Chemically selective adhesion and strength promoters in semiconductor patterning.
By diffusing a solubility modifier into the photoresist to create a footer layer with altered solubility, the method addresses uneven exposure in EUV lithography, enhancing pattern accuracy and regularity by preventing undercutting and ensuring uniform structure formation in semiconductor patterning.
Patent Information
- Application Number
- JP2024525012
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-10-26
- Filing Date
- 2022-10-25
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-10-25
Smart Images

Figure 2024542979000001_ABST
Abstract
Description
[Background technology]
[0001] Microfabrication of semiconductor devices involves various steps such as film deposition, patterning, and pattern transfer. Materials and films are deposited on substrates by spin-coating, evaporation, and other deposition processes. Patterning is typically performed by exposing a photosensitive film, also known as photoresist, to a pattern of actinic radiation and then developing the photoresist to form a relief pattern. The relief pattern then acts as an etch mask that covers the portions of the substrate that are not to be etched when the substrate is subjected to one or more etching processes.
[0002] In semiconductor patterning, it is desirable for the lithographic exposure to be uniform across the feature to enhance etch resistance and local mechanical strength. In extreme ultraviolet (EUV) patterning, the absorption of photons in the photoresist is high enough that the bottom of the photoresist is significantly less exposed than the surface. This leads to a decrease in strength across the photoresist and a large variation in etch resistance. In other words, the photoresist is exposed by EUV patterning in a top-down gradient. For example, the top of the EUV photoresist tends to receive more photons than the bottom portion, and therefore may be more insoluble in a given developer. This tends to result in feature narrowing or pattern undercutting, since the bottom portion of the EUV photoresist is only partially soluble in a given developer. Therefore, there is a need for local pattern strength enhancement to improve pattern accuracy and regularity, especially in cases where multiple patterning is used. Summary of the Invention [Means for solving the problem]
[0003] This Summary is provided to introduce a selection of concepts that are further described below in the Detailed Description. This Summary is not intended to identify key or essential features of the claimed subject matter, nor is it intended to be used as an aid in limiting the scope of the claimed subject matter.
[0004] In one aspect, embodiments disclosed herein relate to a method of patterning a substrate, including depositing an underlayer on a substrate, coating the underlayer with a solubility modifier, laminating a photoresist onto the substrate such that the photoresist covers the solubility modifier, and diffusing the solubility modifier a predetermined distance into the photoresist to provide a solubility-modified region of the photoresist, which forms a footer layer at a bottom portion of the photoresist. The method then includes exposing the photoresist to a pattern of actinic radiation, developing the photoresist to form a relief pattern on the footer layer, the relief pattern including structures separated by gaps, and etching the substrate to remove portions of the footer layer under the gaps, thereby providing uniform structures.
[0005] In another aspect, embodiments disclosed herein relate to a method of patterning a substrate, comprising depositing an underlayer on a substrate, coating the underlayer with a solubility modifier, laminating a photoresist on the substrate such that the photoresist covers the solubility modifier, and exposing the photoresist to a pattern of actinic radiation. The method then comprises diffusing the solubility modifier into the photoresist a predetermined distance to provide a solubility-modified region of the photoresist, which forms a footer layer at a bottom portion of the photoresist, developing the photoresist to form a relief pattern on the footer layer, the relief pattern including structures separated by gaps, and etching the substrate to remove portions of the footer layer that reside under the gaps, thereby providing uniform structures.
[0006] In yet another aspect, embodiments disclosed herein relate to a method of patterning a substrate including depositing an underlayer on a substrate, the underlayer including a secondary electron emitter; stacking a photoresist on the substrate such that the photoresist covers the underlayer; exposing the photoresist to a pattern of actinic radiation, the secondary electron emitter layer enhancing exposure of a bottom portion of the photoresist and providing a footer layer having a different polarity than a top portion of the photoresist; developing the photoresist to form a relief pattern on the footer layer, the relief pattern including structures separated by gaps; and etching the substrate to remove portions of the footer layer under the gaps, thereby providing uniform structures.
[0007] Other aspects and advantages of the claimed subject matter will become apparent from the following description and the appended claims. [Brief description of the drawings]
[0008] [Figure 1] FIG. 2 is a block flow diagram of a method in accordance with one or more embodiments of the present disclosure.
[0009] [Figure 2A] 2A-2D are schematic diagrams of a coated substrate at various points in a method in accordance with one or more embodiments of the present disclosure. [Figure 2B] 2A-2D are schematic diagrams of a coated substrate at various points in a method in accordance with one or more embodiments of the present disclosure. [Figure 2C] 2A-2D are schematic diagrams of a coated substrate at various points in a method in accordance with one or more embodiments of the present disclosure. [Figure 2D] 2A-2D are schematic diagrams of a coated substrate at various points in a method in accordance with one or more embodiments of the present disclosure. [Figure 2E] 2A-2D are schematic diagrams of a coated substrate at various points in a method in accordance with one or more embodiments of the present disclosure. [Figure 2F]2A-2D are schematic diagrams of a coated substrate at various points in a method in accordance with one or more embodiments of the present disclosure.
[0010] [Diagram 3] FIG. 2 is a block flow diagram of a method in accordance with one or more embodiments of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present disclosure generally relates to a method for patterning a semiconductor substrate. As used herein, the terms "semiconductor substrate" and "substrate" are used interchangeably and may be any semiconductor material, including but not limited to a semiconductor wafer, a layer of semiconductor material, and combinations thereof. The method may include treating a bottom portion of a photoresist to improve patterning regularity on the substrate. In one or more embodiments, the adhesion and strength of the photoresist is locally improved by increasing the amount of polymerization-enhancing chemical reaction in a portion of the photoresist. The method may be particularly useful in EUV lithography.
[0012] As mentioned above, in one aspect, the present disclosure relates to a method for improving the regularity of a photoresist pattern in a lithography process. FIG. 1 shows a method 100 in the present disclosure, and the method 100 will be described with reference to FIG. First, in the method 100, in block 102, an underlayer is deposited on a substrate. Then, in block 104, a solubility modifier can be coated on the underlayer, and in block 106, a photoresist is laminated on the solubility modifier. Next, the method 100 includes, in block 108, diffusing the solubility modifier into a bottom portion of the photoresist. By diffusing the solubility modifier into the bottom portion of the photoresist, a footer layer having a different solubility than the top portion of the photoresist can be provided. After the solubility modifier is diffused into the bottom portion of the photoresist to provide a footer layer, in block 110, the photoresist can be exposed to a pattern of actinic radiation and baked, and then developed in block 112. Developing the photoresist can provide a relief pattern of photoresist on the footer layer that includes structures separated by gaps. Thus, some portions of the footer layer can be under the structures and other portions of the footer layer can be under the gaps. The method 100 then includes, at block 114, removing portions of the footer layer that are under the gaps and between the structures in the photoresist to provide a pattern of photoresist with a physically stable footer layer that is free of undercuts.
[0013] Schematic diagrams of the coated substrate at various times during the method are shown in Figures 2A, 2B, 2C, 2D, 2E, and 2F. As used herein, "coated substrate" refers to a substrate that has been coated with one or more layers, such as a first photoresist layer and a second resist layer. Figure 2A shows a substrate that includes an underlayer. Figure 2B shows a substrate that includes an underlayer coated with a solubility modifier. In Figure 2C, photoresist is layered on the solubility modifier. Figure 2D shows the coated substrate after the solubility modifier has diffused into the photoresist, thereby providing a footer layer. In Figure 2E, the photoresist is developed to provide a relief pattern of photoresist on the footer layer that includes structures separated by gaps. Finally, Figure 2F shows the coated substrate that has been directionally etched to remove portions of the footer that reside under the gaps in the relief pattern.
[0014] As mentioned above, in block 102, the method first includes depositing an underlayer on a substrate. FIG. 2A shows an example of an underlayer 202 on a substrate 201. In one or more embodiments, the underlayer is a bottom anti reflection coating (BARC). A bottom anti reflection coating may be desirable because the substrate and / or underlayer would otherwise reflect a significant amount of incident radiation during photoresist exposure, which would adversely affect the quality of the formed pattern. Such a coating can improve depth of focus, exposure latitude, line width uniformity, and CD control. Anti-reflective coatings are typically used when the resist is exposed to deep ultraviolet radiation (300 nm or less), such as, for example, KrF (248 nm), ArF (193 nm), or EUV (13.5 nm) radiation. Anti-reflective coatings may consist of a single layer or multiple different layers. Suitable anti-reflective materials and methods of formation are known in the art. Antireflective materials are commercially available, for example, those sold under the AR™ trade name by DuPont (Wilmington, Del. USA), such as AR™ 3, AR™ 40A, and AR™ 124 antireflective materials.
[0015] In one or more embodiments, the underlayer includes an existing adhesion layer and a separate layer. The existing adhesion layer can be a coating, such as a silane, to modify the surface energy of the substrate. Suitable silanes include, but are not limited to, hexamethyldisilizane (HMDS).
[0016] Then, in block 104, the method 100 includes coating a solubility modifier on the underlayer. The coated substrate from block 104 is shown in FIG. 2B. When the underlayer is a separate layer, an adhesion layer may be disposed between the underlayer 202 and the solubility modifier 203 (not shown). The solubility modifier 203 is shown as a thin coating on the underlayer 202. The thickness of the solubility modifier coating is not particularly limited and may vary based on the desired line cut width. The solubility modifier may be a material that is absorbed into the underlayer upon baking, and in some cases may be referred to herein as an "absorbing material." The process of absorbing the solubility modifier into the underlayer is described in detail below.
[0017] The composition of the solubility modifier may depend on the tone of the photoresist to be layered on in block 106 of method 100. In general, the solubility modifier may be any chemical that is activated using light or heat. For example, when the photoresist is a developed negative tone developed (NTD) photoresist, the solubility modifier may include an acid or a thermal acid generator. The acid, or in the case of TAG, the generated acid, by heat, must be sufficient to cause the decomposition of the bonds of the polymeric acid labile groups in the surface region of the first photoresist pattern to increase the solubility of the first photoresist polymer in the particular developer to be applied. The acid or TAG is typically present in the composition in an amount of about 0.01 to 20% by weight based on the total solids content of the solubility modifier.
[0018] Preferred acids are organic acids, including non-aromatic or aromatic acids, each of which may optionally have fluorine substitution. Suitable organic acids include, for example, carboxylic acids such as alkanoic acids, including formic acid, acetic acid, propionic acid, butyric acid, dichloroacetic acid, trichloroacetic acid, perfluoroacetic acid, perfluorooctanoic acid, oxalic acid, malonic acid, and succinic acid; hydroxyalkanoic acids, such as citric acid; aromatic carboxylic acids, such as benzoic acid, fluorobenzoic acid, hydroxybenzoic acid, and naphthoic acid; organic phosphoric acids, such as dimethylphosphoric acid and dimethylphosphinic acid; and sulfonic acids, such as optionally fluorinated alkylsulfonic acids, including methanesulfonic acid, trifluoromethanesulfonic acid, ethanesulfonic acid, 1-butanesulfonic acid, 1-perfluorobutanesulfonic acid, 1,1,2,2-tetrafluorobutane-1-sulfonic acid, 1,1,2,2-tetrafluoro-4-hydroxybutane-1-sulfonic acid, 1-pentanesulfonic acid, 1-hexanesulfonic acid, and 1-heptanesulfonic acid.
[0019] Exemplary fluorine-free aromatic acids include aromatic acids of the general formula (I): [ka] [In the formula, R1 independently represents a substituted or unsubstituted C1-C20 alkyl group, a substituted or unsubstituted C5-C20 aryl group, or a combination thereof, and optionally contains one or more groups selected from carbonyl, carbonyloxy, sulfonamide, ether, thioether, substituted or unsubstituted alkylene group, or a combination thereof; Z1 independently represents a group selected from carboxyl, hydroxy, nitro, cyano, C1-C5 alkoxy, formyl, and sulfonic acid; a and b independently represent integers of 0 to 5, and a+b is 5 or less]
[0020] An exemplary aromatic acid may be of the following general formula (II): [ka] [wherein R2 and R3 each independently represent a substituted or unsubstituted C1-C20 alkyl group, a substituted or unsubstituted C5-C16 aryl group, or a combination thereof, and optionally contain one or more groups selected from carbonyl, carbonyloxy, sulfonamide, ether, thioether, substituted or unsubstituted alkylene group, or a combination thereof; Z2 and Z3 each independently represent a group selected from carboxyl, hydroxy, nitro, cyano, C1-C5 alkoxy, formyl, and sulfonic acid; c and d each independently represent an integer of 0 to 4, c+d is 4 or less; and e and f each independently represent an integer of 0 to 3, and e+f is 3 or less]
[0021] Additional aromatic acids that may be included in the solubility modifier include those of the general formula (III) or (IV) below. [ka] [wherein R4, R5, and R6 each independently represent a substituted or unsubstituted C1-C20 alkyl group, a substituted or unsubstituted C5-C12 aryl group, or a combination thereof, and optionally contain one or more groups selected from carbonyl, carbonyloxy, sulfonamide, ether, thioether, substituted or unsubstituted alkylene group, or a combination thereof; Z4, Z5, and Z6 each independently represent a group selected from carboxyl, hydroxy, nitro, cyano, C1-C5 alkoxy, formyl, and sulfonic acid; g and h each independently represent an integer of 0 to 4, g+h is 4 or less; i and j each independently represent an integer of 0 to 2, i+j is 2 or less; k and 1 each independently represent an integer of 0 to 3, and k+l is 3 or less] [ka] [wherein R4, R5, and R6 each independently represent a substituted or unsubstituted C1-C20 alkyl group, a substituted or unsubstituted C5-C12 aryl group, or a combination thereof, and optionally contain one or more groups selected from carbonyl, carbonyloxy, sulfonamide, ether, thioether, substituted or unsubstituted alkylene group, or a combination thereof; Z4, Z5, and Z6 independently represent a group selected from carboxyl, hydroxy, nitro, cyano, C1-C5 alkoxy, formyl, and sulfonic acid; g and h independently represent integers of 0 to 4, and g+h is 4 or less; i and j independently represent integers of 0 to 1, and i+j is 1 or less; and k and l independently represent integers of 0 to 4, and k+l is 4 or less]
[0022] A suitable aromatic acid may alternatively be of the following general formula (V): [ka] [In the formula, R7 and R8 each independently represent a substituted or unsubstituted C1-C20 alkyl group, a substituted or unsubstituted C5-C14 aryl group, or a combination thereof, and optionally contain one or more groups selected from carboxyl, carbonyl, carbonyloxy, sulfonamide, ether, thioether, substituted or unsubstituted alkylene group, or a combination thereof; Z7 and Z8 each independently represent a group selected from hydroxy, nitro, cyano, C1-C5 alkoxy, formyl, and sulfonic acid; m and n each independently represent an integer of 0 to 5, m+n is 5 or less; o and p each independently represent an integer of 0 to 4, and o+p is 4 or less]
[0023] Further, exemplary aromatic acids can have the following general formula (VI): [ka] [wherein X is O or S; R9 independently represents a substituted or unsubstituted C1-C20 alkyl group, a substituted or unsubstituted C5-C20 aryl group, or a combination thereof, and optionally contains one or more groups selected from carbonyl, carbonyloxy, sulfonamide, ether, thioether, substituted or unsubstituted alkylene group, or a combination thereof; Z9 independently represents a group selected from carboxyl, hydroxy, nitro, cyano, C1-C5 alkoxy, formyl, and sulfonic acid; q and r independently represent integers of 0 to 3, and q+r is 3 or less]
[0024] In one or more embodiments, the acid is a free acid with fluorine substitution.Suitable free acids with fluorine substitution can be aromatic or non-aromatic.For example, free acids with fluorine substitution that can be used as solubility modifiers include, but are not limited to: [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka]
[0025] Suitable TAGs include those capable of generating non-polymerizable acids as described above. TAGs can be non-ionic or ionic. Suitable non-ionic thermal acid generators include, for example, cyclohexyl trifluoromethylsulfonate, methyl trifluoromethylsulfonate, cyclohexyl p-toluenesulfonate, methyl p-toluenesulfonate, cyclohexyl 2,4,6-triisopropylbenzenesulfonate, nitrobenzyl esters, benzoin tosylate, 2-nitrobenzyl tosylate, tris(2,3-dibromopropyl)-1,3,5-triazine-2,4,6-trione, alkyl esters of organic sulfonic acids, p-toluenesulfonic acid, dodecylbenzenesulfonic acid, oxalic acid, Examples of suitable ionic thermal acid generators include phthalic acid, phosphoric acid, camphorsulfonic acid, 2,4,6-trimethylbenzenesulfonic acid, triisopropylnaphthalenesulfonic acid, 5-nitro-o-toluenesulfonic acid, 5-sulfosalicylic acid, 2,5-dimethylbenzenesulfonic acid, 2-nitrobenzenesulfonic acid, 3-chlorobenzenesulfonic acid, 3-bromobenzenesulfonic acid, 2-fluorocaprylnaphthalenesulfonic acid, dodecylbenzenesulfonic acid, 1-naphthol-5-sulfonic acid, 2-methoxy-4-hydroxy-5-benzoyl-benzenesulfonic acid, and their salts, and combinations thereof. Suitable ionic thermal acid generators include, for example, dodecylbenzenesulfonic acid triethylamine salt, dodecylbenzenedisulfonic acid triethylamine salt, p-toluenesulfonic acid-ammonium salt, p-toluenesulfonic acid-pyridinium salt, sulfonates such as carbocyclic aryl and heteroaryl sulfonates, aliphatic sulfonates, and benzenesulfonates. Compounds that generate sulfonic acid upon activation are generally suitable. Preferred thermal acid generators include ammonium p-toluenesulfonate and heteroarylsulfonates.
[0026] Preferably, the TAG is ionic in the reaction scheme for generating a sulfonic acid as shown below. [ka] In the formula, RSO3 - is the TAG anion, and X + is a TAG cation, preferably an organic cation. The cation may be a nitrogen-containing cation of the following general formula (I): (BH) + (I) This is the monoprotonated form of the nitrogen-containing base B. Suitable nitrogen-containing bases B include, for example, ammonia, difluoromethylammonia, optionally substituted amines such as C1-20 alkylamines and C3-30 arylamines, nitrogen-containing heteroaromatic bases such as pyridine or substituted pyridines (e.g., 3-fluoropyridine), pyrimidines and pyrazines, and nitrogen-containing heterocyclic groups such as oxazole, oxazoline or thiazoline. The aforementioned nitrogen-containing bases B can be optionally substituted with one or more groups selected from, for example, alkyl, aryl, halogen atoms (preferably fluorine), cyano, nitro and alkoxy. Of these, base B is preferably a heteroaromatic base.
[0027] The base B typically has a pKa of 0-5.0, 0-4.0, 0-3.0, or 1.0-3.0. As used herein, terms such as "pKa" are used according to their art-recognized meanings. That is, pKa is the pKa of the conjugate acid (BH) of the basic moiety (B) in aqueous solution at about room temperature. + C. is the negative logarithm (to the base 10) of the dissociation constant of . In certain embodiments, base B has a boiling point of less than about 170.degree. C., less than about 160.degree. C., less than 150.degree. C., less than 140.degree. C., less than 130.degree. C., less than 120.degree. C., less than 110.degree. C., less than 100.degree. C., or less than 90.degree.
[0028] Suitable exemplary nitrogen-containing cations (BH) + As for NH4 + , CF2HNH2 + , CF3CH2NH3 + , (CH3)3NH + , (C2H5)3NH + , (CH3)2(C2H5)NH + and the following: [ka] wherein Y is alkyl, preferably methyl or ethyl.
[0029] In certain embodiments, the solubility modifier can be an acid such as trifluoromethanesulfonic acid, perfluoro-1-butanesulfonic acid, p-toluenesulfonic acid, 4-dodecylbenzenesulfonic acid, 2,4-dinitrobenzenesulfonic acid, and 2-trifluoromethylbenzenesulfonic acid, an acid generator such as triphenylsulfonium antimonate, pyridinium perfluorobutanesulfonate, 3-fluoropyridinium perfluorobutanesulfonate, 4-t-butylphenyltetramethylenesulfonium perfluoro-1-butanesulfonate, 4-t-butylphenyltetramethylenesulfonium 2-trifluoromethylbenzenesulfonate, and 4-t-butylphenyltetramethylenesulfonium 4,4,5,5,6,6-hexafluorodihydro-4H-1,3,2-dithiazine 1,1,3,3-tetraoxide, or a combination thereof.
[0030] Alternatively, when the photoresist is a positive tone developed (PTD) photoresist, the solubility modifier may include a base or a base generator. In such embodiments, suitable solubility modifiers include, but are not limited to, hydroxides, carboxylates, amines, imines, amides, and mixtures thereof. Specific examples of bases include ammonium carbonate, ammonium hydroxide, ammonium hydrogen phosphate, ammonium phosphate, tetramethylammonium carbonate, tetramethylammonium hydroxide, tetramethylammonium hydrogen phosphate, tetramethylammonium phosphate, tetraethylammonium carbonate, tetraethylammonium hydroxide, tetraethylammonium hydrogen phosphate, tetraethylammonium phosphate, and combinations thereof. Amines include aliphatic amines, cycloaliphatic amines, aromatic amines, and heterocyclic amines. The amines may be primary, secondary, or tertiary amines. The amines may be monoamines, diamines, or polyamines. Suitable amines may include C1-30 organic amines, imines or amides, or may be C1-30 quaternary ammonium salts of strong bases (eg, hydroxides or alkoxides) or weak bases (eg, carboxylates).Exemplary bases include amines such as tripropylamine, dodecylamine, tris(2-hydroxypropyl)amine, tetrakis(2-hydroxypropyl)ethylenediamine, arylamines such as diphenylamine, triphenylamine, aminophenol and 2-(4-aminophenyl)-2-(4-hydroxyphenyl)propane, Troeger's base, hindered amines such as diazabicycloundecene (DBU) or diazabicyclononene (DBN), amides such as tert-butyl 1,3-dihydroxy-2-(hydroxymethyl)propan-2-ylcarbamate and tert-butyl 4-hydroxypiperidine-1-carboxylate, or ionic quenchers including quaternary alkylammonium salts such as tetrabutylammonium hydroxide (TBAH) or tetrabutylammonium lactate. In another embodiment, the amine is a hydroxyamine. Examples of hydroxyamines include hydroxyamines having one or more hydroxyalkyl groups (e.g., hydroxymethyl, hydroxyethyl, and hydroxybutyl groups), each having 1 to about 8 carbon atoms, preferably 1 to about 5 carbon atoms. Specific examples of hydroxyamines include monoethanolamine, diethanolamine, triethanolamine, 3-amino-1-propanol, 2-amino-2-methyl-1-propanol, 2-amino-2-ethyl-1,3-propanediol, tris(hydroxymethyl)aminomethane, N-methylethanolamine, 2-diethylamino-2-methyl-1-propanol, and triethanolamine.
[0031] A suitable base generator may be a thermal base generator, which forms a base when heated above a first temperature, typically above about 140° C. The thermal base generator may include functional groups such as amides, sulfonamides, imides, imines, O-acyloximes, benzoyloxycarbonyl derivatives, quaternary ammonium salts, nifedipine, carbamates, and combinations thereof. Exemplary thermal base generators include o-{(β-(dimethylamino)ethyl)aminocarbonyl}benzoic acid, o-{(γ-(dimethylamino)propyl)aminocarbonyl}benzoic acid, 2,5-bis{(β-(dimethylamino)ethyl)aminocarbonyl}terephthalic acid, 2,5-bis{(γ-(dimethylamino)propyl)aminocarbonyl}terephthalic acid, 2,4-bis{(β-(dimethylamino)ethyl)aminocarbonyl}isophthalic acid, 2,4-bis{(γ-(dimethylamino)propyl)aminocarbonyl}isophthalic acid, and combinations thereof.
[0032] In one or more embodiments, the solubility modifier comprises a solvent. The solvent can be any suitable solvent capable of facilitating the coating of the solubility modifier on the underlayer. Thus, the solvent can be miscible with or capable of dissolving or suspending other components contained in the solubility modifier, such as, for example, an acid, an acid generator, a base, or a base generator. The solvent is typically selected from water, an organic solvent, and mixtures thereof. In some embodiments, the solvent can comprise an organic-based solvent system comprising one or more organic solvents. The term "organic-based" means that the solvent system comprises more than 50% organic solvent by weight based on the total solvent of the solubility modifier composition, and more typically comprises more than 90%, more than 95%, more than 99%, or 100% organic solvent by weight based on the total solvent of the solubility modifier composition. The solvent component is typically present in an amount of 90-99% by weight based on the solubility modifier composition.
[0033] Suitable organic solvents for the solubility modifier composition include, for example, alkyl esters such as alkyl propionates, such as n-butyl propionate, n-pentyl propionate, n-hexyl propionate, and n-heptyl propionate, and alkyl butyrates, such as n-butyl butyrate, isobutyl butyrate, and isobutyl isobutyrate; ketones, such as 2,5-dimethyl-4-hexanone and 2,6-dimethyl-4-heptanone; n-heptane; Aliphatic hydrocarbons such as hexane, n-nonane, n-octane, n-decane, 2-methylheptane, 3-methylheptane, 3,3-dimethylhexane, and 2,3,4-trimethylpentane, as well as fluorinated aliphatic hydrocarbons such as perfluoroheptane, 1-butanol, 2-butanol, isobutyl alcohol, tert-butyl alcohol, 3-methyl-1-butanol, 1-pentanol, 2-pentanol, 4-methyl-2-pentanol, 1-hexanol, 1-hexane, linear, branched or cyclic C4-C9 monohydric alcohols such as 2,2,3,3,4,4-hexafluoro-1-butanol, 2,2,3,3,4,4,5,5-octafluoro-1-pentanol and 2,2,3,3,4,4,5,5,6,6-decafluoro-1-hexanol; and C5-C9 fluorinated diols such as 2,2,3,3,4,4-hexafluoro-1,5-pentanediol, 2,2,3,3,4,4,5,5-octafluoro-1,6-hexanediol, and 2,2,3,3,4,4,5,5,6,6,7,7-dodecafluoro-1,8-octanediol; ethers such as isopentyl ether and dipropylene glycol monomethyl ether; and mixtures containing one or more of these solvents.
[0034] In one or more embodiments, the solvent preferably comprises one or more polar organic solvents. For example, the solubility modifier may comprise a polar solvent such as methyl isobutyl carbinol (MIBC). The solubility modifier may also comprise aliphatic hydrocarbons, esters and ethers as co-solvents, such as, for example, decane, isobutyl isobutyrate, isoamyl ether and combinations thereof. In certain embodiments, the solvent comprises MIBC and a co-solvent. In such embodiments, the MIBC may be contained in the solvent in an amount ranging from 60 to 99%, based on the total volume of the solvent. Thus, the co-solvent may be contained in an amount ranging from 1 to 40%, based on the total volume of the solvent.
[0035] Alternatively, in one or more embodiments, the solvent preferably comprises one or more non-polar organic solvents. Terms such as "non-polar organic system" mean that the solvent system comprises greater than 50% by weight of total non-polar organic solvents based on the total solvents of the solubility modifier composition, and more typically greater than 70%, 85% or 100% by weight of total non-polar organic solvents based on the total solvents of the solubility modifier composition. The non-polar organic solvents are typically present in the solvent in a total amount of 70-98% by weight, preferably 80-95% by weight, more preferably 85-98% by weight, based on the total solvents.
[0036] Suitable non-polar solvents include, for example, ethers, hydrocarbons, and combinations thereof, with ethers being preferred. Suitable ether solvents include, for example, alkyl monoethers and aromatic monoethers, with those having a total carbon number of 6 to 16 being particularly preferred. Suitable alkyl monoethers include, for example, 1,4-cineole, 1,8-cineole, pinene oxide, di-n-propyl ether, diisopropyl ether, di-n-butyl ether, di-n-pentyl ether, diisoamyl ether, dihexyl ether, diheptyl ether, and dioctyl ether, with diisoamyl ether being preferred. Suitable aromatic monoethers include, for example, anisole, ethyl benzyl ether, diphenyl ether, dibenzyl ether, and phenetole, with anisole being preferred. Suitable aliphatic hydrocarbons include, for example, n-heptane, 2-methylheptane, 3-methylheptane, 3,3-dimethylhexane, 2,3,4-trimethylpentane, n-octane, n-nonane, n-decane, and fluorinated compounds such as perfluoroheptane. Suitable aromatic hydrocarbons include, for example, benzene, toluene, and xylene.
[0037] In some embodiments, the solvent comprises one or more alcohol and / or ester solvents. For certain compositions, the alcohol and / or ester solvents may provide enhanced solubility for the solid components of the composition. Suitable alcohol solvents include, for example, linear, branched or cyclic C alcohols such as 1-butanol, 2-butanol, isobutyl alcohol, tert-butyl alcohol, 3-methyl-1-butanol, 1-pentanol, 2-pentanol, 4-methyl-2-pentanol, 1-hexanol, 1-heptanol, 1-octanol, 2-hexanol, 2-heptanol, 2-octanol, 3-hexanol, 3-heptanol, 3-octanol, 4-octanol, 2,2,3,3,4,4-hexafluoro-1-butanol, 2,2,3,3,4,4,5,5-octafluoro-1-pentanol and 2,2,3,3,4,4,5,5,6,6-decafluoro-1-hexanol. 4-9Monohydric alcohols and C such as 2,2,3,3,4,4-hexafluoro-1,5-pentanediol, 2,2,3,3,4,4,5,5-octafluoro-1,6-hexanediol and 2,2,3,3,4,4,5,5,6,6,7,7-dodecafluoro-1,8-octanediol 5-9 The alcohol solvent is preferably C 4-9 It is a monohydric alcohol, and 4-methyl-2-pentanol is preferred. Suitable ester solvents include, for example, alkyl esters having a total carbon number of 4 to 10, such as alkyl propionates, such as n-butyl propionate, n-pentyl propionate, n-hexyl propionate, and n-heptyl propionate, and alkyl butyrates, such as n-butyl butyrate, isobutyl butyrate, and isobutyl isobutyrate. When used in the solvent, one or more alcohol solvents and / or ester solvents are typically present in a total amount of 2 to 50% by weight, more typically 2 to 30% by weight, based on the total amount of solvent.
[0038] The solvent may also include one or more additional solvents selected from, for example, one or more of ketones, such as 2,5-dimethyl-4-hexanone and 2,6-dimethyl-4-heptanone, and polyethers, such as dipropylene glycol monomethyl ether and tripropylene glycol monomethyl ether. Such additional solvents, if used, are typically present in a total amount of 1 to 20% by weight based on the total amount of solvent.
[0039] As described above, the solubility modifier is coated on the underlayer. In order to coat the underlayer properly, the solubility modifier may include a matrix polymer. Any matrix polymer commonly used in the art may be included in the solubility modifier. The matrix polymer must have good solubility in the solvent included in the solubility modifier. The matrix polymer may be formed from one or more monomers selected from monomers having ethylenically unsaturated polymerizable double bonds, such as (meth)acrylate monomers such as isopropyl (meth)acrylate and n-butyl (meth)acrylate; aromatic vinyl monomers such as (meth)acrylic acid, styrene, hydroxystyrene, vinyl naphthalene and acenaphthylene; vinyl alcohol; vinyl chloride; vinyl pyrrolidone; vinyl pyridine; vinyl amine; vinyl acetal; maleic anhydride; maleimide; norbornene; and combinations thereof.
[0040] In some embodiments, the polymer contains one or more functional groups selected from acid groups, such as hydroxy, carboxyl, sulfonic acid and sulfonamide, silanol, fluoroalcohol, such as hexafluoroisopropyl alcohol [-C(CF3)2OH], anhydride, lactone, ester, ether, allylamine, pyrrolidone, and combinations thereof. The polymer can be a homopolymer or a copolymer having multiple distinct repeat units, such as 2, 3, 4 or more repeat units. In one aspect, the repeat units of the polymer are formed entirely from (meth)acrylate monomers, formed entirely from aromatic (vinyl) monomers, or formed entirely from (meth)acrylate monomers and aromatic (vinyl) monomers. When the polymer contains more than one type of repeat unit, it is typically in the form of a random copolymer.
[0041] The solubility modifier typically comprises a single polymer, but may optionally comprise one or more additional polymers. The content of polymer in the solubility modifier depends, for example, on the target thickness of the layer, with higher polymer contents being used when thicker layers are desired. The polymer is typically present in the solubility modifier composition in an amount of 80-99.9 wt%, more typically 90-99 wt%, or 95-99 wt%, based on the total solids content of the solubility modifier composition. The weight average molecular weight (Mw) of the polymer is typically less than 400,000, preferably 3000-50,000, more preferably 3000-25,000, as measured by GPC against polystyrene standards. Typically, the polymer has a polydispersity index (PDI=Mw / Mn) of 3 or less, preferably 2 or less, as measured by GPC against polystyrene standards.
[0042] Suitable polymers for use in the solubility modifier composition are commercially available and / or can be easily made by those skilled in the art. For example, the polymer can be synthesized by dissolving selected monomers corresponding to the units of the polymer in an organic solvent, adding a radical polymerization initiator, and carrying out thermal polymerization to form the polymer. Examples of suitable organic solvents that can be used to polymerize the polymer include, for example, toluene, benzene, tetrahydrofuran, diethyl ether, dioxane, ethyl lactate, and methyl isobutyl carbinol. Suitable polymerization initiators include, for example, 2,2'-azobisisobutyronitrile (AIBN), 2,2'-azobis(2,4-dimethylvaleronitrile), dimethyl 2,2-azobis(2-methylpropionate), benzoyl peroxide, and lauroyl peroxide.
[0043] The solubility modifier including the matrix polymer can be coated onto the underlayer according to methods known in the art. Typically, the solubility modifier including the matrix polymer can be coated onto the first relief pattern by spin coating. The solids content of the solubility modifier can be adjusted to provide a desired thickness of film of the solubility modifier on the first relief pattern. For example, the solids content of the solubility modifier solution can be adjusted to provide a desired film thickness based on the particular coating equipment utilized, the viscosity of the solution, the speed of the coating tool, and the time it can be spun. Typical thicknesses of the solubility modifier can range from about 200 Å to about 1500 Å.
[0044] In one or more embodiments, the solubility modifier comprises an active agent (i.e., an acid, an acid generator, a base or a base generator), a solvent and a matrix polymer, as described above. A typical formulation of such a solubility modifier may comprise about 1-10% by weight solids and 90-99.9% by weight solvent, based on the total weight of the solubility modifier, the solids comprising the active agent and the matrix polymer. Within the solids content, the active agent may be contained in an amount ranging from about 1 to about 5% by weight.
[0045] The solubility modifier may contain additives with various purposes, depending on the particular chemistry used. In some embodiments, surfactants may be included in the solubility modifier. Surfactants may be included in the solubility modifier to aid in coating quality, especially when thin gaps between features of the first photoresist need to be filled. Suitable surfactants known in the art may be included in the solubility modifier.
[0046] As noted above, in one or more embodiments, the solubility modifier is absorbed into the underlayer. Absorption of the solubility modifier into the underlayer may be accomplished by performing a thermal pretreatment, such as a bake. The bake may be a soft bake. The temperature and time of the soft bake may depend on the properties of the first resist and the desired amount of diffusion of the solubility modifier into the first resist. Typically, the soft bake may be performed at a temperature ranging from about 50 to about 150° C. for about 30 seconds to about 90 seconds.
[0047] After absorption into the underlayer, the coating layer may remain on the first resist with little or no effective solubility modifying material. In one or more embodiments, the coating layer may be removed by rinsing. Rinsing may be accomplished by rinsing the coated substrate with a solvent that dissolves the coating layer but not the underlayer. Rinsing may be performed using a suitable method, for example, by immersing the substrate in a bath filled with the solvent for a period of time (immersion method), by allowing the solvent to rise to the substrate surface by the action of surface tension and remain there for a period of time, thereby dissolving the coating layer (puddle method), by spraying the solvent onto the substrate surface (spray method), or by continuously spraying the solvent onto the substrate rotating at a constant speed while scanning the solvent nozzle at a constant speed (dynamic dispense method).
[0048] In block 106 of method 100, a photoresist is deposited on the substrate. A coated substrate with an underlayer 202, a solubility modifier 203, and a photoresist 204 is shown in FIG. 2C. The photoresist may be deposited on the substrate to completely coat the underlayer and the solubility modifier. The photoresist may be deposited on the substrate according to any suitable method known in the art, such as, for example, spin-on deposition or vapor phase processing.
[0049] Generally, a photoresist is a chemically amplified photosensitive composition that includes a polymer, a photoacid generator, and a solvent. In a particular embodiment, the photoresist is an EUV resist. In this case, the term EUV resist refers to a resist that is sensitive to EUV light. The photoresist may include a polymer. A suitable polymer may be any standard polymer typically used in photoresist materials, particularly a polymer that has acid labile groups. For example, the polymer may be a polymer made from monomers that include aromatic vinyl monomers such as styrene and p-hydroxystyrene, acrylates, methacrylates, norbornene, and combinations thereof. Monomers that include reactive functional groups may be present in the polymer in a protected form. For example, the -OH group of p-hydroxystyrene may be protected with a tert-butyloxycarbonyl protecting group. Such a protecting group may modify the reactivity and solubility of the polymer included in the first photoresist. As will be appreciated by those skilled in the art, a variety of protecting groups may be used for this reason. Acid labile groups include, for example, tertiary alkyl ester groups, secondary or tertiary aryl ester groups, secondary or tertiary ester groups having a combination of alkyl and aryl groups, tertiary alkoxy groups, acetal groups, or ketal groups. Acid labile groups are also commonly referred to in the art as "acid decomposable groups", "acid dissociable groups", "acid dissociable protecting groups", "acid labile protecting groups", "acid leaving groups", and "acid sensitive groups".
[0050] The polymer may contain acid labile groups that upon degradation form a carboxylic acid on the polymer, preferably of the formula -C(O)OC(R 1 )3, or a tertiary ester group of the formula -C(O)OC(R 2 )2OR 3 where R 1 are each independently a linear C 1-20 Alkyl, branched C 3-20 Alkyl, monocyclic or polycyclic C 3-20 Cycloalkyl, linear C 2-20 Alkenyl, branched C 3-20 Alkenyl, monocyclic or polycyclic C 3-20Cycloalkenyl, monocyclic or polycyclic C 6-20 Aryl, or monocyclic or polycyclic C 2-20 Heteroaryl, preferably linear C 1-6 Alkyl, branched C 3-6 Alkyl, or monocyclic or polycyclic C 3-10 cycloalkyl, each of which is substituted or unsubstituted; and each R 1 optionally includes one or more groups selected from -O-, -C(O)-, -C(O)-O-, or -S- as part of its structure, and any two R 1 The groups together optionally form a ring, R 2 are independently hydrogen, fluorine, linear C 1-20 Alkyl, branched C 3-20 Alkyl, monocyclic or polycyclic C 3-20 Cycloalkyl, linear C 2-20 Alkenyl, branched C 3-20 Alkenyl, monocyclic or polycyclic C 3-20 Cycloalkenyl, monocyclic or polycyclic C 6-20 Aryl, or monocyclic or polycyclic C 2-20 Heteroaryl, preferably hydrogen, linear C 1-6 Alkyl, branched C 3-6 Alkyl, or monocyclic or polycyclic C 3-10 cycloalkyl, each of which is substituted or unsubstituted; and each R 2 optionally includes one or more groups selected from -O-, -C(O)-, -C(O)-O-, or -S- as part of its structure, and a plurality of R 2 The groups together optionally form a ring, R 3 is a linear C 1-20 Alkyl, branched C 3-20 Alkyl, monocyclic or polycyclic C 3-20 Cycloalkyl, linear C 2-20 Alkenyl, branched C 3-20 Alkenyl, monocyclic or polycyclic C 3-20 Cycloalkenyl, monocyclic or polycyclic C 6-20 Aryl, or monocyclic or polycyclic C 2-20Heteroaryl, preferably linear C 1-6 Alkyl, branched C 3-6 Alkyl or monocyclic or polycyclic C 3-10 cycloalkyl, each of which is substituted or unsubstituted; R 3 optionally includes one or more groups selected from -O-, -C(O)-, -C(O)-O-, or -S- as part of its structure, and one R 2 is R 3 and optionally form a ring. Such monomers are typically aromatic vinyl, (meth)acrylate or norbornyl monomers. The total content of polymerized units containing acid-decomposable groups that form carboxylic acid groups in the polymer is typically 10 to 100 mol %, more typically 10 to 90 mol %, or 30 to 70 mol %, based on the total polymerized units of the polymer contained in the photoresist.
[0051] The polymer may further comprise a monomer that, upon polymerization, comprises an acid labile group, the decomposition of which forms an alcohol or fluoroalcohol group on the polymer. Suitable such groups include, for example, monomers of the formula -COC(R 2 )2OR 3 -, an acetal group of the formula -OC(O)O-, or a carbonate group of the formula -OC(O)O-, where R is as defined above. Such monomers are typically aromatic vinyl, (meth)acrylate or norbornyl monomers. When present in the polymer, the total content of polymerized units containing acid decomposable groups, the decomposition of which forms an alcohol group or a fluoroalcohol group in the polymer, is typically 10-90 mol %, more typically 30-70 mol %, based on the total polymerized units of the polymer.
[0052] In one or more embodiments, the photoresist includes a photoacid generator. The photoacid generator can be a compound capable of generating an acid upon irradiation with actinic or radiation. The photoacid generator can be selected from known compounds capable of generating an acid upon irradiation with actinic or radiation used as photoinitiators for cationic photopolymerization, photoinitiators for radical photopolymerization, photobleachers for dyes, photochromic agents, microresists, etc., and mixtures thereof can be used. Examples of photoacid generators include diazonium salts, phosphonium salts, sulfonium salts, iodonium salts, imidosulfonates, oximesulfonates, diazodisulfones, disulfones, and o-nitrobenzylsulfonates.
[0053] Suitable photoacids include onium salts such as triphenylsulfonium trifluoromethanesulfonate, (p-tert-butoxyphenyl)diphenylsulfonium trifluoromethanesulfonate, tris(p-tert-butoxyphenyl)sulfonium trifluoromethanesulfonate, triphenylsulfonium p-toluenesulfonate; di-t-butylphenyliodonium perfluorobutanesulfonate, and di-t-butylphenyliodonium camphorsulfonate. Nonionic sulfonate and sulfonyl compounds are used as photoacid generators. They are also known to function as photocatalyst generators, for example, nitrobenzyl derivatives, such as 2-nitrobenzyl-p-toluenesulfonate, 2,6-dinitrobenzyl-p-toluenesulfonate and 2,4-dinitrobenzyl-p-toluenesulfonate; sulfonic acid esters, such as 1,2,3-tris(methanesulfonyloxy)benzene, 1,2,3-tris(trifluoromethanesulfonyloxy)benzene and 1,2,3-tris(p-toluenesulfonyloxy)benzene; diazomethane derivatives, such as bis(benzenesulfonyl)diazomethane, bis(p-toluenesulfonyl)diazomethane; Glyoxime derivatives such as bis-O-(p-toluenesulfonyl)-α-dimethylglyoxime and bis-O-(n-butanesulfonyl)-α-dimethylglyoxime; sulfonate derivatives of N-hydroxyimide compounds such as N-hydroxysuccinimide methanesulfonate and N-hydroxysuccinimide trifluoromethanesulfonate; and halogen-containing triazine compounds such as 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-1,3,5-triazine and 2-(4-methoxynaphthyl)-4,6-bis(trichloromethyl)-1,3,5-triazine. Suitable non-polymeric photoacid generators are further described in U.S. Patent No. 8,431,325 to Hashimoto et al. (column 37, lines 11-47 and columns 41-91).Other suitable sulfonate PAGs include sulfonated esters and sulfonyloxyketones, nitrobenzyl esters, s-triazine derivatives, benzoin tosylate, t-butylphenyl α-(p-toluenesulfonyloxy)-acetate and t-butyl α-(p-toluenesulfonyloxy)-acetate, as described in U.S. Patents 4,189,323 and 8,431,325. PAGs that are onium salts typically contain anions with sulfonate or non-sulfonate groups, such as sulfonamidate, sulfonimidate, methide or borate groups.
[0054] The photoresist may optionally include multiple PAGs. The multiple PAGs may be polymeric, non-polymeric, or may include both polymeric and non-polymeric PAGs. Preferably, each of the multiple PAGs is non-polymeric. Preferably, when multiple PAGs are used, the first PAG includes a sulfonate group in the anion, and the second PAG includes an anion that does not include a sulfonate group, such an anion containing, for example, the above-mentioned sulfonamidate group, sulfonimidate group, methide group, or borate group.
[0055] In one or more embodiments, the photoresist is an EUV resist. In this case, the term EUV resist refers to a resist that is sensitive to EUV light. Suitable EUV resists can be chemically amplified resists, organometallic resists, and dry resists. Chemically amplified EUV resists can include the polymers described above and a photoacid generator.
[0056] In one or more embodiments, the EUV resist is an organometallic resist. Thus, in one or more embodiments, the photoresist is an organometallic or metal-based resist based on metal oxide chemistry, including metal oxo / hydroxo compositions that utilize radiation-sensitive ligands to enable patterning by actinic radiation. One class of radiation-based resists uses peroxo ligands as radiation-sensitive stabilizing ligands. Peroxo-based metal oxo-hydroxo compounds are described, for example, in U.S. Pat. No. 9,176,377 by Stowers et al., entitled "Patterned Inorganic Layers, Radiation Based Patterning Compositions and Corresponding Methods," which is incorporated herein by reference. Related resist compounds are discussed in U.S. Patent Application Publication No. 2013 / 0224652 by Bass et al., entitled "Metal Peroxo Compounds With Organic Co-ligands for Electron Beam, Deep UV and Extreme UV Resist Applications," which is incorporated herein by reference. An effective type of resist is developed with alkyl ligands as described in U.S. Pat. No. 9,310,684 to Meyers et al., entitled "Organometallic Solution Based High Resolution Patterning Compositions," U.S. Patent Application Publication No. 2016 / 0116839 to Meyers et al., entitled "Organometallic Solution Based High Resolution Patterning Compositions and Corresponding Methods," and U.S. Patent Application No. 15 / 291,738, entitled "Organotin Oxide Hydroxide Patterning Compositions, Precursors, and Patterning," all of which are incorporated by reference herein in their entireties.Although tin compositions are exemplified in these publications and the edge bead removal solutions described herein are expected to be effective for other metal-based resists, as described below, the data presented herein focuses on tin-based resists.
[0057] Regarding tin-based photoresists that particularly attract attention, these photoresists are based on the chemical reaction of an organometallic composition represented by the formula RzSnO(2-(z / 2)-(x / 2))(OH)x [where 0 < z ≤ 2 and 0 < (z + x) ≤ 4, and R is a hydrocarbyl group having 1 to 31 carbon atoms]. However, at least a part of the oxo / hydroxo ligands can be formed after deposition based on in-situ hydrolysis based on a composition represented by the formula RnSnX4-n [where n = 1 or 2, and X is a ligand having a hydrolyzable M-X bond]. Generally, suitable hydrolyzable ligands (X in RSnX3) can include alkynide RC≡C, alkoxide RO-, azide N3-, carboxylate RCOO-, halide, and dialkylamide. Therefore, in some embodiments, all or part of the oxo-hydroxo composition can be replaced with an Sn-X composition or a mixture thereof. The R-Sn bond is generally radiation-sensitive and forms the basis for the aspect where the resist can be radiation-treated. However, some of the RzSnO(2-(z / 2)-(x / 2))(OH)x compositions can be replaced with MO((m / 2)-l / 2)(OH)x [where 0 < z ≤ 2, 0 < (z + w) ≤ 4, m is the formal valence of Mm+, 0 ≤ l ≤ m, and y / z = (0.05 to 0.6)], M = M' or Sn, M' is a non-tin metal in Groups 2 to 16 of the periodic table, and R is a hydrocarbyl group having 1 to 31 carbon atoms. Therefore, the photoresist processed during edge bead rinsing can include a selected blend of RzSnO(2-(z / 2)-(x / 2))(OH)x, R'nSnX4-n, and / or MO((m / 2)-l / 2)(OH)x, and generally many fractions of this composition contain alkyl-tin bonds. Other photoresist compositions include, for example, compositions having a metal carboxylate bond (such as ligands like acetate, propanoate, butanoate, benzoate, etc.), like dibutyltin diacetate.
[0058] While the metal oxo / hydroxo or carboxylate-based photoresists mentioned above are particularly desirable, in some embodiments, a number of other high performance photoresists may be suitable, particularly other metal-based photoresists that have high etch selectivity to substrate and hardmask materials. These may include photoresists such as metal oxide nanoparticle resists (e.g., Jiang, Jing; Chakrabarty, Souvik; Yu, Mufei; et al., "Metal Oxide Nanoparticle Resists for EUV Patterning", Journal Of Photopolymer Science And Technology 27(5), 663-666 2014, incorporated herein by reference), or other metal-containing resists (A Platinum-Fullerene Complex for Patterning Metal Containing Nanostructures, DX Yang, A. Frommhold, DS He, ZY Li, RE Palmer, MA Lebedeva, TW Chamberlain, ANKhlobystov, APG Robinson, Proc SPIE Advanced Lithography, 2014, incorporated herein by reference). Other metal-based resists are described in U.S. Patent Application Publication No. 2009 / 0155546 by Yamashita et al., entitled "Film-Forming Composition, Method for Pattern Formation, and Three-Dimensional Mold," and U.S. Patent No. 6,566,276 by Maloney et al., entitled "Method of Making Electronic Materials," both of which are incorporated herein by reference.
[0059] In another embodiment, the photoresist is an EUV-sensitive film applied by a deposition process known as "dry resist". The film may be formed by mixing a vapor stream of an organometallic precursor with a vapor stream of a counter reactant to form a polymerized organometallic material. A hard mask may also be formed by depositing a polymeric organometallic material onto a semiconductor substrate surface. The mixing and deposition operation may be performed in chemical vapor deposition (CVD), ALD with CVD equipment such as atomic layer deposition (ALD), and discontinuous ALD-like processes where the metal precursor and the counter reactant are separated in either time or space.
[0060] Such EUV-sensitive films include materials that undergo changes upon exposure to EUV, such as loss of bulky pendant substituents bonded to metal atoms in less dense M-OH rich materials, which allows crosslinking to denser MOM-bonded metal oxide materials. Through EUV patterning, regions of the film are created that have altered physical or chemical properties relative to unexposed regions. These properties can be exploited in subsequent processing, for example, to dissolve either the unexposed or exposed regions, or to selectively deposit material onto either the unexposed or exposed regions. In some embodiments, under conditions under which such subsequent processing is performed, the unexposed film has a hydrophobic surface and the exposed film has a hydrophilic surface (it being recognized that the hydrophilicity of the exposed and unexposed regions is relative to one another). For example, material removal can be achieved by exploiting differences in the chemical composition, density, and crosslinking of the film. Removal can be by wet or dry processing.
[0061] The thin films, in various embodiments, are organometallic materials that contain SnOx or other metal oxide moieties. The organometallic compounds can be made in a gas phase reaction of an organometallic precursor with a counter reactant. In various embodiments, the organometallic compounds are formed by mixing specific combinations of organometallic precursors with bulky alkyl or fluoroalkyl groups and counter reactants, and polymerizing the mixture in the gas phase to create a low density EUV sensitive material that is deposited on the substrate.
[0062] In various embodiments, the organometallic precursors contain at least one alkyl group on each metal atom that can survive gas phase reaction, but other ligands or ions coordinated to the metal atom can be replaced with counter reactants. MaRbLc (Formula 1) where M is a metal with a high EUV absorption cross section, R is alkyl, e.g., CnH2n+1, preferably n≧3, L is a ligand, ion or other moiety reactive with a counter reactant, and a≧1, b≧1, and c≧1.
[0063] In various embodiments, M is 1×10 7 cm 2 / mol or more. M can be, for example, selected from the group consisting of tin, bismuth, antimony, and combinations thereof. In some embodiments, M is tin. R can be fluorinated, for example, having the formula CnFxH(2n+1). In various embodiments, R has at least one β-hydrogen or β-fluorine. For example, R can be selected from the group consisting of i-propyl, n-propyl, t-butyl, i-butyl, n-butyl, sec-butyl, n-pentyl, i-pentyl, t-pentyl, sec-pentyl, and mixtures thereof. L can be any moiety that is readily displaced by a counter reactant, such as a moiety selected from the group consisting of amines (dialkylamino, monoalkylamino), alkoxy, carboxylate, halogen, and mixtures thereof, to produce the M-OH moiety.
[0064] The organometallic precursor can be any of a wide variety of possible organometallic precursors. For example, when M is tin, such precursors include t-butyltris(dimethylamino)tin, i-butyltris(dimethylamino)tin, n-butyltris(dimethylamino)tin, sec-butyltris(dimethylamino)tin, i-propyl(tris)dimethylaminotin, n-propyltris(diethylamino)tin, and similar alkyl(tris)(t-butoxy)tin compounds, such as t-butyltris(t-butoxy)tin. In some embodiments, the organometallic precursor is partially fluorinated.
[0065] The counter reactant preferably has the ability to replace the ligand or ion of the reactive moiety (e.g., L in Formula 1 above) and link at least two metal atoms via a chemical bond. Counter reactants may include water, peroxides (e.g., hydrogen peroxide), di- or polyhydroxy alcohols, fluorinated di- or polyhydroxy alcohols, fluorinated glycols, and other sources of hydroxy moieties. In various embodiments, the counter reactant reacts with the organometallic precursor by forming oxygen bridges between adjacent metal atoms. Other potential counter reactants include hydrogen sulfide and hydrogen disulfide, which can bridge metal atoms via sulfur bridges.
[0066] In addition to the organometallic precursor and counter reactant, the thin film may include optional materials to modify the chemical or physical properties of the film, such as to modify the film's sensitivity to EUV or to enhance etch resistance. Such optional materials may be introduced, such as by doping, during vapor formation prior to deposition on the substrate, after deposition of the film, or both. In some embodiments, a mild remote H2 plasma may be introduced to replace some Sn-L bonds with Sn-H, which may enhance the reactivity of the resist under EUV.
[0067] In various embodiments, the EUV patternable film is prepared and deposited on the substrate using deposition equipment and processes, among others known in the art. In such processes, a polymerized organometallic material is formed in the gas phase or in situ on the surface of the substrate. Suitable processes include, for example, chemical vapor deposition (CVD), atomic layer deposition (ALD) with CVD equipment, such as ALD, and discontinuous ALD-like processes where the metal precursor and counter reactant are separated in either time or space.
[0068] In general, the method includes mixing a vapor flow of an organometallic precursor with a vapor flow of a counter reactant to form a polymerized organometallic material, and depositing the organometallic material on a surface of a semiconductor substrate. As will be appreciated by those skilled in the art, the mixing and deposition aspects of the process can be simultaneous in a substantially continuous process.
[0069] In an exemplary sequential CVD process, two or more gas flows of organometallic precursors and a source of counter reactant in separate inlet paths are introduced into a deposition chamber of a CVD apparatus, where they mix and react in the gas phase to form an aggregated polymeric material (e.g., via metal-oxygen-metal bond formation). The flows can be introduced, for example, using separate inlets or a dual plenum showerhead. The apparatus is configured to mix the flows of organometallic precursors and counter reactants in the chamber, allowing them to react to form a polymerized organometallic material. Without limiting the mechanism, function, or utility of the present technology, it is believed that the products of such gas phase reactions have a heavier molecular weight due to metal atoms being cross-linked by the counter reactant, which are then condensed or otherwise deposited onto a substrate. In various embodiments, the steric hindrance of the bulky alkyl groups prevents the formation of a close-packed network, producing a porous, low-density film.
[0070] CVD processes are typically carried out at reduced pressures, such as between 10 mTorr and 10 Torr. In some embodiments, the processes are carried out at between 0.5 and 2 Torr. The temperature of the substrate is preferably equal to or less than the temperature of the reaction stream. For example, the temperature of the substrate can be between 0° C. and 250° C., or between ambient temperature (e.g., 23° C.) and 150° C. In various processes, deposition of the polymerized organometallic material on the substrate occurs inversely proportional to the surface temperature.
[0071] The thickness of the EUV patterning formed on the substrate surface may vary according to the surface characteristics, the material used, and the processing conditions. In various embodiments, the film thickness may range from 0.5 nm to 100 nm, and is preferably thick enough to absorb most of the EUV light under the EUV patterning conditions. For example, the total absorption of the resist film may be 30% or less (e.g., 10% or less or 5% or less) so that the resist material at the bottom of the resist film is fully exposed. In some embodiments, the film thickness is 10 to 20 nm. Without limiting the mechanism, function, or utility of the present technology, it is believed that unlike the wet spin-coating processes of the art, the process of the present technology has fewer limitations on the surface adhesion characteristics of the substrate and therefore can be applied to a variety of substrate types. Furthermore, as discussed above, the deposited film may closely conform to surface features, which is advantageous in forming a mask on a substrate, such as an underlying substrate, without planarizing such features by "filling" such features.
[0072] After depositing the photoresist on the substrate, the method 100 includes diffusing the solubility modifier into the photoresist at block 108. The diffusion of the solubility modifier into the photoresist can provide a layer of polarity modified resist. In one or more embodiments, the diffusion of the solubility modifier into the photoresist is accomplished by performing a bake. The bake can be performed on a hot plate or in an oven. The temperature and time of the bake can depend on the composition of the photoresist and the desired amount of diffusion of the solubility modifier into the photoresist. Suitable conditions for the bake can include a temperature in the range of 50° C. to 160° C. and a time in the range of about 30 to 90 seconds. In one or more embodiments, after baking, a solubility modified region, i.e., a layer of polarity modified resist, can be present at the bottom portion of the photoresist. The solubility modified region of the first photoresist can also be referred to herein as a “footer layer.” The amount of diffusion of the solubility modifier can correspond to the thickness of the footer layer. In some embodiments, the footer layer extends into the second resist and has a thickness of about 1 to about 60 nm. For example, the thickness of the footer layer may range from a lower limit of one of 1 nm, 5 nm, 10 nm, 15 nm, 20 nm, and 25 nm to an upper limit of one of 40 nm, 45 nm, 50 nm, 55 nm, and 60 nm, where any lower limit may be paired with any mathematically compatible upper limit.
[0073] As described above, diffusion of the solubility modifier may provide a footer layer on the bottom portion of the photoresist. A coated substrate including a footer layer is shown in FIG. 2D. As shown in FIG. 2D, the coated substrate includes a substrate 201 and an underlayer 202. Underlayer 202 is coated with a solubility modifier 203. Photoresist 204 is coated on the solubility modifier and substrate. A footer layer 205 is shown on the bottom portion of photoresist 204.
[0074] The footer layer may have a different solubility than the areas of the photoresist that were not exposed to the solubility modifier, i.e., the top part of the photoresist. Thus, the footer layer and the unexposed areas of the photoresist may be soluble in different developers.
[0075] In block 112 of method 100, the photoresist is exposed to a pattern of actinic radiation. The photoresist can be exposed to actinic radiation using a KrF excimer laser at 248 nm, an ArF excimer laser at 193 nm, or an extreme ultraviolet (EUV) exposure tool at 13.5 nm. In a particular embodiment, the photoresist is exposed to an EUV exposure tool at 13.5 nm.
[0076] To impart a shape or relief pattern to the photoresist, a mask may be used to block portions of the photoresist from the actinic radiation. After exposure to actinic radiation, the unexposed portions of the resist may have a different solubility than the exposed portions of the resist. Thus, subsequent development of the photoresist, such as rinsing with a photoresist developer, as shown in block 114 of method 100, will dissolve either the unexposed or exposed portions. Notably, in one or more embodiments, a footer layer at the bottom portion of the photoresist is not dissolved by the photoresist developer. FIG. 2E illustrates the substrate after the photoresist has been exposed to a pattern of actinic radiation and developed with a photoresist developer. As shown in FIG. 2E, the relief pattern includes structures 204' created by the photoresist that are separated by gaps. At the base of the structures, a footer layer 205 remains.
[0077] As noted above, development of a photoresist after exposure to a pattern of actinic radiation dissolves either the unexposed or exposed portions. When the unexposed portions of the resist remain after rinsing with a developer, the relief pattern provided is a positive-tone developed resist. In contrast, when the exposed portions of the resist remain after rinsing with a developer, the relief pattern provided is either a negative-tone developed resist or a negative-tone developed resist.
[0078] In some embodiments, the photoresist is a positive tone developed (PTD) resist. In such embodiments, the relief pattern may include a polymer made from the above monomers, where any monomers containing reactive functional groups are protected. Thus, the PTD photoresist may be organic soluble, whereby a relief pattern may be provided by rinsing with a photoresist developer that is basic. Suitable basic photoresist developers include quaternary ammonium hydroxides, such as tetramethylammonium hydroxide (TMAH).
[0079] In other embodiments, the photoresist is a negative resist. In such embodiments, the first relief pattern can include a polymer made from the above monomers, and any monomers that include reactive functional groups are not protected. Exposure to actinic radiation causes crosslinking of the polymer in the exposed areas, making the polymer insoluble to the developer. The unexposed and thus uncrosslinked areas can then be removed using a suitable developer to form the relief pattern.
[0080] In yet other embodiments, the photoresist is a negative tone developed (NTD) photoresist. Similar to PTD photoresists, NTD photoresists may include polymers made from the monomers described above, with any monomers that contain reactive functional groups being protected. Thus, NTD photoresists may be organic soluble, but rather than developing exposed areas with a resist developer that is basic, a relief pattern may be provided by rinsing the photoresist with a photoresist developer that includes an organic solvent. Suitable organic solvents that may be used as the first resist developer include n-butyl acetate (NBA) and 2-heptanone.
[0081] As described above and shown in FIG. 2E, a relief pattern is provided on a footer layer and includes structures of photoresist separated by gaps. In one or more embodiments, the presence of the footer layer provides the structures with a structurally strong base. For example, the presence of the footer layer may limit or prevent undercutting of the photoresist that typically occurs during development.
[0082] Finally, in block 114, the method 100 includes removing the portions of the footer layer that reside under the gaps of the relief pattern. The portions of the footer layer that reside under the gaps of the relief pattern may be removed by methods known in the art, such as, for example, a plasma dry etching process. In one embodiment, the etching process may be an anisotropic etching process, such as a reactive ion etching process. In some embodiments, if the organic material is a purely hydrocarbon-based material, the etchant may be a dry etchant, such as O2 or a halide-based plasma. In one or more embodiments, the solubility modifier coating may remain on the underlying layer. In such embodiments, the remaining solubility modifier coating is removed along with the portions of the footer layer that reside under the gaps of the relief pattern. Thus, an etched photoresist that includes a uniform structure may be provided. For example, FIG. 2F shows a coated substrate that includes a footer layer 205′, a layer of solubility modifier 203′, and a structure of etched photoresist 204′ provided on an underlying layer 202 on a substrate 201. In embodiments in which the solubility modifier is absorbed into the underlying layer, no film of solubility modifier is present at this point in the method. The etched photoresist produced according to method 100 can provide uniform structures with a structurally strong base without undercuts.
[0083] Method 100 represents one possible embodiment and is not intended to limit the invention. As will be appreciated by those skilled in the art, the invention may encompass a variety of alternative methods, such as a method in which the photoresist is exposed to a pattern of actinic radiation before the solubility modifier is diffused into the photoresist. In such alternative embodiments, the components and techniques used in the method may be as described above with respect to method 100.
[0084] In one or more embodiments, actinic radiation is applied to the photoresist prior to diffusion of the solubility modifier. In such embodiments, the method may include first depositing an underlayer on the substrate and then coating the underlayer with the solubility modifier. Photoresist may then be laminated onto the substrate, thereby covering the solubility modifier. At this point, the photoresist may be exposed to a pattern of actinic radiation, such as by using an EUV exposure tool. The solubility modifier may then be diffused into the photoresist a predetermined distance to provide a footer layer composed of solubility-modified photoresist. After the solubility modifier has diffused into the photoresist, the substrate may be developed and etched as described with respect to method 100 to provide a relief pattern including a uniform structure of photoresist without undercuts.
[0085] Alternatively, in one or more embodiments, the non-amplified chemical resist is a photoresist and the strong secondary electron emitter is an underlayer. Secondary electron emission is a method of electron emission from a surface, typically a metal or metal oxide surface. When actinic radiation is injected into a metal oxide, secondary electrons are emitted from the surface. This phenomenon can be used to create the desired effect of a footer layer or adhesion layer at the resist and substrate interface. In such an embodiment, the method is shown in and described with reference to FIG. 3. As shown, in block 302, the method 100 first includes depositing an underlayer on a substrate. The substrate is as previously described. The underlayer can be a secondary electron emitter layer. Suitable secondary electron emitting underlayers include, but are not limited to, magnesium oxide, beryllium oxide, and combinations thereof. In some embodiments, the secondary electron emitter layer is deposited with a strong absorber, such as tin oxide (SnO). In some embodiments, the underlayer includes multiple secondary electron emitter layers.
[0086] Method 300 then includes depositing a photoresist on the substrate at block 304. In one or more embodiments, the photoresist is an EUV resist. Suitable EUV resists include organometallic resists and dry resists, as described above with respect to method 100. Additionally, in some embodiments, the photoresist includes other additives, such as those additives described above with respect to method 100.
[0087] After depositing the photoresist on the substrate, the method 300 includes exposing the photoresist to a pattern of actinic radiation at block 306. In one or more embodiments, the pattern of actinic radiation has a wavelength in the EUV spectrum, such as, for example, 13.5 nm.
[0088] Due to the presence of the secondary electron emitter layer, the photoresist can receive additional chemical exposure near the surface; that is, the region at the interface between the secondary electron emitter layer and the photoresist layer can become polarity-changed or cross-linked, depending on the tone of the resist. Unlike conventional adhesion techniques, the process is based on improving the exposure of the bottom part of the photoresist. Thus, the secondary electron emitter layer provides a "footer layer" for the photoresist in improving the exposure of the bottom part of the photoresist to the pattern of actinic radiation. This reduces the roughness of the line edges and allows direct patterning into the resist.
[0089] As described above, a mask may be used to block portions of the photoresist from actinic radiation to impart a feature or relief pattern to the photoresist. After exposure to actinic radiation, the unexposed portions of the resist may have a different solubility than the exposed portions of the resist. Thus, subsequent development of the photoresist, such as rinsing with a photoresist developer, as shown in block 308 of method 300, dissolves either the unexposed or exposed portions. Notably, in one or more embodiments, a footer layer at the bottom portion of the photoresist is insoluble in the photoresist developer. In one or more embodiments, the presence of the footer layer provides a structure with a structurally strong base. For example, the presence of the footer layer may limit or prevent undercutting of the photoresist that typically occurs during development.
[0090] Finally, in block 310, the method 300 includes removing the portions of the footer layer that reside under the gaps in the relief pattern. Removal of the footer layer may be performed as described above with respect to method 100. The etched photoresist produced according to method 300 can provide a uniform structure with a structurally strong base without undercuts.
[0091] Although only a few exemplary embodiments have been described in detail above, those skilled in the art will readily appreciate that many modifications are possible in the exemplary embodiments without materially departing from the invention, and all such modifications are therefore intended to be included within the scope of this disclosure, as defined in the following claims.
Claims
1. 1. A method of patterning a substrate, comprising the steps of: depositing an underlayer on the substrate; coating the underlayer with a solubility modifier; depositing a photoresist onto the substrate such that the photoresist covers the solubility modifier; diffusing the solubility modifier a predetermined distance into the photoresist to provide a solubility modified region of the photoresist, the solubility modified region forming a footer layer on a bottom portion of the photoresist; exposing the photoresist to a pattern of actinic radiation; developing the photoresist to form a relief pattern on the footer layer, the relief pattern including structures separated by gaps; and e.g., etching the substrate to remove portions of the footer layer under the gap, thereby providing a uniform structure.
2. 1. A method of patterning a substrate, comprising the steps of: depositing an underlayer on the substrate; coating the underlayer with a solubility modifier; depositing a photoresist onto the substrate such that the photoresist covers the solubility modifier; exposing the photoresist to a pattern of actinic radiation; diffusing the solubility modifier a predetermined distance into the photoresist to provide a solubility modified region of the photoresist, the solubility modified region forming a footer layer on a bottom portion of the photoresist; developing the photoresist to form a relief pattern on the footer layer, the relief pattern including structures separated by gaps; and e.g., etching the substrate to remove portions of the footer layer underlying the gap, thereby providing a uniform structure.
3. The method of claim 1 or 2, wherein the underlayer is a bottom antireflective coating (BARC) layer.
4. The method of claim 1 or 2, wherein the solubility modifier comprises an acid generator.
5. The method of claim 4 , wherein the acid generator is fluorine-free.
6. 5. The method of claim 4, wherein the acid generator is selected from the group consisting of pyridinium perfluorobutanesulfonate, 3-fluoropyridinium perfluorobutanesulfonate, 4-t-butylphenyl tetramethylenesulfonium perfluoro-1-butanesulfonate, 4-t-butylphenyl tetramethylenesulfonium 2-trifluoromethylbenzenesulfonate, 4-t-butylphenyl tetramethylenesulfonium 4,4,5,5,6,6-hexafluorodihydro-4H-1,3,2-dithiazine 1,1,3,3-tetraoxide, triphenylsulfonium antimonate, and combinations thereof.
7. The method of claim 1 or 2, wherein the solubility modifier comprises an acid.
8. The method of claim 7 , wherein the acid is fluorine-free.
9. 8. The method of claim 7, wherein the acid is selected from the group consisting of trifluoromethanesulfonic acid, perfluoro-1-butanesulfonic acid, p-toluenesulfonic acid, 4-dodecylbenzenesulfonic acid, 2,4-dinitrobenzenesulfonic acid, 2-trifluoromethylbenzenesulfonic acid, and combinations thereof.
10. The method of claim 1 or 2, wherein the solubility modifier comprises a base.
11. The method of claim 1 or 2, wherein the solubility modifier comprises a base generator.
12. 3. The method of claim 1 or 2, wherein the solubility modifier comprises a matrix polymer comprising monomers having ethylenically unsaturated polymerizable double bonds, including (meth)acrylate monomers; (meth)acrylic acid; aromatic vinyl monomers such as styrene, hydroxystyrene, vinyl naphthalene, and acenaphthylene; vinyl alcohol; vinyl chloride; vinyl pyrrolidone; vinyl pyridine; vinyl amine; vinyl acetal; maleic anhydride; maleimide; norbornene; and combinations thereof.
13. 3. The method of claim 1 or 2, wherein the solubility modifier comprises a matrix polymer comprising monomers containing one or more functional groups selected from hydroxy, carboxyl, sulfonic acid, sulfonamide, silanol, fluoroalcohol, anhydride, lactone, ester, ether, allylamine, pyrrolidone, and combinations thereof.
14. 3. The method of claim 1 or 2, further comprising diffusing the solubility modifier into the underlayer immediately after coating the underlayer with the solubility modifier.
15. The method of claim 14 , wherein diffusing the solubility modifier into the underlayer is accomplished by performing a bake.
16. The method of claim 1 or 2, wherein the photoresist is an EUV resist.
17. The method of claim 1 or 2, wherein the footer layer comprises areas where the solubility of the photoresist is altered.
18. The method of claim 1 or 2, further comprising removing the solubility modifier remaining on the underlayer after removing the portion of the footer layer that resides under the gap.
19. After coating the underlayer with the solubility modifier, allowing the solubility modifier to diffuse into the underlayer; 3. The method of claim 1 or 2, further comprising rinsing to remove residual solubility modifier.
20. 1. A method of patterning a substrate, comprising the steps of: depositing an underlayer on the substrate, the underlayer including a secondary electron emitter; depositing a photoresist onto the substrate such that the photoresist covers the underlayer; exposing the photoresist to a pattern of actinic radiation, where the secondary electron emitter layer enhances exposure of a bottom portion of the photoresist and provides a footer layer having a different polarity than a top portion of the photoresist; developing the photoresist to form a relief pattern on the footer layer, the relief pattern including structures separated by gaps; and etching the substrate to remove portions of the footer layer under the gap, thereby providing a uniform structure.
21. 21. The method of claim 20, wherein the secondary electron emitter is selected from the group consisting of magnesium oxide, beryllium oxide, and combinations thereof.
22. 21. The method of claim 20, wherein the photoresist is an EUV resist.
Citation Information
Patent Citations
Forming method for photoresist pattern and semiconductor element
JP2003195521A
Silicon-containing surface modifier, composition for resist underlayer film formation containing the same, and method for pattern formation
JP2013166812A
Mask blank, method for manufacturing mask blank, and method for manufacturing transfer mask
JP2016066019A
Mask formation method
JP2020030291A
Composition for forming silicon-containing resist underlayer film and patterning process
JP2020184062A