-containing precursor may be a liquid carbon compound such as methanol (CH3OH) or a gaseous carbon compound such as a gaseous hydrocarbon such as acetylene (C2H2) or propylene (C3H6). Among these, the liquid carbon compound must be accompanied by a separate vaporizer, and the gaseous carbon compound may be more advantageous for depositing an amorphous carbon film having a high selectivity. The selectivity in the present invention is the selectivity to SiO2 unless otherwise specified. Therefore, it is more preferable to use a gaseous carbon compound as the carbon-containing precursor.
[0047] The supply amount of the carbon-containing precursor may be set differently depending on the thickness of the amorphous carbon film to be deposited, the temperature of the process chamber, etc., and may be supplied at a flow rate of, for example, 500 to 1500 sccm.
[0048] The carbon-containing precursor may be supplied into the chamber together with an inert gas such as helium gas (He) or argon gas (Ar). The inert gas may be supplied into the process chamber at a flow rate of about 4000 sccm or less. As an example, the argon gas may be supplied into the chamber at a flow rate of 2000 to 4000 sccm, and the helium gas may be supplied into the chamber at a flow rate of 200 to 1000 sccm, but is not limited thereto.
[0049] On the other hand, when an amorphous carbon film with high selectivity is deposited using only a gaseous carbon compound, the compressive stress may be excessively increased. In order to solve this problem, the present invention deposits an amorphous carbon film doped with oxygen and nitrogen using a precursor containing carbon, an oxygen-containing precursor, and a nitrogen-containing precursor.
[0050] The oxygen-containing precursor may be a gas containing oxygen such as oxygen gas (O2) or ozone gas (O3), among which oxygen gas is more preferred.The nitrogen-containing precursor may be a gas containing nitrogen such as nitrogen gas (N2) or ammonia gas (NH3), among which nitrogen gas is more preferred.
[0051] Meanwhile, precursors containing both oxygen and nitrogen, such as nitrogen oxides such as NO, NO2, and N2O, are also contemplated. However, when nitrogen oxides are used, the deposition rate of the amorphous carbon film may be excessively low compared to when oxygen gas and nitrogen gas are used separately.
[0052] The oxygen-containing precursor may be supplied into the chamber at a flow rate of 80 to 500 sccm. The nitrogen-containing precursor may be supplied into the chamber at a flow rate of 100 to 1000 sccm. If the flow rate of the oxygen-containing precursor or the nitrogen-containing precursor is too low, it may be difficult to simultaneously achieve the targeted high selectivity and low compressive stress due to insufficient doping of oxygen and / or nitrogen. Conversely, if the flow rate of the oxygen-containing precursor or the nitrogen-containing precursor is too high, there is no further effect and the properties such as the modulus of the amorphous carbon film may be reduced.
[0053] The ONACL deposition step (S120) can be performed under typical deposition conditions for an amorphous carbon film. For example, the ONACL deposition step (S120) can be performed under conditions of a process pressure of 3 to 8 Torr, a plasma power of 1000 to 3000 W, and a substrate temperature of 400 to 650° C. That is, in the present invention, an amorphous carbon film is deposited using a typical PECVD process, but a precursor containing oxygen and a precursor containing nitrogen are supplied into the chamber together with a precursor containing carbon.
[0054] According to the method for depositing an amorphous carbon film according to the present invention, an amorphous carbon film doped with oxygen and nitrogen can be deposited by using a precursor containing carbon, an oxygen-containing precursor, and a nitrogen-containing precursor.
[0055] In the amorphous carbon film according to the present invention, the carbon matrix is doped with oxygen and nitrogen. Since the amorphous carbon film according to the present invention is doped with oxygen and nitrogen, it can have a compressive stress of 200 MPa or less and a modulus of 40 MPa or more. Amorphous carbon films deposited by a high temperature PECVD process using gaseous hydrocarbons can also have a modulus of 40 MPa or more, but in most cases have a high compressive stress of 200 MPa or more. In contrast, the amorphous carbon film according to the present invention has a modulus of 40 MPa or more, but unusually has a relatively low compressive stress of 200 MPa or less. This can be seen from FIG. 4.
[0056] As a result, the oxygen and nitrogen doped amorphous carbon film according to the present invention can have a high modulus while having a low compressive stress, and can be used, for example, as a hard mask for manufacturing a vertical NAND device without increasing the thickness of the amorphous carbon film.
[0057] In addition, the amorphous carbon film according to the present invention can exhibit a Vickers hardness of 5.0 GPa or more. Similarly, the amorphous carbon film according to the present invention exhibits a high hardness of 5.0 GPa or more and has a relatively low compressive stress of 200 MPa or less. This can be confirmed from FIG. 3.
[0058] Working Example Hereinafter, the configuration and operation of the present invention will be described in more detail with reference to preferred embodiments of the present invention, which are presented as preferred examples of the present invention and are not to be construed as limiting the present invention in any sense.
[0059] Contents not described here will not be explained since they can be easily inferred by those skilled in the art.
[0060] Under the conditions shown in Table 1, the amorphous carbon films according to Examples 1 to 14 were deposited, and under the conditions shown in Table 2, the amorphous carbon films according to Comparative Examples 1 to 8 were deposited.
[0061] [Table 1]
[0062] [Table 2]
[0063] FIG. 3 shows the stress and hardness of an amorphous carbon film (ONACL) deposited according to an embodiment and an amorphous carbon film (ACL) deposited according to a comparative example. FIG. 4 shows the stress and modulus of an amorphous carbon film deposited according to an embodiment and a comparative example. FIG. 5 shows the hardness and modulus of an amorphous carbon film deposited according to an embodiment and a comparative example. In FIG. 3 to FIG. 5, the amorphous carbon film deposited according to an embodiment is represented as ONACL, and the amorphous carbon film deposited according to a comparative example is represented as ACL.
[0064] 3, it can be seen that the amorphous carbon films deposited according to the embodiments and the amorphous carbon films deposited according to the comparative examples have a Vickers hardness of about 5.0 GPa or more, except for exceptional cases. In particular, the amorphous carbon films deposited according to the embodiments have a Vickers hardness similar to that of the amorphous carbon films deposited according to the comparative examples, but the amorphous carbon films deposited according to the comparative examples have a relatively large compressive stress, while the amorphous carbon films deposited according to the embodiments have a relatively small compressive stress.
[0065] 4, it can be seen that the amorphous carbon films deposited according to the Examples and the Comparative Examples have moduli of about 40 MPa or more, except for exceptional cases. In particular, it can be seen that the amorphous carbon films deposited according to the Examples have moduli similar to those of the Comparative Examples, but the amorphous carbon films deposited according to the Comparative Examples have relatively large compressive stress, whereas the amorphous carbon films deposited according to the Examples have relatively small compressive stress.
[0066] Meanwhile, referring to FIG. 5, in the case of the amorphous carbon film deposited according to the embodiment and the amorphous carbon film deposited according to the comparative example, as the hardness increases, the modulus also tends to increase.
[0067] Table 3 shows the properties of the amorphous carbon films prepared according to Comparative Examples 9 and 10 and Examples 15 and 16. In Comparative Examples 9 and 10 and Examples 15 and 16, the same process conditions were applied except for the conditions shown in Table 3.
[0068] [Table 3]
[0069] The selectivity in Table 3 is the selectivity to SiO2, and the selectivity of the amorphous carbon film according to Comparative Example 9 is set to 100%, and the relative selectivity of the other amorphous carbon films is shown.
[0070] Referring to Table 3, the amorphous carbon film according to Comparative Example 10, in which the deposition rate is very slow without the supply of O2 and N2, shows a higher selectivity than the amorphous carbon film according to Comparative Example 9, but the compressive stress also increases significantly.
[0071] In contrast, in the case of the amorphous carbon films of Examples 15 and 16 in which O and N were supplied together with C3H6, the film showed a high selectivity similar to that of the amorphous carbon film of Comparative Example 10, but the compressive stress was relatively low and the deposition rate was faster than that of Comparative Example 10.
[0072] Moreover, the amorphous carbon films of Examples 15 and 16 exhibited a relatively high absorption coefficient compared to Comparative Example 9. The higher the absorption coefficient, the closer to black the amorphous carbon film became, indicating an increase in film density.
[0073] Therefore, based on the results in Table 3, it can be said that using oxygen-containing and nitrogen-containing precursors along with gaseous hydrocarbons is more advantageous for depositing amorphous carbon films with high selectivity and low compressive strength.
[0074] Although the present invention has been described above with a focus on the embodiments, various modifications and variations may be made by those skilled in the art. These modifications and variations are within the scope of the present invention. Therefore, the scope of the present invention should be determined by the scope of the claims set forth below. [Explanation of symbols]
[0075] 1 PECVD equipment 2 Chamber 3. Shower head 4 Susceptor 5 RF power supply 6 1st electrode 7 RF Filters 8 Ground Line
Claims
1. (a) loading a substrate into a chamber; (b) discharging a carbon-containing precursor, an oxygen-containing precursor, and a nitrogen-containing precursor to deposit an oxygen- and nitrogen-doped amorphous carbon film on the substrate; Characterized in that it comprises A method for depositing amorphous carbon films.
2. The carbon-containing precursor is a gaseous carbon compound. The method for depositing an amorphous carbon film according to claim 1 .
3. The oxygen-containing precursor is oxygen gas. The method for depositing an amorphous carbon film according to claim 1 .
4. The oxygen-containing precursor is supplied into the chamber at a flow rate of 80 to 500 sccm. The method for depositing an amorphous carbon film according to claim 3.
5. The nitrogen-containing precursor is nitrogen gas. The method for depositing an amorphous carbon film according to claim 1 .
6. The nitrogen-containing precursor is supplied into the chamber at a flow rate of 100 to 1000 sccm. The method for depositing an amorphous carbon film according to claim 5 .
7. The step (b) is performed under the conditions of a process pressure of 3 to 8 Torr, a plasma power of 1000 to 3000 W, and a substrate temperature of 400 to 650° C. The method for depositing an amorphous carbon film according to claim 1 .
8. A carbon matrix is doped with oxygen and nitrogen, and has a compressive stress of 200 MPa or less and a modulus of 40 MPa or more. Amorphous carbon film.
9. The amorphous carbon film has a Vickers hardness of 5.0 GPa or more. The amorphous carbon film according to claim 8.
Citation Information
Patent Citations
Gas barrier coating and vessel
JP2006111967A
Amorphous carbon film and vessel
JP2006289836A
Recombinant E. coli for carotenoid production and use thereof
KR102710048B1