Alumina aqueous dispersion for ceramics and refractories and its manufacturing method

The alumina aqueous dispersion with controlled particle size, pH, and organic acid composition addresses residual carbon issues, enabling low-temperature thermal decomposition and effective use in ceramics and refractories.

JP7560190B1Active Publication Date: 2024-10-02ASADA KAGAKU IND
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024003209
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-01-12
Publication Date
2024-10-02
Estimated Expiration
2044-01-12

AI Technical Summary

Technical Problem

Existing alumina aqueous dispersions leave residual carbon when fired at temperatures below 600°C, making them unsuitable for low-temperature firing applications in ceramics and refractories.

Method used

An alumina aqueous dispersion with specific properties: average particle diameter of 10 to 1000 nm, amorphous and/or χ alumina crystal system, pH of 2.0 to 5.3, containing formic acid or a mixture of formic and acetic acid as organic acids, and ammonia as alkali, with a thixotropic index of 2 to 10, and low alkali metal or halogen content, produced through a method involving precipitation, washing, and concentration steps.

Benefits of technology

The dispersion allows for complete thermal decomposition at low temperatures, ensuring no residual carbon, excellent transparency, and sinterability, suitable for inorganic binders, surface modification, and abrasive applications without agglomeration or alkali/halogen issues.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007560190000001_ABST
    Figure 0007560190000001_ABST
Patent Text Reader

Abstract

The present invention provides an aqueous alumina dispersion which leaves no residual carbon even when fired at 600° C. or less and is useful for forming refractories by firing ceramics and the like. [Solution] The present invention relates to an alumina aqueous dispersion containing alumina particles as dispersed particles, and the dispersion has the following characteristics: (1) an average particle size of 10 to 1000 nm when the alumina dispersed particles are measured on a number basis, (2) the crystal system of the alumina particles when the alumina aqueous dispersion is dried at 100°C is amorphous and / or x-alumina, (3) the pH of the alumina aqueous dispersion is in the range of 2.0 to 5.3, (4) the alumina aqueous dispersion contains an organic acid and an alkali, the organic acid being formic acid or a combination of formic acid and acetic acid, and the alkali being ammonia, and (5) the alumina (Al 2 O 3 The present invention provides an alumina aqueous dispersion satisfying the above condition: its alumina concentration in terms of 0.5 to 11.5 mass %; and a method for producing the same.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an aqueous alumina dispersion for use in ceramics and refractories, and a method for producing the same. [Background technology]

[0002] Alumina aqueous dispersions in which alumina particles are dispersed in water are currently used for various purposes.

[0003] Japanese Patent No. 7308650 (Patent Document 1) describes a large particle size alumina dispersion that satisfies all of the following: alumina particles are dispersed, the dispersed particles have an average particle size of 50 to 3000 nm, the crystal form of the alumina when dried at 100°C is boehmite or pseudo-boehmite, the pH is 5.5 to 9, the alumina particle dispersion contains an organic acid and an alkali, the organic acid is lactic acid and / or malic acid, and the alkali is at least one of ammonia and an alkali metal. This large particle size alumina dispersion has a problem in that it cannot be used for low temperature firing applications because residual carbon remains when fired at a firing temperature of 600°C or less. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 7308650 Summary of the Invention [Problem to be solved by the invention]

[0005] An object of the present invention is to provide an aqueous alumina dispersion which leaves no residual carbon even when fired at 600° C. or less and is useful for forming refractories by firing ceramics and the like. [Means for solving the problem]

[0006] That is, the present invention provides the following aspects: [1] An alumina aqueous dispersion containing alumina particles as dispersed particles, the dispersion having the following characteristics: (1) The average particle size of the alumina dispersed particles measured by number is in the range of 10 to 1000 nm; (2) When the aqueous alumina dispersion is dried at 100°C, the crystal system of the alumina particles is amorphous and / or chi-alumina, (3) The pH of the aqueous alumina dispersion is in the range of 2.0 to 5.3; (4) Alumina water dispersion is an organic acid and an alkali, the organic acid being formic acid or a combination of formic acid and acetic acid, and the alkali being ammonia; (5) Alumina (Al) contained in the alumina aqueous dispersion 2 O 3 ) converted concentration is 0.5 to 11.5 mass%, An alumina aqueous dispersion that satisfies the above requirements. [2] The alumina aqueous dispersion according to [1], wherein the alumina aqueous dispersion has a thixotropic index (TI value=rotation speed 6 rpm / rotation speed 60 rpm) of 2 to 10 as measured by a Brookfield viscometer. [3] The alumina aqueous dispersion according to [1] or [2], wherein the alumina aqueous dispersion contains an alkali metal or a halogen element in a range of 0 to 0.03 mass % based on the total weight of the solid components in the alumina aqueous dispersion. [4] The alumina aqueous dispersion according to [1] or [2], which is used for forming a ceramic or a refractory material. [5] a first step of adding aqueous ammonia to an aqueous solution of an aluminum salt selected from aluminum nitrate and aluminum sulfate to adjust the pH to 5 to 8, and then stirring the solution at a temperature in the range of 15 to 45° C. for 0.5 to 3 hours to form a precipitate of amorphous aluminum hydroxide; A second step of washing the produced amorphous aluminum hydroxide and then drying it to a moisture content of 60 to 80%; a third step of adding water to the dried amorphous aluminum hydroxide, dispersing the mixture, and then adding 1.8 to 10 moles of formic acid or a mixture of formic acid and acetic acid per mole of aluminum, followed by stirring at 40 to 80° C. for 1 to 3 hours to obtain an aqueous solution of aluminum formate or an aqueous solution of a mixture of aluminum formate and aluminum acetate; and a fourth step of concentrating the obtained aqueous aluminum formate solution or the aqueous solution of a mixture of aluminum formate and aluminum acetate at a temperature of 90 to 120° C. for 1 to 24 hours; The method for producing an aqueous alumina dispersion according to [1], [6] The production method according to [5], characterized in that, when the volume of the aqueous aluminum formate solution or the aqueous solution of a mixture of aluminum formate and aluminum acetate obtained in the third step is taken as C, and the volume obtained by subsequent heating and concentrating at 90 to 120°C for 1 to 24 hours in the fourth step is taken as D, the solution is concentrated so that the volume concentration ratio (D / C) is 0.3 to 0.8. Effect of the Invention

[0007] The alumina aqueous dispersion according to the present invention can be used as alumina by pyrolyzing organic components at a low temperature of 600°C or less, and has an average particle size of 10 to 1000 nm, and is excellent in transparency and sinterability, so it can be used as an alumina coating for glass, metal, etc., an inorganic binder for bonding inorganic powder of ceramics and refractories, surface modification of catalyst carriers, fine abrasives, etc. The alumina aqueous dispersion of the present invention does not leave any carbon residue even when fired at a low temperature of 600°C or less, and contains almost no alkali metals or halogens that cause problems during firing. Furthermore, the alumina aqueous dispersion of the present invention has a thixotropic property that allows it to have shape retention when mixed with an inorganic filler. [Brief description of the drawings]

[0008] [Figure 1] 1 is an electron microscope photograph of the alumina aqueous dispersion of Example 1 dried in a glass evaporating dish at 100° C. for 10 minutes, observed at 100,000 times with an FE-SEM (JSM-7001F manufactured by JEOL Ltd.). [Diagram 2]FIG. 2 is an X-ray diffraction diagram of a powder obtained by drying the alumina aqueous dispersion of Example 1 in a glass evaporating dish at 100° C. for 20 minutes in a hot air circulation dryer, and measuring the powder with an X-ray diffractometer (Smartlab 9 kW: manufactured by Rigaku Corporation). [Diagram 3] The alumina aqueous dispersion of Example 1 was dried in a glass evaporating dish using a hot air circulation dryer at 100°C for 20 minutes, the powder was placed in an alumina crucible, and fired in an electric furnace (FO200: manufactured by Yamato Scientific Co., Ltd.) at 700°C for 2 hours. This shows an X-ray diffraction pattern of the powder measured using an X-ray diffractometer (Smartlab 9kw: manufactured by Rigaku Corporation). [Figure 4] 2 is a graph showing the results of measuring the particle size distribution of the alumina aqueous dispersion of Example 1 on a number basis. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The present invention will be described in detail below based on preferred embodiments, but the present invention is not limited to the following embodiments and various modifications are possible within the scope of the claims. In this specification, the expression "numeric value 1 to numerical value 2" in a numerical range indicates that numerical value 1 is the lower limit and numerical value 2 is the upper limit. This means a range including numerical value 1 and numerical value 2 at both ends, and is synonymous with "numerical value 1 or more and numerical value 2 or less."

[0010] Since aluminum has an oxidation number of 3, when it forms a salt with an acid, not all of the bonds form bonds with the acid group, but some may bond. Specifically, as described below, the salt with formic acid is Al(OH) 2 (OOCH), Al(OH)(OOCH) 2 and Al(OOCH) 3 In the present specification, the salt with an acid includes all three of these cases.

[0011] (Alumina water dispersion) The average particle size of the alumina dispersion particles in the alumina aqueous dispersion of the present invention measured by number distribution is preferably 10 to 1000 nm, more preferably 30 to 100 nm. If the average particle size is less than 10 nm, the binding with inorganic particles is poor, and there is a problem that the shape retention during molding is poor. On the other hand, if it exceeds 1000 nm, the average particle size is too large, and when inorganic powders of several hundred nm in size are bound and sintered, the primary particles may become foreign matter and become the starting point of destruction. Here, the "average particle size" means the average particle size measured by number standard by dynamic light scattering method using Zetasizer Nano ZS (manufactured by Spectris Co., Ltd.) in an aqueous solvent.

[0012] The alumina crystal system in the alumina aqueous dispersion of the present invention is preferably amorphous and / or chi-alumina, since it undergoes phase transition to gamma alumina or alpha alumina during high-temperature sintering of ceramics or the like depending on the firing conditions.

[0013] The pH of the alumina aqueous dispersion of the present invention is 2.0 to 5.3, and more preferably 3.0 to 4.7. If the pH is less than 2.0, it becomes strongly acidic, and tends to alter inorganic particles when mixed with inorganic particles, or to corrode metals when the alumina aqueous dispersion comes into contact with them. On the other hand, if the pH exceeds 5.3, the alumina dispersion will aggregate when an acidic environment is required for refractory molding, catalyst carrier production, etc. The pH of the alumina aqueous dispersion is measured using a portable pH meter "HM-40P" and a pH composite electrode "GST-2739C" manufactured by Toa DKK Co., Ltd.

[0014] The alumina aqueous dispersion of the present invention contains a short-chain carboxylic acid such as formic acid or a mixture of formic acid and acetic acid, and is designed to have good thermal decomposition properties at low temperatures. Alumina aqueous dispersions containing lactic acid, malic acid, etc. as described in Patent Document 1 have poor thermal decomposition properties and leave carbon residue, so they are considered to be unsuitable for thermal decomposition at low temperatures (for example, 500 to 600°C).

[0015] The alumina (Al) in the alumina aqueous dispersion of the present invention 2 O 3The alumina-equivalent concentration is preferably 0.5 to 11.5 mass%. The alumina-equivalent concentration is preferably in the range of 0.8 to 10.5 mass%, more preferably 2 to 10 mass%. If it is less than 0.3 mass%, the alumina concentration in the alumina aqueous dispersion is too low, resulting in poor adhesion when used as a binder for inorganic particles and no thixotropy. If it exceeds 11.5 mass%, the storage stability of the aluminum formate or the mixture of aluminum formate and aluminum acetate is poor, and there is a problem that precipitates are precipitated in the alumina aqueous dispersion over time.

[0016] The alumina (Al) in the alumina aqueous dispersion of the present invention 2 O 3 The calculated concentration is calculated as follows: The aluminum concentration in the alumina aqueous dispersion was measured using an emission spectrometer (Agilent 5110 ICP-OCS: manufactured by Agilent Technologies). The atomic weight of aluminum was 27, the atomic weight of oxygen was 16, and the atomic weight of Al was 27. 2 O 3 The molecular weight is calculated using the following formula: Al 2 O 3 Converted concentration (mass%) = Al concentration (mass%) × (102 / 27)

[0017] The alumina aqueous dispersion of the present invention preferably has a TI value (thixotropic index value) of 2 to 10, more preferably 2.5 to 7, and even more preferably 3 to 8, measured with a B-type viscometer (using a TVB10M TM-3 spindle rotor manufactured by Toki Sangyo Co., Ltd.). The TI value was calculated by (rotation speed 6 rpm) / (rotation speed 60 rpm). If the TI value is less than 2, the liquid property does not have structural viscosity, so that it becomes difficult to maintain the shape when a mixture of inorganic particles and the alumina aqueous dispersion is placed in a mold and molded, and the shape collapses. If the TI value exceeds 10, the structural viscosity is too strong, so that it becomes difficult to deform unless the shear rate is increased, and it becomes difficult to perform pouring or the like when molding using a mold.

[0018] The alumina aqueous dispersion of the present invention preferably contains almost no alkali metal or halogen element. The alkali metal or halogen element is preferably contained in the alumina aqueous dispersion of the present invention in a range of 0 to 0.03 mass%, preferably 0 to 0.02 mass%. Specific examples of the alkali metal include sodium and potassium, and specific examples of the halogen element include chlorine, bromine, and iodine. If the content of the alkali metal exceeds 0.03 mass%, when used in refractories, ceramics, etc., the sintering temperature tends to decrease when firing is performed, and defects in the sintered body tend to occur. If the content of the halogen element exceeds 0.03 mass%, when used in refractories, ceramics, etc., gases derived from each element are generated when firing is performed, and there is a problem of corrosion in the furnace. The content of these elements is measured by drying the alumina aqueous dispersion at 80°C for 30 minutes and measuring the powder obtained by drying with an energy dispersive X-ray fluorescence (EDX) equipped with a scanning electron microscope JCM-7000 manufactured by JEOL Ltd.

[0019] The alumina aqueous dispersion of the present invention does not leave any carbon residue at low temperatures of 600°C or less, and does not generate halogen gases or the like during firing. In addition, it is possible to impart shape retention by mixing it with an inorganic filler, and it can be used without coagulation even in an acidic region. The alumina aqueous dispersion of the present invention can be effectively used for forming ceramics and refractories.

[0020] (Method of producing alumina aqueous dispersion) The alumina aqueous dispersion of the present invention can be produced by the following method: a first step of adding aqueous ammonia to an aqueous solution of an aluminum salt selected from aluminum nitrate and aluminum sulfate to adjust the pH to 5 to 8, and then stirring the solution at a temperature in the range of 15 to 45° C. for 0.5 to 3 hours to form a precipitate of amorphous aluminum hydroxide; A second step of washing the produced amorphous aluminum hydroxide and then drying it to a moisture content of 60 to 80%; a third step of adding water to the dried amorphous aluminum hydroxide, dispersing the mixture, and then adding 1.8 to 10 moles of formic acid or a mixture of formic acid and acetic acid per mole of aluminum, followed by stirring at 40 to 80° C. for 1 to 3 hours to obtain an aqueous solution of aluminum formate or an aqueous solution of a mixture of aluminum formate and aluminum acetate; and a fourth step of concentrating the obtained aqueous aluminum formate solution or the aqueous solution of a mixture of aluminum formate and aluminum acetate at a temperature of 90 to 120° C. for 1 to 24 hours; Includes:

[0021] In the first step, ammonia water is added to an aqueous solution of an aluminum salt (specifically, aluminum nitrate or aluminum sulfate) to form a precipitate of amorphous aluminum hydroxide. This step is carried out by stirring at a temperature range of 15 to 45°C for 0.5 to 3 hours. This step is preferably carried out by stirring at 20 to 35°C for 1 to 2 hours. If the temperature is less than 15°C, the reactivity of aluminum nitrate or aluminum sulfate with ammonia becomes poor, and the reaction takes time, while if the temperature exceeds 45°C, the ammonia content volatilizes violently, and the pH tends to be unstable. In addition, if the stirring time is less than 0.5 hours, the reaction time tends to be insufficient and amorphous aluminum hydroxide does not precipitate sufficiently, and if it exceeds 3 hours, amorphous aluminum hydroxide can be synthesized, but the reaction time takes too long, resulting in poor productivity. At the time of adding ammonia water, the pH is 5 to 8. More preferably, the pH is 6 to 7. If the pH is less than 5, it takes a very long time for the amorphous aluminum hydroxide precipitate to settle, resulting in poor productivity, whereas if the pH exceeds 8, dispersibility tends to deteriorate when water is added to the amorphous aluminum hydroxide and dispersed.

[0022] In the second step, the produced amorphous aluminum hydroxide is washed and then dried so that the moisture content is 60 to 80%. Washing is performed by washing with water and then separating the water. Separation of the water may be performed by various methods, including centrifugation. Washing may be performed once, but water is usually added and separated several times, preferably about three times.

[0023] Drying is carried out after the separation of water. A drying step is required so that the moisture content is 60-80%. A more preferable moisture content is 65-75%. If the moisture content is less than 60%, dispersibility will be poor when adding water to the amorphous aluminum hydroxide and dispersing it, and if the moisture content exceeds 80%, the moisture content of the amorphous aluminum hydroxide will be too high, making it difficult to handle and reducing productivity. The moisture content is measured using a heat-drying moisture meter (MX50, manufactured by A&D Co., Ltd.) at 105°C for 40 minutes. Drying may be performed using a shelf dryer.

[0024] The third step is a step of adding water to the dried amorphous aluminum hydroxide, dispersing it, and then adding 1.8 to 10 moles, preferably 1.8 to 6 moles, more preferably 1.8 to 3 moles of formic acid or a mixture of formic acid and acetic acid per mole of aluminum, and stirring at 40 to 80°C for 1 to 3 hours to obtain an aqueous solution of aluminum formate or an aqueous solution of a mixture of aluminum formate and aluminum acetate. If the amount of formic acid or the mixture of formic acid and acetic acid is less than 1.8 moles per mole of aluminum, there is a tendency that the amount of formic acid or the mixture of formic acid and acetic acid is insufficient and an aqueous alumina dispersion is not produced. If the amount of formic acid or the mixture of formic acid and acetic acid is more than 10 moles per mole of aluminum, the amount of formic acid or the mixture of formic acid and acetic acid becomes excessive, the pH of the aqueous alumina dispersion becomes less than 2, and the aqueous alumina dispersion cannot be used because it corrodes metals or dissolves inorganic powders during use.

[0025] The stirring is carried out at 40°C to 80°C, preferably 45°C to 65°C. If the temperature is lower than 40°C, the reaction between the amorphous aluminum hydroxide and formic acid or the mixture of formic acid and acetic acid is insufficient, and unreacted formic acid or the mixture of formic acid and acetic acid remains in the system, resulting in poor storage stability. On the other hand, if the temperature exceeds 80°C, evaporation of water and formic acid becomes significant, and precipitates may form on the walls of the reaction vessel during synthesis.

[0026] The moles of aluminum in the amorphous aluminum hydroxide in the third step are: aluminum atomic weight: 27, oxygen atomic weight: 16, hydrogen atomic weight: 1, Al(OH) 3 The molecular weight of the compound is 78, and is calculated from the following formula: Moles of aluminum = (weight of aluminum hydroxide) x (100 - moisture content) / 100 x (27 / 78) / 27

[0027] When using a combination of formic acid and acetic acid, the ratio (B / A) of the number of moles of formic acid: A to the number of moles of acetic acid: B must be 0 to 0.25, preferably 0 to 0.15. If B / A exceeds 0.25, the amount of acetic acid in the system increases, and precipitation may occur during storage over time.

[0028] The fourth step is a step of concentrating the obtained aqueous aluminum formate solution or the aqueous mixture of aluminum formate and aluminum acetate at a temperature of 90 to 120°C for 1 to 24 hours. The heating method when heating and stirring aluminum formate or aluminum acetate is not particularly limited, and a normal heating method or an autoclave can be used. The stirring method is also no problem as long as it is a normal stirring method, and the reaction temperature is preferably 90 to 120°C, more preferably 95 to 110°C. The reaction time can be arbitrarily determined within 1 to 24 hours, including the productivity. If the heating temperature is less than 90°C, the reaction does not proceed sufficiently and an alumina particle dispersion liquid is not obtained. If the heating temperature exceeds 120°C, a special reaction environment such as applying pressure to increase the temperature is required, which deteriorates the productivity.

[0029] When the volume of the aqueous aluminum formate solution or the aqueous solution of a mixture of aluminum formate and aluminum acetate obtained in the third step is C, and the volume when the aqueous aluminum formate solution is heated and concentrated for 1 to 24 hours at 90 to 120°C in the fourth step is D, it is preferable to concentrate the aqueous aluminum formate solution so that the volume concentration ratio (D / C) is 0.3 to 0.8. Usually, an aqueous alumina dispersion is synthesized by applying heat in a sealed reaction vessel, so that concentration is not performed, but in the present invention, a concentration step is actively provided. If the volume concentration ratio (D / C) is less than 0.3, the aqueous alumina dispersion is excessively concentrated, and it is difficult to maintain the form of the aqueous alumina dispersion. On the other hand, if the volume concentration ratio (D / C) exceeds 0.8, the concentration is insufficient, and there is a problem that an aqueous alumina dispersion cannot be obtained.

[0030] The alumina aqueous dispersion of the present invention must be designed by selecting materials that do not contain halogen gases such as chlorine and bromine that damage furnaces when fired at high temperatures for ceramics and refractories, or alkali metals such as sodium and potassium that lower the sintering temperature of ceramics, refractories, etc. Therefore, when producing an alumina aqueous dispersion, it is necessary to use raw materials that do not contain these elements (i.e., alkali metals and halogen elements) as main components.

[0031] It is important that the alumina aqueous dispersion obtained in the present invention is pyrolyzed by low-temperature firing, and the temperature at which the weight loss is completed is preferably in the range of 400 to 600 ° C, more preferably 450 to 550 ° C. The firing time is preferably in the range of 2 to 300 minutes, more preferably 5 to 60 minutes. If the temperature at which the weight loss due to firing is completed is less than 400 ° C, decomposition will begin when resin is blended and molding is performed at a temperature of about 300 ° C, and there is a problem that the molded body will become unstable. On the other hand, if the temperature at which the weight loss is completed exceeds 600 ° C, when the substrate is exposed to high temperatures during coating on metals, glass, etc., it may melt and deform, making it impossible to coat. If the firing time is less than 2 minutes, the pyrolysis rate is too fast when coating large objects, refractories, and ceramics at a specified temperature, making it easy to generate firing variations between the ends and the center, and if the firing time exceeds 300 minutes, productivity tends to deteriorate. EXAMPLES

[0032] The present invention will be described in more detail with reference to examples, but the present invention is not limited thereto.

[0033] Example 1 2250g of 0.5mol / l aluminum nitrate aqueous solution was put into a 20L separable flask, and then 1160.6g of 13.3mol / l ammonia water was put in while stirring at 250rpm. After stirring at 30℃ for 1 hour, the pH was 6.6. The precipitated amorphous aluminum hydroxide gel was washed by centrifuging at 2,000rpm for 1 minute with a centrifuge (KBS-12 available from Kansai Centrifugal Separation Manufacturing Co., Ltd.) and adding 4L of water three times, and then dried at 100℃ for 1 hour in a tray dryer. The moisture content was 65%. 6695g of water was added to 1137.5g of the dried amorphous aluminum hydroxide gel, and the mixture was stirred and dispersed, and then 2386.6g of 23.1mol / l formic acid was added and stirred at 45℃ for 1 hour at 250rpm to synthesize a basic aluminum formate aqueous solution. 500 ml of the obtained basic aluminum formate aqueous solution (C) was collected in a measuring cylinder, transferred to a separable flask, and heated and concentrated at 250 rpm at 110°C for 8 hours to obtain an alumina aqueous dispersion. The obtained alumina aqueous dispersion was poured into a measuring cylinder, and the volume was measured to be 235 ml (D).

[0034] Example 2 2250g of 0.17mol / l aluminum sulfate aqueous solution was put into a 20L separable flask, and then 1260.6g of 13.3mol / l ammonia water was put in while stirring at 250rpm. After stirring at 30℃ for 1 hour, the pH was 7.0. The precipitated amorphous aluminum hydroxide gel was washed by centrifuging at 2,000rpm for 1 minute with a centrifuge (KBS-12 available from Kansai Centrifugal Separation Manufacturing Co., Ltd.) and adding 4L of water three times, and then dried at 100℃ for 1 hour in a tray dryer. The moisture content was 65%. 6695g of water was added to 1137.5g of the dried amorphous aluminum hydroxide gel, and the mixture was stirred and dispersed, and then 2386.6g of 23.1mol / l formic acid was added and stirred at 45℃ and 250rpm for 1 hour to synthesize a basic aluminum formate aqueous solution. 500 ml of the obtained basic aluminum formate aqueous solution (C) was collected in a measuring cylinder, transferred to a separable flask, and heated and concentrated at 250 rpm at 110°C for 8 hours to obtain an alumina aqueous dispersion. The obtained alumina aqueous dispersion was poured into a measuring cylinder, and the volume was measured to be 225 ml (D).

[0035] Example 3 2250g of 0.5mol / l aluminum nitrate aqueous solution was put into a 20L separable flask, and then 1060.6g of 13.3mol / l ammonia water was put in while stirring at 250rpm. After stirring at 30℃ for 1 hour, the pH was 6.2. The precipitated amorphous aluminum hydroxide gel was centrifuged at 2,000rpm for 1 minute with a centrifuge (KBS-12 available from Kansai Centrifugal Separation Manufacturing Co., Ltd.) and 4L of water was added, which was repeated three times to wash the amorphous aluminum hydroxide gel, and then dried at 100℃ for 1 hour in a tray dryer. The moisture content was 65%. 6695g of water was added to 1137.5g of the dried amorphous aluminum hydroxide gel, and the mixture was stirred and dispersed, and then 2386.6g of 23.1mol / l formic acid was added and stirred at 45℃ and 250rpm for 1 hour to synthesize a basic aluminum formate aqueous solution. 500 ml of the obtained basic aluminum formate aqueous solution (C) was collected in a measuring cylinder, transferred to a separable flask, and heated and concentrated at 250 rpm at 110°C for 8 hours to obtain an alumina aqueous dispersion. The obtained alumina aqueous dispersion was poured into a measuring cylinder, and the volume was measured to be 250 ml (D).

[0036] Example 4 2250g of 0.5mol / l aluminum nitrate aqueous solution was put into a 20L separable flask, and then 1160.6g of 13.3mol / l ammonia water was put in while stirring at 250rpm. After stirring at 30℃ for 1 hour, the pH was 6.6. The precipitated amorphous aluminum hydroxide gel was washed by centrifuging at 2,000rpm for 1 minute with a centrifuge (KBS-12 available from Kansai Centrifugal Separation Manufacturing Co., Ltd.) and adding 4L of water three times, and then dried at 100℃ for 1 hour in a tray dryer. The moisture content was 65%. 6695g of water was added to 1137.5g of the dried amorphous aluminum hydroxide gel, and the mixture was stirred and dispersed, and then 2386.6g of 23.1mol / l formic acid was added and stirred at 45℃ for 1 hour at 250rpm to synthesize a basic aluminum formate aqueous solution. The obtained basic aluminum formate aqueous solution (500 ml) (C) was collected in a measuring cylinder, transferred to a separable flask, and heated and concentrated at 250 rpm at 120°C for 6 hours to obtain an alumina aqueous dispersion. The obtained alumina aqueous dispersion was poured into a measuring cylinder, and the volume was measured to be 200 ml (D).

[0037] Example 5 2250g of 0.5mol / l aluminum nitrate aqueous solution was put into a 20L separable flask, and then 1160.6g of 13.3mol / l ammonia water was put in while stirring at 250rpm. After stirring at 30℃ for 1 hour, the pH was 6.6. The precipitated amorphous aluminum hydroxide gel was washed by centrifuging at 2,000rpm for 1 minute with a centrifuge (KBS-12 available from Kansai Centrifugal Separation Manufacturing Co., Ltd.) and adding 4L of water three times, and then dried at 100℃ for 1 hour in a tray dryer. The moisture content was 65%. 6695g of water was added to 1137.5g of the dried amorphous aluminum hydroxide gel, and the mixture was stirred and dispersed, and then 2386.6g of 23.1mol / l formic acid was added and stirred at 45℃ for 1 hour at 250rpm to synthesize a basic aluminum formate aqueous solution. 500 ml of the obtained basic aluminum formate aqueous solution (C) was collected in a measuring cylinder, transferred to a separable flask, and heated and concentrated at 250 rpm at 100°C for 20 hours to obtain an alumina aqueous dispersion. The obtained alumina aqueous dispersion was poured into a measuring cylinder, and the volume was measured to be 235 ml (D).

[0038] Example 6 2250g of 0.5mol / l aluminum nitrate aqueous solution was put into a 20L separable flask, and then 1160.6g of 13.3mol / l ammonia water was put in while stirring at 250rpm. After stirring at 30℃ for 1 hour, the pH was 6.6. The precipitated amorphous aluminum hydroxide gel was centrifuged at 2,000rpm for 1 minute in a centrifuge (KBS-12 available from Kansai Centrifugal Separation Manufacturing Co., Ltd.) and 4L of water was added, which was repeated three times to wash the amorphous aluminum hydroxide gel, and then dried at 100℃ for 1 hour in a tray dryer. The moisture content was 72%. 6695g of water was added to 1137.5g of the dried amorphous aluminum hydroxide gel, and the mixture was stirred and dispersed, and then 1431.9g of 23.1mol / l formic acid was added and stirred at 45℃ and 250rpm for 1 hour to synthesize a basic aluminum formate aqueous solution. 500 ml of the obtained basic aluminum formate aqueous solution (C) was collected in a measuring cylinder, transferred to a separable flask, and heated and concentrated at 250 rpm at 100°C for 20 hours to obtain an alumina aqueous dispersion. The obtained alumina aqueous dispersion was poured into a measuring cylinder, and the volume was measured to be 225 ml (D).

[0039] Example 7 2250g of 0.5mol / l aluminum nitrate aqueous solution was put into a 20L separable flask, and then 1160.6g of 13.3mol / l ammonia water was put in while stirring at 250rpm. After stirring at 30℃ for 1 hour, the pH was 6.6. The precipitated amorphous aluminum hydroxide gel was centrifuged at 2,000rpm for 1 minute with a centrifuge (KBS-12 available from Kansai Centrifugal Separation Manufacturing Co., Ltd.) and 4L of water was added, which was repeated three times to wash the amorphous aluminum hydroxide gel, and then dried at 100℃ for 1 hour in a tray dryer. The moisture content was 65%. 6695g of water was added to 1137.5g of the dried amorphous aluminum hydroxide gel, and the mixture was stirred and dispersed, and then 2386.6g of 23.1mol / l formic acid was added and stirred at 60℃ for 1 hour at 250rpm to synthesize a basic aluminum formate aqueous solution. 500 ml of the obtained basic aluminum formate aqueous solution (C) was collected in a measuring cylinder, transferred to a separable flask, and heated and concentrated at 250 rpm at 110°C for 8 hours to obtain an alumina aqueous dispersion. The obtained alumina aqueous dispersion was poured into a measuring cylinder, and the volume was measured to be 225 ml (D).

[0040] Example 8 2250g of 0.5mol / l aluminum nitrate aqueous solution was added to a 20L separable flask, and then 1160.6g of 13.3mol / l ammonia water was added while stirring at 250rpm. After stirring for 1 hour at 30℃, the pH was 6.6. The precipitated amorphous aluminum hydroxide gel was centrifuged at 2,000rpm for 1 minute in a centrifuge (KBS-12 available from Kansai Centrifugal Separation Manufacturing Co., Ltd.) and 4L of water was added, which was repeated three times to wash the amorphous aluminum hydroxide gel, and then dried for 1 hour at 100℃ in a tray dryer. The moisture content was 65%. After adding 6695g of water to 1137.5g of the dried amorphous aluminum hydroxide gel and stirring to disperse it, 2000g of 23.1mol / l formic acid and 386.6g of 17.4mol / l acetic acid were added and stirred at 60℃ and 250rpm for 1 hour to synthesize a mixture of basic aluminum formate aqueous solution and basic aluminum acetate aqueous solution. 500ml of the obtained basic aluminum formate aqueous solution (C) was collected in a measuring cylinder, transferred to a separable flask, and heated and concentrated at 110℃ for 8 hours at 250rpm to obtain an alumina aqueous dispersion. The obtained alumina aqueous dispersion was poured into a measuring cylinder, and the volume was measured to be 225ml (D).

[0041] Comparative Example 1 2250g of 0.5mol / l aluminum nitrate aqueous solution was put into a 20L separable flask, and then 1960.6g of 13.3mol / l ammonia water was put in while stirring at 250rpm. After stirring at 30℃ for 1 hour, the pH was 8.9. The precipitated amorphous aluminum hydroxide gel was washed by centrifuging at 2,000rpm for 1 minute with a centrifuge (KBS-12 available from Kansai Centrifugal Separation Manufacturing Co., Ltd.) and adding 4L of water three times, and then dried at 100℃ for 1 hour in a tray dryer. The moisture content was 65%. 6695g of water was added to 1137.5g of the dried amorphous aluminum hydroxide gel, and the mixture was stirred and dispersed, and then 2386.6g of 23.1mol / l formic acid was added and stirred at 45℃ for 1 hour at 250rpm to synthesize a basic aluminum formate aqueous solution.

[0042] Comparative Example 2 2250g of 0.5mol / l aluminum nitrate aqueous solution was put into a 20L separable flask, and then 1160.6g of 13.3mol / l ammonia water was put in while stirring at 250rpm. After stirring at 30℃ for 1 hour, the pH was 6.6. The precipitated amorphous aluminum hydroxide gel was washed by centrifuging at 2,000rpm for 1 minute with a centrifuge (KBS-12 available from Kansai Centrifugal Separation Manufacturing Co., Ltd.) and adding 4L of water three times, and then dried in a tray dryer at 100℃ for 8 hours. The moisture content was 45%. 6695g of water was added to 1137.5g of the dried amorphous aluminum hydroxide gel, and the mixture was stirred and dispersed, and then 2386.6g of 23.1mol / l formic acid was added and stirred at 45℃ and 250rpm for 1 hour to synthesize a basic aluminum formate aqueous solution.

[0043] Comparative Example 3 2250g of 0.5mol / l aluminum nitrate aqueous solution was put into a 20L separable flask, and then 1160.6g of 13.3mol / l ammonia water was put in while stirring at 250rpm. After stirring at 30℃ for 1 hour, the pH was 6.6. The precipitated amorphous aluminum hydroxide gel was centrifuged at 2,000rpm for 1 minute in a centrifuge (KBS-12 available from Kansai Centrifugal Separation Manufacturing Co., Ltd.) and 4L of water was added, which was repeated three times to wash the amorphous aluminum hydroxide gel, and then dried at 100℃ for 1 hour in a tray dryer. The moisture content was 65%. 6695g of water was added to 1137.5g of the dried amorphous aluminum hydroxide gel, and the mixture was stirred and dispersed, and then 2386.6g of 23.1mol / l formic acid was added and stirred at 10℃ and 250rpm for 1 hour to synthesize a basic aluminum formate aqueous solution. 500 ml of the obtained basic aluminum formate aqueous solution (C) was collected in a measuring cylinder, transferred to a separable flask, and heated and concentrated at 250 rpm at 110° C. for 8 hours to obtain an aqueous alumina dispersion.

[0044] Comparative Example 4 2250g of 0.5mol / l aluminum nitrate aqueous solution was put into a 20L separable flask, and then 1160.6g of 13.3mol / l ammonia water was put in while stirring at 250rpm, and after stirring at 30℃ for 1 hour, the pH was 6.6. The precipitated amorphous aluminum hydroxide gel was centrifuged at 2,000rpm for 1 minute with a centrifuge (KBS-10 available from Kansai Centrifugal Separation Manufacturing Co., Ltd.) and 4L of water was added, which was repeated three times to wash the amorphous aluminum hydroxide gel, and then dried at 100℃ for 1 hour in a tray dryer. The moisture content was 65%. 6695g of water was added to 1137.5g of the dried amorphous aluminum hydroxide gel, and the mixture was stirred and dispersed, and then 2386.6g of 23.1mol / l formic acid was added, and the mixture was stirred at 45℃ and 250rpm for 1 hour to synthesize a basic aluminum formate aqueous solution. 500 ml of the resulting basic aluminum formate aqueous solution (C) was collected in a measuring cylinder, transferred to a separable flask, and heated and concentrated at 250 rpm at 50° C. for 24 hours to obtain an aqueous alumina dispersion.

[0045] Comparative Example 5 2250g of 0.5mol / l aluminum nitrate aqueous solution was put into a 20L separable flask, and then 1160.6g of 13.3mol / l ammonia water was put in while stirring at 250rpm, and after stirring at 30℃ for 1 hour, the pH was 6.6. The precipitated amorphous aluminum hydroxide gel was centrifuged at 2,000rpm for 1 minute in a centrifuge (KBS-12 available from Kansai Centrifugal Separation Manufacturing Co., Ltd.) and 4L of water was added, which was repeated three times to wash the amorphous aluminum hydroxide gel, and then dried at 100℃ for 1 hour in a tray dryer. The moisture content was 65%. 6695g of water was added to 1137.5g of the dried amorphous aluminum hydroxide gel, and the mixture was stirred and dispersed, and then 315.0g of 23.1mol / l formic acid was added, and the mixture was stirred at 45℃ and 250rpm for 1 hour to synthesize a basic aluminum formate aqueous solution. 500 ml of the obtained basic aluminum formate aqueous solution (C) was collected in a measuring cylinder, transferred to a separable flask, and heated and concentrated at 250 rpm at 110° C. for 8 hours to obtain an aqueous alumina dispersion.

[0046] Comparative Example 6 2250g of 0.5mol / l aluminum nitrate aqueous solution was put into a 20L separable flask, and then 386.9g of 8.0mol / l sodium hydroxide aqueous solution was put in while stirring at 250rpm. After stirring at 30℃ for 1 hour, the pH was 6.9. The precipitated amorphous aluminum hydroxide gel was washed by centrifuging at 2,000rpm for 1 minute with a centrifuge (KBS-12 available from Kansai Centrifugal Separation Manufacturing Co., Ltd.) and adding 4L of water three times, and then dried at 100℃ for 1 hour in a tray dryer. The moisture content was 65%. 6695g of water was added to 1137.5g of the dried amorphous aluminum hydroxide gel, and the mixture was stirred and dispersed, and then 2386.6g of 23.1mol / l formic acid was added and stirred at 45℃ for 1 hour at 250rpm to synthesize a basic aluminum formate aqueous solution. 500 ml of the obtained basic aluminum formate aqueous solution (C) was collected in a measuring cylinder, transferred to a separable flask, and heated and concentrated at 250 rpm at 110°C for 8 hours to obtain an alumina aqueous dispersion. The obtained alumina aqueous dispersion was poured into a measuring cylinder, and the volume was measured to be 225 ml (D).

[0047] Comparative Example 7 2250g of 0.5mol / l aluminum nitrate aqueous solution was put into a 20L separable flask, and then 1160.6g of 13.3mol / l ammonia water was put in while stirring at 250rpm, and the temperature was 30℃ and stirred for 1 hour, after which the pH was 6.6. The precipitated amorphous aluminum hydroxide gel was centrifuged at 2,000rpm for 1 minute in a centrifuge (KBS-12 available from Kansai Centrifugal Separation Manufacturing Co., Ltd.) and 4L of water was added, which was repeated three times to wash the amorphous aluminum hydroxide gel, and then dried for 1 hour at 100℃ in a tray dryer. The moisture content was 65%. 6695g of water was added to 1137.5g of the dried amorphous aluminum hydroxide gel, and the mixture was stirred and dispersed, and then 2386.6g of 23.1mol / l lactic acid was added, and the mixture was stirred at 45℃ and 250rpm for 1 hour to synthesize a basic aluminum lactate aqueous solution. 500 ml of the obtained basic aluminum lactate aqueous solution (C) was collected in a measuring cylinder, transferred to a separable flask, and heated and concentrated at 250 rpm at 110°C for 8 hours to obtain an alumina aqueous dispersion. The obtained alumina aqueous dispersion was poured into a measuring cylinder, and the volume was measured to be 210 ml (D).

[0048] Comparative Example 8 2250g of 0.5mol / l aluminum chloride aqueous solution was put into a 20L separable flask, and then 1160.6g of 13.3mol / l ammonia water was put in while stirring at 250rpm, and after stirring at a temperature of 30℃ for 1 hour, the pH was 6.6. The precipitated amorphous aluminum hydroxide gel was centrifuged at 2,000rpm for 1 minute with a centrifuge (KBS-12 available from Kansai Centrifugal Separation Manufacturing Co., Ltd.) and 4L of water was added, which was repeated three times to wash the amorphous aluminum hydroxide gel, and then dried at 100℃ for 1 hour in a tray dryer. The moisture content was 65%. 6695g of water was added to 1137.5g of the dried amorphous aluminum hydroxide gel, and the mixture was stirred and dispersed, and then 2386.6g of 23.1mol / l acetic acid was added, and the mixture was stirred at 45℃ and 250rpm for 1 hour to synthesize a basic aluminum acetate aqueous solution. The obtained basic aluminum acetate aqueous solution (500 ml) (C) was collected in a measuring cylinder, transferred to a separable flask, and heated and concentrated at 250 rpm at 110°C for 8 hours to obtain an alumina aqueous dispersion. The obtained alumina aqueous dispersion was poured into a measuring cylinder, and the volume was measured to be 250 ml (D).

[0049] The average particle size (nm) of the alumina particles, the crystal system when dried at 100°C, the pH of the alumina aqueous dispersion, and Al 2 O 3 The converted concentration (mass %) was measured as follows, and the results are shown in Tables 1 to 4. In Comparative Examples 1 to 5, the formation state of the alumina aqueous dispersion was insufficient, and the final state is shown in Table 3.

[0050] (Average particle size of alumina particles (nm)) The average particle diameters of Examples 1 to 8 and Comparative Examples 6 to 8 were measured by dynamic light scattering in an aqueous solvent using a Zetasizer Nano ZS (manufactured by Spectris, Inc.), and the average particle diameters measured by number are shown in Tables 1 to 4.

[0051] (Crystal system when dried at 100℃) The crystal systems of Examples 1 to 8 and Comparative Examples 6 to 8 when dried at 100° C. were measured using an X-ray diffractometer (Smartlab 9kw: manufactured by Rigaku Corporation). The results are shown in Tables 1 to 3.

[0052] (pH) Measurements were performed using a portable pH meter "HM-40P" and a pH composite electrode "GST-2739C" manufactured by Toa DKK Corporation, and the results are shown in Tables 1 to 3.

[0053] (Al 2 O 3 (equivalent concentration) Al in Examples 1 to 8 and Comparative Examples 6 to 8 2 O 3 The aluminum concentration was first measured using an emission spectrometer (Agilent 5110 ICP-OCS: manufactured by Agilent Technologies), and the aluminum concentration was calculated using the following formula: 2 O 3 The results were converted into concentrations and shown in Tables 1 to 4. Al 2 O 3 Converted concentration (mass%) = Al concentration (mass%) × (102 / 27)

[0054] (Thixotropic index (TI value)) The TI (thixotropic index) value was measured using a B-type viscometer (Toki Sangyo Co., Ltd., TVB10M TM-3 spindle rotor) and calculated as (rotation speed 6 rpm) / (rotation speed 60 rpm).

[0055] (D / C) The volume of the aqueous aluminum formate solution or the aqueous solution of a mixture of aluminum formate and aluminum acetate was 500 ml (C), and the volume of the finally obtained aqueous alumina dispersion was (D). The volume concentration ratio (D / C) is shown in Tables 1 to 4.

[0056] (Concentrations of chlorine, bromine, iodine, sodium and potassium) The concentrations of chlorine, bromine, iodine, sodium, and potassium in Examples 1 to 8 and Comparative Examples 6 to 8 were measured using SEM (JCM-7000, manufactured by JEOL Ltd.) and EDS (energy dispersive fluorescent X-ray), and are shown in Tables 1 to 4. Those that were not detected were indicated as nd.

[0057] (Thermal decomposition evaluation) 1 g of each of the aqueous alumina dispersions of Examples 1 to 8 and Comparative Examples 6 to 8 was dropped onto a glass surface measuring 30 mm x 50 mm x 2 mm, and then the glass was dried at 100°C for 5 minutes using a hot air circulation dryer. The glass was then baked at 600°C for 5 minutes in an electric furnace (FO200: manufactured by Yamato Scientific Co., Ltd.). The appearance of what remained on the glass was visually confirmed, and the color thereof is shown in Tables 1 to 4.

[0058] [Table 1]

[0059] [Table 2]

[0060] [Table 3]

[0061] [Table 4]

[0062] The alumina aqueous dispersion of Example 1 was dried in a glass evaporating dish at 100° C. for 10 minutes, and the result of observing the result at 100,000 times magnification with an FE-SEM (JSM-7001F manufactured by JEOL Ltd.) is shown in FIG.

[0063] The alumina aqueous dispersion of Example 1 was placed in a glass evaporating dish and dried in a manual hot air circulation dryer at 100° C. for 20 minutes to obtain powder. The powder was measured and evaluated using an X-ray diffractometer (Smartlab 9kW: manufactured by Rigaku Corporation). The results are shown in FIG. 2.

[0064] The alumina aqueous dispersion of Example 1 was placed in a glass evaporating dish and dried in a hot air circulation dryer at 100°C for 20 minutes, and the powder was placed in an alumina crucible and fired in an electric furnace (FO200: manufactured by Yamato Scientific Co., Ltd.) at 700°C for 2 hours. The powder was measured using an X-ray diffraction device (Smartlab 9kw: manufactured by Rigaku Corporation) and the evaluation results are shown in Figure 3.

[0065] The alumina aqueous dispersion of Example 1 was measured in an aqueous solvent by dynamic light scattering using a Zetasizer Nano ZS (manufactured by Spectris Corporation), and the results measured on a number basis are shown in FIG.

[0066] As shown in Tables 1 and 2, in Examples 1 to 3 and Examples 5 to 8, amorphous alumina aqueous dispersions were produced, and the average particle size, pH, Al 2 O 3 The average particle size, pH and Al content of the alumina dispersion liquid of amorphous + chi-alumina are shown in Table 1. 2 O 3 The values ​​of the TI and TI values ​​were within the range of the present invention, and when fired at 600°C for 5 minutes, white matter was confirmed, no fired organic matter was found, and it was confirmed that the thermal decomposition of the organic matter was completed.

[0067] As shown in Table 3, in Comparative Example 1, the pH of the amorphous aluminum hydroxide was too high, so that the amorphous aluminum hydroxide could not be dispersed in water in the next step. In Comparative Example 2, the moisture content during drying was too low, so that the amorphous aluminum hydroxide could not be dispersed in water in the next step. In Comparative Example 3, after the amorphous aluminum hydroxide gel was dispersed in water, the temperature after formic acid was added was too low, so that basic aluminum formate was not synthesized, and an alumina aqueous dispersion was not produced even when heated at a high temperature.

[0068] As shown in Table 3, in Comparative Example 4, after dispersing the amorphous aluminum hydroxide gel in water, the temperature during stirring after adding formic acid was too low, so a large amount of aluminum formate was produced and an alumina aqueous dispersion was not obtained. As shown in Table 3, in Comparative Example 5, the amount of formic acid added to the amorphous aluminum hydroxide gel was too small, so the amount of aluminum formate produced was small, and although an alumina aqueous dispersion was produced upon further heating, its concentration was low.

[0069] As shown in Table 4, in Comparative Example 6, the amorphous aluminum hydroxide gel is neutralized with sodium hydroxide instead of ammonia, so that there is a possibility that a large amount of sodium remains when an alumina aqueous dispersion is synthesized. As shown in Table 4, in Comparative Example 7, basic aluminum lactate was synthesized by using lactic acid instead of formic acid for the amorphous aluminum hydroxide gel, and an alumina aqueous dispersion was synthesized. Although an alumina aqueous dispersion could be synthesized, when a thermal decomposition evaluation was performed, the glass surface was black, and it was confirmed that the organic matter was not completely decomposed by thermal decomposition and carbon was generated, and it was not converted to alumina, and it was confirmed that there was a problem with low-temperature thermal decomposition. In Comparative Example 8, aluminum acetate was synthesized using aluminum chloride without using formic acid, and an alumina aqueous dispersion was synthesized, but the product contained a lot of chlorine and at the same time had low water solubility containing basicity, so precipitation occurred preferentially when additional heating was performed, and an alumina aqueous dispersion could not be synthesized.

[0070] As shown in FIG. 1, the alumina aqueous dispersion of Example 1 was dried at 100° C. for 10 minutes and observed with a FE-SEM. It was found that the majority of particles had a primary particle size of 100 nm or less, confirming that the desired alumina aqueous dispersion had been synthesized.

[0071] FIG. 2 shows the X-ray diffraction of the alumina aqueous dispersion of Example 1 dried at 100° C. for 20 minutes. No clear peaks were observed, confirming that an amorphous alumina particle dispersion was produced.

[0072] As shown in FIG. 3, the X-ray diffraction of the alumina aqueous dispersion of Example 1 which was dried at 100° C. for 20 minutes and calcined at 700° C. for 2 hours is shown. It shows a gamma alumina peak pattern, and it was confirmed that a phase transition to gamma alumina can be caused by increasing the calcination temperature from an amorphous alumina particle dispersion.

[0073] As shown in FIG. 4, the particle size distribution of the alumina aqueous dispersion of Example 1 was measured on a number basis, and it was confirmed that the alumina aqueous dispersion had an average particle size of 55 nm and did not contain coarse particles exceeding 100 nm.

[0074] Furthermore, the following aspects can be proposed. [1] An alumina aqueous dispersion containing alumina particles as dispersed particles, the dispersion having the following characteristics: (1) The average particle size of the alumina dispersed particles measured by number is in the range of 10 to 1000 nm; (2) When the aqueous alumina dispersion is dried at 100°C, the crystal system of the alumina particles is amorphous and / or chi-alumina, (3) The pH of the aqueous alumina dispersion is in the range of 2.0 to 5.3; (4) Alumina water dispersion is an organic acid and an alkali, the organic acid being formic acid or a combination of formic acid and acetic acid, and the alkali being ammonia; (5) Alumina (Al) contained in the alumina aqueous dispersion 2 O 3 ) converted concentration is 0.5 to 11.5 mass%, An alumina aqueous dispersion that satisfies the above requirements. [2] The alumina aqueous dispersion according to [1], wherein the alumina aqueous dispersion has a thixotropic index (TI value=rotation speed 6 rpm / rotation speed 60 rpm) of 2 to 10 as measured by a Brookfield viscometer. [3] The alumina aqueous dispersion according to [1] or [2], wherein the alumina aqueous dispersion contains an alkali metal or a halogen element in a range of 0 to 0.03 mass % based on the total weight of the solid components in the alumina aqueous dispersion. [4] The alumina aqueous dispersion according to any one of [1] to [3], which is used for forming a ceramic or a refractory material. [5] a first step of adding aqueous ammonia to an aqueous solution of an aluminum salt selected from aluminum nitrate and aluminum sulfate to adjust the pH to 5 to 8, and then stirring the solution at a temperature in the range of 15 to 45° C. for 0.5 to 3 hours to form a precipitate of amorphous aluminum hydroxide; A second step of washing the produced amorphous aluminum hydroxide and then drying it to a moisture content of 60 to 80%; a third step of adding water to the dried amorphous aluminum hydroxide, dispersing the mixture, and then adding 1.8 to 10 moles of formic acid or a mixture of formic acid and acetic acid per mole of aluminum, followed by stirring at 40 to 80° C. for 1 to 3 hours to obtain an aqueous solution of aluminum formate or an aqueous solution of a mixture of aluminum formate and aluminum acetate; and a fourth step of concentrating the obtained aqueous aluminum formate solution or the aqueous solution of a mixture of aluminum formate and aluminum acetate at a temperature of 90 to 120° C. for 1 to 24 hours; The method for producing an aqueous alumina dispersion according to any one of [1] to [5], [6] The production method according to [5], characterized in that, when the volume of the aqueous aluminum formate solution or the aqueous solution of a mixture of aluminum formate and aluminum acetate obtained in the third step is taken as C, and the volume obtained by subsequent heating and concentrating at 90 to 120°C for 1 to 24 hours in the fourth step is taken as D, the solution is concentrated so that the volume concentration ratio (D / C) is 0.3 to 0.8.

Claims

1. An alumina aqueous dispersion containing alumina particles as dispersed particles, the dispersion having the following characteristics: (1) The average particle size of the alumina dispersion particles measured by number is in the range of 10 to 1000 nm; (2) When the alumina aqueous dispersion is dried at 100° C., the crystal system of the alumina particles is amorphous and / or chi-alumina, (3) The pH of the aqueous alumina dispersion is in the range of 2.0 to 5.3; (4) The alumina aqueous dispersion contains an organic acid and an alkali, the organic acid is formic acid or a combination of formic acid and acetic acid, and the alkali is ammonia; (5) Alumina (Al) contained in the alumina aqueous dispersion 2 O 3 ) converted concentration is 0.5 to 11.5 mass%; The aqueous alumina dispersion is used to form a ceramic or refractory material that satisfies the above requirements.

2. 2. The alumina aqueous dispersion used for forming a ceramic or refractory material according to claim 1, wherein the alumina aqueous dispersion has a thixotropic index (TI value=rotational speed 6 rpm / rotational speed 60 rpm) of 2 to 10 as measured by a Brookfield viscometer.

3. The alumina aqueous dispersion used for forming a ceramic or refractory material according to claim 1 or 2, wherein the alumina aqueous dispersion contains an alkali metal or a halogen element in a range of 0 to 0.03 mass% based on the total weight of the solid components in the alumina aqueous dispersion.

4. a first step of adding aqueous ammonia to an aqueous solution of an aluminum salt selected from aluminum nitrate and aluminum sulfate to adjust the pH to 5 to 8, and then stirring the solution at a temperature in the range of 15 to 45° C. for 0.5 to 3 hours to form a precipitate of amorphous aluminum hydroxide; A second step of washing the produced amorphous aluminum hydroxide and then drying it to a moisture content of 60 to 80%; a third step of adding water to the dried amorphous aluminum hydroxide, dispersing the aluminum hydroxide, and then adding 1.8 to 10 moles of formic acid or a mixture of formic acid and acetic acid per mole of aluminum, followed by stirring at 40 to 80° C. for 1 to 3 hours to obtain an aqueous solution of aluminum formate or an aqueous solution of a mixture of aluminum formate and aluminum acetate; and A fourth step of concentrating the obtained aqueous solution of aluminum formate or the aqueous solution of a mixture of aluminum formate and aluminum acetate at a temperature of 90 to 120° C. for 1 to 24 hours; A method for producing the alumina aqueous dispersion used for forming the ceramic or refractory material according to claim 1, comprising the steps of:

5. The method according to claim 4, characterized in that the aluminum formate aqueous solution or the aqueous solution of a mixture of aluminum formate and aluminum acetate obtained in the third step is concentrated to a volume concentration ratio (D / C) of 0.3 to 0.8, where C is the volume of the aqueous aluminum formate solution or the aqueous solution of a mixture of aluminum formate and aluminum acetate obtained in the third step, and D is the volume of the aqueous aluminum formate solution obtained by heating and concentrating the aqueous aluminum formate and aluminum acetate at 90 to 120° C. for 1 to 24 hours in the fourth step.

Citation Information

Patent Citations

  • JP1965-014292B

  • Manufacture of liquid composition for alumina coating

    JP1978045314A

  • Recording medium, image forming method using this recording medium, manufacture of this recording medium, alumina dispersion and preparation of alumina dispersion

    JP2000071609A

  • Hexagonal-plate-like boehmite, hexagonal-plate-like alumina, and method for producing them

    JP2003002642A

  • α-aluminum oxide precursor sol, method for producing the same, and method for producing yttrium-aluminum-garnet

    JP2013010652A