Polyester molding and its manufacturing method

Inorganic tin compounds address the issues of acetaldehyde and formaldehyde generation in polyester production, providing environmentally safe and high-quality containers with improved physical properties.

JP7587022B2Active Publication Date: 2024-11-19HYOSUNG TNC CORP
View PDF 15 Cites 0 Cited by

Patent Information

Application Number
JP2023512233
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-08-19
Filing Date
2021-08-18
Publication Date
2024-11-19
Estimated Expiration
2041-08-18

AI Technical Summary

Technical Problem

Existing polyester production methods using antimony-based catalysts result in high acetaldehyde and formaldehyde generation, toxicity issues, and environmental contamination, while alternative catalysts like titanium and germanium face stability and cost challenges.

Method used

Employing inorganic tin compounds as polymerization catalysts, specifically stannous compounds, to produce polyester molded articles that reduce acetaldehyde and formaldehyde content, ensuring environmental safety and improved physical properties.

Benefits of technology

The use of inorganic tin compounds minimizes harmful substance generation, enhances heat resistance and moldability, and produces environmentally friendly containers without toxicity, maintaining taste and aroma integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587022000001
    Figure 0007587022000001
  • Figure 0007587022000002
    Figure 0007587022000002
  • Figure 0007587022000003
    Figure 0007587022000003
Patent Text Reader

Abstract

The present invention relates to a polyester molded product containing a polyester obtained by polymerization in the presence of an inorganic tin compound catalyst, and a method for producing the same. The polyester molded product containing the inorganic tin compound of the present invention can overcome problems caused by residual antimony-based catalysts, and has reduced contents of acetaldehyde and formaldehyde, so that it does not affect the taste or aroma when used as a food storage container, and can be used as an environmentally friendly container that is non-toxic to the human body.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyester molded article and a method for producing the same, and more particularly to an environmentally friendly polyester molded article and a method for producing the same which eliminates the problems caused by the residue of antimony-based catalysts. [Background technology]

[0002] In general, polyester has excellent mechanical and chemical properties and is used in a wide range of applications, such as beverage containers, automotive molded parts, etc. However, acetaldehyde and formaldehyde are produced as additional substances during the polycondensation process of polyester, which may be harmful if consumed through products that contain them.

[0003] In particular, acetaldehyde present in drinking water bottles gradually leaks out and mixes with the contents, negatively affecting the flavor and aroma of the product being consumed. In addition, formaldehyde present in the bottles is a toxic substance that is strictly regulated in developed countries because even trace amounts can cause diseases such as cancer in the body.

[0004] Therefore, much research has been conducted to suppress the production of aldehyde substances such as acetaldehyde and formaldehyde that are formed during the polycondensation process of polyester.

[0005] In addition, when the polyester molded article after use is to be incinerated, it is preferable that the content of metals which become a source of ash requiring additional treatment is small.

[0006] In addition, even when a used polyester resin is depolymerized to recover and recycle monomers, it is preferable that the recovered monomers contain as little metal as possible, which may cause impurities. Therefore, there is an urgent need to develop a technique for reducing the content of metals, particularly heavy metals, contained in polyester resins that are used as materials for polyester molded articles.

[0007] Antimony-based catalysts are a typical material for polycondensation of polyesters used to manufacture molded products such as drinking water bottles. However, in the case of polyester food containers made with antimony-based catalysts, large amounts of acetaldehyde and formaldehyde are generated as additional substances during the polycondensation process.

[0008] For example, Patent Document 1 discloses a technology for producing polyester molded bodies by polymerizing polyester resin under an antimony compound catalyst. However, in the case of molded bodies such as drinking water bottles made with antimony-based catalysts, a large amount of antimony must be used in the polymerization process, and because of the toxicity of the metal itself, if antimony is leaked and flows into the body after long-term use, it can cause diseases such as fetal growth inhibition and carcinogenicity, as well as environmental problems (Anal.Bioanal.Chem.2006,385,821).

[0009] In addition, antimony catalysts do not have high polymerization activity per metal mass, so they must be used at relatively high concentrations when polyester resins are to be produced at industrially satisfactory production rates. As a result, polyester resins produced using these compounds contain 50 ppm to 300 ppm of antimony as metal atoms.

[0010] In addition, when used in polyester polymerization reaction, catalyst reduction products are generated at about 10 to 15% of the input amount, which may cause a problem of lowering the L value of the color of the polyester molded product.

[0011] Despite attempts to apply antimony-free catalysts such as titanium or aluminum catalysts, the generation of acetaldehyde and formaldehyde during the composite process or during the product forming process remains a serious problem.

[0012] Patent Document 2 discloses a polyester resin molded product having a multilayer structure including a surface layer made of polyethylene terephthalate containing a metal catalyst selected from the group consisting of a germanium-based catalyst, a titanium-based catalyst, and a mixture thereof, and a back layer made of polyethylene terephthalate containing an antimony-based catalyst.

[0013] However, while titanium catalysts have high polycondensation activity per metal mass, they also have a strong tendency to cause undesirable polyester decomposition reactions, which may lead to discoloration of the resin during the polycondensation reaction process, or deterioration of resin quality due to the production of low molecular weight compounds as by-products or a decrease in molecular weight during the melt molding process.

[0014] As a result, polyester resins produced using these titanium compounds as polycondensation catalysts have low stability and are more susceptible to the generation of acetaldehyde and the decrease in molecular weight due to thermal decomposition during melt molding than polyester resins produced using conventional antimony compounds as polycondensation catalysts, making them difficult to use as materials for molded bodies such as beverage filling containers.

[0015] On the other hand, although the germanium compound catalyst itself has high activity, there is a limitation in that if a large amount of germanium catalyst is used for polymerization, it is difficult to apply it commercially due to the high price of the catalyst. [Prior art documents] [Patent documents]

[0016] [Patent Document 1] Korean Patent Publication No. 2001-0043209 [Patent Document 2] Korean Patent Publication No. 2010-0020223 Summary of the Invention [Problem to be solved by the invention]

[0017] The present invention has been made to solve the above-mentioned problems of the prior art, and an object of the present invention is to provide an environmentally friendly polyester molding that does not affect the taste and aroma of the contents and is non-toxic to the human body by minimizing the amount of acetaldehyde and formaldehyde generated during the polyester polycondensation process and the product molding process.

[0018] Another object of the present invention is to provide a polyester molding which is less includ ed in foreign matter and excels in strength and elongation, heat resistance and shape stability.

[0019] It is still another object of the present invention to provide a method for producing a polyester resin molding having reduced contents of acetaldehyde and formaldehyde. [Means for solving the problem]

[0020] One aspect of the present invention for solving the above-mentioned technical problem is to The present invention relates to a polyester molded article obtained by melting and molding a polyester produced using an inorganic tin compound as a polymerization catalyst.

[0021] The inorganic tin compound is an inorganic stannous compound or an inorganic stannic tin compound.

[0022] Non-limiting examples of the inorganic stannous compounds include stannous oxide, stannous pyrophosphate, stannous phosphate, stannous tartrate, stannous acetate, stannous oxalate, stannous stearate, stannous oleate, stannous gluconate, stannous citrate, stannous 2-ethylhexanoate, stannous ethoxide, stannous acetylacetonate, and stannous glycolate.

[0023] Non-limiting examples of the inorganic stannous compounds include stannous oxide, stannous pyrophosphate, stannous phosphate, stannous tartrate, stannous acetate, stannous oxalate, stannous stearate, stannous oleate, stannous gluconate, stannous citrate, stannous 2-ethylhexanoate, stannous ethoxide, stannous acetylacetonate, and stannous glycolate. The inorganic tin compounds may be composites of various kinds, and may be used in combination with a conventionally known catalyst.

[0024] The polyester molded body contains one or more of polyethylene terephthalate, polytrimethylene terephthalate, polytetramethylene terephthalate, and polybutylene terephthalate, and contains 10 ppm to 200 ppm of inorganic tin compound residues therein.

[0025] Another aspect of the present invention for solving the above-mentioned technical problems relates to a method for producing a polyester molded product, which comprises melting and molding a polyester polymer polymerized in the presence of an inorganic tin compound catalyst. Effect of the Invention

[0026] According to the present invention, a catalyst that does not contain heavy metals that are harmful to humans and the environment is used, so that a polyester molded product that does not pollute the environment or contain components that are harmful to the human body can be provided, and the burden on the environment can be reduced even during the incineration or recycling of the molded product.

[0027] The polyester molded article of the present invention has reduced aldehyde-based compounds, so that it does not affect the taste and aroma when used as a food storage container, and can be used as an environmentally friendly container that is non-toxic to the human body.

[0028] The polyester molded article of the present invention has the effects of providing excellent heat resistance, dimensional stability, and moldability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] The present invention will now be described in more detail.

[0030] In describing the present invention, if it is determined that a detailed description of related prior art may make the gist of the present invention unclear, the detailed description will be omitted. In this specification, when a part "contains" a certain component, this does not mean that the part "contains" other components, but that the part further contains other components, unless otherwise specified.

[0031] The polyester molded article according to one embodiment of the present invention is characterized in that it is produced by melting and molding polyester produced using an inorganic tin compound as a polymerization catalyst. The inorganic tin compound catalyst may be used alone, or in combination of two or more kinds, or in combination with a conventionally known catalyst.

[0032] Organotin compound catalysts are excluded from the present invention because they are subject to stricter environmental regulations than the inorganic tin compounds used in the present invention.

[0033] The inorganic tin compound used in the present invention has a significant advantage in that it has a lower standard reduction potential energy value than the conventionally used antimony (Sb) catalyst and is not easily reduced during the polyester polymerization reaction and molding process. The inorganic tin compound catalyst used in the present invention does not have the problems of being easily reduced during the polymerization reaction to reduce activity or leaving catalyst residue in the polymerization reactor due to the reduction product, and there is little increase in the filter pressure of the extruder and little generation of nozzle foreign matter during the molding process, resulting in improved processability.

[0034] TIFF0007587022000001.tif27170

[0035] The higher the standard reduction potential, the greater the reducibility, and the lower the standard reduction potential, the lower the reducibility. Antimony (Sb), which has been used mainly in polyester polymerization, has a positive standard reduction potential (+) and reducing power when it is in the oxidation state of 3 or 5, which has catalytic activity. In contrast, the inorganic tin compound catalyst used in the present invention maintains its catalytic activity because it is non-spontaneous when reduced in the oxidation state of 2 (RPE is negative), and can reduce the reduction products (catalyst residues) generated during the polyester polymerization and extrusion process.

[0036] The inorganic tin compound is preferably tin oxalate, tin acetate, or tin glycolate.

[0037] The inorganic tin compound catalyst is an inorganic stannous compound or an inorganic stannic compound.

[0038] The inorganic stannous compound is selected from the group consisting of stannous oxide, stannous pyrophosphate, stannous phosphate, stannous tartrate, stannous acetate, stannous oxalate, stannous stearate, stannous oleate, stannous gluconate, stannous citrate, stannous 2-ethylhexanoate, stannous ethoxide, stannous acetylacetonate, and stannous glycolate.

[0039] The inorganic stannic compound is selected from the group consisting of stannic oxide, stannic pyrophosphate, stannic phosphate, stannic tartrate, stannic acetate, stannic oxalate, stannic stearate, stannic oleate, stannic gluconate, stannic citrate, stannic 2-ethylhexanoate, stannic ethoxide, stannic acetylacetonate, and stannic glycolate.

[0040] The inorganic tin compound catalyst used in the present invention can be added at any step during polyester polymerization, for example, only during the preparation of a slurry (EG / TPA mixture) before the esterification reaction step, only during the esterification reaction step, only during the polycondensation step of the esterification reaction step, or all during the preparation of a slurry before the esterification reaction step, the esterification reaction step, and the polycondensation step.

[0041] However, when a polyester is produced by esterifying a dicarboxylic acid component and a glycol component and then polycondensing the reactant, the inorganic tin compound catalyst is preferably added in the step of polycondensing the esterified reactant.

[0042] The inorganic tin compound catalyst may be added to the polyester polymerization process in the form of a powder or in the form of a catalyst solution, or may be prepared in an ethylene glycol solution and then added. However, when the catalyst is prepared in an ethylene glycol solution and then added, it is preferable to react the ethylene glycol solution with the inorganic tin compound to prepare tin glycolate and then add the resulting solution.

[0043] Antimony catalysts, which are generally used as polyester polymerization catalysts, have low catalytic activity and are used in an amount of 50 ppm to 500 ppm (Sb element amount) based on polyester. In contrast, the inorganic tin compound catalysts newly applied in the present invention can sufficiently ensure the same polycondensation reactivity even with a small amount of 10 ppm to 200 ppm, preferably 10 ppm to 100 ppm (Sn element amount).

[0044] Due to such a low catalyst content, the catalyst foreign matter of polyester is improved, and the generation of foreign matter in the molding process due to the catalyst reduction product is low, so that the effect of improving the foreign matter in the molding process is obtained. In addition, when the catalyst is used at a high concentration, the polyester polymer may become grayish, but in the present invention, the low catalyst content has a remarkable effect of improving the color (Color L) of the polyester polymer and the molding.

[0045] In addition, by providing the catalyst of the present invention, the heat resistance of the polyester can be improved, thereby reducing the content of acetaldehyde generated from polyester decomposition products, and the content of cyclic oligomers can be improved by carrying out the polycondensation reaction at a low polymerization temperature.

[0046] Unlike antimony-based catalysts, the catalyst of the present invention is less likely to cause problems for humans and the environment because the toxicity of the metal itself is relatively low, and even a small amount of the catalyst shows high activity within a short reaction time. In addition, polyesters produced using the catalyst of the present invention have excellent physical properties such as viscosity and color.

[0047] The polyester used in the polyester molded article of the present invention is a homopolyester or a copolymer polyester. In the case of a homopolyester, it is preferable that the homopolyester is obtained by polycondensation of an aromatic dicarboxylic acid and an aliphatic glycol. Examples of the aromatic dicarboxylic acid include terephthalic acid and 2,6-naphthalenedicarboxylic acid.

[0048] Aliphatic glycols include ethylene glycol, diethylene glycol, 1,4-cyclohexanedimethanol, etc. Preferably, the polyester is polyethylene terephthalate (PET), polybutylene terephthalate, polytrimethylene terephthalate, and polytetramethylene terephthalate.

[0049] On the other hand, examples of the dicarboxylic acid component of the copolymer polyester include one or more of isophthalic acid, phthalic acid, terephthalic acid, 2,6-naphthalenedicarboxylic acid, adipic acid, sebacic acid, etc., and examples of the glycol component include one or more of ethylene glycol, diethylene glycol, propylene glycol, butanediol, 1,4-cyclohexanedimethanol, neopentyl glycol, etc.

[0050] In either case, the polyester in the present invention is preferably polyethylene terephthalate, which is generally composed of 60 mol % or more, and preferably 80 mol % or more of ethylene terephthalate units.

[0051] In the method for producing a polyester resin molded product of the present invention, a toning agent is added to improve the hue of the resin molded product produced. Examples of the toning agent include cobalt acetate, cobalt acetylacetonate, cobalt benzoylacetonate, cobalt hydroxide, cobalt bromide, cobalt chloride, cobalt iodide, cobalt fluoride, cobalt cyanide, cobalt nitrate, cobalt sulfate, cobalt selenide, cobalt phosphate, cobalt oxide, cobalt thiocyanate, and cobalt propionate, and other cobalt-containing compounds, but are not limited thereto. In addition to the cobalt-based inorganic toning agent, non-cobalt-based organic toning agents (blue, red series) may also be used to improve the hue.

[0052] The toning agent is added in an amount such that the content of cobalt element based on the final polyester resin is about 150 ppm or less, for example, about 10 to about 150 ppm, and preferably about 10 to about 100 ppm. Although it is known that cobalt compounds themselves have a certain degree of catalytic activity, if an excessive amount that can exert a catalytic effect is added, the residual metal in the polyester increases, which may induce toxicity and reduce brightness.

[0053] Therefore, when added within the above range, it is possible to minimize coloring by generating trace amounts of additional substances such as acetaldehyde and formaldehyde in the polyester. However, in the present invention, a non-cobalt-based organic toning agent is used as the toning agent in order to provide an environmentally friendly polyester molding.

[0054] In the present invention, Blue (Polysynthren Blue RLS) and Red (Polysynthren Red GFP) manufactured by Clariant are used as organic toning agents.

[0055] The polyester molded article of the present invention has a reduced content of acetaldehyde and formaldehyde, and therefore can be used as an environmentally friendly container that does not affect the taste and aroma of food and drink when used as a storage container for food and drink and is non-toxic to the human body. More specifically, the polyester resin molded article is used in drinking water bottles, food packaging materials, fibrous plastics, etc., and is preferably used as a drinking water bottle.

[0056] Another aspect of the present invention relates to a method for producing a polyester molded article, in which a polyester resin composition comprising a polyester produced using an inorganic tin compound catalyst is melt-extruded to produce a molded article.

[0057] When producing a polyester polymer of the polyester resin composition for producing a molded article, an inorganic tin compound is used as a polymerization catalyst to polymerize a dicarboxylic acid component and a glycol component.

[0058] The step of polymerizing the dicarboxylic acid component and the glycol component includes a step of esterifying the dicarboxylic acid component and the glycol component, and a step of polycondensing the reaction product of the esterification reaction. In the esterification reaction step, a low polymer is obtained by transesterification, and then organic polymer particles and various additives are added, and an inorganic tin compound is added as a polycondensation catalyst to carry out a polycondensation reaction to obtain a high molecular weight polyester.

[0059] More specifically, first, a dicarboxylic acid component and a glycol component are subjected to an ester reaction.

[0060] According to an embodiment of the present invention, examples of the dicarboxylic acid component include, but are not limited to, terephthalic acid, oxalic acid, malonic acid, azelaic acid, fumaric acid, pimelic acid, suberic acid, isophthalic acid, dodecanedicarboxylic acid, naphthalenedicarboxylic acid, biphenyldicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, succinic acid, glutaric acid, adipic acid, sebacic acid, 2,6-naphthalenedicarboxylic acid, 1,2-norbornanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, 1,3-cyclobutanedicarboxylic acid, 1,4-cyclobutanedicarboxylic acid, 5-sodium sulfoisophthalic acid, 5-potassium sulfoisophthalic acid, 5-lithium sulfoisophthalic acid, and 2-sodium sulfoterephthalic acid.

[0061] In addition to the above dicarboxylic acids, other dicarboxylic acids not exemplified above may be used within the scope of the present invention. According to one embodiment of the present invention, terephthalic acid is used as the dicarboxylic acid component.

[0062] According to an embodiment of the present invention, examples of the glycol component include ethylene glycol, 1,2-propylene glycol, 1,2-butylene glycol, 1,3-butylene glycol, 2,3-butylene glycol, 1,4-butylene glycol, 1.5-pentanediol, neopentyl glycol, 1,3-propylene glycol, diethylene glycol, triethylene glycol, 1,2-cyclohexanediol, 1,3-cyclohexanediol, 1,4-cyclohexanediol, propanediol, 1,6-hexanediol, neopentyl glycol, tetramethylcyclobutanediol, 1,4-cyclohexanediethanol, 1,10-decamethylene glycol, 1,12-dodecanediol, polyoxyethylene glycol, polyoxymethylene glycol, polyoxytetramethylene glycol, and glycerol, but are not limited thereto, and other glycols may be used as long as they do not impair the object of the present invention.

[0063] Preferably, ethylene glycol is used as the glycol component.

[0064] According to one embodiment of the present invention, the step of esterifying the dicarboxylic acid component and the glycol component is preferably carried out by reacting for about 1 to 6 hours at a temperature of about 200° C. to about 300° C. Then, the reaction product of the esterification reaction is polycondensed. The step of polycondensing the reaction product of the esterification reaction is carried out by reacting for about 1 to about 3 hours at a temperature of about 200° C. to about 300° C. and under reduced pressure of about 0.1 to about 1 torr.

[0065] The inorganic tin compound catalyst of the present invention is introduced during the preparation of the slurry prior to the esterification reaction or during the esterification reaction and prior to the polycondensation step after the esterification reaction.

[0066] However, although the inorganic tin compound catalyst of the present invention is effective in improving the esterification reaction, it has little effect in improving the polycondensation time and there is a concern that the content of diethylene glycol (DEG), a by-product of the esterification reaction, increases slightly, so in the present invention, it is preferable to add the reactant after the esterification reaction to the polycondensation step. By doing so, the polycondensation time can be significantly shortened and productivity can be increased compared to when using conventional catalysts.

[0067] In the polymerization process of the polyester resin for producing the polyester molded product of the present invention, the inorganic tin compound catalyst is used in an amount of about 200 ppm or less, for example, about 10 to about 200 ppm, preferably about 10 ppm to 100 ppm, based on the content of tin contained in the inorganic tin compound catalyst relative to the mass of the finally produced polyester.

[0068] In the present invention, if the amount of inorganic tin compound catalyst during the polyester polycondensation reaction is less than 10 ppm, the polymerization reaction rate will be slow and the polymerization efficiency will decrease, and if it is more than 200 ppm, the inorganic tin compound in excess of the required amount will act as a foreign matter, which may decrease the workability of the molding process.

[0069] The content of tin in the polyester molded product is preferably 200 ppm or less, more preferably 10 to 100 ppm. If the content of tin exceeds 200 ppm, oligomers are by-produced in the process of melting and extruding the polyester, and a molded product having low oligomer content and high transparency may not be obtained.

[0070] According to the present invention, the use of an inorganic tin compound allows the polymerization reaction to be carried out using a small amount of catalyst. Also, a product with high viscosity can be obtained in a short reaction time. As the amount of catalyst used can be reduced, the blackening phenomenon of the polyester aggregate generated after polymerization can be reduced and the conventional low viscosity can be increased, which is very advantageous commercially. The polyester molded product according to the present invention is characterized by a superior Color-L value compared to polyester molded products produced using other types of metal catalysts.

[0071] In the present invention, the polyester resin for producing the polyester molded article has an intrinsic viscosity in the range of 0.70 dl / g to 1.3 dl / g, more preferably 0.70 dl / g to 0.85 dl / g, in order to ensure appropriate physical properties and moldability of the molded article.

[0072] If the intrinsic viscosity of the polyester is less than 0.70 dl / g, the tensile strength of the polyester molded article may decrease, whereas if the intrinsic viscosity of the polyester is more than 1.3 dl / g, the productivity of the polyester molded article may decrease.

[0073] The units of intrinsic viscosity are all dl / g, and the intrinsic viscosity was measured at 30°C in a 60 / 40 (mass ratio) phenol / 1,1,2,2-tetrachloroethane solution of a 0.5 mass% PET resin solution according to ASTM D4603-96.

[0074] The polyester resin produced by the polymerization reactor of the present invention may be solidified and pelletized, and then remelted and used for molding, or may be transferred to a molding machine in a molten state without being solidified and used for molding.

[0075] Here, "molten state" refers to the state in which the resin melts and flows when heat is applied to the resin, and resin in this molten state generally has a viscosity of 500,000 Pa s or less.

[0076] When producing a polyester molded article according to the present invention, first, a polyester resin composition containing a polyester produced using an inorganic tin compound catalyst is melted, the molten polyester resin composition is then filled into a mold, and the polyester resin composition filled into the mold is cooled and then released from the mold to produce the polyester molded article.

[0077] In the present invention, the molding step of the polyester molded article is carried out by a method such as compression molding, transfer molding, lamination molding, injection molding, extrusion molding, blow molding, calendar molding, gas molding, insert molding, or vacuum molding. Methods and devices that can be used in such a molding step are not particularly limited as long as they are known to be usable for the manufacture of plastic molded products.

[0078] For example, when the polyester resin is used to manufacture a plastic drinking water bottle, a blow molding method is used.

[0079] The step of molding the polyester resin further includes a step of forming a preform of a resin molding using the molded polyester resin. In the step of forming the preform of the resin molding, the formed polyester resin is dried to remove moisture, and the polyester resin from which moisture has been removed is injected or extruded to manufacture a preform suitable for a final product. The final product is then provided by applying the preform to the above-mentioned molding method.

[0080] In the present invention, the polyester resin produced using the inorganic tin compound catalyst contains less than 3 ppm of aldehyde compounds, more preferably less than 2 ppm of acetaldehyde and less than 1 ppm of formaldehyde based on the weight of the polyester resin.

[0081] The polyester molded article of the present invention is an environmentally friendly container that has a reduced content of acetaldehyde and formaldehyde and does not affect the taste and aroma when used as a food storage container and is non-toxic to the human body. Specific examples include drinking water bottles, food packaging materials, fibrous plastics, etc.

[0082] The present invention will be described in more detail with reference to the following examples, however, these examples are merely presented as examples of the invention and do not limit the scope of the invention.

[0083] Working Example Example 1 Preparation of catalyst solution 5 g of the inorganic tin compound catalyst shown in Table 2 below was diluted with ethylene glycol to a total mass of 2 kg, and the mixture was stirred at a stirring speed of 400 rpm to prepare an inorganic tin compound catalyst at a concentration of 0.25% in ethylene glycol. Next, the mixture was reacted in a reactor capable of refluxing at a reaction temperature of 160 to 180°C for 2 hours to produce an inorganic tin compound catalyst.

[0084] Polyester resin manufacturing A slurry was prepared from 7.8 kg of terephthalic acid (TPA) and 3.3 kg of ethylene glycol (EG) (EG / TPA molar ratio = 1.13), which was then introduced into an esterification reactor in a semi-batch manner and reacted in a nitrogen atmosphere at normal pressure until the reaction temperature reached 265°C to produce a polyester oligomer. At this time, the esterification reaction temperature was 253°C when the slurry was introduced, and 265°C at the end of the final esterification reaction, and the reaction time was about 3 hours and 30 minutes.

[0085] The PET oligomer produced in the esterification reactor was transferred to a polycondensation reactor, where 200 ppm of tin oxide catalyst was added based on the final PET, and polycondensation was carried out for about 2 hours and 30 minutes under high vacuum and reduced pressure until the reaction temperature reached 288°C, producing raw chips. The raw chips were then solid-phase polymerized at a temperature of about 250°C under vacuum to have an intrinsic viscosity of 0.76 dl / g.

[0086] Manufacturing of polyester moldings Using a bottle manufacturing model (equipment: Erontier), the temperature applied to the preform is 70-80°C, and the pressure is nitrogen pressure (5-8Kgf / cm 2 The preform, which was manufactured by fixing the strength to a certain level, was placed in the machine and heated while rotating automatically along the lane. The preform rotated at a speed of 8.4 seconds and the air pressure (1st: 11, 2nd: 40, 3rd: 7Kgf / cm) was adjusted in three steps. 2 ) was added in the mold.

[0087] The preform was pressed into the mold, and the thickness of the bottom of the bottle was determined by the pressure applied to it, while the strength of the air being blown in determined the overall thickness of the surface of the bottle.

[0088] Examples 2 to 50 A polyester molding was manufactured in the same manner as in Example 1, except that polyester chips manufactured using an inorganic tin compound shown in Table 2 below as a catalyst were used.

[0089] Comparative Example 1 A polyester molding was produced in the same manner as in Example 1, except that no catalyst was used.

[0090] Comparative Example 2 40 g of antimony was dissolved in ethylene glycol to a total weight of 2 kg, and the solution was stirred at 400 rpm to prepare a catalyst solution. The mixture was reacted in a refluxable reactor at a reaction temperature of 180-190°C for 2 hours to prepare an antimony glycolate solution. A polyester molded product was manufactured in the same manner as in Example 1, except that the polyester polymerized using the obtained antimony catalyst solution was used.

[0091] Comparative Examples 2 to 9 A polyester molding was manufactured in the same manner as in Example 1, except that a polyester polymer prepared using an antimony catalyst shown in Table 1 below was used as a catalyst.

[0092] Comparative Example 10 40g of titanium compound was dissolved in ethylene glycol to a total weight of 2kg, and stirred at 400rpm to prepare a catalyst solution. The mixture was reacted in a refluxable reactor at a reaction temperature of 180~190℃ for 2 hours to prepare a titanium glycolate solution. A polyester molded product was prepared in the same manner as in Example 1, except that the polyester polymerized using the obtained titanium catalyst solution was used.

[0093] Comparative Examples 11 to 17 A polyester molding was produced in the same manner as in Example 1, except that a polyester polymer produced using a titanium compound catalyst shown in Table 1 below was used as the catalyst.

[0094] Comparative Examples 18 to 47 Polyester moldings were manufactured in the same manner as in Example 1, except that polyester polymers prepared using 1 ppm, 8 ppm, or 500 ppm of an inorganic tin compound shown in Table 2 below as a catalyst were used.

[0095] Test Example The physical properties of the polyester molded articles produced in Examples 1 to 50 and Comparative Examples 1 to 47 were evaluated by the following methods, and the results are shown in Tables 1 and 2 below.

[0096] (1) Intrinsic viscosity According to ASTM D 4603, 0.1g of sample was dissolved in a 6:4 mass ratio mixture of phenol and 1,1,2,2-tetrachloroethane (raw chip 90℃, SSP 130℃) for 90 minutes to a concentration of 0.4g / 100ml, then transferred to an Ubbelohde viscometer and kept in a 30℃ thermostatic bath for 10 minutes, and the time it took for the solution to fall was measured using a viscometer and an aspirator. The time it took for the solvent to fall was also measured in the same way, and the RV (relative viscosity) and IV (intrinsic viscosity) values ​​were calculated using Equations 1 and 2.

[0097] [Number 1] RV = sample drop time / solvent drop time

[0098] [Number 2] IV=1 / 4×[(RV-1) / C]+3 / 4×(lnR.V. / C)

[0099] In the above formula, C represents the concentration of the sample in the solution (g / 100 ml).

[0100] (2) Concentration of carboxy end group (CEG) According to ASTM D 7409, the sample was dissolved using 0-cresol and then analyzed using acid-base neutralization titration. In detail, about 0.2g of sample was taken and 10ml of benzyl alcohol was added to it.

[0101] The mixture was heated in a 200℃ heating block for 10 minutes to dissolve, and then cooled in a water bath for 1 minute. 10 ml of chloroform and a few drops of phenol red and phenolphthalein indicator were added, and titrated using 0.02N KOH (or NaOH). The titration amount was used to calculate the carboxy end group (CEG) concentration using Equation 3. The number of carboxy groups is expressed as carboxy milliequivalents / kg of polymer (meq / kg).

[0102] [Number 3] CEG = (AB) x 0.02 x 1000 / W A: ml consumed by sample, B: blank, W: mass of sample

[0103] (3) Polymer and acetaldehyde (AA) content (ppm) Polyester samples freeze-shattered according to ASTM F 2013 were placed in headspace sampler vials and sealed, then thermally extracted at 160°C for 2 h and analyzed by gas chromatography GC (Agilent 7890).

[0104] (4) Hue measurement (Color L) Using a color difference meter (BYK Gardner Color view-9000), the color L value was measured under D65 light source and 10° conditions. The L value measured by a spectrophotometer is a color measurement value calculated from the CIE 1976 CIE Lab color difference formula after measuring the reflectance of the sample.

[0105] (5) Analysis of acetaldehyde (AA) content (ppb) of mineral water in the molded body Drinking water was poured into the polyester molded product to be measured, and trace amounts (ppb level) of acetaldehyde in the drinking water were analyzed using HPLC / UV-VIS after derivatization with DNPH (2,4-dinitrophenylhydrazine).

[0106] The DNPH derivatization solution was prepared with 0.2g of 2,4-dinitrophenylhydrazine / 100ml of acetonitrile, and the derivatization reaction procedure was as follows: 2ml of the solution to be measured was taken in a 4ml vial, 100μL of the DNPH derivatization solution was added, and the mixture was stirred. After stirring, 100μL of 45% H3PO4 was added to the sample, and the mixture was derivatized by sonication for 30 minutes. The sample solution after derivatization was analyzed and evaluated using HPLC / UV-VIS (Waters LC Module 1 plus).

[0107] The column used for the analysis was Kromasil KR100-10C18 (25 cm*4.6 mm), and the solvent conditions used in the instrument were CH3CN / Water=2 / 1.

[0108] The UV-VIS detection wavelength was evaluated at 356 nm, and the content of acetaldehyde in the sample was measured.

[0109] [Table 1]

[0110] [Table 2] TIFF0007587022000004.tif199170

[0111] Referring to Tables 1 and 2, it was confirmed that in Examples 1 to 50, the physical properties of the polyester containers produced were equal to or better than those of Comparative Examples 2 to 7, which used polyester resins using an antimony catalyst.

[0112] In addition, it was confirmed that the content of acetaldehyde in the drinking water contained in the polyester containers manufactured in Examples 1 to 50 was significantly reduced and the color was good. As a result, it was confirmed that the polyester resin molded products of the above Examples contain a very small amount of acetaldehyde, which does not affect the taste and aroma of the beverage, and can be used to manufacture environmentally friendly containers that are non-toxic to the human body.

[0113] In contrast, in the bottles of Comparative Examples 1 to 47, relatively large amounts of acetaldehyde were detected in the drinking water contained in the containers, and it was confirmed that using these bottles as storage containers for food and drink would be harmful to both the environment and human body, and the color was also poor.

[0114] Although the present invention has been described above by way of limited examples, the present invention is not limited thereto, and it is obvious that those skilled in the art to which the present invention pertains can make various modifications and variations of the technical concept of the present invention. Therefore, the true scope of protection of the present invention should be determined by the following claims and their equivalents.

Claims

1. A polyester molded body obtained by melting and molding a polyester produced using an inorganic stannous tin compound as a polymerization catalyst, The polyester molded body contains 10 ppm to 200 ppm of an inorganic tin compound residue, and the inorganic tin compound catalyst is an inorganic tin compound selected from the group consisting of stannous pyrophosphate, stannous phosphate, stannous tartrate, stannous acetate, stannous stearate, stannous oleate, stannous gluconate, stannous citrate, stannous ethoxide, stannous acetylacetonate, and stannous glycolate.

2. The polyester is at least one selected from the group consisting of polyethylene terephthalate, polytrimethylene terephthalate, and polytetramethylene terephthalate. The polyester molded article according to claim 1.

3. A polyester resin composition comprising a polyester produced using an inorganic stannous tin compound as a polymerization catalyst is melted and molded; A method for producing a polyester molded body, the method comprising the steps of: When polymerizing the polyester, an inorganic tin compound catalyst is added to the polyester in an amount of 10 ppm to 200 ppm; The inorganic stannous compound used is an inorganic stannous compound selected from the group consisting of stannous pyrophosphate, stannous phosphate, stannous tartrate, stannous acetate, stannous stearate, stannous oleate, stannous gluconate, stannous citrate, stannous ethoxide, stannous acetylacetonate, and stannous glycolate. A method for producing a polyester molded article.

4. The method comprises: Melting the polyester resin composition; Filling a mold with the molten polyester resin composition; and cooling and releasing the polyester resin composition filled in the mold. A method for producing the polyester molded article according to claim 3. A method for producing a polyester molding.

5. The molding step is carried out by the method of compression molding, transfer molding, lamination molding, injection molding, extrusion molding, blow molding, calendar molding, gas molding, insert molding, or vacuum molding; A method for producing the polyester molded article according to claim 3.

Citation Information

Patent Citations

  • Preparation of polyester

    JP1982190020A

  • Production of polybutylene terephthalate of low terminal-carboxyl group content

    JP1984086622A

  • Hollow polyester container

    JP1997208679A

  • Method for preparing polytrimethylene terephthalate

    JP2004224895A

  • Polybutylene terephthalate resin

    JP2005029581A