Electrodeposition coating, method for producing electrodeposition coating and method for producing insulating material
By employing a polyimide precursor compound with a specific structure and inorganic particles in a solvent system, the paintability issues in electrodeposition paints are resolved, resulting in improved coating and insulating materials with enhanced mechanical and thermal properties.
Patent Information
- Application Number
- JP2023076955
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-08
- Publication Date
- 2024-11-20
AI Technical Summary
Existing electrodeposition paints containing polyimide precursors and inorganic particles suffer from poor paintability due to coagulation, leading to increased viscosity and poor film formation properties.
The use of a polyimide precursor compound with a specific structure represented by general formula (A1) and inorganic particles, such as aluminum oxide, is combined with a solvent system to prevent aggregation, ensuring excellent paintability and film formation.
The solution results in an electrodeposition paint with improved coating properties, allowing for uniform film formation and enhanced insulating materials with better mechanical properties and heat resistance.
Smart Images

Figure 2024161853000015 
Figure 2024161853000001 
Figure 2024161853000002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a paint for electrodeposition coating, a method for producing the paint for electrodeposition coating, and a method for producing an insulating material. [Background technology]
[0002] Insulated electric wires having an insulating coating are used as electric wires for electric devices such as motors. For electric wires for motors that require high efficiency, high output, and compact size, such as drive motors for electric and hybrid vehicles, rectangular enameled wires with a high conductor occupancy rate in the coil are used. For the manufacture of rectangular enameled wires, an electrodeposition coating method is sometimes used (see, for example, Patent Documents 1 to 5). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 1127047 [Patent Document 2] Special Publication No. 54-41617 [Patent Document 3] Patent No. 2098020 [Patent Document 4] Patent No. 475189 [Patent Document 5] Patent No. 1311182 Summary of the Invention [Problem to be solved by the invention]
[0004] Polyimide resins have been used in electrodeposition coating paints for forming insulating materials (e.g., insulating films) by electrodeposition coating, and resins with low solubility in solvents, such as fully aromatic polyimide resins, are also used as the polyimide resins. When using such resins with low solubility in solvents, they are made into paint in the form of polyamic acid, which is a polyimide precursor, in order to increase the solubility in solvents, and after forming a coating film using this paint, the insulating material is formed by imidizing it by baking or the like. However, when inorganic particles are added to a coating material for electrodeposition coating that contains a polyimide precursor, the polyimide precursor and the inorganic particles aggregate, causing the coating material to thicken, which can result in poor coating properties (film formability).
[0005] Therefore, an object of the present disclosure is to provide an electrodeposition coating paint that has excellent paintability even when it contains a polyimide precursor compound and inorganic particles, a method for producing the electrodeposition coating paint, and a method for producing an insulating material using the electrodeposition coating paint. [Means for solving the problem]
[0006] Means for solving the above problems include the following means. <1> A solvent; A polyimide precursor compound having a structure represented by the following general formula (A1); Inorganic particles; A paint for electrodeposition coating containing the above.
[0007] [ka]
[0008] (In general formula (A1), R 1 is an organic group containing at least one selected from the group consisting of an aliphatic group and an aromatic group, 1 represents an organic group containing an aromatic group, Ar 2 represents an organic group containing an aromatic group. <2> In the general formula (A1), 1The organic group containing at least one selected from the group consisting of an aliphatic group and an aromatic group represented by the formula: <1> The electrocoating paint according to claim 1. <3> In the general formula (A1), the Ar 1 The organic group containing an aromatic group represented by the formula (I) has a structure that does not contain a linear or branched aliphatic group or a sulfonyl group in the main chain, and the Ar 2 The organic group containing an aromatic group represented by the formula (I) has a structure that does not contain a linear or branched aliphatic group or a sulfonyl group in the main chain, <1> or <2> The electrocoating paint according to claim 1. <4> The absolute value of the zeta potential is 5 mV or more. <1> ~ <3> 13. The electrocoating paint according to claim 12 . <5> The inorganic particles are particles containing at least one selected from the group consisting of aluminum oxide, silicon oxide, titanium oxide, and magnesium oxide. <1> ~ <4> 13. The electrocoating paint according to claim 12 . <6> reacting a tetracarboxylic dianhydride derivative with an esterifying agent to prepare an esterified tetracarboxylic dianhydride derivative; a step of reacting the esterified tetracarboxylic dianhydride derivative and a diamine compound in a solvent A to synthesize a polyimide precursor compound having a structure represented by the following general formula (A1), and preparing a first mixed solution containing the polyimide precursor compound and the solvent A; A step of mixing the first mixed liquid with inorganic particles to obtain a second mixed liquid; mixing the second mixed liquid with a solvent B.
[0009] [ka]
[0010] (In general formula (A1), R 1 is an organic group containing at least one selected from the group consisting of an aliphatic group and an aromatic group,1 represents an organic group containing an aromatic group, Ar 2 represents an organic group containing an aromatic group. <7> The esterification agent is a compound having a hydroxyl group and a boiling point of 250° C. or less. <6> A method for producing the electrocoating paint according to claim 1. <8> <1> ~ <5> A step of forming a coating film by electrodeposition coating the coating material for electrodeposition coating according to any one of the above items; and baking the coating film. Effect of the Invention
[0011] The present disclosure provides an electrodeposition coating paint that has excellent paintability even when it contains a polyimide precursor compound and inorganic particles, a method for producing the electrodeposition coating paint, and a method for producing an insulating material using the electrodeposition coating paint. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is a schematic diagram showing an example of an electrodeposition apparatus used in the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, an embodiment that is an example of the present disclosure will be described. These descriptions and examples are merely illustrative of the embodiment, and are not intended to limit the scope of the invention. In the present specification, the upper or lower limit of one numerical range may be replaced with the upper or lower limit of another numerical range. In addition, in the present specification, the upper or lower limit of the numerical range may be replaced with a value shown in the examples.
[0014] Each component may contain multiple types of the corresponding substance. When referring to the amount of each component in a composition, if the composition contains multiple substances corresponding to each component, the amount refers to the total amount of those multiple substances present in the composition, unless otherwise specified. The term "process" includes not only independent processes, but also processes that cannot be clearly distinguished from other processes as long as the intended effect of the process is achieved.
[0015] <Electrodeposition coating paint> The electrodeposition coating paint according to the present disclosure (hereinafter also referred to as the "disclosed paint") contains a solvent, a polyimide precursor compound having a structure represented by general formula (A1) described below (hereinafter also referred to as the "specific polyimide precursor compound"), and inorganic particles.
[0016] Due to the above-mentioned configuration, the coating material of the present disclosure is a coating material for electrodeposition coating that has excellent coatability (film formability) even though it contains a polyimide precursor compound and inorganic particles. This is presumably due to the following reasons.
[0017] Conventionally, in electrodeposition coating paints for forming insulating materials (e.g., insulating films), resins with low solubility in solvents, such as fully aromatic polyimide resins, have been used. When using such resins with low solubility in solvents, the paint is prepared by dissolving the polyimide precursor, polyamic acid, in a solvent. Then, after forming a coating film using this paint, the insulating material is formed by imidizing it by baking or the like.
[0018] On the other hand, a method of adding inorganic particles to an electrodeposition coating paint is considered from the viewpoint of, for example, increasing the uniformity of the thickness of the insulating material to be formed or reducing the wear of the organic components of the insulating material due to partial discharge. However, when inorganic particles are further added to an electrodeposition coating paint containing a polyimide precursor compound, the polyimide precursor and the inorganic particles aggregate, causing the paint to thicken and, in some cases, to gel. As a result, the paintability (formability of the coating film) decreases, and in some cases, a coating film cannot be formed.
[0019] One of the possible reasons for this is that, for example, the carboxylic acid group (-COOH) contained in the polyimide precursor compound is electrically attracted to the inorganic particles, causing the polyimide precursor compound and the inorganic particles to aggregate. In particular, inorganic particles with a positive zeta potential (e.g., boehmite alumina, etc.) tend to aggregate easily with the polyimide precursor compound.
[0020] In contrast, the coating material disclosed herein uses a polyimide precursor compound (specific polyimide precursor compound) having the structure shown in the general formula (A1) described below. The specific polyimide precursor compound has a structure in which H in the carboxylic acid group (-COOH) is substituted to form an organic group containing at least one selected from the group consisting of an aliphatic group and an aromatic group, that is, R 1 is an organic group containing at least one of an aliphatic group and an aromatic group, it is believed that this suppresses the polyimide precursor compound and the inorganic particles from electrically attracting each other and aggregating, thereby providing excellent coating properties.
[0021] Each component constituting the coating material of the present disclosure will be described below.
[0022] (solvent) Examples of the solvent include ether-based solvents, ketone-based solvents, alcohol-based solvents, aprotic polar solvents, and water.
[0023] An ether solvent is a solvent that has an ether bond in one molecule. Examples of the ether solvent include tetrahydrofuran (THF), dioxane, trioxane, 1,2-dimethoxyethane, diethylene glycol dimethyl ether, and diethylene glycol diethyl ether.
[0024] A ketone solvent is a solvent that has a ketone group in one molecule. Examples of the ketone solvent include acetone, methyl ethyl ketone, and cyclohexanone.
[0025] An alcohol-based solvent is a solvent that has an alcoholic hydroxyl group in one molecule. Examples of alcohol-based solvents include methanol, ethanol, 1-propanol, 2-propanol, tert-butyl alcohol, ethylene glycol, monoalkyl ethers of ethylene glycol, propylene glycol, monoalkyl ethers of propylene glycol, diethylene glycol, monoalkyl ethers of diethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 1,5-pentanediol, 2-butene-1,4-diol, 2-methyl-2,4-pentanediol, glycerin, 2-ethyl-2-hydroxymethyl-1,3-propanediol, and 1,2,6-hexanetriol.
[0026] Aprotic polar solvents are solvents that are highly polar and have no acidic hydrogens. Examples of aprotic polar solvents include N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAc), dimethylsulfoxide (DMSO), hexamethylene phosphoramide (HMPA), N-methylcaprolactam, N-acetyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone (DMI), N,N'-dimethylpropyleneurea, tetramethylurea, trimethyl phosphate, and triethyl phosphate.
[0027] The solvent may be used alone or in combination of two or more.
[0028] The solvent content is preferably 50% by mass or more and 98% by mass or less, more preferably 60% by mass or more and 95% by mass or less, and even more preferably 70% by mass or more and 85% by mass or less, based on the entire electrocoating paint.
[0029] The solvent is preferably a mixed solution of two or more kinds. The solvent preferably contains solvent A and solvent B, which will be described later. The ratio of solvent B to solvent A (solvent B / solvent A) is preferably from 0.1 to 4.0, more preferably from 0.5 to 3.0, and even more preferably from 0.8 to 2.5, on a mass basis.
[0030] (Specific polyimide precursor compound) The coating material of the present disclosure contains a polyimide precursor compound having a structure shown in the following general formula (A1).
[0031] [ka]
[0032] (In general formula (A1), R 1 is an organic group containing at least one selected from the group consisting of an aliphatic group and an aromatic group, 1 represents an organic group containing an aromatic group, Ar 2 represents an organic group containing an aromatic group.
[0033] Here, an organic group containing at least one selected from the group consisting of an aliphatic group and an aromatic group means a group containing at least one of an aliphatic group and an aromatic group in its structure, which may further contain an element other than carbon (C) and hydrogen (H) (e.g., O, F, N, S, etc.). An organic group containing an aromatic group means a group containing an aromatic group in its structure, which may further contain an aliphatic group in the group structure, and may further contain an element other than carbon (C) and hydrogen (H) (e.g., O, F, N, S, etc.).
[0034] R 1 The organic group containing at least one selected from the group consisting of an aliphatic group and an aromatic group represented by the formula (I) can be, for example, an organic group containing at least one selected from the group consisting of an aliphatic group and an aromatic group derived from an esterifying agent described below. R 1The number of carbon atoms in the organic group containing at least one selected from the group consisting of aliphatic groups and aromatic groups represented by the following formula (I) is preferably from 1 to 10, more preferably from 1 to 8, and even more preferably from 1 to 6. The aliphatic group may be linear, branched, or cyclic, and is preferably linear or branched. R 1 Examples of the organic group containing at least one selected from the group consisting of aliphatic groups and aromatic groups represented by the formula (I) include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a 2-butyl group, an isobutyl group, a t-butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, a phenyl group, and a benzyl group (Ph-CH2-: Ph represents a phenyl group), etc. Among these, a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a 2-butyl group, a phenyl group, and a benzyl group are preferred.
[0035] The esterifying agent will be described in detail later.
[0036] Ar 1 The organic group containing an aromatic group represented by the formula (3) can be, for example, an organic group derived from a tetracarboxylic dianhydride. That is, it can be a tetravalent group excluding the carboxylic anhydride group (-C(=O)-OC(=O)-) in the tetracarboxylic dianhydride. Examples of the tetracarboxylic dianhydride include "tetracarboxylic dianhydride", "tetracarboxylic dianhydride having an ester group", "tetracarboxylic dianhydride having an amide bond" and "tetracarboxylic dianhydride represented by formula (3)" which will be described later. However, Ar 1 In order to improve the heat resistance of an insulating material obtained by using the coating material of the present disclosure, it is preferable that the main chain does not contain a linear or branched aliphatic group or a sulfonyl group (-S(=O)2-). 1 The "main chain" in 1In the structure of (A1), it means a chain that directly connects four bonds (four bonds bonded to the -C(=O)- group in general formula (A1)) together. In other words, it refers to a portion that is not a side chain. In addition, as described above, the aliphatic groups that are preferably not included in the main chain are "straight-chain and branched-chain" aliphatic groups, and cyclic aliphatic groups do not fall under the group that is preferably not included in the main chain.
[0037] Ar 2 The organic group containing an aromatic group represented by the formula (I) can be, for example, an organic group derived from a diamine compound. In other words, it can be a divalent group obtained by removing the amino group (-NH2) in the diamine compound. Examples of this diamine compound include the "diamine compound" described below. However, Ar 2 In order to improve the heat resistance of an insulating material obtained by using the coating material of the present disclosure, it is preferable that the main chain does not contain a linear or branched aliphatic group or a sulfonyl group (-S(=O)2-). 2 The "main chain" in the formula (I) is a divalent group, Ar 2 In the structure of the compound, it means the chain that directly connects the two bonds. In other words, it refers to the part that is not a side chain.
[0038] The specific polyimide precursor compound preferably has a ratio (%) of the number of repeating units having the structure represented by general formula (A1) to the number of all repeating units contained in the compound of 50% or more, more preferably 80% or more, even more preferably 90% or more, and even more preferably 95% or more. The "repeating unit" in a polyimide precursor compound means a structural unit that is repeated every two amide bonds (-CO-NH-) on the polymer chain of the polyimide precursor compound, which is a polymer. For example, when the polyimide precursor compound is a polymer of a tetracarboxylic dianhydride and a diamine compound, one repeating unit is composed of two amide bonds, one residue of the tetracarboxylic dianhydride, and one residue of the diamine compound.
[0039] The specific polyimide precursor compound is thermally or chemically imidized to form -CO-NH- bonds and -COOR 1 The specific polyimide precursor compound can be obtained by polymerizing an esterified tetracarboxylic dianhydride and a diamine compound.
[0040] -Types of specific polyimide precursor compounds The specific polyimide precursor compound is preferably at least one selected from the group consisting of, for example, a polyimide precursor, a polyesterimide precursor, a polyetherimide precursor, and a polyamideimide precursor. The polyimide precursor as used herein refers to a specific polyimide precursor compound that does not contain an ester group, an ether group, or an amide group in the constituent unit represented by the general formula (A1). The polyesterimide precursor refers to a specific polyimide precursor compound that further contains an ester group in addition to the structural unit represented by the general formula (A1) above. The polyetherimide precursor refers to a specific polyimide precursor compound that further contains an ether group in addition to the structural unit represented by the general formula (A1) above. The polyamideimide precursor refers to a specific polyimide precursor compound that further contains an amide group in addition to the structural unit represented by the general formula (A1) above.
[0041] Polyimide precursor The polyimide precursor, which is one type of specific polyimide precursor compound, will now be described. The polyimide precursor is obtained by polymerizing a tetracarboxylic dianhydride and a diamine compound. The tetracarboxylic dianhydride is preferably esterified with an esterifying agent before being polymerized with the diamine compound. The esterification method will be described later.
[0042] First, the tetracarboxylic dianhydride before esterification will be described. The tetracarboxylic dianhydride is an aromatic compound, that is, a specific polyimide precursor compound represented by the general formula (A1) Ar 1 A compound capable of introducing an organic group containing an aromatic group into the copolymer is used. Examples of aromatic tetracarboxylic dianhydrides include pyromellitic dianhydride (PMDA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride (BPADA), 3,3',4,4'-biphenylsulfonetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, 2,3,6,7-naphthalenetetracarboxylic dianhydride, 3,3',4,4'-biphenylethertetracarboxylic dianhydride, 3,3',4,4'-dimethyldiphenylsilanetetracarboxylic dianhydride, 3,3',4,4'-tetraphenylsilanetetracarboxylic dianhydride, 1,2,3,4-furantetracarboxylic dianhydride, 4,4 '-bis(3,4-dicarboxyphenoxy)diphenyl sulfide dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenyl sulfone dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenylpropane dianhydride, 3,3',4,4'-perfluoroisopropylidenediphthalic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, bis(phthalic acid)phenylphosphine oxide dianhydride, p-phenylene-bis(triphenylphthalic acid) dianhydride, m-phenylene-bis(triphenylphthalic acid) dianhydride, bis(triphenylphthalic acid)-4,4'-diphenyl ether dianhydride, bis(triphenylphthalic acid)-4,4'-diphenylmethane dianhydride, 3,3',4,4'-diphenylsulfonetetracarboxylic dianhydride (DSDA), and the like.
[0043] As the aromatic tetracarboxylic dianhydride, for example, the following tetracarboxylic dianhydrides are preferable.
[0044] [ka]
[0045] However, from the viewpoint of improving the heat resistance of the insulating material obtained by using the coating material of the present disclosure, the aromatic tetracarboxylic dianhydride is preferably a compound that does not contain a linear or branched aliphatic group or a sulfonyl group (-S(=O)2-) in the main chain in the structure of the portion excluding the carboxylic anhydride group (-C(=O)-OC(=O)-). From this viewpoint, the above-mentioned BTDA, PMDA, and BPDA are more preferable as the aromatic tetracarboxylic dianhydride.
[0046] In addition to the aromatic tetracarboxylic dianhydride, an aliphatic tetracarboxylic dianhydride may be used in combination as the tetracarboxylic dianhydride. However, the proportion of aliphatic tetracarboxylic dianhydrides among all the tetracarboxylic dianhydrides used in the synthesis of the specific polyimide precursor compound is preferably 10 mol % or less, more preferably 5 mol % or less, even more preferably 1 mol % or less, and particularly preferably 0 mol % (i.e., no aliphatic tetracarboxylic dianhydride is used).
[0047] Examples of the aliphatic tetracarboxylic dianhydride include butane tetracarboxylic dianhydride, 1,2,3,4-cyclobutane tetracarboxylic dianhydride, 1,3-dimethyl-1,2,3,4-cyclobutane tetracarboxylic dianhydride, 1,2,3,4-cyclopentane tetracarboxylic dianhydride, 2,3,5-tricarboxycyclopentyl acetic dianhydride, 3,5,6-tricarboxynorbonane-2-acetic dianhydride, 2,3,4,5-tetrahydrofuran tetracarboxylic dianhydride, 5-(2,5-dioxotetrahydrofuryl)-3-methyl-3-cyclohexene-1,2-dicarboxylic dianhydride, bicyclo[2,2,2]-oct-7-ene aliphatic or alicyclic tetracarboxylic acid dianhydrides such as 1,3,3a,4,5,9b-hexahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-c]furan-1,3-dione, 1,3,3a,4,5,9b-hexahydro-5-methyl-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-c]furan-1,3-dione, and 1,3,3a,4,5,9b-hexahydro-8-methyl-5-(tetrahydro-2,5-dioxo-3-furanyl)-naphtho[1,2-c]furan-1,3-dione.
[0048] Next, the diamine compound will be described. The diamine compound is a diamine compound having two amino groups in its molecular structure. The diamine compound is an aromatic compound, that is, a specific polyimide precursor compound represented by the general formula (A1) when it is formed. 2 A compound capable of introducing an organic group containing an aromatic group into the copolymer is used.
[0049] Examples of aromatic diamine compounds include p-phenylenediamine (PDA), m-phenylenediamine, 4,4'-diaminodiphenylmethane (DAM), 4,4'-diaminodiphenylethane, 4,4'-diaminodiphenylether (ODA), 4,4'-diaminodiphenylsulfide, 4,4'-diaminodiphenylsulfone, 1,5-diaminonaphthalene, 3,3'-dimethyl-4,4'-diaminobiphenyl, and 2,2'-dimethyl-4,4'-diaminobiphenyl (m-Tolidine). , 5-amino-1-(4'-aminophenyl)-1,3,3-trimethylindan, 6-amino-1-(4'-aminophenyl)-1,3,3-trimethylindan, 4,4'-diaminobenzanilide, 3,5-diamino-3'-trifluoromethylbenzanilide, 3,5-diamino-4'-trifluoromethylbenzanilide, 3,4'-diaminodiphenyl ether, 2,7-diaminofluorene, 2,2-bis(4-aminophenyl)hexafluoropropane, 4,4'-methylene-bis(2-chlorophenyl) aniline), 2,2',5,5'-tetrachloro-4,4'-diaminobiphenyl, 2,2'-dichloro-4,4'-diamino-5,5'-dimethoxybiphenyl, 3,3'-dimethoxy-4,4'-diaminobiphenyl, 4,4'-diamino-2,2'-bis(trifluoromethyl)biphenyl, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 1,4-bis(4-aminophenoxy)benzene , 4,4'-bis(4-aminophenoxy)-biphenyl (BAPB), 2,2'-bis(3-amino-4-hydroxyphenyl)propane (AHPP), 1,3'-bis(4-aminophenoxy)benzene, 9,9-bis(4-aminophenyl)fluorene, 4,4'-(p-phenyleneisopropylidene)bisaniline, 4,4'-(m-phenyleneisopropylidene)bisaniline, 2,2'-bis[4-(4-amino-2-trifluoromethylphenoxy)phenyl]hexafluoropropane, 4,Examples of aromatic diamines include 4'-bis[4-(4-amino-2-trifluoromethyl)phenoxy]-octafluorobiphenyl, bis[4-(4-aminophenoxy)phenyl]sulfone (BAPS), bis(3-amino-4-hydroxyphenyl)sulfone (AHPS), 2,4-diaminotoluene (DAT), and 4,4'-methylenebis(2,6-diethylaniline) (MBDEA); and aromatic diamines having two amino groups bonded to an aromatic ring and a heteroatom other than the nitrogen atom of the amino group, such as diaminotetraphenylthiophene.
[0050] In addition to the aromatic diamine compound, an aromatic diisocyanate may be used in combination. Examples of the aromatic diisocyanate include toluene diisocyanate (TDI) and diphenylmethane diisocyanate (MDI).
[0051] As the aromatic diamine compound and aromatic diisocyanate, for example, the following diamine compounds and diisocyanates are preferable.
[0052] [ka]
[0053] However, from the viewpoint of improving the heat resistance of the insulating material obtained by using the coating material of the present disclosure, the aromatic diamine compound is preferably a compound that does not contain a linear or branched aliphatic group or a sulfonyl group (-S(=O)2-) in the main chain in the structure of the portion excluding the amino group. From this viewpoint, the above-mentioned ODA, BAPB, PDA, DAT, and m-Tolidine are more preferable as the aromatic diamine compound.
[0054] In addition to the above-mentioned aromatic diamine compounds and their derivatives, aliphatic diamine compounds can also be used in combination as diamine compounds. However, among all diamine compounds used in the synthesis of the specific polyimide precursor compound, the ratio of aliphatic diamine compounds is preferably 10 mol % or less, more preferably 5 mol % or less, even more preferably 1 mol % or less, and particularly preferably 0 mol % (i.e., no aliphatic diamine compounds are used).
[0055] Examples of the aliphatic diamine compounds include 1,1-meta-xylylenediamine, 1,3-propanediamine, tetramethylenediamine, pentamethylenediamine, octamethylenediamine, nonamethylenediamine, 4,4-diaminoheptamethylenediamine, 1,4-diaminocyclohexane, isophoronediamine, tetrahydrodicyclopentadienylenediamine, hexahydro-4,7-methanoindanylenediamine, tricyclo[6,2,1,0 2.7 ]-undecylenedimethyldiamine, 4,4'-methylenebis(cyclohexylamine), and other aliphatic diamines (including alicyclic diamines).
[0056] The tetracarboxylic dianhydrides and diamine compounds may be used alone or in combination of two or more.
[0057] Polyesterimide precursor The polyesterimide precursor, which is one type of specific polyimide precursor compound, will now be described. The polyesterimide precursor is obtained by polymerizing a tetracarboxylic dianhydride having an ester group with a diamine compound. The tetracarboxylic dianhydride having an ester group is preferably esterified with an esterifying agent before being polymerized with the diamine compound.
[0058] The number of ester groups contained in the tetracarboxylic dianhydride is not particularly limited, but is preferably 1 to 4, more preferably 2 to 3, and even more preferably 2.
[0059] The tetracarboxylic dianhydride having an ester group is preferably one obtained by reacting a tricarboxylic anhydride with a diol. Specifically, for example, it is preferable that the compound is represented by the following formula (1).
[0060] [ka]
[0061] (In formula (1), each X independently represents a trivalent organic group, and Y represents a divalent organic group.)
[0062] In the formula, X is a residue obtained by removing a carboxy group and a 1,3-oxo-2-oxapropylene (-CO-O-CO-) group from a tricarboxylic acid anhydride, and Y is a residue obtained by removing two hydroxyl groups from a diol.
[0063] Examples of tricarboxylic acid anhydrides used in the synthesis of tetracarboxylic acid dianhydrides having an ester group include benzenetricarboxylic acid anhydride (1,2,3-benzenetricarboxylic acid anhydride, trimellitic acid anhydride [1,2,4-benzenetricarboxylic acid anhydride], etc.), naphthalenetricarboxylic acid anhydride (1,2,4-naphthalenetricarboxylic acid anhydride, 1,4,5-naphthalenetricarboxylic acid anhydride, 2,3,6-naphthalenetricarboxylic acid anhydride, 1,2,8-naphthalenetricarboxylic acid anhydride, etc.), 3,4,4'-benzophenonetricarboxylic acid anhydride, 3,4,4'-biphenylethertricarboxylic acid anhydride, 3,4,4'-biphenyltricarboxylic acid anhydride, 2,3,2'-biphenyltricarboxylic acid anhydride, 3,4,4'-biphenylmethanetricarboxylic acid anhydride, and 3,4,4'-biphenylsulfonetricarboxylic acid anhydride.
[0064] Examples of diols used in the synthesis of tetracarboxylic dianhydrides having an ester group include ethylene glycol, propylene glycol, butanediol, pentanediol, neopentyl glycol, methylpentanediol, hexanediol, heptanediol, octanediol, nonanediol, decanediol, and dodecanediol. aliphatic diols such as those listed above; alicyclic diols such as cyclohexanediol and hydrogenated xylylene glycol; aromatic diols such as xylylene glycol; and polyether polyols obtained by addition polymerization of alkylene oxides (ethylene oxide, propylene oxide, etc.) to dihydric alcohols.
[0065] Examples of the diamine compound used in the synthesis of the tetracarboxylic dianhydride having an ester group are the same as those described above.
[0066] Polyamide-imide precursor A polyamideimide precursor, which is one type of specific polyimide precursor compound, will now be described. The polyamide-imide precursor is obtained by polymerizing a tetracarboxylic dianhydride having an amide group with a diamine compound. The tetracarboxylic dianhydride having an amide group is preferably esterified with an esterifying agent before being polymerized with the diamine compound.
[0067] The number of amide groups contained in the tetracarboxylic dianhydride is not particularly limited, but is preferably 1 to 4, more preferably 2 to 3, and even more preferably 2.
[0068] The diamine compound used in the synthesis of the tetracarboxylic dianhydride having an amide group is preferably the same as that described above. The tetracarboxylic dianhydride having an amide group is preferably one obtained by reacting an acid chloride of a tricarboxylic anhydride, such as trimellitic anhydride chloride, with a diamine compound. Specifically, for example, it is preferable that the compound is represented by the following formula (2).
[0069] [ka]
[0070] In formula (2), each X2 independently represents a trivalent organic group, and Y2 represents a divalent organic group.
[0071] In formula (2), X2 is a residue obtained by removing a carboxy group and a 1,3-oxo-2-oxapropylene (-CO-O-CO-) group from a tricarboxylic acid anhydride, or a residue obtained by removing a -COOCl group and a 1,3-oxo-2-oxapropylene (-CO-O-CO-) group from an acid chloride of a tricarboxylic acid anhydride, and Y is a residue obtained by removing two isocyanate groups from a diisocyanate, or a residue obtained by removing two amino groups from a diamine compound.
[0072] Examples of tricarboxylic acid anhydrides used in the synthesis of tetracarboxylic acid dianhydrides having an amide group include the same tricarboxylic acid anhydrides as those used in the synthesis of the above-mentioned tetracarboxylic acid dianhydrides having an ester group. Examples of tricarboxylic acids used in the synthesis of tetracarboxylic dianhydrides having an amide group include 1,2,3-benzenetricarboxylic acid, trimellitic acid (1,2,4-benzenetricarboxylic acid), naphthalenetricarboxylic acids (1,2,4-naphthalenetricarboxylic acid, 1,4,5-naphthalenetricarboxylic acid, 2,3,6-naphthalenetricarboxylic acid, 1,2,8-naphthalenetricarboxylic acid, etc.), 3,4,4'-benzophenonetricarboxylic acid, 3,4,4'-biphenylethertricarboxylic acid, 3,4,4'-biphenyltricarboxylic acid, 2,3,2'-biphenyltricarboxylic acid, 3,4,4'-biphenylmethanetricarboxylic acid, and 3,4,4'-biphenylsulfonetricarboxylic acid. Examples of the acid chloride of a tricarboxylic acid anhydride include the acid chloride of a tricarboxylic acid anhydride used in the synthesis of the above-mentioned tetracarboxylic acid dianhydride having an ester group.
[0073] Examples of diisocyanates used in the synthesis of tetracarboxylic dianhydrides having an amide group include metaphenylene diisocyanate, p-phenylene diisocyanate, o-tolidine diisocyanate, p-phenylene diisocyanate, m-phenylene diisocyanate, 4,4'-oxybis(phenylisocyanate), 4,4'-diisocyanate diphenylmethane, bis[4-(4-isocyanate phenoxy)phenyl]sulfone, 2,2'-bis[4-(4-isocyanate phenoxy)phenyl]sulfone, phenyl]propane, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, 3,3'-dimethyldiphenyl-4,4'-diisocyanate, 3,3'-diethyldiphenyl-4,4'-diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, m-xylene diisocyanate, p-xylene diisocyanate, naphthalene diisocyanate, and the like. The diamine compound used in the synthesis of the tetracarboxylic dianhydride having an amide group may be, for example, the same as the diamine compound used in the synthesis of the polyimide precursor described above.
[0074] Molecular weight of specific polyimide precursor compound The number average molecular weight of the specific polyimide precursor compound is preferably 5,000 or more and 100,000 or less, more preferably 10,000 or more and 70,000 or less, and further preferably 20,000 or more and 50,000 or less. By setting the number average molecular weight of the specific polyimide precursor compound to 5000 or more, the strength of the formed film is likely to be improved. On the other hand, by setting the number average molecular weight of the specific polyimide precursor compound to 100000 or less, the viscosity of the paint is prevented from increasing. When the molecular weight is within the above range, mechanical properties such as flexibility are improved, the insulated wire and insulating parts can be easily processed, and the paint can be easily produced.
[0075] The number average molecular weight of the specific polyimide precursor compound is a value measured by gel permeation chromatography (GPC).
[0076] The content of the specific polyimide precursor compound is preferably from 0.1% by mass to 50% by mass, more preferably from 1% by mass to 30% by mass, and even more preferably from 5% by mass to 20% by mass, based on the entire electrocoating paint.
[0077] (Inorganic particles) The coating material of the present disclosure contains inorganic particles. The inorganic particles are preferably particles containing at least one type selected from the group consisting of metals and metal oxides.
[0078] The metal is not particularly limited, and examples thereof include aluminum, gold, silver, platinum, palladium, zinc, iron, copper, titanium, and magnesium. Examples of metal oxides include aluminum oxide, silver oxide, zinc oxide, iron oxide, and copper oxide. , silicon oxide (silica), titanium oxide, magnesium oxide, etc. In addition, when a metal oxide can form a hydrate, the metal oxide includes the hydrate. For example, aluminum oxide can form aluminum oxide monohydrate (i.e., boehmite alumina), so aluminum oxide monohydrate is a type of aluminum oxide.
[0079] From the viewpoint of uniformity of the thickness of the coating film, the inorganic particles are preferably particles containing a metal oxide, more preferably particles containing at least one selected from the group consisting of aluminum oxide, silicon oxide, titanium oxide, and magnesium oxide, and even more preferably particles containing aluminum oxide.
[0080] From the viewpoint of uniformity of the coating thickness, the particle size of the inorganic particles is preferably 1 nm or more and 50 nm or less, more preferably 2 nm or more and 40 nm or less, and even more preferably 3 nm or more and 30 nm or less.
[0081] The particle size of the inorganic particles is measured using a nanoparticle analyzer, nanoPartica SZ-100, manufactured by Horiba, Ltd. The procedure for measuring the particle size of inorganic particles will be specifically described below. The dispersion liquid containing inorganic particles is diluted with a solvent having the same composition as the solvent to a concentration of 0.01%, and then placed in a glass cell to measure the particle size.
[0082] From the viewpoint of uniformity of the thickness of the coating film, the absolute value of the zeta potential of the inorganic particles is preferably 5 mV or more, more preferably 20 mV or more, and even more preferably 30 mV or more. The upper limit of the absolute value of the zeta potential of the inorganic particles is not particularly limited, but may be, for example, 110 mV or less.
[0083] The absolute value of the zeta potential of the inorganic particles is measured using a nanoparticle analyzer, nanoPartica SZ-100, manufactured by Horiba, Ltd. The procedure for measuring the absolute value of the zeta potential of inorganic particles will be specifically described below. The dispersion liquid containing the inorganic particles to be measured is diluted with a solvent having the same composition as the dispersion liquid to a concentration of 0.01% to prepare a measurement solution. The measurement solution is placed in a glass cell and the zeta potential is measured.
[0084] The content of the inorganic particles is preferably from 1% by mass to 80% by mass, more preferably from 2% by mass to 70% by mass, and further preferably from 3% by mass to 60% by mass, based on the content of the resin.
[0085] (Other Ingredients) The paint according to the present embodiment may contain various known and commonly used paint additives within the scope of the present invention. Examples of paint additives include thickeners, leveling agents, thixotropic agents, defoamers, freeze stabilizers, matting agents, crosslinking reaction catalysts, antiskinning agents, dispersants, wetting agents, light stabilizers, antioxidants, ultraviolet absorbers, fillers, plasticizers, lubricants, reducing agents, preservatives, antifungal agents, deodorants, anti-yellowing agents, antistatic agents, and charge regulators.
[0086] (Absolute value of zeta potential) From the viewpoint of uniformity of the coating thickness, the absolute value of the zeta potential of the coating material disclosed herein is preferably 5 mV or more, more preferably 20 mV or more, and even more preferably 30 mV or more, 40 mV or more, or 50 mV or more. The upper limit of the absolute value of the zeta potential of the paint disclosed herein is not particularly limited, but may be, for example, 110 mV or less, 5 mV or more and 110 mV or less, 20 mV or more and 90 mV or less, or 30 mV or more and 80 mV or less.
[0087] The absolute value of the zeta potential of the coating material of the present disclosure is measured using a nanoparticle analyzer nanoPartica SZ-100 manufactured by Horiba, Ltd. The procedure for measuring the absolute value of the zeta potential of the paint of the present disclosure will be specifically described below. The paint to be measured is diluted with a solvent of the same composition as the solvent contained in the paint to be measured to a concentration of 0.01 mass % (i.e., diluted so that the total content of resin and inorganic particles is 0.01 mass % of the total measurement solution), and the measurement solution is then placed in a glass cell and the zeta potential measurement is performed.
[0088] <Method of manufacturing electrocoating paint> The method for producing a paint for electrodeposition coating according to the present disclosure comprises: A step of reacting a tetracarboxylic dianhydride derivative with an esterifying agent to prepare an esterified tetracarboxylic dianhydride derivative (step 0: esterification step); a step (first step) of synthesizing a polyimide precursor compound (specific polyimide precursor compound) having a structure represented by the above general formula (A1) by reacting the esterified tetracarboxylic dianhydride derivative and a diamine compound in a solvent A to prepare a first mixed solution containing the specific polyimide precursor compound and a solvent A; A step (second step) of mixing the first mixed liquid with inorganic particles to obtain a second mixed liquid; and mixing the second mixture with a solvent B (third step).
[0089] Each step will be described in detail below.
[0090] (Step 0: Esterification Step) The esterification step is a step in which a tetracarboxylic dianhydride derivative and an esterifying agent are reacted (esterified) to prepare an esterified tetracarboxylic dianhydride derivative.
[0091] Esterification reaction By reacting a tetracarboxylic dianhydride derivative with an esterifying agent, the carboxylic anhydride group (-C(=O)-OC(=O)-) in the tetracarboxylic dianhydride derivative is opened, and one becomes a carboxyl group (-COOH) and the other becomes a group with a structure in which H in the carboxyl group is replaced (-COOR 1 (R 1 represents an organic group containing at least one selected from the group consisting of an aliphatic group and an aromatic group, hereinafter referred to as an "ester group"). Of the carboxyl groups generated by ring-opening of the carboxylic anhydride groups in the esterified tetracarboxylic dianhydride derivative, the proportion that becomes ester groups through esterification (i.e., the proportion of the number of ester groups to the sum of the number of carboxyl groups and the number of ester groups) is preferably 10% or more, more preferably 30% or more, even more preferably 45% or more, and even more preferably 50%.
[0092] The ratio of the number of ester groups to the sum of the number of carboxyl groups and the number of ester groups in the esterified tetracarboxylic dianhydride derivative can be measured by quantifying hydrogen derived from the ester groups using nuclear magnetic resonance analysis (NMR).
[0093] Tetracarboxylic acid dianhydride derivatives As the tetracarboxylic dianhydride derivative, the above-mentioned "tetracarboxylic dianhydride", "tetracarboxylic dianhydride having an ester group", "tetracarboxylic dianhydride having an amide bond", and "tetracarboxylic dianhydride represented by formula (3)" can be used.
[0094] Esterification agent As the esterification agent, a compound having an organic group containing at least one selected from the group consisting of an aliphatic group and an aromatic group, and a hydroxyl group (-OH) is used. For example, an alcohol (R 1 -OH(R 1 R represents an organic group containing at least one selected from the group consisting of an aliphatic group and an aromatic group. 1 The number of carbon atoms in the organic group containing at least one selected from the group consisting of aliphatic groups and aromatic groups represented by the following formula (I) is preferably from 1 to 10, more preferably from 1 to 8, and even more preferably from 1 to 6. The aliphatic group may be linear, branched, or cyclic, and is preferably linear or branched. Examples of the esterifying agent include methanol, ethanol, propanol, isopropanol, butanol, 2-butanol, isobutanol, t-butanol, pentanol, hexanol, heptanol, octanol, nonanol, decanol, phenol, and benzyl alcohol (Ph-CH2-OH: Ph represents a phenyl group), etc. Among these, methanol, ethanol, propanol, isopropanol, butanol, 2-butanol, phenol, and benzyl alcohol are preferred.
[0095] The esterification agent is preferably removed by evaporation after reacting with the tetracarboxylic dianhydride derivative as described below, and from this viewpoint, the esterification agent preferably has a low boiling point. The low boiling point of the esterification agent allows the heating temperature when evaporating the esterification agent to be kept low, and the site that has been opened by esterification and turned into an ester group on one side is prevented from closing the ring again to become a carboxylic anhydride group. Specifically, the boiling point of the esterification agent is preferably 250°C or less, more preferably 200°C or less, and even more preferably 150°C or less. The lower limit of the boiling point of the esterification agent is not particularly limited, but can be 30°C or more.
[0096] ·Esterification method A specific method for reacting (esterifying) a tetracarboxylic dianhydride derivative with an esterifying agent includes, for example, a method in which the tetracarboxylic dianhydride derivative and the esterifying agent are mixed and heated under reflux. The heating temperature is, for example, preferably from 30° C. to 150° C., and more preferably from 60° C. to 120° C. The reaction time is, for example, preferably from 1 hour to 10 hours, and more preferably from 2 hours to 6 hours.
[0097] Removal of esterification agents It is preferable to remove the esterification agent after reacting (esterifying) the tetracarboxylic dianhydride derivative with the esterification agent. By removing the esterification agent before reacting the esterified tetracarboxylic dianhydride derivative with the diamine compound, the reaction of the esterification agent with the condensation agent or the diisocyanate compound can be suppressed, and the reaction rate of the esterified tetracarboxylic dianhydride derivative with the diamine compound can be increased. Specifically, after the esterification is completed, it is preferable to further heat the mixture at a temperature equal to or higher than the boiling point of the esterification agent to evaporate and remove the esterification agent. The heating temperature when evaporating the esterification agent is, for example, preferably 20°C to 100°C, more preferably 40°C to 80°C. When the boiling point of the esterification agent is high, it is preferable to lower the boiling point by evaporating it under reduced pressure. The heating time is, for example, preferably 1 hour to 24 hours, more preferably 3 hours to 8 hours. The esterifying agent is preferably a compound having a hydroxyl group and a boiling point of 250° C. or less.
[0098] (1st step) The first step is a step of synthesizing a specific polyimide precursor compound by reacting an esterified tetracarboxylic dianhydride derivative and a diamine compound in a solvent A, and preparing a first mixed solution containing the specific polyimide precursor compound and the solvent A.
[0099] ·reaction By reacting an esterified tetracarboxylic dianhydride derivative with a diamine compound, a carboxyl group (-COOH) of the esterified tetracarboxylic dianhydride derivative reacts with an amino group (-NH2) of the diamine compound to form an amide bond (-CO-NH-), and a polyimide precursor compound having the structure represented by the above-mentioned general formula (A1) is synthesized.
[0100] A specific example of the method for the first step includes a method in which the esterified tetracarboxylic dianhydride derivative obtained in the esterification step and a diamine compound are added to a solvent A, and a condensing agent is further added as necessary, followed by reaction with stirring.
[0101] Diamine compounds As the diamine compound, the above-mentioned "diamine compound" can be used.
[0102] Condensation Agent Examples of the condensation agent include diphenyl(2,3-dihydro-2-thioxo-3-benzoxazolyl)phosphonate (DBOP), (benzotriazol-1-yloxy)tris(dimethylamino)phosphonium hexafluorophosphate (BOP), (benzotriazol-1-yloxy)tripyrrolidinophosphonium hexafluorophosphate (PyBOP), 1-[bis(dimethylamino)methylene]-1H-benzotriazolium 3-oxide tetrafluoroborate (TBT U), 1-[bis(dimethylamino)methylene]-1H-benzotriazolium 3-oxide hexafluorophosphate (HBTU), 1-[bis(dimethylamino)methylene]-1H-1,2,3-triazolo[4,5-b]pyridinium 3-oxide tetrafluoroborate (TATU), and 1-[bis(dimethylamino)methylene]-1H-1,2,3-triazolo[4,5-b]pyridinium 3-oxide hexafluorophosphate (HATU), etc. can be used. Alternatively, an active ester method may be used, for example, by forming an active ester using 1-hydroxybenzotriazole (HOBt), 1-hydroxy-7-azabenzotriazole (HOAt), ethyl (hydroxyimino)cyanoacetate (Oxyma), or the like, followed by the use of a condensing agent such as diphenylphosphoryl azide (DPPA).
[0103] Solvent A The solvent A is preferably a solvent that dissolves the specific polyimide precursor compound. Therefore, in the first step, it is preferable to dissolve the synthesized specific polyimide precursor compound in the solvent A. Here, in this embodiment, "dissolved" means that the specific polyimide precursor compound dissolves in the solvent A at 25°C in an amount of 90% by mass or more. Specific examples of the solvent A include the aprotic polar solvents described above.
[0104] The amount of solvent A added is not particularly limited as long as it is an amount capable of dissolving the specific polyimide precursor compound, but it is preferably from 1000% by mass to 6000% by mass based on the mass of the synthesized specific polyimide precursor compound.
[0105] -Content of specific polyimide precursor compounds In the first mixed liquid prepared in the first step, the content of the specific polyimide precursor compound is preferably 5% by mass or more and 45% by mass or less, more preferably 10% by mass or more and 40% by mass or less, and even more preferably 15% by mass or more and 35% by mass or less, relative to the first mixed liquid.
[0106] (2nd process) The second step is a step of mixing the first mixed liquid with inorganic particles to obtain a second mixed liquid. The second step may be, for example, a method in which inorganic particles are added to the first mixed liquid and mixed. The method of adding the inorganic particles is not particularly limited, and examples thereof include a method of adding the inorganic particles alone and a method of adding a dispersion liquid containing the inorganic particles. From the viewpoint of dispersibility, the method of adding a dispersion liquid containing the inorganic particles is preferred.
[0107] The dispersion liquid containing inorganic particles preferably contains inorganic particles and a solvent A or a solvent B described below. The content of the inorganic particles in the entire dispersion liquid containing the inorganic particles is preferably from 5% by mass to 30% by mass, and more preferably from 10% by mass to 20% by mass.
[0108] The amount of inorganic particles added is not particularly limited, and is, for example, preferably 1% by mass or more and 80% by mass or less, more preferably 2% by mass or more and 70% by mass or less, and even more preferably 3% by mass or more and 60% by mass or less, relative to the resin content in the first mixed liquid.
[0109] (3rd step) The third step is a step of mixing the second mixed liquid with a solvent B. The third step may be, for example, a method in which solvent B is added dropwise to the second mixed liquid while being mixed.
[0110] Solvent B is preferably a solvent that does not dissolve the specific polyimide precursor compound. In this specification, the term "not soluble" also includes the case where the specific polyimide precursor compound is soluble in the solvent B at 25°C within a range of 3% by mass or less. Examples of the solvent B include the above-mentioned ether-based solvents, the above-mentioned ketone-based solvents, the above-mentioned alcohol-based solvents, and water.
[0111] The method for mixing the second mixed liquid with the solvent B is not particularly limited, and can be performed using a known stirring device, etc. Examples of the stirring device that can be used include a homomixer, a homogenizer, and a dissolver.
[0112] The amount of solvent B added is not particularly limited, but for example, it is preferably 50% by mass or more and 90% by mass or less, more preferably 55% by mass or more and 85% by mass or less, and even more preferably 60% by mass or more and 80% by mass or less, relative to the second mixed liquid.
[0113] Here, the combination of solvent A and solvent B is not particularly limited to the specific examples described above. It is preferable that solvent A is a solvent that dissolves the specific polyimide precursor compound contained in the electrodeposition coating paint to be produced, and solvent B is a solvent that does not dissolve the specific polyimide precursor compound contained in the electrodeposition coating paint to be produced. For example, although water is given as a specific example of solvent B, depending on the type of the specific polyimide precursor compound used, it may be solvent A. For example, when the specific polyimide precursor compound contained in the electrodeposition coating paint to be produced is soluble in water, it is preferable that solvent A is water and solvent B is a solvent other than water.
[0114] <Insulation material manufacturing method> The method for producing an insulating material according to the present disclosure preferably includes a step of forming a coating film by electrodeposition coating paint (coating film forming step), and a step of baking the coating film (baking step). Each step will be described in detail below.
[0115] (Coating film formation process) The coating film forming step is a step of forming a coating film by electrodeposition coating the coating material for electrodeposition coating according to the present disclosure. The method of electrodeposition coating is not particularly limited, and a known electrodeposition coating method can be used. For example, it is preferable to apply a voltage of 1 V to 400 V between the substrate as the anode and the cathode. It is also preferable to apply a voltage of 1 V to 400 V between the substrate as the cathode and the anode. The temperature of the paint during electrodeposition coating is preferably, for example, 10° C. to 45° C.
[0116] The substrate to be coated is not particularly limited, but examples thereof include plate-shaped conductors, rod-shaped conductors, coil-shaped conductors, and conductors of irregular shape. The material of the substrate is not particularly limited as long as it is electrically conductive, but examples include metals such as platinum, gold, silver, copper, aluminum, zinc, nickel, titanium, and bismuth, alloys of the above metals, and carbon. The substrate may also be one having a conductor surface plated with nickel or the like.
[0117] The thickness of the coating film is not particularly limited, and it is preferable to adjust it appropriately within the range of 5 μm or more and 100 μm or less depending on the application and the type of substrate to be coated.
[0118] FIG. 1 shows an example of an electrodeposition apparatus 100 used for electrodeposition coating. The stainless steel container 10 contains the paint 11 . A glass container lid 12 is provided on the top of the stainless steel container 10. Pipes 16 and 17 are passed through the stainless steel container 10 via the glass container lid 12, and an inert gas (e.g., nitrogen, argon, etc.) is blown in through pipe 16 and flows out of the stainless steel container 10 through pipe 17. A DC power supply 13 is connected to an electric field generating electrode 14 which is a positive electrode and a coating substrate 15 which is a negative electrode, and applies a voltage between the electrodes.
[0119] By applying a voltage between the electrodes, the specific polyimide precursor compound (hereinafter also referred to as the resin component) and inorganic particles contained in the coating material 11 electrophores toward the negative electrode of the coating substrate 15, and the resin component and inorganic particles aggregate on the surface of the coating substrate 15 to form a coating film. When the resin component and inorganic particles are materials that electrophores toward the positive electrode side, it is preferable to connect the coating substrate 15 to the positive terminal of the DC power source 13 (i.e., the coating substrate 15 is the positive electrode) and connect the electric field generating electrode 14 to the negative terminal of the DC power source 13 (i.e., the electric field generating electrode 14 is the negative electrode), and electrophores the resin component and inorganic particles to form a coating film of the resin component and inorganic particles on the surface of the coating substrate 15, which is the positive electrode.
[0120] (Firing process) The baking step is a step of baking the coating film obtained through the coating film forming step. The baking can promote imidization of the specific polyimide precursor compound in the coating film, and an insulating material containing a polyimide resin (for example, a polyimide insulating film) can be formed.
[0121] The firing step may be carried out by increasing the heating temperature stepwise. The coating film may be heated in stages by drying the coating film by heating it at a relatively low temperature (e.g., below 200°C) and then baking the dried coating film at a high temperature (e.g., around 300°C).
[0122] The coating film can be dried, for example, by methods such as heat drying, natural drying, and vacuum drying, and from the viewpoint of production efficiency, heat drying is preferred. The conditions for heat drying are preferably changed as appropriate depending on the film thickness of the coating film, etc., but for example, drying is preferably performed under conditions of 70°C or higher and 200°C or lower for 20 minutes or longer and 300 minutes or shorter, and more preferably 20 minutes or longer and 200 minutes or shorter.
[0123] The coating film after drying may be baked at 150° C. or more and 400° C. or less (preferably around 300° C.) for 20 minutes or more and 120 minutes or less. The firing may be carried out by increasing the temperature stepwise. The heating method for firing may be heater heating, hot air heating, dielectric heating, or the like.
[0124] It is preferable that the insulating material is manufactured through the above steps.
[0125] The insulating material obtained by the above-mentioned production method can be used for applications such as insulated wires, insulating parts, mobile communication devices (including 5th generation (5G)), and films. EXAMPLES
[0126] Examples will be described below, but the present disclosure is not limited to these examples. In the following description, unless otherwise specified, all "parts" and "%" are based on mass.
[0127] <Example 1> (Preparation of polyimide precursor solution) First, the tetracarboxylic dianhydride was reacted with an esterifying agent. A flask equipped with a condenser was charged with the type and amount (mol) of tetracarboxylic dianhydride and the type and amount (mol) of esterifying agent shown in Table 1, and the two were reacted with each other by heating at 65°C for 4 hours under reflux. Next, the condenser was removed, and the remaining esterifying agent was evaporated by heating at 60°C under reduced pressure for 3 hours. As a result, an esterified tetracarboxylic dianhydride powder was obtained in which the tetracarboxylic dianhydride and the esterifying agent had reacted.
[0128] Next, a 1 L three-necked separable flask equipped with a stirrer and a thermometer was charged with the type and amount (mol) of diamine compound shown in Table 1 and NMP as solvent A (an amount to give a polyimide precursor compound concentration of 20.0% by mass), and dissolved while stirring by flowing in nitrogen. Next, a condensation agent shown in Table 1 was added with the type and amount (mol) of condensation agent, and the powder of esterified tetracarboxylic dianhydride obtained above was gradually added and stirred to obtain a solution containing a polyimide precursor with a concentration of 20.0% by mass (the content of the polyimide precursor compound relative to the entire solution containing the polyimide precursor is 20% by mass; the same applies below).
[0129] (Preparation of paint for electrodeposition coating) 20 g of the solution containing the polyimide precursor was diluted with 80 g of NMP as solvent A (first step). Next, while vigorously stirring, 7.06 g of boehmite alumina A10 (containing inorganic particles containing aluminum oxide monohydrate and NMP as solvent A. The content of the inorganic particles is 10 mass% with respect to the entire dispersion) was dropped into the solution containing inorganic particles (second step), and then 180 g of ethanol was dropped into the solution as solvent B (third step) to obtain a coating material for electrodeposition coating.
[0130] <Examples 2 to 17> A solution containing a polyimide precursor was prepared and a coating material for electrodeposition coating was obtained in the same manner as in Example 1, except that the diamine compound, acid component (tetracarboxylic dianhydride), esterification agent, and condensation agent used were changed to the types and amounts (mol) shown in Tables 1 to 4, and the inorganic particles added were changed to the types shown in Tables 1 to 4. It should be noted that no condensation agent was used in Examples 12 and 14. Moreover, in Examples 8 to 17, methanol was used as the solvent B in (preparation of the paint for electrodeposition coating).
[0131] <Comparative Example 1> (Preparation of polyimide precursor solution) In a 1 L three-necked separable flask equipped with a stirrer and a thermometer, the type and amount (mol) of diamine compound shown in Table 4 and NMP (amount to give a polyimide precursor compound concentration of 20.0% by mass) as solvent A were charged, and nitrogen was introduced and dissolved while stirring. Next, the type and amount (mol) of acid component (tetracarboxylic dianhydride) shown in Table 4 was gradually added and stirred to obtain a solution containing a polyimide precursor with a concentration of 20.0% by mass (the content of the polyimide precursor compound relative to the entire solution containing the polyimide precursor is 20% by mass. The same applies below).
[0132] (Preparation of paint for electrodeposition coating) 20 g of the solution containing the polyimide precursor was diluted with 80 g of NMP as solvent A (first step). Next, while vigorously stirring, 7.06 g of boehmite alumina A10 (containing inorganic particles containing aluminum oxide monohydrate and NMP as solvent A. The content of the inorganic particles was 10 mass% relative to the entire dispersion) was added dropwise (second step), and then 180 g of methanol was added dropwise as solvent B (third step) to obtain a coating material for electrodeposition coating.
[0133] <Comparative Example 2> A solution containing a polyimide precursor was prepared and a coating material for electrodeposition coating was obtained in the same manner as in Comparative Example 1, except that the diamine compound and acid component (tetracarboxylic dianhydride) used were changed to the types and amounts (mol) shown in Table 4, and the inorganic particles added were changed to the types shown in Table 4.
[0134] <Electrodeposition coating> (electrodeposition, drying and firing) Using the electrodeposition equipment shown in Figure 1, electrodeposition coating was performed using the electrodeposition coating paint obtained in each example. The substrate (cathode electrode) was oxygen-free copper with a width of 10 mm, thickness of 1 mm, and corner radius of 0.1 mm. DC 250V was applied for 5 minutes while nitrogen was flowing in, forming an electrodeposition film. After the solvent was dried off from the substrate at around 120°C in a thermostatic chamber, the temperature was raised in stages, and finally, the substrate was baked at 300°C for 10 minutes to produce a substrate with an insulating film (hereinafter, insulating material).
[0135] <Evaluation> (Appearance of electrocoating paint) The electrodeposition coating paint obtained in each example was visually inspected to evaluate whether the components contained in the electrodeposition coating paint were dispersed in a nearly uniform state. In the tables, when the components contained in the electrodeposition coating paint are dispersed in a nearly uniform state, it is recorded as "dispersed." On the other hand, when agglomerates occur in the electrodeposition coating paint, it is described as "agglomeration."
[0136] (Storage of paint for electrodeposition coating) The electrodeposition coating paint obtained in each example was stored at 5°C, and the electrodeposition coating paint was taken out at regular intervals and used to prepare insulating materials under the same conditions as described above (electrodeposition, drying, and baking). The insulating materials thus prepared were used to perform the dielectric breakdown test described below, and the storage time at which the breakdown voltage value fell to 50% or less of the initial value was measured.
[0137] (Appearance of the insulating film) The insulating film of the insulating material prepared using the electrodeposition coating paint obtained in each example was visually inspected, and the surface smoothness of the insulating film was evaluated. In the table, when the surface of the insulating film is smooth, it is recorded as "good." On the other hand, if there are many irregularities on the surface of the insulating coating, it is rated as "poor."
[0138] (Coating thickness) The outer diameters of the insulating material prepared using the electrocoating paint obtained in each example were measured at three random points in the thickness direction and width direction. The arithmetic mean value of the outer diameters of the insulating material in the thickness direction and the arithmetic mean value of the outer diameters of the insulating material in the width direction were calculated. The thickness direction coating thickness was calculated by subtracting the thickness direction diameter of the coated object (anode electrode) included in the insulating material from the arithmetic mean value of the outer diameters of the insulating material in the thickness direction (referred to as "thickness (mm)" in the table). The width direction coating thickness was calculated by subtracting the width direction diameter of the coated object (anode electrode) included in the insulating material from the arithmetic mean value of the outer diameters of the insulating material in the width direction (referred to as "width (mm)" in the table). In addition, the smallest value among the thicknesses of the insulating coating of the insulating material measured when calculating the arithmetic average thickness of the coating was taken as the thickness at the thinnest part (referred to as "thinnest part thickness" in the table). Here, the width and thickness of the coating film were measured using a micrometer.
[0139] (Flexibility) The insulating material made using the electrocoating paint obtained in each example was bent 90 degrees around a cylindrical mandrel with a diameter of 5 mm, and the presence or absence of cracks in the insulating film was checked with a magnifying glass. If no cracks were found, it was judged as "passed", and if cracks were found, it was judged as "failed".
[0140] (Voltage Test) A 10mm wide metal foil was tightly wrapped around the outer circumference of the insulating material made using the electrocoating paint obtained in each example, and a voltage of AC 2000Vrms, 50Hz was applied between the insulating material and the metal foil for 10 seconds. If the leakage current was less than 5mA, it was judged as "passed", and if the leakage current was 5mA or more, it was judged as "failed".
[0141] (Dielectric breakdown test) A 10 mm wide metal foil was tightly wrapped around the outer circumference of the insulating material made using the electrocoating paint obtained in each example, and a sine wave (50 Hz) voltage was applied between the insulating material and the metal foil, increasing the voltage at approximately 500 V / sec. The voltage at which the leakage current became 5 mA or more was taken as the breakdown voltage.
[0142] (Heat deterioration resistance test) The insulating coating of the insulating material produced using the electrocoating paint obtained in each example was subjected to a heat treatment at 300° C. for 500 hours. Next, the insulating coating after the heat treatment was subjected to the film elongation test described below, and a film whose elongation (%) was 50% or more of the initial value was judged as "passed", and a film whose elongation was less than 50% was judged as "failed".
[0143] (5% mass reduction temperature) The insulating film of the insulating material produced using the electrocoating paint obtained in each example was peeled off, and TG-DTA measurement was performed using a Shimadzu DTG-60H. If the temperature at which the mass of the insulating film was reduced by 5% by mass was 500°C or higher, it was judged as "passed", and if it was less than 500°C, it was judged as "failed".
[0144] (Film elongation test) A 5 mm wide cut was made with a sharp blade in the insulating film of the insulating material prepared using the electrocoating paint obtained in each example, and the film was cut into a film piece of about 100 mm by peeling it off from the end face with tweezers. A tensile test was carried out on the film piece with a chuck length of 50 mm, and the elongation rate of the film until the film piece broke was measured.
[0145] [Table 1]
[0146] [Table 2]
[0147] [Table 3]
[0148] [Table 4]
[0149] The contents of Tables 1 to 4 will be explained below. Resin: Indicates the type and amount (in moles) of diamine compound, diisocyanate, and tetracarboxylic dianhydride used in preparing the electrodeposition coating paint. Also indicates the amount (in moles) of methacrylic anhydride used in preparing the electrodeposition coating paint. If a commercially available resin is used, indicate the product name. Good solvent: Indicates the type of solvent A contained in the paint for electrodeposition coating. -Poor solvent: Indicates the type of solvent B contained in the paint for electrodeposition coating. Resin type: Indicates the type of resin contained in the electrocoating paint. Inorganic particles: Indicates the type of inorganic particles contained in the electrocoating paint. "A10" indicates boehmite alumina A10. Boehmite alumina is a particle that contains aluminum oxide, and silica is a particle that contains silicon oxide.
[0150] From the above results, it can be seen that the electrodeposition coating paint of the Example has suppressed the occurrence of aggregation and has excellent coating properties compared to the electrodeposition coating paint of the Comparative Example. 1 It can be seen that, compared with Examples 16 and 17 in which polyimide precursors having a structure containing an aliphatic group in the main chain are synthesized, Examples 1 to 15 in which polyimide precursors having a structure not containing an aliphatic group in the main chain are synthesized, insulating materials having excellent heat resistance are obtained. [Explanation of symbols]
[0151] 10 Stainless steel containers 11 Paint 12 Glass container lids 13 DC power supply 14 Electric field generating electrode 15 Substrate for coating 16, 17 tube 100 Electrodeposition equipment
Claims
1. A solvent; A polyimide precursor compound having a structure represented by the following general formula (A1); Inorganic particles; A paint for electrocoating containing the above. [Formula 1] (In general formula (A1), R 1 is an organic group containing at least one selected from the group consisting of an aliphatic group and an aromatic group, 1 represents an organic group containing an aromatic group, Ar 2 represents an organic group containing an aromatic group.
2. In the general formula (A1), R 1 2. The electrocoating paint according to claim 1, wherein the organic group containing at least one selected from the group consisting of an aliphatic group and an aromatic group represented by the following formula (I) has 1 to 10 carbon atoms.
3. In the general formula (A1), the Ar 1 The organic group containing an aromatic group represented by the formula (I) has a structure that does not contain a linear or branched aliphatic group or a sulfonyl group in the main chain, and the Ar 2 2. The electrocoating paint according to claim 1, wherein the organic group containing an aromatic group represented by the formula (I) has a structure which does not contain linear or branched aliphatic groups or sulfonyl groups in the main chain.
4. 2. The electrocoating paint according to claim 1, which has an absolute value of a zeta potential of 5 mV or more.
5. 2. The electrocoating paint according to claim 1, wherein the inorganic particles are particles containing at least one type selected from the group consisting of aluminum oxide, silicon oxide, titanium oxide, and magnesium oxide.
6. reacting a tetracarboxylic dianhydride derivative with an esterifying agent to prepare an esterified tetracarboxylic dianhydride derivative; a step of reacting the esterified tetracarboxylic dianhydride derivative and a diamine compound in a solvent A to synthesize a polyimide precursor compound having a structure represented by the following general formula (A1), and preparing a first mixed solution containing the polyimide precursor compound and the solvent A; A step of mixing the first mixture with inorganic particles to obtain a second mixture; and mixing the second mixed liquid with a solvent B. [chemical 2] (In general formula (A1), R 1 is an organic group containing at least one selected from the group consisting of an aliphatic group and an aromatic group, 1 represents an organic group containing an aromatic group, Ar 2 represents an organic group containing an aromatic group.
7. The method for producing a paint for electrodeposition coating according to claim 6, wherein the esterifying agent is a compound having a hydroxyl group and a boiling point of 250°C or less.
8. A step of forming a coating film by electrodeposition coating the coating material for electrodeposition coating according to any one of claims 1 to 5; and baking the coating film.
Citation Information
Patent Citations
JP1311182B
JP1972005189A
Signal storage and memory unit
JP1979041617A
Production of temperature compensation crystal oscillator
JP1999027047A
JP2098020B