Characterization and measurement in a small box with multi-measurement using XPS

By employing multiple XPS measurements with varying beam sizes and modeling the signal attenuation, the technique addresses the challenge of accurately measuring film layer thickness in small semiconductor structures, enhancing characterization and measurement precision.

JP2024538229APending Publication Date: 2024-10-18NOVA MEASURING INSTRUMENTS INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024524420
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-12-30
Filing Date
2022-10-24
Publication Date
2024-10-18

AI Technical Summary

Technical Problem

As semiconductor structures become smaller, X-ray photoelectron spectroscopy (XPS) measurements face challenges in accurately determining the thickness of film layers within small box regions due to X-ray beam sizes that exceed the box area, causing spillage of the signal outside the box and making it difficult to distinguish the signal from inside and outside the box material.

Method used

The technique involves multiple XPS measurements using X-ray beams of different sizes to determine the mixing ratio of the beam within and outside the box, allowing for the calculation of film layer thickness by modeling the attenuation of the XPS signal using effective attenuation lengths and contribution factors.

Benefits of technology

This method enhances the analytical accuracy of XPS measurements in small box regions by precisely determining the thickness and composition of film layers within semiconductor structures, improving characterization and measurement capabilities.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024538229000011
    Figure 2024538229000011
  • Figure 2024538229000012
    Figure 2024538229000012
  • Figure 2024538229000013
    Figure 2024538229000013
Patent Text Reader

Abstract

A system is disclosed for characterizing a film layer within a measurement box. The system acquires a first mixing fraction corresponding to a first X-ray beam, the mixing fraction representing a fraction of the first X-ray beam within a measurement box of a wafer sample, the measurement box representing a bore structure disposed on a substrate, the measurement box having a film layer disposed within the bore structure. The system acquires a measurement box contribution value corresponding to the first X-ray beam, the contribution value representing a seed signal outside the measurement box that contributes to a same seed signal within the measurement box. The system acquires a first measurement detection signal corresponding to a measurement of the measurement box with the first X-ray beam. The system determines a measurement value of the film layer based on the first measurement detection signal, the contribution value, and the first mixing fraction.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This disclosure relates generally to techniques for characterizing and measuring semiconductor structures, and specifically to techniques for characterizing and measuring layers of material in small boxes with multiple measurements using X-ray photoelectron spectroscopy (XPS). [Background technology]

[0002] Integrated circuits (ICs) are typically constructed from multiple layers formed on a silicon substrate. As integrated circuits become smaller and the layers that make up the IC become thinner, the operation of devices constructed from these multiple layers becomes more dependent on the thickness of a particular layer. For example, transistors formed on a silicon substrate may have different characteristics depending on the thickness of the transistor's gate.

[0003] Layers on an IC are deposited on a substrate by deposition techniques where patterns are etched onto the layers to form the various IC components. Such patterns include trenches or paddings (boxes). When the trenches or boxes are coated with additional layers of material, it can be difficult to ascertain the proper layer thickness and to ascertain the coating material deposited within the trenches or boxes if the trenches or boxes are small. Therefore, it can be useful to determine the thickness of the film layer within the small box area.

[0004] The thickness of a film layer deposited on a substrate can be determined using one of several techniques, one of which is X-ray photoelectron spectroscopy (XPS), in which an X-ray beam is irradiated onto the substrate while simultaneously measuring the kinetic energy and number of electrons that escape from the top layer of the substrate, resulting in an XPS spectrum. Summary of the Invention [Problem to be solved by the invention]

[0005] As IC components become smaller, the X-ray beam for XPS measurements may not fit inside a box region. If an X-ray beam with a beam size larger than the box region is used, the X-ray beam will irradiate the area inside the box and the area around the box, so the collected XPS signal will come from the material inside the box and the material around the box. Therefore, it is difficult to determine which part of the XPS signal corresponds only to the material inside the box. There is a need to improve the analytical accuracy of XPS measurements for small box regions. [Means for solving the problem]

[0006] The following summary of the disclosure is included to provide a basic understanding of some aspects and features of the disclosure. This summary is not an extensive overview of the disclosure, and as such is not intended to particularly identify key or critical elements of the disclosure or to delineate the scope of the disclosure. Its sole purpose is to present some concepts of the disclosure in a simplified form as a prelude to the more detailed description that is presented below.

[0007] The disclosed embodiments allow for characterization and measurement of film layers within small boxes using multiple measurements using XPS. In some disclosed embodiments, XPS measurements are used to analyze specific properties of film layers within small boxes, such as thickness or composition, where the XPS signal has some spillage outside the small boxes.

[0008] Other aspects and features of the present disclosure will become apparent from the following detailed description taken in conjunction with the drawings, in which it is understood that the detailed description and drawings provide various non-limiting examples of various embodiments of the present disclosure as defined by the appended claims.

[0009] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments of the disclosure and, together with the description of the specification, serve to explain and illustrate the principles of the disclosure. The drawings are intended to diagrammatically illustrate major features of exemplary embodiments. The drawings are not intended to depict all features of actual embodiments or the relative dimensions of the depicted elements, and are not drawn to scale. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a partial cross-sectional view of a wafer sample showing measurements according to some embodiments, FIG. 1A is a schematic diagram showing an example of determining the layer thickness of a film stack outside a box structure, and FIG. 1B is a schematic diagram showing an example of determining the layer thickness of a film stack inside a box structure. [Diagram 2] 1 shows an example of a measuring device. [Diagram 3] FIG. 3A shows an example of a measurement of a reference wafer sample using a nominal beam 1, and FIG. 3B shows an example of a measurement of a reference wafer sample using a beam 2 with a large spot diameter. [Figure 4]FIG. 4A shows an example of measurement of a measurement wafer sample using a nominal beam 1, and FIG. 4B shows an example of measurement of a measurement wafer sample using a beam 2 with a large spot diameter. [Diagram 5] An example of a measurement of a measurement wafer sample using nominal beam 1 is shown. [Figure 6] FIG. 1 is a flow diagram illustrating an example method. [Figure 7] FIG. 1 is a partial cross-sectional view of an example wafer sample with boxes showing two film layers. [Figure 8] FIG. 8A shows an example of measurement of a reference wafer sample using an X-line scan, and FIG. 8B shows an example of measurement of a reference wafer sample using a Y-line scan. [Figure 9] 1 shows an example of a simulation of beam parameters for an X-ray beam. [Figure 10] FIG. 10A shows a simulation and measurement example of the mixing ratio versus central cross-sectional area in the Y direction, FIG. 10B shows a simulation and measurement example of the mixing ratio versus central cross-sectional area in the X direction, and FIG. 10C shows an example of the mixing ratio versus beam position relative to the box center in an X line scan. [Figure 11] FIG. 11A shows an example of measurement of a measurement wafer sample using X-line scanning, and FIG. 11B shows an example of measurement of a measurement wafer sample using Y-line scanning. [Figure 12] FIG. 1 is a flow diagram illustrating an example method. [Figure 13] FIG. 1 is a flow diagram illustrating an example method. [Figure 14] FIG. 1 is a flow diagram illustrating an example method. [Figure 15] FIG. 1 is a flow diagram illustrating an example method. [Figure 16] 1 is an example of a pad disposed above a substrate. [Figure 17] FIG. 1 is a flow diagram illustrating an example method. [Figure 18] 1 is an example of a simulation of a material thickness. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The embodiments of the characterization and measurement method / system are described with reference to the drawings. Different embodiments or combinations thereof can be used for different applications or to achieve different advantages. The various features disclosed in this specification can be used alone or in combination with other features, partially or fully utilized, balancing the advantages with requirements and constraints, depending on the results to be achieved. Thus, certain advantages are highlighted with reference to various embodiments, but are not limited to the disclosed embodiments. That is, the features disclosed in this specification are not limited to the embodiments in which they are described, but may be "mixed and matched" with other features and incorporated into other embodiments.

[0012] In the following detailed description, numerous specific details are set forth in order to provide a thorough understanding of the present invention. However, it will be understood by those skilled in the art that the present invention may be practiced without these specific details. In other instances, well-known methods, procedures, and components have not been described in detail so as not to obscure the present invention.

[0013] The subject matter which is regarded as the invention is particularly pointed out and distinctly claimed in the concluding portion of the specification, however, the invention, both as to its organization and method of operation, together with its objects, features, and advantages, may best be understood by reference to the following detailed description when read in conjunction with the accompanying drawings.

[0014] It will be understood that for simplicity and clarity of illustration, elements shown in the figures have not necessarily been drawn to scale. For example, the dimensions of some elements may be exaggerated relative to other elements for clarity. Further, where considered appropriate, reference numerals may be repeated among the figures to indicate corresponding or analogous elements.

[0015] In this specification, any reference to a system, method, and non-transitory computer-readable medium should be applied mutatis mutandis to any other of the system, method, and non-transitory computer-readable medium. For example, any reference to a system should be applied mutatis mutandis to a method executable by the system, and to a non-transitory computer-readable medium capable of storing instructions executable by the system.

[0016] At least one illustrated embodiment of the present invention can, for the most part, be implemented using electronic components and circuits known to those skilled in the art, and therefore details will not be described beyond what is considered necessary as described above for an understanding and appreciation of the concepts underlying the present invention and in order not to obscure or deviate from the teachings of the present invention.

[0017] The following illustrative values ​​should be considered as non-limiting examples.

[0018] In various examples, reference is made to a film layer (thin film layer) made of SiO2, and a substrate made of Si. It should be noted that these are merely non-limiting examples of materials, and the film layer can be made of a material different from SiO2, and / or the substrate can be made of a material other than Si. References to SiO2 and Si should apply mutatis mutandis to any film layer material and substrate material, respectively.

[0019] FIG. 1 shows a cross section of a portion of a semiconductor wafer sample 100 illustrating a characterization or measurement process, e.g. a process for determining species and / or species thickness of a thin film layer (e.g. about 0-10 nm thick) on the sample. A base layer 101, e.g. a wafer substrate, is made of silicon, on which an insulator layer 105 is formed. In this example, a silicon-dioxide layer is formed on the silicon substrate base layer. The silicon-dioxide layer 105 is patterned by etching bores (holes) in the shape of a square or circular box 110, in a particular example having a side length of 30 μm in length or diameter. In a practical manufacturing process many such bores are formed in the insulator layer 105, but for the sake of understanding the embodiment, the description will proceed with respect to only one such bore. In this example the bore does not reach the substrate, and a thin film 115 of silicon dioxide remains at the bottom of the bore on the base layer 101. 1, a layer of silicon dioxide 105 is formed on a silicon substrate 101 and etched to form the box 110, but any other material (silicon nitride, other oxides or nitrides, etc.) or manufacturing process (e.g., selective deposition, etc.) can be used to form the box 110. The box 110 can be rectangular, circular, trench-shaped, etc. Also, there may be an intervening layer of a different material between the substrate 101 and the dielectric layer 105 in which the bore is formed.

[0020] In one embodiment, XPS is used to characterize box 110, i.e., to determine the presence, composition and thickness of a film layer within (or beneath) box 110. Referring to the example of Figure 1, in this embodiment, XPS is used to determine whether a silicon dioxide film layer remains within (or beneath) box 110, and if so, the thickness of that film layer.

[0021] In one embodiment, the sample shown in FIG. 1 is irradiated with X-rays and the resulting photoelectron emission from the sample (indicated by the arrow) is examined. If the X-ray beam produces a spot 120 that fits within the 30 μm box 110, the thickness of the SiO2 layer 115 can be calculated using the attenuation by the SiO2 layer 115 of the emission (light emission) from the Si substrate 101, referred to herein as the Si signal. However, in a particular example, the X-ray beam produced has a spot 120 with a diameter larger than the 30 μm dimension, so that the XPS signal spills outside the box 110. In this case, the attenuation of the emission from the SiO2 has a signal component inside the box and a signal component (e.g. spill) outside the box. In one embodiment, multiple measurements are performed on the reference box 110 to determine a mixing fraction of the beam (fraction of beam that is inside the box). Using the mixture fraction, multiple measurements are performed on the box 110 to determine a contribution value for species signal outside the box that contribute to a same species signal inside the box. The mixture fraction and contribution value can then be used to calculate the thickness of the SiO2 layer 115.

[0022] 2 illustrates an example of an X-ray system 200 for characterization or measurement processes for various embodiments disclosed herein. The operation of the system and the analyses described herein may be performed by one or more computers 205. In one embodiment, computer 205 may be a stand-alone computer at a customer's location. Computer 205 may store instructions used in software on a suitable non-volatile computer readable storage medium and cause hardware to execute the instructions using one or more processors to implement the techniques of this specification.

[0023] An electron gun 210 emits an electron beam, which strikes an anode 215, here made of aluminum. As a result, X-rays are generated at the anode and directed to a monochromator 220. The X-rays are then diffracted in the monochromator. In this embodiment, the monochromator 220 is made of quartz crystal and is configured to focus only AlKα X-rays onto the wafer 225. A small amount of AlKα is also collected by a flux detector 230. The signal of the flux detector 230 can be converted from an X-ray count to a flux number. The flux number can be used as a reference indicator of the X-rays hitting the wafer.

[0024] A primary AlKα X-ray beam is directed to strike the wafer 225. As the X-rays pass through the layers of the wafer 225, electrons and secondary X-rays are emitted from each layer of the wafer. The XPS energy analyzer 240 collects the emitted electrons and directs them to the XPS detector 245. The XPS energy analyzer 240 separates the emitted electrons according to their energy, roughly like a prism separating white light into photon frequencies. As a result, the signal generated by the XPS detector 245 can be used to measure the number of electrons at each specific energy (i.e., intensity). A sample graph generated by the computer 205 plotting intensity (number of electrons) versus binding energy is displayed on the monitor 250.

[0025] The plot illustrated on monitor 250 shows how materials within a sample can be identified. In this particular example, wafer 225 is made of silicon and has a first layer of silicon dioxide 105 or a film layer of silicon monoxide 115. The various peaks in the plot can be used to identify the materials present in the sample being inspected, here wafer 225.

[0026] In one embodiment, the attenuation of the XPS signal from a layer is used to infer the presence of a layer of a different material above it. Furthermore, the amount of attenuation can be used to quantify the thickness of the upper layer when the X-ray beam is contained within the box 110. For an X-ray beam that has a spillover of a species signal outside the box 110, a mixing fraction f can be used to quantify the fraction of the beam inside the box (e.g., f) and the fraction of the beam outside the box (e.g., 1-f), which can be used to calculate the spillover of the species.

[0027] Focusing on the specific example in Figure 1, as illustrated in Figure 1B, for an overlayer SiO2 with a mixing ratio of f = 1 and a thickness of t0, the signal of species S (Figure 1B) is Isi = Isi'e (-t0 / λsi,SiO) where Isi' (sometimes called reference intensity or reference electron count) is the intensity of the photoelectrons from the species Si before passing through the layer SiO2, and λsi,sio are material parameters (effective attenuation length (EAL) for a particular type of photoelectron from the species Si passing through the material SiO2, e.g. silicon 2p photoelectrons emitted from silicon and passing through SiO2. In this document, the abbreviation EAL is sometimes used for material A in material B, but should be understood to refer to the particular photoelectrons emitted from said material). In the presence of other species (other than a thin layer of SiO2 and / or other than a Si substrate), the indices of intensity (si for Isi, and / or SiO for Isio), as well as the indices of other constants and variables (e.g. Ksi, Ksio, λsi, SiO, and / or λsio) are modified to reflect the different species (different materials).

[0028] As illustrated in Figure 1B, based on the above formula, for an X-ray beam with a mixing ratio of less than 1, the species Si signal attenuation is Isi Model=fe (-t0 / λsi,SiO) / Ksi, where f is the mixing fraction and Ksi is a constant representing the effective contribution of Si to the signal strength. Thus, the attenuation signal of silicon through a SiO2 overlayer is expressed as an exponential of the ratio of the overlayer thickness to the effective attenuation length of silicon through SiO2, scaled by the silicon scaling factor Ksi, which is further scaled by the mixing fraction f.

[0029] The signal generation of the seed SiO2 is similar to that of Isio Model =f(1-e (-t0 / λsi,SiO) ) / Ksio, where Ksio is a constant representing the effective contribution of SiO2 to the intensity of the signal, and λsio is a material parameter (the effective attenuation length (EAL) for a particular type of photoelectron from the species SiO2 passing through the material SiO2). Thus, the SiO2 signal generated from the SiO2 overlayer is expressed as a function of the ratio of the overlayer thickness to the effective attenuation length of silicon passing through SiO2, scaled by the silicon scaling factor Ksio, which is further scaled by the blend fraction f.

[0030] Focusing on FIG. 1A, for a thick overlayer 105 (about 100 nm), the attenuation of the seed Si signal can be approximated to zero. That is, the overlayer 105 is assumed to be thick enough so that Isi is not generated outside the box. The seed SiO2 signal is attenuated by Isio. Model = (1-f) / Ksio, that is, the SiO2 signal can be expressed as a SiO2 scaling coefficient Ksio, which is further scaled by the runoff coefficient (1-f).

[0031] Referring again to FIG. 1, the wafer sample to be characterized is a substrate of material B having a thickness t thick A first layer of material A (e.g., about 100 nm in Fig. 1) and a thickness of t thin(e.g., about 2 nm in FIG. 1) and a residual film layer of material A. Intensity I A and I B The optical emissions from species A and B in box 110 having layer A are independently attenuated by the presence of layer A, reduced by a mixing ratio representing the proportion of the X-ray beam directed at species A and B in the box, and the intensity modified by a contribution value representing the X-ray beam that escapes outside the box. In subsequent figures, the substrate may be referred to as material B and the overlayer as material A.

[0032] In one embodiment, the raw intensity numbers are not used directly because the flux variation from each measurement and from tool to tool needs to be taken into account. That is, the X-ray flux numbers can be used to normalize the raw intensities. In one embodiment, the raw intensity numbers are used directly as the seed signal. In one embodiment, the value of Isi' or 1 / Ksi is known and can be used as a constant to scale the seed signal based on requirements or experience. For example, the value of Isi' can be obtained by performing an XPS measurement of the wafer substrate before depositing the top layer, which can be the intensity of photoelectrons per some unit of incident X-ray flux, or the intensity of photoelectrons at some nominal flux, etc.

[0033] In some embodiments, the ratio of measured intensities (Isio / Isi) from the XPS measurement is expressed as the total model intensity ratio (Isio M / Isi M ), the sample in Figure 1 can be further characterized. For example, the residual function (or merit function (M)) can be determined as follows:

[0034]

number

[0035] where M is the merit function, Isio / Isi is the measured intensity ratio, and Isio M / Isi M represents the modeled ratio of species intensity, Isi represents the species intensity measured for Si, Isio represents the species intensity measured for SiO2, t0 represents the thickness of the SiO2 film layer 115 in the box 110, Ksi denotes a constant representing the effective contribution of Si to the intensity of the seed signal, Ksio denotes a constant representing the effective contribution of SiO2 to the intensity of the seed signal, f denotes the mixing fraction representing the fraction of the incident beam in the box, etc.

[0036] Assuming that Isi is not generated outside box 110, there is no contribution from Ksi, and Isio M and Isi M can be approximated as follows:

[0037]

number

[0038] The M function can be λ / (λ with a dashed line over it). In this example, there are more unknowns than there are intensity ratios. Therefore, additional data points are needed to characterize box 110.

[0039] In the following disclosure, as further described in Figures 3-6, multiple measurements (first beam and second beam) are used in conjunction with a reference wafer sample to characterize box 110 of Figure 1 and solve for multiple unknowns.

[0040] FIG. 3A shows a measurement to characterize a reference sample 300 using a nominal beam 1, and FIG. 3B shows a measurement to characterize a reference sample 300 using a beam 2 with a large spot diameter according to an embodiment. The reference sample 300 represents the sample 100 of FIG. 1 with a box 310 with a side length of 30 μm. The reference sample 300 has a substrate (not shown) of known material Si and an overlay 305 of known material SiO2. Here, to increase the number of data points, beam 1 and beam 2 are used to characterize the reference sample 300. Beam 1 has a spot with a diameter of 40 μm providing a first mixture fraction f1, and beam 2 has a spot with a diameter of 50 μm providing a second mixture fraction f2. Furthermore, to reduce the number of unknowns, the reference wafer is of the same dimensions of 30 μm with known species and species thicknesses, for example, a SiO2 film layer 315 with a thickness of 2 nm.

[0041] In one embodiment, to create a sample 300 with a known thickness, the wafer sample 300 can be etched in a similar box (bore structure) with a side length of 200 μm (not shown), and the known thickness is obtained by characterizing the 200 μm box using a 40 μm beam. Here, it is assumed that the 200 μm box is etched in a similar process to the 30 μm box, and both the 200 μm box and the 30 μm box have the same film layer thickness in these boxes. Since the 40 μm beam applied to the 200 μm box should have a signal of all species within the box (e.g., no leakage), the thickness is determined by the attenuation equation Isi=Isi'e, as described above. (-t0 / λsi,SiO) can be determined by:

[0042] Given a 30 μm box with a film layer of known material (SiO2) and known thickness (2 nm), the merit function for characterizing sample 300 with beam 1 is:

[0043]

number

[0044] where M1 represents the merit function of beam 1, Isio1 / Isi1 represents the measured intensity ratio of beam 1, and Isio1 M / Isi1 M denotes the modeled species intensity ratio for beam 1, Isi1 denotes the measured species intensity of Si using beam 1, Isio1 denotes the measured species intensity of SiO2 using beam 1, t denotes the thickness of the SiO2 film layer 315 in box 310, Ksio denotes a constant representing the effective contribution of SiO2 to the intensity of the species signal, and f1 denotes the first mixing fraction.

[0045] The merit function for characterizing sample 300 using beam 2 is:

[0046]

number

[0047] where M2 represents the merit function of beam 2, Isio2 / Isi2 represents the measured intensity ratio of beam 2, and Isio2 M / Isi2 M denotes the modeled species intensity ratio for beam 2, Isi2 denotes the measured species intensity of Si with beam 2, Isio2 denotes the measured species intensity of SiO2 with beam 2, t denotes the thickness of the SiO2 film layer 315 in box 310, Ksio denotes a constant representing the effective contribution of SiO2 to the intensity of the species signal, and f2 denotes the second mixture fraction. (Note that in the merit function, the notations SiO1 and SiO2 refer to the silicon dioxide signals obtained from beam 1 and beam 2, not silicon monoxide and silicon dioxide.)

[0048] Referring to the first and second merit functions (M1, M2), the known values ​​are seed signals Isi1, Isio1 (first measurement with beam 1), seed signals Isi2, Isio2 (second measurement with beam 2), t, and Ksio. The unknown values ​​are the mixture fractions f1 and f2. Since there are two equations with two unknowns, the mixture fractions f1 and f2 can be calculated independently using the merit functions M1, M2. In another embodiment, the mixture fractions can be calculated using the merit functions by regression techniques.

[0049] Once the mixing ratios for Beam 1 and Beam 2 are known, the characterization process can perform additional measurements on a measurement sample 400 of unknown material and unknown thickness using the same Beam 1 and Beam 2, respectively, as shown in Figures 4A-4B, as long as the size of the box remains the same as the reference sample.

[0050] Figure 4A shows measurements of a measurement sample 400 using nominal beam 1, and Figure 4B shows measurements characterizing a reference sample 400 using beam 2 according to one embodiment. Measurement sample 400 may be representative of sample 100 of Figure 1. Measurement sample 400 may be provided by a customer and, similar to reference sample 300 of Figures 3A-B, box 410 has known box dimensions of 30 μm x 30 μm.

[0051] As described above, Beam 1 has a 40 μm diameter spot providing a first mixture fraction f1, and Beam 2 has a 50 μm diameter spot providing a second mixture fraction f2. Furthermore, since the measurement sample 400 has the same 30 μm box dimension as the reference sample 300, the mixture fractions f1 and f2 will be the same as those calculated above for the reference sample 300 of Figures 3A-3B. Here, the measurement sample 400 has a substrate (not shown) of unknown material B and an overlayer 405 of unknown material A. Within the box 410 is a film layer 415 of material A on the surface of the substrate of material B.

[0052] The measurement sample 400 can be characterized using multiple measurements, for example, beam 1 (40 μm spot) in measurement 1, and raw intensity data is collected and stored for measurement 1. The beam of x-rays can then be adjusted to provide beam 2 (larger than 50 μm spot) to characterize the measurement sample 400 in measurement 2, and raw intensity data is collected and stored for measurement 2.

[0053] After the above measurements, the merit functions characterizing beam 1 and beam 2 are as follows:

[0054]

number

[0055] Here I A1,2 M represents the modeled intensity of seed signal A for beam 1 or beam 2, and I B1,2 M represents the modeled intensity of the seed signal B for beam 1 or beam 2, M denotes the merit function, and I A1 denotes the seed intensity measured for material A using beam 1, and I B1 denotes the seed intensity measured for material B using beam 1, and I A2 denotes the seed intensity measured for material A using beam 2, and I B2 denotes the seed intensity measured for material B using beam 2, f1 denotes the first blending fraction, f2 denotes the second blending fraction, t denotes the thickness of the film layer 415 of material A in box 410, K A represents a constant that represents the effective contribution of A to the intensity of the seed signal, and λ 1,2 is the material parameter (effective attenuation length (EAL)) of a particular type of photoelectron from species A and B passing through material A. λ can be estimated based on the binding energy of the species signals from a look-up table or the NIST database.

[0056] In this case, the merit function M contains two measurement signal ratios and two unknowns (t and KA ) exists. The merit function M is solved by a numerical method, and the unknowns (t and K A In one embodiment, regression can be used to determine the measured raw spectral ratios (e.g., I A1 / I B1 and I A2 / I B2 ) and the modeled or estimated light emission intensity ratio (e.g., I A1 M / I B1 M and I A2 M / I B2 M ) to simultaneously minimize the merit function between t and K A The value of can be calculated.

[0057] For example, various t values ​​and K A The values ​​are used iteratively in the above formula to model the intensity ratio I A1 M / I B1 M Various values ​​of t and K can be generated, and the resulting values ​​are those that minimize the value of the merit function M1. A is inserted into the merit function M1 until it is determined. At the same time, the t value and K A The values ​​are used iteratively in the above formula to model the strength I A2 M and I B2 M Various values ​​for t and K can be generated, and the resulting values ​​are then the values ​​of M1 and M2 that minimize A are plugged into the merit function M2 until they are simultaneously determined, where the signal generated by the overlayer material A (1-f 1,2 ) / K A A part of contributes to the seed signal from outside the box to inside the box.

[0058] FIG. 5 illustrates the thermal expansion of known overlayer materials (K A)505 and the known material K A shows the measurement of a sample 500 having an unknown thickness (t) of the film layer 515 of A . The measurement sample 500 can represent the sample 400 of FIGS. 4A-4B having a box 510 with a side length of 30 μm. In one embodiment, the sample 500 can be made of the same overlay material as the sample 400 of FIGS. 4A-4B in batch processing. Since the mixing ratio and the overlay material 505 are known from prior measurements, the measured value of the film layer thickness can be calculated.

[0059] For example, the merit function for the measurement sample 500 using beam 1 is as follows.

[0060] [Number]

[0061] Measured species signal I A1 / I B1 The ratio of can be obtained from the XPS measurement of the measurement sample 500. K A And f1 are known from prior measurements (the measurements of FIGS. 4A-4B), so t can be calculated from the merit function M1.

[0062] FIG. 6 is a flowchart showing a method for characterizing a box 110 according to one embodiment. Step 600 can be executed by processing logic that can include software, hardware, or a combination thereof. For example, step 600 can be executed by the computer 205 of FIG. 2.

[0063] Referring to FIG. 6, in block 601, the processing logic obtains a first mixing ratio f1 corresponding to a first X-ray beam (beam 1). The mixing ratio represents the ratio (fraction) of the first X-ray beam within a measurement box (box 510) of a measurement wafer sample (sample 500), and the measurement box represents a bore structure disposed on a substrate and having a film layer disposed within the bore structure.

[0064] For example, a reference sample 300 with known thickness and known material Ksio as described in FIG. 3A can be used to determine a first mixing fraction f1 corresponding to a first X-ray beam (Beam 1). The mixing fraction can be calculated using merit function M1 as described above. The mixing fraction f1 can represent the portion of the X-ray beam inside a box where the X-ray beam is directed into the box, and the spillage (1-f1) represents the portion of the X-ray beam outside the box.

[0065] The measurement box (box 510) can be represented by sample 500 in Figure 5, where sample 500 is provided by a customer and has at least one bore with known dimensions of 30 μm x 30 μm, similar to reference sample 300, with known overlay material A and unknown thickness of the film layer at the bottom of the bore.

[0066] In one embodiment, in order to obtain the first mixture ratio f1 corresponding to the first X-ray beam (beam 1), a first reference detection signal (XPS signal for measuring the reference sample 300 using beam 1) for a reference sample (sample wafer having the reference sample 300) is obtained, and a first reference measurement ratio (I SiO1 / I Si1 ) and the first reference measurement ratio (I SiO1 / I Si1 ) to determine the first mixing ratio f1.

[0067] In one embodiment, obtaining a first reference detection signal (XPS signal) includes providing a reference sample (reference sample 300) with an illuminated reference box 310, where the reference box is a film layer (SiO2) with a known thickness (e.g., 2 nm) and a known contribution factor (Ksio), generating a first X-ray beam (Beam 1) under first conditions (spot size of 40 μm diameter), directing the first X-ray beam (Beam 1) at the reference sample (reference sample 300), and collecting measurements to obtain a first reference detection signal (XPS signal), where the contribution factor Ksio represents the effective contribution of SiO2 electrons to the intensity of the species in the XPS signal.

[0068] In one embodiment, the first reference measurement ratio (I SiO1 / I Si1 The determination of the first mixing ratio f1 based on the first reference measurement ratio (I SiO1 / I Si1 ) and the first modeled intensity ratio (I SiO1 M / I Si1 M ) and calculating a first blending fraction f1 based on the first reference measurement ratio and the first modeled intensity ratio.

[0069] In block 603, processing logic calculates a contribution value (1-f1) / K for the measurement box (box 510) corresponding to the first x-ray beam. A where the contribution values ​​represent the seed signals outside the measurement box that contribute to the same seed signal within the measurement box.

[0070] For example, as shown in Figures 4A-4B, the seed signal contribution value (1-f1) / K A,K A As described above, the measurement sample 400 can be calculated using the K A A sample 400 is provided by a customer to calculate a thickness of 30 μm×30 μm, where sample 400 has at least a bore structure (box 410) with known dimensions of 30 μm×30 μm, the same as reference sample 300. Additionally, the overlayer material 405 of sample 400 is unknown, and a film layer 415 within bore structure 410 has an unknown thickness of unknown material.

[0071] Using beam 1 with a 40 μm diameter spot, a measurement can be performed to collect a measured species intensities ratio for beam 1. Using beam 2 with a 50 μm diameter spot (e.g., a larger spot), a measurement can be performed to collect a measured species intensities ratio for beam 2. Using the measured species intensity ratios and the calculated mixture fractions f1 and f2, the thicknesses t and K A can be calculated simultaneously using regression. A and f1, the species signal contribution is (1-f1) / K A It can be calculated as:

[0072] In one embodiment, the processing logic further calculates a second mixture fraction f2 by obtaining a second reference detection signal for the reference sample (XPS measurement using beam 2 for reference sample 300) and calculating a second reference measurement ratio (I SiO2 / I Si2 ) and the second reference measurement ratio (I SiO2 / I Si2 ) determining a second blending proportion f2 based on

[0073] In one embodiment, obtaining a second reference detection signal (XPS signal) includes providing a reference sample (reference sample comprising sample 300) comprising an irradiated reference box 310 having a film layer with a known thickness (2 nm) and a known contribution coefficient (Ksio), generating a second X-ray beam (beam 2) having second conditions (spot diameter = 50 μm), directing the second X-ray beam (beam 2) at the reference sample, and collecting measurements to obtain the second reference detection signal (XPS signal).

[0074] In one embodiment, the second reference measurement ratio (I SiO1 / I Si1 The determination of the second mixing ratio f2 based on the second reference measurement ratio (I SiO2 / I Si2 ) and the second modeled intensity ratio (I SiO2 M / I Si2 M ) and calculate the second reference measurement ratio (I SiO2 / I Si2 ) and the second modeled intensity ratio (I SiO2 M / I Si2 M and determining a second mixing ratio f2 based on the second mixing ratio f2.

[0075] In one embodiment, the acquisition of the contribution value for the measurement box corresponding to the first X-ray beam includes acquiring a second measurement detection signal (XPS signal for sample 400 using beam 1) and a third measurement detection signal (XPS signal for sample 400 using beam 2) for the measurement sample (sample 400), and deriving a first measurement ratio (I A1 / I B1 ) and the second measurement ratio (I A2 / I B2 ) is obtained, and the contribution value (1-f1) / K is calculated based on the first and second measurement ratios. A This includes determining:

[0076] As shown in Figure 4A-B, the seed signal contribution value (1-f1) / K A ,K A can be calculated using the values ​​of f1 and f2, where t is the thickness and K A ,K A can be calculated simultaneously for sample 400 by measurements with beam 1 and measurements with beam 2 to obtain

[0077] In one embodiment, obtaining the second and third measurement detection signals includes providing a first measurement sample (wafer sample 400 in FIGS. 4A-4B) with an illuminated measurement box 410, where within the measurement box 410 is an unknown thickness and an unknown contribution factor (K A ) film layer, generating a first X-ray beam (Beam 1) under first conditions (40 μm spot), directing the first X-ray beam (Beam 1) at the measurement sample, collecting measurements to obtain the second measurement detection signal (XPS signal), generating a second X-ray beam (Beam 2) under second conditions (50 μm spot), directing the second X-ray beam (Beam 2) at the measurement sample, collecting measurements to obtain a third measurement detection signal (XPS signal).

[0078] In one embodiment, the first measurement ratio (I A1 / I B1 ) and the second measurement ratio (I A2 / I B2 ) based on the contribution value (1-f1) / K A The determination of the first measurement ratio (I A1 / I B1 ) and the second measurement ratio (I A2 / I B2 ) and the first (I A1 M / I B1M ) and the second (I A2 M / I B2 M ) to minimize the difference in the modeled strength ratios, and the contribution value (K A or (1-f1) / K A ) and the thickness value t of the film layer are determined simultaneously.

[0079] In block 605, processing logic obtains a first measurement detection signal (XPS signal) corresponding to a measurement of the measurement box (box 510) using a first X-ray beam (beam 1).

[0080] 5, a customer can provide a wafer sample having a sample 500 to be measured, the sample 500 having a known overlayer material A with an unknown film thickness. An XPS measurement can be performed on the sample 500 and an XPS signal / raw intensity (e.g., a first measured detection signal) can be obtained for the measured sample 500.

[0081] In block 607, the processing logic calculates the first measured detection signal (the XPS signal measured on sample 500 of FIG. 5 using beam 1), the contribution value (1-f1) / K A and determining a measurement value of the film layer based on the first mixing ratio f1.

[0082] For example, from the XPS signal intensity / raw intensity collected for sample 500 of FIG. 5 having known overlayer material A, the processing logic may determine a measured ratio of intensities from the XPS signals (e.g., I A / I B ) can be obtained. The above measured intensity ratio (I A / I B ),K A , and f1, the processing logic calculates the modeled intensity ratio (I A M / I B M ) can be used to calculate the thickness value t from the merit function M1.

[0083] In one embodiment, the contribution value (1-f1) / K A The measurement value (e.g., thickness t) of the film layer based on the first mixture ratio f1 is determined based on a seed signal of the first measurement detection signal (XPS signal measuring sample 500 using beam 1) by a third measurement ratio (I A / I B ), determining a first residual function M1 having the first mixing ratio f1 corresponding to the first X-ray beam (beam 1), and determining a third measurement ratio (I A / I B ) and the modeled intensity ratio (I A M / I B M ) to calculate the film layer measurement (thickness, t).

[0084] Thus, Figures 3-6 illustrate the XPS characterization technique to characterize the material composition of film layers and the thickness of film layers within a small 30 μm box (bore). Although 40 μm and 50 μm beams are illustrated, any spot size X-ray beam can be used to calculate the respective mixing percentages. Furthermore, this characterization technique can be extended to multiple film layers within the box, as further explained in Figure 7.

[0085] FIG. 7 is a partial cross-sectional view of a portion of a wafer sample 700 showing two film layers (715, 735) according to one embodiment. Sample 700 can be represented as a representation of sample 100 of FIG. 1 with a box 710 measuring 30 μm on a side, and with two film layers within the box 710. As shown in FIG. 7, the box 710 is formed in an overlay 705 of material A deposited on a substrate of material B. A thin film layer 725 of material C is deposited on the overlay 705. Within the box 700 is a film layer 715 (thickness=t1) of material A on a film layer 735 (thickness=t2) of material C, which is on a substrate 700 of material B.

[0086] To characterize box 700, the merit function can be:

[0087]

number

[0088] where M is the merit function, Mi is the merit function for the i-th beam, and I Ai M represents the modeled intensity of the seed signal A for the i-th beam, and I Bi M represents the modeled intensity of the seed signal B for the i-th beam, and I Ci M represents the modeled intensity of the seed signal C for the i-th beam, and I Ai represents the measured seed intensity of material A for the i-th beam, and I Bi represents the measured species intensity of material B for the i-th beam, and I Ci represents the measured seed intensity of material C for the i-th beam, and f i represents the i-th mixture ratio, t1 represents the thickness of the film layer of material A in box 110, and K A represents a constant representing the effective contribution of A to the intensity of the seed signal, t2 represents the thickness of the film layer of material C in box 110, and K C represents a constant that represents the effective contribution of C to the intensity of the seed signal, and λ 1,2,3,4,5 is the material parameter (effective attenuation length (EAL)) for a particular type of photoelectron from species A, B or C passing through material A or C. Note that λ can be estimated by a look-up table or from the NIST database based on the binding energy of the species signal.

[0089] The merit function above has t1, t2, and K A ,K C To solve these four unknowns, two beams of different sizes are used to obtain four separate measurement ratios I B1 / I A1 ,I C1 / I A1 ,I B2 / I A2 , and I C2 / I A2 With the four measurement ratios and four unknowns, the regression method can be applied to the merit function to solve the unknowns.

[0090] As discussed above, different beam conditions provide different blending ratios to solve the merit function, e.g., condition 1 provides a beam with a 40 μm spot diameter, condition 2 provides a beam with a 50 μm spot diameter, etc. In some embodiments, different beam positions (x or y offsets) provide different blending ratios to solve the merit function, as further described in Figures 8A-10.

[0091] FIG. 8A shows the measurement of a reference sample 800 using an X-line scan and FIG. 8B shows the measurement of a reference sample 800 using a Y-line scan according to one embodiment. The reference sample 800 can be, for example, a 30 μm box, representing the sample 300 of FIG. 3A-3B with a film layer of unknown thickness with a known film layer material SiO2 in the box 810. As shown in FIG. 8A-8B, multiple measurements with a beam 1 having a spot diameter of 40 μm can be performed on the measurement sample 800 with x and / or y offsets. The x and y offsets refer to the movement of the stage containing the sample 800 in the x or y direction. In the case of an X-scan, scans can be performed using the same stage settings, for example, at time 1 with (x1,y1)=(0,0), at time 2 with (x2,y2)=(10 μm,0), at time 3 with (x2,y2)=(20 μm,0), etc.

[0092] In one embodiment, the mixing fraction can be expressed as a Gaussian equation, assuming that the x-ray beam directed at the wafer sample is Gaussian. The characteristics of beam 1 are shown in Figures 9-10C. For example, the beam can be expressed by its center coordinates (xc, yc) relative to the center of the box 810. (σx, σy) is the one standard deviation of the Gaussian beam 1 in the x and y directions. With reference to Figures 10A-10C, the measured mixing fraction at the y,x center cross section and the modeled mixing fraction on the Gaussian are shown in plots 1000-1003. The modeled mixing fraction versus beam location is shown in plot 1005, and shows that the Gaussian equation is suitable to model the mixing fraction, as explained further below. The center of the beam does not always coincide with the center of the box (due to slight displacement errors in the stage setup), so there is a slight offset in the X / Y scan. Since these offsets are unknown, (xc, yc) can be used to optimize the alignment of the model and measured data, and (σx, σy) can be optimized as one standard deviation of an assumed Gaussian x-ray beam impinging on the sample.

[0093] 8A-10, the blending ratio can be expressed by a Gaussian equation using the stage position, e.g. (xi, yi), and the measured offsets of the beam, e.g. (xc, yc, σx, σy). The blending ratio for each scan is:

[0094]

number

[0095] Here, fi represents the ith mixing fraction for the ith beam scan, (xi, yi) represents the x, y position of the stage relative to the center of box 810, (xc, yc) represents the optimized center coordinates of the beam relative to the center of box 810, and (σx, σy) are the x, y lengths of one standard deviation of the Gaussian X-ray beam.

[0096] Each X / y measurement scan can then be described with a merit function. The merit function for sample 800 is:

[0097]

number

[0098] where M represents the merit function, Mi represents the merit function of the i-th scan, fi represents the blending fraction of the i-th scan (fi can be expressed as the stage position (xi, yi) and the beam measurement offset (xc, yc, σx, σx)), (xi, yi) represent the x and y positions of the stage relative to the center of the box 810 of the i-th scan, n represents the total number of scans, and Isi i represents the measured intensity of species Si in the i-th scan, and Isio i represents the measured intensity of seed SiO2 for the i-th scan, Ksio represents a constant representing the effective contribution of SiO2 to the intensity of the seed signal, (xc, yc) represents the optimized center coordinate of the beam relative to the center of the box 810, t represents the thickness of the film layer 815 of material SiO2 in the box 810, and (σx, σy) represents one standard deviation value in the x or y direction.

[0099] If multiple X / Y scans are performed, then for each of the i-th scans, xi, yi, and Isi i ,Isio ivalues ​​are obtained. The Ksio value is known since the sample 800 has a known SiO2 layer 805 and a SiO2 film in the box 810. The unknown variables in this case are xc, yc, t, σx, σy. That is, five measurement scans can provide five species intensity ratios to solve for the five unknown variables xc, yc, t, σx, σy, and the unknowns can be solved by applying regression techniques to the merit function M. After characterizing the beam offset, for example, after determining (xc, yc, t, σx, σy), a new measurement sample 1100 of unknown film thickness of unknown material A can be characterized as shown in Figure 11A-Figure 11B.

[0100] FIG 11A shows the measurement of a measurement sample 1100 using an X-line scan and FIG 11B shows the measurement of a measurement sample 1100 using a Y-line scan according to one embodiment. The sample 1100 may represent the reference sample 800 of FIG 8A and FIG 8B with a box 1110 having a side length of 30 μm and with an overlayer 1105 of material A. The measurement scan may be described by a merit function. The merit function may be as follows:

[0101]

number

[0102] where M represents the merit function, Mi represents the merit function of the i-th scan, and I Ai / I Bi represents the intensity ratio of the measured species for the i-th scan, and I Ai M / I Bi M represents the modeled species intensity ratio for the i-th scan, (xi, yi) represents the x and y positions of the stage relative to the center of the box 1110 for the i-th scan, and I Ai represents the measured intensity of species A in the i-th scan, and I Birepresents the measured intensity of species B for the i-th scan, (σx,σy) is the one standard deviation value in the x or y direction, (xc,yc) represents the optimized center coordinate of the beam relative to the center of the box 1110, t represents the thickness of the film layer 1115 of material A in the box 1110, and K A,B represents a constant that represents the effective contribution of A and B to the intensity of the seed signal.

[0103] In this case, the unknown variables are xc, yc, t, and K. A,B Therefore, we use regression techniques to find the four unknown variables xc, yc, t, and K. A,B Four measurement scans can provide four species intensity ratios to solve for K. Although in FIG. 11 only one film layer of unknown material with unknown thickness is characterized, the X / Y line scan characterization technique can be applied to box samples with multiple film layers with one or more unknown materials, where additional scans can be performed to characterize additional unknown parameters. Alternatively, additional measurement data can be provided from additional measurement scans to characterize K. B Other parameters such as

[0104] 12 is a flow diagram illustrating a method according to one embodiment. Process 1200 may be performed by processing logic that may include software, hardware, or a combination thereof. For example, process 1200 may be performed by computer 205 of FIG. 2.

[0105] 12, in block 1201, processing logic obtains beam Gaussian parameters (xc, yc, σx, σy), where the beam Gaussian parameters include at least offset coordinates (xc, yc) of an X-ray beam relative to a center of a box (e.g., box 1110) of a sample (e.g., box 1110), where the measurement box (e.g., box 1110) represents a bore structure having a film layer 1115 disposed inside the bore structure, the bore structure being formed on a layer 1105 fabricated on a substrate inside the bore structure.

[0106] For example, as shown in Figures 8A-8B, a wafer sample 800 is provided for characterization using X / Y line scans to obtain beam Gaussian parameters (xc, yc, σx, σy). A merit function of the sample 800 is used to solve for unknown parameters, e.g., (xc, yc, σx, σy) beam Gaussian parameters, using species intensities ratios obtained from the X / Y line scans. In one embodiment, the beam Gaussian parameters include the offset coordinates (xc, yc) of the X-ray beam relative to the center of the box.

[0107] In one embodiment, the beam Gaussian parameters include optimized standard deviation values ​​(σx, σy).

[0108] In one embodiment, the unknowns include a measured value of the thickness t of the film layer 815. In this case, additional X / Y line scans can be performed to obtain additional measured intensity ratios, such that the number of known measured intensity ratios is equal to or greater than the unknown variables to be solved for. The measured value of the thickness t and the beam Gaussian parameters can then be determined simultaneously using regression.

[0109] In block 1203, processing logic obtains a measurement detection signal (XPS signal) corresponding to a measurement of a measurement box (eg, box 1110) using an X-ray beam (beam 1).

[0110] In block 1205, processing logic determines a measurement value (thickness) of the film layer based on the measurement detection signal (XPS signal) and the scan parameters (xc, yc).

[0111] In one embodiment, the processing logic obtains additional scan parameters for stage adjustments that adjust the stage coordinates of the measurement box, obtains additional measurement detection signals corresponding to measurements at each stage adjustment, and calculates additional measurement values ​​(K) of the measurement box based on the measurement additional detection signals, the contribution values, and the scan parameters. B ) to get the

[0112] In one embodiment, processing logic performs a stage adjustment in the X or Y direction and performs a measurement scan after the stage adjustment to obtain additional measurement detection signals.

[0113] Thus, there is provided a method for characterizing a film layer in a measurement box using electron spectroscopy, the method comprising: acquiring a first mixing proportion corresponding to a first X-ray beam, where the mixing proportion represents a proportion of the first X-ray beam in a measurement box of a measurement wafer sample, the measurement box representing a bore structure disposed on a substrate and having a film layer disposed within the bore structure; acquiring a measurement box contribution value corresponding to the first X-ray beam, where the contribution value represents a seed signal outside the measurement box that contributes to a same seed signal inside the measurement box; acquiring a first measurement detection signal corresponding to a measurement of the measurement box using the first X-ray beam; and determining a measurement value of the film layer based on the first measurement detection signal, the contribution value, and the first mixing proportion.

[0114] Obtaining a first mixing ratio corresponding to the first X-ray beam includes obtaining a first reference detection signal for a reference wafer sample, obtaining a first reference measurement ratio from a seed signal of the first reference detection signal, and determining the first mixing ratio based on the first reference measurement ratio.

[0115] Obtaining the first reference detection signal includes providing a reference wafer sample having an irradiated reference box, the reference box having a film layer having a known thickness and a known contribution factor, generating a first X-ray beam having a first condition, directing the first X-ray beam at the reference wafer sample, and collecting measurements to obtain the first reference detection signal.

[0116] Determining a first mixing ratio based on the first reference measurement ratio includes determining a first residual error function having a first mixing ratio corresponding to the first X-ray beam, calculating a first reference measurement ratio and a first modeled intensity ratio, and calculating a first mixing ratio based on the first reference measurement ratio and the first modeled intensity ratio.

[0117] In addition, calculating the second mixing ratio includes obtaining a second reference detection signal for a reference wafer sample, obtaining a second reference measurement ratio from a seed signal of the second reference detection signal, and determining the second mixing ratio based on the second reference measurement ratio.

[0118] Obtaining the second reference detection signal includes providing a reference wafer sample with an irradiated reference box, the reference box having a film layer with a known thickness and a known contribution coefficient, generating a second X-ray beam having second conditions, directing the second X-ray beam at the reference wafer sample, and collecting measurements to obtain a second reference detection signal.

[0119] Determining the second mixing ratio based on the second reference measurement ratio further includes determining a second residual function having a second mixing ratio corresponding to the second X-ray beam, calculating a second reference measurement ratio and a second modeled intensity ratio, and calculating the second mixing ratio based on the second reference measurement ratio and the second modeled intensity ratio.

[0120] Obtaining a contribution value for the measurement box corresponding to the first X-ray beam includes obtaining second and third measurement detection signals for the measurement wafer sample, obtaining first and second measurement ratios from seed signals of the second and third measurement detection signals, and determining a contribution value based on the first and second measurement ratios.

[0121] Obtaining the second and third measurement detection signals includes preparing a measurement wafer sample with an irradiated measurement box, the measurement box having a film layer of unknown thickness and unknown contribution coefficient, generating a first X-ray beam having a first condition, directing the first X-ray beam at the measurement wafer sample, collecting measurement values ​​to obtain a second measurement detection signal, generating a second X-ray beam having a second condition, directing the second X-ray beam at the measurement wafer sample, collecting measurement values ​​to obtain a third measurement detection signal.

[0122] Determining a contribution value based on the first and second measurement ratios includes determining a first residual function having a first mixing ratio corresponding to a first X-ray beam, determining a second residual function having a second mixing ratio corresponding to a second X-ray beam, and performing a regression on the first and second residual functions to minimize a difference between the first and second measurement ratios and a modeled intensity ratio to simultaneously determine the contribution value and a thickness value of the film layer.

[0123] Determining a measurement value of the film layer based on the contribution value and the first mixing ratio includes determining a third measurement ratio based on a seed signal of the first measurement detection signal, determining a first residual function having a first mixing ratio corresponding to the first X-ray beam, and calculating the measurement value of the film layer by minimizing a difference between a third measurement ratio and a modeled intensity ratio for the first residual function.

[0124] In some embodiments, a system is provided for characterizing a film layer within a measurement box, the system comprising: a stage for supporting a measurement wafer sample; an X-ray source for generating a first X-ray beam to irradiate the measurement wafer sample over at least a region of the measurement wafer sample having a measurement box, the measurement wafer sample including a first layer of a first material disposed on a substrate made from a substrate material, the first layer having a bore structure formed therein, thereby forming a wall of the measurement box, and a first film layer of a first material disposed within the bore structure; an electron analyzer for splitting electrons emitted from the measurement wafer sample according to different electron energies; an electron detector for detecting the electrons after passing through the electron analyzer and outputting a detection signal; the measurement signal is received by a first detector, and a processor for receiving the detection signal and determining, based on the detection signal, a seed signal of an energy band corresponding to electrons emitted from a first material and a substrate material, the processor further performing the operations of: acquiring a first mixing proportion corresponding to a first X-ray beam, the mixing proportion representing a proportion of the first X-ray beam within a measurement box of the measurement wafer sample; acquiring a contribution value for the measurement box corresponding to the first X-ray beam, the contribution value representing a seed signal outside the measurement box that contributes to the same seed signal in the measurement box; acquiring a first measurement detection signal corresponding to a measurement in the measurement box using the first X-ray beam; and determining a measurement value of the film layer based on the first measurement detection signal, the contribution value, and the first mixing proportion.

[0125] Obtaining a first mixing ratio corresponding to the first X-ray beam includes obtaining a first reference detection signal for a reference wafer sample, obtaining a first reference measurement ratio from a seed signal of the first reference detection signal, and determining the first mixing ratio based on the first reference measurement ratio.

[0126] Obtaining the first reference detection signal includes providing a reference wafer sample with an irradiated reference box, the reference box having a film layer with a known thickness and a known contribution coefficient, generating a first X-ray beam having a first condition, directing the first X-ray beam at the reference wafer sample, and collecting measurements to obtain a first reference detection signal.

[0127] Determining a first mixing ratio based on the first reference measurement ratio includes determining a first residual function having a first mixing ratio corresponding to the first X-ray beam, calculating a first reference measurement ratio and a first modeled intensity ratio, and calculating the first mixing ratio based on the first reference measurement ratio and the first modeled intensity ratio.

[0128] The operations further include calculating a second mixing ratio, which includes obtaining a second reference detection signal for a reference wafer sample, obtaining a second reference measurement ratio from a seed signal of the second reference detection signal, and determining a second mixing ratio based on the second reference measurement ratio.

[0129] Obtaining the second reference detection signal includes providing a reference wafer sample with a reference box to be irradiated, the reference box having a film layer with a known thickness and a known contribution coefficient, generating a second X-ray beam having second conditions, directing the second X-ray beam at the reference wafer sample, and collecting measurements to obtain the second reference detection signal.

[0130] Also provided is a method for characterizing a film layer in a measurement box using electron spectroscopy, the method comprising obtaining beam Gaussian parameters corresponding to an X-ray beam, the beam Gaussian parameters including at least an offset coordinate of the X-ray beam relative to a center of a measurement box of a measurement wafer sample, the measurement box representing a bore structure disposed on a substrate having a film layer disposed within the bore structure, obtaining a measurement detection signal corresponding to a measurement of the measurement box using the X-ray beam, and determining a measurement value of the film layer based on the measurement detection signal and the beam Gaussian parameters.

[0131] Further, additional scan parameters for stage adjustments that adjust the stage coordinates for the measurement box are obtained, additional measurement detection signals corresponding to measurements at each stage adjustment are obtained, and additional measurement values ​​of the measurement box are determined based on the measurement additional detection signals, the contribution values, and the scan parameters.

[0132] In addition, a stage adjustment is performed in the X direction or the Y direction, and a measurement scan is performed after the stage adjustment to obtain an additional measurement detection signal.

[0133] An embodiment of the disclosure includes a method for characterizing a film layer in a measurement box (small box) using electron spectroscopy, the method comprising: obtaining a first mixing ratio corresponding to a first X-ray beam, the mixing ratio representing a ratio of the first X-ray beam in the measurement box of a sample, the measurement box representing a film layer disposed on a bore structure and a substrate; obtaining a contribution value for the measurement box corresponding to the first X-ray beam, the contribution value representing a seed signal outside the measurement box that contributes to the same seed signal in the measurement box; obtaining a first measurement detection signal corresponding to a measurement in the measurement box using the first X-ray beam; and determining a measurement value of the film layer based on the first measurement detection signal, the contribution value, and the first mixing ratio. The film layer may be disposed between bore structures or may be disposed inside the bore structure. Reference to a film layer in a bore structure should also apply mutatis mutandis to a film layer located below a bore structure.

[0134] In a further aspect, a system is provided for characterizing a film layer in a measurement box using electron spectroscopy, the system comprising: a stage for supporting a wafer sample; an X-ray source for generating an X-ray beam that irradiates the wafer sample over at least a region of the wafer sample with a measurement box, the wafer sample including a first layer of a first material disposed on a substrate made of a substrate material, the first layer having a bore structure formed therein, thereby forming a wall of the measurement box, and a first film layer of a first material disposed within the bore structure; an electron analyzer for splitting electrons emitted from the wafer sample according to different electron energies; an electron detector for detecting the electrons after passing through the electron analyzer and outputting a detection signal; and a detector for receiving the detection signal and, based on the detection signal, determining whether the electrons are in a predetermined range or not. The system includes a processor for determining a seed signal of an energy band corresponding to electrons emitted from a first material and a substrate material, the processor further performing the operations of obtaining a first mixing ratio corresponding to the first X-ray beam, the mixing ratio representing a ratio of the first X-ray beam within a measurement box of the wafer sample, obtaining a measurement box contribution value corresponding to the first X-ray beam, the contribution value representing a seed signal outside the measurement box that contributes to the same seed signal in the measurement box, obtaining a first measurement detection signal corresponding to a measurement in the measurement box using the first X-ray beam, and determining a measurement value of the film layer based on the first measurement detection signal, the contribution value, and the first mixing ratio.

[0135] In a further aspect, a method is provided for characterizing a film layer within a measurement box using electron spectroscopy, the method comprising obtaining beam Gaussian parameters corresponding to an X-ray beam, the beam Gaussian parameters including at least an offset coordinate of the X-ray beam relative to a center of a measurement box of a sample, the measurement box representing a bore structure within which a film layer is disposed, obtaining a measurement detection signal corresponding to a measurement of the measurement box using the X-ray beam, and determining a measurement value of the film layer based on the measurement detection signal and the beam Gaussian parameters.

[0136] A system for characterizing a first film layer of a sample is provided that includes electron optics and a processor. Figure 2 illustrates a non-limiting example of such a system, where the processor can be or can be included in a computer 205, and the electron optics can include at least some of, for example, an electron gun 210, an anode 215, a monochromator 220, a flux detector 230, an XPS energy analyzer 240, and an XPS detector 245.

[0137] The electron optics is configured to irradiate an X-ray spot onto a first sample area (e.g., measurement box 110 in FIG. 1 ) and onto first sample sub-areas (which are irradiated but located on the sides of the measurement box) comprising a first film layer, said first film layer being made of a first film layer material and being arranged on a substrate made of a substrate material.

[0138] The electron-optics system is also configured to detect electrons emitted from the first sample region to provide a detection signal.

[0139] The processor can be configured to determine species signals based on the detection signals, the species signals including: (i) a first film layer material species signal in an energy band corresponding to electrons emitted from the first film layer material, and (ii) a substrate material species signal in an energy band corresponding to electrons emitted from the substrate material.

[0140] The processor may also be configured to determine a measurement value of the first film layer based on (i) the seed signals, (ii) mixing information (e.g., f) indicative of the proportion of the X-ray spot that is incident on the first film layer, and (ii) a first film layer material contribution value (e.g., Ksio) representing the effective contribution of the first film layer material to at least one of the seed signals.

[0141] The detection signal may be an X-ray photoelectron spectroscopy (XPS) detection signal.

[0142] The measurement may be a thickness of a film layer. The material(s) of the film layer may be determined based on the frequency band(s) of the species signals.

[0143] The processor is configured to determine a thickness of the film layer based on a value of a merit function (e.g., M), the value of the merit function being determined based on a difference between an actual attenuation of the film layer and a modeled attenuation of the film layer. The actual attenuation of the film layer can be expressed by Isio / Isi, while the modeled attenuation of the film layer can be expressed by Isio / Isi. M / Isi M Various examples of merit functions are given above.

[0144] The processor can be configured to determine the thickness of the film layer based on a value of a merit function, the value of the merit function being a function of (i) a first film layer material species signal (e.g., Isio), (ii) a substrate material species signal (e.g., Isi), (iii) a modeled first film layer material species signal (e.g., Isio), M ) and (iv) modeled substrate material species signals (e.g., Isi M ) is determined based on

[0145] A modeled first film layer material species signal can be calculated based on the mixing information, a first film layer attenuation parameter (e.g., λsio) associated with photoelectrons generated within the first film layer, the film layer thickness, and the first film layer material contribution value.

[0146] A substrate material seed signal is calculated based on the mixing information, the film layer thickness, a first film layer attenuation parameter (e.g., λsi, sio) associated with photoelectrons generated within the substrate, and a substrate material contribution value (Ksi) representing the effective contribution of the substrate material to at least one of the seed signals.

[0147] The mixed information may indicate a beam intensity distribution associated with one or more film layers. Thus, the mixed information may indicate a beam intensity distribution above one or more film layers, for example the proportion of radiation incident on the measurement box relative to the total radiation.

[0148] The mixture information may include one or more beam Gaussian parameters, examples of which are given above.

[0149] The film layer may be disposed above the top surface of additional sample sub-regions, see for example pad of interest 1610 disposed above substrate 1620 in Figure 16. The X-ray spot 1620 irradiates the pad of interest 1610 and a first sample sub-region, also called an irrelevant region or contaminating region, which results in a bleed-through signal in the signal sensed by the detector.

[0150] The film layer may be located below the top surface of the additional sample sub-area, see, for example, Figures 1 and 7.

[0151] The sample area may include a second film layer located outside the first sample sub-area, made from a second film layer material. For example, referring to Figure 7, two film layers 715 and 735 are shown, where the second film layer is designated by the numeral 715.

[0152] In this case, the processor is further configured to determine a second film layer material species signal in an energy band corresponding to electrons emitted from the second film layer material based on the detection signal, and the processor is also configured to determine a measurement value of the second film layer based on (i) the species signal, (ii) the mixture information, and (ii) a second film layer material contribution value representing an effective contribution of the second film layer material to at least one of the species signals.

[0153] When there are two film layers, more information may need to be collected since there are more unknown variables associated with the two film layers. In this case, the electron optics may need to perform one or more additional measurements including irradiating a second sample area, including a second film layer and a second sample sub-area, with an X-ray spot and detecting electrons emitted from the second sample area to provide a detection signal. Examples of additional measurements are shown in Figures 8A and 8B.

[0154] 13 is a flow diagram illustrating a method according to one embodiment. The method 1300 is performed by processing logic that may include software, hardware, or a combination thereof. For example, the method 1300 may be performed by the computer 205 of FIG. 2.

[0155] The method 1300 starts in step 1310 by irradiating a first sample area, including a first film layer and a first sample sub-area, with an X-ray spot by an electron optics system. The first film layer is made from a first film layer material and is disposed on a substrate made from a substrate material.

[0156] Step 1310 is followed by step 1320, in which electron optics detects electrons emitted from the first sample region to provide a detection signal.

[0157] Step 1320 is followed by step 1330, in which a processor determines a seed signal based on the detection signal, the seed signal including (i) a first film layer material species signal in an energy band corresponding to electrons emitted from the first film layer material, and (ii) a substrate material species signal in an energy band corresponding to electrons emitted from the substrate material.

[0158] Step 1330 is followed by step 1340, in which the processor determines a measurement value of the first film layer based on (i) the seed signal, (ii) mixing information (e.g., f) indicative of the proportion of the X-ray spot incident on the first film layer, and (ii) a first film layer material contribution value (e.g., Ksio) representing the effective contribution of the first film layer material to at least one of the seed signals.

[0159] The detection signal may be an X-ray Photoelectron Spectroscopy (XPS) detection signal.

[0160] The measurement may be a thickness of a film layer, the material of which may be determined based on a frequency band of the seed signal.

[0161] Step 1340 may include at least one of the following: a. Determine the thickness of the film layer based on a value of a merit function (e.g., M). The value of the merit function is determined based on the difference between the actual attenuation of the film layer and the modeled attenuation of the film layer. The actual attenuation of the film layer can be expressed by Isio / Isi, while the modeled attenuation of the film layer can be expressed by Isio / Isi. M / Isi M Various examples of merit functions are given above. b. Determine the thickness of the film layer based on a value of a merit function. The value of the merit function is a function of (i) a first film layer material species signal (e.g., Isio), (ii) a substrate material species signal (e.g., Isi), and (iii) a modeled first film layer material species signal (e.g., Isio). M ) and (iv) modeled substrate material species signals (e.g., IsiM ) is determined based on c. Calculating the modeled first film layer material species signal based on the mixing information, a first film layer attenuation parameter (e.g., λsio) associated with photoelectrons generated in the first film layer, a film layer thickness, and a first film layer material contribution value. d. Calculating the substrate material seed signal based on the mixing information, a film layer thickness, a first film layer attenuation parameter (e.g., λsi,sio) associated with photoelectrons generated in the substrate, and a substrate material contribution value (e.g., Ksi) representing an effective contribution of the substrate material to at least one of the seed signals.

[0162] The sample area may include a second film layer made from a second film layer material and positioned outside the first sample sub-area. For example, referring to Figure 7, two film layers 715 and 735 are shown, where the second film layer is designated by the numeral 715.

[0163] In this case, step 1340 may include determining a second film layer material species signal in an energy band corresponding to electrons emitted from the second film layer material based on the detection signal. The processor is also configured to determine a measurement of the second film layer based on (i) the species signal, (ii) the mixture information, and (ii) a second film layer material contribution value representing an effective contribution of the second film layer material to at least one of the species signals.

[0164] If there are two film layers, more information may need to be gathered since there are more unknown variables associated with the two film layers. In this case, one or more additional measurements may need to be performed. Step 1310 may be repeated and may include illuminating, by the electron optics system, a second sample area including the second film layer and the second sample sub-area with an X-ray spot. Step 1320 may be repeated and may include detecting electrons emitted from the second sample area to provide a detection signal.

[0165] 14 is a flow diagram illustrating a method 1400 according to one embodiment. The method 1400 may be performed by processing logic including software, hardware, or a combination thereof. For example, the method 1400 may be performed by the computer 205 of FIG. 2.

[0166] The method 1300 starts at step 1410 by obtaining a detection signal indicative of electrons emitted from a first sample area as a result of irradiation by an x-ray spot, the first sample area being comprised of a first film layer and a first sample sub-area, the first film layer being made of a first film layer material and being disposed on a substrate made of a substrate material.

[0167] Step 1410 is followed by step 1320, where electron optics detects electrons emitted from the first sample region to provide a detection signal.

[0168] Step 1320 is followed by step 1330, in which a processor determines a seed signal based on the detection signal, the seed signal including (i) a first film layer material species signal in an energy band corresponding to electrons emitted from the first film layer material, and (ii) a substrate material species signal in an energy band corresponding to electrons emitted from the substrate material.

[0169] Step 1330 is followed by step 1340, in which the processor determines a measurement value of the first film layer based on (i) the seed signal, (ii) mixing information (e.g., f) indicative of the proportion of the X-ray spot incident on the first film layer, and (ii) a first film layer material contribution value (e.g., Ksio) representing the effective contribution of the first film layer material to at least one of the seed signals.

[0170] The detection signal may be an X-ray Photoelectron Spectroscopy (XPS) detection signal.

[0171] The measurement may be a thickness of a film layer, the material of which may be determined based on a frequency band of the seed signal.

[0172] The sample area may include a second film layer made from a second film layer material and positioned outside the first sample sub-area. For example, referring to Figure 7, two film layers 715 and 735 are shown, where the second film layer is designated by the numeral 715.

[0173] In this case, step 1340 may include determining a second film layer material species signal in an energy band corresponding to electrons emitted from the second film layer material based on the detection signal. The processor is also configured to determine a measurement of the second film layer based on (i) the species signal, (ii) the mixture information, and (ii) a second film layer material contribution value representing an effective contribution of the second film layer material to at least one of the species signals.

[0174] When there are two film layers, more information may need to be collected since there are more unknown variables related to the two film layers.

[0175] Step 1410 may be repeated, including obtaining a detection signal indicative of electrons emitted from a second sample area as a result of irradiating the first sample area with the X-ray spot, the second sample area being comprised of a second film layer and a second sample sub-area, the second film layer being made from a second film layer material and being disposed above a substrate made from a substrate material.

[0176] Step 1320 may be repeated and may include detecting electrons emitted from the second sample volume to provide a detection signal.

[0177] The detected signal can be considered to be a weighted sum of a signal of interest (S) from the film layer or layers and a signal from the spill region (area irradiated by the x-ray beam but outside the film layer or layers) (C) (also called the spillage signal). The weight assigned to signal S is f and the weight assigned to signal C is 1-f.

[0178] The values ​​of f and C or f and S need to be determined.

[0179] The bleed-through signal can be determined by knowledge of the semiconductor process provided by the manufacturer or by measuring an area larger than the XPS spot size, where the unpatterned parts of the die may be located. Another way to determine the bleed-through signal is to scan the measurement area in a systematic way, allowing the known amount of bleed-through to vary in the measurement data. See for example Figures 8A and 8. The more the spot covers the contaminated area, the more the bleed-through signal increases, while the signal of interest decreases. This information can be used to determine the contamination signal by taking multiple points at different offsets from the center of the measurement pad. An additional way to determine the bleed-through signal is to extrapolate the scan data to determine the signal in the case of zero bleed-through.

[0180] There are several ways to determine the coefficients mentioned above. One is to float the coefficients in the regression routine. Another is to fully characterize the power density throughout the XPS spot, which may not be stable over time.

[0181] Another method is to determine the spill rate using a well-characterized reference wafer sample, see for example Figure 5.

[0182] Yet another aspect of determining the weights can include feed-forward, where the structural element is measured before the formation of the film layer and after the formation of the film layer, and the detection signal after the formation is compared with the detection signal after the formation, thereby providing an indication of the influence of the film layer on the detection signal, which in turn can provide an indication of the measurement value of the film layer. If C is the same before and after the formation, it can be determined and removed from the detection signal.

[0183] The pre-formation detection signal may be used to normalize the post-formation detection signal since the pre-formation detection signal contains information about layers below the film layer.

[0184] Carrying out pre- and post-formation measurements can provide a very high accuracy assessment of the measurements, overcoming inaccuracies in the formation of the structural elements, differences between evaluation systems and even deviations of the measurements over time.

[0185] FIG. 15 illustrates an example method 1500 for characterizing a first film layer of a sample.

[0186] The method 1500 starts at step 1510 by irradiating a preliminary first sample area (which is the first sample area prior to forming a first film layer within the first sample area) with an X-ray spot. The preliminary first sample area may include a substrate and an additional structural element. The substrate is made of a substrate material.

[0187] Step 1510 is followed by step 1520, which detects electrons emitted from the preliminary first sample region to provide a preliminary detection signal.

[0188] Step 1520 is followed by step 1530 of determining, by a processor, a preliminary species signal based on the detection signal. The preliminary species signal may include a preliminary substrate material species signal in an energy band corresponding to electrons emitted from the substrate material.

[0189] The method may resume after forming a first sample area that includes a film layer (step 1540).

[0190] Step 1540 includes irradiating a first sample area (here including a first film layer and a first sample sub-area) with an X-ray spot. The first film layer is made from a first film layer material and is disposed over a substrate.

[0191] Step 1540 is followed by step 1550, which detects electrons emitted from the first sample region to provide a detection signal.

[0192] Step 1550 is followed by step 1560 of determining, by a processor, seed signals based on the detection signals, the seed signals including (i) a first film layer material species signal in an energy band corresponding to electrons emitted from the first film layer material, and (ii) a substrate material species signal in an energy band corresponding to electrons emitted from a substrate material.

[0193] A processor determines a measurement value of the first film layer based on the preliminary seed signal of step 1530 and the seed signal of step 1560. The determining includes determining an influence of the film layer based on a difference between the preliminary seed signal and the seed signal, and determining a measurement value based on the difference. This may include, for example, using variables such as a material contribution value of the first film layer and / or using any of the models described above. For example, the formula I=1 / k(1-e -t / σ ) to determine the thickness, where K is the standard k factor for generating a photoelectron of a given species from a particular material, t is the layer thickness, and σ is the effective attenuation length of the material. It is assumed that k and σ are known.

[0194] In another embodiment, the film layer measurements can be determined using an effective material model, where the effluent signal is modeled as an effective substrate material. The effective substrate material is used as a variable in a modeled intensity equation, and the method includes solving the modeled intensity equation. An example of the modeled intensity equation is shown below.

[0195] In standard XPS film analysis, the thickness of the sample is I = 1 / k(1-e -t / σ ), where K is the standard k-factor for generating a photoelectron of a given species from a particular material, t is the layer thickness, and σ is the effective attenuation length for the material.

[0196] The above modeled intensity equation may be I=1 / k', where the k' factor for each species of interest is assumed to arise from a bulk substrate instead, and would be floated during a regression.

[0197] The value of k' can be determined by irradiating the structural element of interest with x-ray spots of different radii. X-ray spots of different radii cover the entire film layer, but need to cover different areas of the effusion area. Although Figures 4A and 4B show two x-ray spots with different radii, it may be beneficial in determining k' for each of the first and second x-ray spots to cover the entire film layer.

[0198] FIG. 17 illustrates an example method 1700 for characterizing a first film layer of a sample.

[0199] The method 1700 starts at step 1710 by irradiating a first sample area, including a first film layer and a first sample subarea, with a first x-ray spot of a first radius by an electron-optical system. The first film layer is made from a first film layer material and is disposed on a substrate made from a substrate material.

[0200] Step 1710 is followed by step 1720, detecting electrons emitted from the first sample region by electron-optics to provide a first detection signal.

[0201] Step 1720 is followed by step 1730 of determining, by a processor, first species signals based on the first detection signals, the first species signals including (i) a first film layer material species signal in an energy band corresponding to electrons emitted from the first film layer material, and (ii) a substrate material species signal in an energy band corresponding to electrons emitted from the substrate material.

[0202] Step 1730 is followed by step 1740, in which the electron-optics system irradiates the first sample area, including the first film layer and the first sample sub-area, with a second x-ray spot of a second radius different than the first radius.

[0203] Step 1740 is followed by step 1750, where electron-optics detects electrons emitted from the first sample region to provide a second detection signal.

[0204] Step 1750 is followed by step 1760 of determining, by the processor, a second species signal based on the second detection signal, the first species signal including (i) a first film layer material species signal in an energy band corresponding to electrons emitted from the first film layer material, and (ii) a substrate material species signal in an energy band corresponding to electrons emitted from the substrate material.

[0205] Step 1760 is followed by step 1770 of determining, by a processor, a measurement of the first film layer based on the first seed signal and the second seed signal.

[0206] Figure 18 shows the simulation of material (film layer) thickness as a function of k' factor for several sizes of beam and pad size. Simulations of SiO film thickness are provided as a function of 1 / k' for three XPS measurements.

[0207] In standard film analysis, 1 / k' is known to be ~0.7, which is used as the input to determine the SiO film thickness. If k is allowed to vary, the solution becomes underdetermined.

[0208] The curves VFIV, f = 0.57 (line 1801) and VFIII, f = 7.05 (line 1802) show the effect on a 30 μm measurement pad with 50 μm and 40 μm spots, respectively, where f is the fraction of the beam in the measurement pad. The effective material model uniquely defines a solution using two beam sizes with different amounts of contamination. The intersection of these curves is the unique solution for k and therefore thickness. The curve VFIII, f = 0.97 (line 1803) shows the relationship between k and film thickness for a 50 μm beam on a 50 μm measurement pad, the lower the spillover, the less sensitive to k'. These curves are merely used as descriptive tools, since the algorithm uses regression to determine the k value for each species of interest.

[0209] A non-transitory computer readable medium for characterizing a first film layer of a sample can be provided, the non-transitory computer readable medium storing instructions that, when executed by a computerized system, cause the computerized system to perform the steps of method 1700.

[0210] A non-transitory computer readable medium for characterizing a first film layer of a sample can be provided, the non-transitory computer readable medium storing instructions that, when executed by a computerized system, cause the computerized system to perform the steps of method 1500.

[0211] A non-transitory computer readable medium for characterizing a first film layer of a sample can be provided, the non-transitory computer readable medium storing instructions that, when executed by a computerized system, cause the computerized system to perform the steps of method 1400.

[0212] A non-transitory computer readable medium for characterizing a first film layer of a sample can be provided, the non-transitory computer readable medium storing instructions that, when executed by a computerized system, cause the computerized system to perform the steps of method 1300.

[0213] A system for characterizing a first film layer of a sample can be configured to perform the method 1300.

[0214] A system for characterizing a first film layer of a sample can be configured to perform the method 1400.

[0215] A system for characterizing a first film layer of a sample can be configured to perform the method 1500.

[0216] A system for characterizing a first film layer of a sample can be configured to perform the method 1700.

[0217] Any arrangement of components to achieve the same functionality is substantially "associated" such that the desired functionality is achieved. Thus, for purposes of this specification, any two components that are combined to achieve a particular functionality may be considered to be "associated" with one another such that the desired functionality is achieved, regardless of architecture or intervening components. Similarly, any two components so associated may also be considered to be "operably connected" or "operably coupled" with one another to achieve the desired functionality.

[0218] Moreover, those skilled in the art will recognize that the boundaries between operations described above are merely illustrative. Multiple operations may be combined into a single operation, a single operation may be distributed among additional operations, and operations may be performed with at least partial overlap in time. Moreover, alternative embodiments may include multiple instances of an operation, and the order of operations may be altered in various other embodiments.

[0219] Also for example, in one embodiment, the illustrated embodiments may be implemented as circuits collocated on a single integrated circuit or within the same device, or the illustrated embodiments may be implemented as any number of separate integrated circuits or separate devices interconnected with each other in any suitable manner.

[0220] Also, for example, embodiments or portions thereof may be implemented as a soft or coded representation of a physical circuit, or a logical representation that can be converted into a physical circuit, such as in any suitable type of hardware description language.

[0221] However, other modifications, variations, and alternatives are possible. Accordingly, the specification and drawings are to be regarded as illustrative rather than restrictive.

[0222] In the claims, any reference signs placed between parentheses shall not be construed as limiting the claim. The word "comprising" does not exclude the presence of other elements or steps than those stated in the claim. Furthermore, as used in this specification, the singular terms "a" or "an" are defined as one or more. Moreover, the use of introductory phrases such as "at least one" and "one or more" in a claim should not be construed as implying that the introduction of an element of another claim by an indefinite article ("a" or "an") limits a particular claim containing such introduced claim element to an invention containing only one such element, even if the same claim also contains the introductory phrases "one or more" or "at least one" and an indefinite article such as "a" or "an". The same applies to the use of definite articles. Unless otherwise stated, terms such as "first" and "second" are used arbitrarily to distinguish between the elements which such terms describe. Thus, these terms are not necessarily intended to indicate a temporal or other priority of such elements. The mere fact that certain measures are recited in mutually different claims does not indicate that a combination of these measures cannot be used to advantage.

[0223] While certain features of the invention have been illustrated and described in this specification, many modifications, substitutions, changes, and equivalents will occur to those skilled in the art. It is therefore to be understood that the appended claims are intended to cover all such modifications and changes as fall within the true spirit of the invention.

[0224] Any reference to the terms "including," "comprising," or "having" may be applied mutatis mutandis to the terms "consisting" and / or "consisting essentially of."

[0225] It should be understood that the processes and techniques described herein are not inherently related to any particular apparatus and can be implemented by any suitable combination of components. Moreover, various types of general purpose apparatus can be used in accordance with the teachings described herein. While this disclosure has been described with reference to specific embodiments, these embodiments are intended in all respects to be illustrative and not restrictive. Those skilled in the art will recognize that many different combinations will be suitable for practicing this disclosure.

[0226] Additionally, other embodiments of this disclosure will be apparent to those skilled in the art from consideration of the specification and embodiments of this disclosure disclosed herein. It should be noted that the representations disclosed herein are provided as examples for the specific geometries of the patterned layers as shown in the disclosed examples. Various aspects and / or components of the described embodiments may be used alone or in any combination. It is intended that the specification and examples be considered as exemplary only, with the true scope and spirit of this disclosure being indicated by the following claims.

Claims

1. 1. A system for characterizing a first film layer of a sample, comprising: Equipped with an electron optical system and a processor, The electron optical system is irradiating a first sample area with an X-ray spot, the first sample area comprising a first film layer and a first sample sub-area, the first film layer being made from a first film layer material and disposed on a substrate made from a substrate material; configured to detect electrons emitted from the first sample volume to provide a detection signal; The processor: determining a species signal based on the detection signal, the species signal including (i) a first film layer material species signal at an energy band corresponding to electrons emitted from the first film layer material, and (ii) a substrate material species signal at an energy band corresponding to electrons emitted from the substrate material; determining a measurement of the first film layer based on (i) the seed signals, (ii) mixing information indicative of a proportion of the x-ray spot incident on the first film layer, and (ii) a first film layer material contribution value indicative of an effective contribution of the first film layer material to at least one of the seed signals; system.

2. 2. The system of claim 1, wherein the detection signal is an X-ray Photoelectron Spectroscopy (XPS) detection signal.

3. 2. The system of claim 1, wherein the detection signal is an X-ray Photoelectron Spectroscopy (XPS) detection signal.

4. The system of claim 1 , wherein the measurement is a thickness of the film layer.

5. 5. The system of claim 4, wherein the processor is configured to determine the thickness of the film layer based on a value of a merit function, the value of the merit function being determined based on a difference between an actual attenuation of the film layer and a modeled attenuation of the film layer.

6. 5. The system of claim 4, wherein the processor is configured to determine the thickness of the film layer based on a value of a merit function, the value of the merit function being determined based on (i) the first film layer material species signal, (ii) the substrate material species signal, (iii) a modeled first film layer material species signal, and (iv) a modeled substrate material species signal.

7. 7. The system of claim 6, wherein the modeled first film layer material type signal is calculated based on the mixing information, a first film layer attenuation parameter associated with photoelectrons generated within the first film layer, a thickness of the film layer, and the first film layer material contribution value.

8. 8. The system of claim 7, wherein the substrate material species signal is calculated based on the mixing information, the film layer thickness, a first film layer attenuation parameter associated with photoelectrons generated within the substrate, and a substrate material contribution value representing an effective contribution of the substrate material to at least one of the species signals.

9. 2. The system of claim 1, wherein the mixture information is indicative of a beam intensity distribution for one or more film layers.

10. The system of claim 1 , wherein the mixture information comprises one or more beam Gaussian parameters.

11. The system of claim 1 , wherein the film layer is disposed on a top surface of the additional sample subarea.

12. The system of claim 1 , wherein the film layer is disposed below a top surface of the additional sample subarea.

13. the sample area comprises a second film layer made from a second film layer material and positioned outside the first sample sub-area; The processor, determining a second film layer material type signal in an energy band corresponding to electrons emitted from the second film layer material based on the detection signal; and determining a measurement of the second film layer based on (i) the seed signals, (ii) the mixing information, and (ii) a second film layer material contribution value representative of an effective contribution of the second film layer material to at least one of the seed signals. The system of claim 1 .

14. The electron optical system is irradiating a second sample area, the second sample area comprising the second film layer and a second sample sub-area, with the x-ray spot; further configured to detect electrons emitted from the second sample volume to provide a detection signal. The system of claim 13.

15. 1. A method for characterizing a first film layer of a sample, comprising: using an X-ray spot to irradiate a first sample area including a first film layer and a second sample sub-area, the first film layer being made from a first film layer material and disposed on a substrate made from a substrate material; detecting electrons emitted from the first sample volume to provide a detection signal; determining, by a processor, a species signal based on the detection signal, the species signal including (i) a first film layer material species signal at an energy band corresponding to electrons emitted from a first film layer material, and (ii) a substrate material species signal at an energy band corresponding to electrons emitted from the substrate material; determining, by a processor, a measurement of the first film layer based on (i) the seed signals, (ii) blending information indicative of a fraction of the x-ray spot incident on the first film layer, and (iii) a first film layer material contribution value indicative of an effective contribution of the first film layer material to at least one of the seed signals; method.

16. 1. A non-transitory computer readable medium for characterizing a first film layer of a sample, comprising: The non-transitory computer-readable medium, when executed by a computerized system, irradiating a first sample area including a first film layer and a first sample sub-area with an X-ray spot, the first film layer being made from a first film layer material and disposed on a substrate made from a substrate material; detecting electrons emitted from the first sample volume to provide a detection signal; determining, by a processor, species signals based on the detection signals, the species signals including (i) a first film layer material species signal at an energy band corresponding to electrons emitted from the first film layer material, and (ii) a substrate material species signal at an energy band corresponding to electrons emitted from the substrate material; determining, by a processor, a measurement value of the first film layer based on (i) the seed signals, (ii) blending information indicative of a fraction of the x-ray spot incident on the first film layer, and (ii) a first film layer material contribution value indicative of an effective contribution of the first film layer material to at least one of the seed signals; storing instructions for causing the computerized system to carry out a process; Medium.

17. 1. A method for characterizing a first film layer of a sample, comprising: obtaining a detection signal indicative of electrons emitted from a first sample area as a result of irradiating the first sample area with an X-ray spot, the first sample area including a first film layer and a first sample sub-area, the first film layer being made from a first film layer material and disposed on a substrate made from a substrate material; determining, by a processor, species signals based on the detection signals, the species signals including (i) a first film layer material species signal at an energy band corresponding to electrons emitted from the first film layer material, and (ii) a substrate material species signal at an energy band corresponding to electrons emitted from the substrate material; determining, by the processor, a measurement of the first film layer based on (i) the seed signals, (ii) blending information indicative of a fraction of the x-ray spot incident on the first film layer, and (ii) a first film layer material contribution value indicative of an effective contribution of the first film layer material to at least one of the seed signals; method.

Citation Information

Patent Citations

  • Pretreatment method for measuring thickness of organic membrane and polymeric membrane

    CN1470849A

  • Device and method for x-ray photoelectron spectroscopy

    JP2001153826A

  • X-ray photoelectron analyzer

    JP2001201470A

  • Inspection method and inspection apparatus

    JP2008164617A

  • Film thickness measuring system, film thickness measuring method, and program

    JP2021148791A