Polyester film, its manufacturing method, and method for recycling polyethylene terephthalate containers using the same

A polyester film with controlled crystallinity and a recycling method for polyethylene terephthalate containers addresses the issues of uneven shrinkage and clumping, enhancing recyclability and productivity by minimizing clumping during the recycling process.

JP7592014B2Active Publication Date: 2024-11-29MICROWORKS AMERICA INC COVINGTON +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021529073
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-10-28
Filing Date
2020-10-29
Publication Date
2024-11-29
Estimated Expiration
2040-10-29

AI Technical Summary

Technical Problem

Existing polyester films used in heat-shrinkable labels and packaging materials exhibit fast shrinkage rates and high shrinkage stress, leading to uneven shrinkage and distortion of plastic containers, and are difficult to recycle due to high crystallinity and thermal characteristics, causing clumping during the recycling process.

Method used

A polyester film with controlled crystallinity, achieved by copolymerizing diol and dicarboxylic acid to set the crystallization temperature between 70°C and 130°C, is used in conjunction with a method for recycling polyethylene terephthalate containers, allowing for heat treatment at 210°C to minimize clumping and enable efficient recycling.

Benefits of technology

The film maintains excellent shrinkage properties and seam properties while significantly reducing clumping during recycling, improving the quality, yield, and productivity of recycled polyester chips, and eliminating the need for separate film removal steps.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007592014000006
    Figure 0007592014000006
  • Figure 0007592014000007
    Figure 0007592014000007
  • Figure 0007592014000008
    Figure 0007592014000008
Patent Text Reader

Abstract

The examples relate to polyester film, its manufacturing method, and a method for recycling polyethylene terephthalate (PET) containers using the same. The crystallization temperature (Tc) of the polyester film measured by a differential scanning calorimetry is either not measurable or satisfies a range of 70°C to 130°C, thereby controlling the crystallinity, providing excellent shrinkage characteristics and recyclability, and causing almost no clumping even during long periods of high-temperature drying in the recycling process.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The embodiment relates to a polyester film, a manufacturing method thereof, and a method for recycling polyethylene terephthalate (PET) containers using the same. Specifically, the embodiment relates to a polyester film with controlled crystallinity and excellent recyclability, a manufacturing method thereof, and a method for recycling polyethylene terephthalate (PET) containers equipped with such a polyester film. [Background technology]

[0002] Recently, heat-shrinkable labels and packaging materials have been attracting attention as beverage and food containers are produced in various shapes and full-surface packaging is often used to attract consumers' attention. Heat-shrinkable labels and packaging materials utilize the property that polymer films shrink back to their pre-stretched shape at a certain temperature or higher after stretching and orientation. A typical heat-shrinkable labeling or packaging process involves cutting a heat-shrinkable film, printing it with the desired design, rolling it up, gluing both ends with an adhesive solvent, loosely covering the container, and applying heat to shrink it.

[0003] The film applied to the heat shrinking process is required to have not only basic properties such as heat resistance, chemical resistance, weather resistance, printability, but also container sealing property, heat shrink uniformity, running property in the length direction, crack resistance, etc. Polyvinyl chloride film, polystyrene film, polypropylene film, etc. have been used in the heat shrinking process, and recently polyester film, which has properties such as high heat resistance, weather resistance, ease of incineration, and excellent printability, has been widely used.

[0004] However, normal polyester films have a high shrinkage rate and high shrinkage stress, which can cause defects due to non-uniform shrinkage and distortion of plastic containers, etc. Patent Document 1 discloses that a heat-shrinkable polyester film is blended with 5% by weight or more of a polyester elastomer to suppress the occurrence of wrinkles, uneven shrinkage, distortion, etc. due to heat shrinkage when packaging plastic bottles on the entire surface.

[0005] In this way, the polyester film used in the heat shrink process is manufactured by lowering the crystallinity by blending a soft component into the polyester resin, and is developed to have thermal properties such as temperature-specific shrinkage rate and shrinkage stress, chemical resistance suitable for the seaming process, and recyclability that has emerged in response to the recent issue of waste plastic.

[0006] In addition, in recent years, as concerns about environmental issues have increased, there has been a demand for responses to the issue of recycling products made using thermoplastic polymers. In particular, polyethylene terephthalate (PET), a thermoplastic resin with excellent properties such as heat resistance, processability, transparency, and non-toxicity, is widely used to manufacture a wide range of products such as films, fibers, bottles, and containers, and research is being conducted to improve the recycling rate. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Korean Patent Publication No. 2002-0062838 Summary of the Invention [Problem to be solved by the invention]

[0008] Therefore, the present invention aims to provide a polyester film that has controlled crystallinity, excellent shrinkage characteristics, and excellent recyclability, and that hardly generates irregular clumping even during long-term high-temperature drying in the recycling process, a manufacturing method thereof, and a recycling method for polyethylene terephthalate containers using the same. [Means for solving the problem]

[0009] The polyester film according to one embodiment is a polyester film including a copolymer polyester resin in which a diol and a dicarboxylic acid are copolymerized, and has a crystallization temperature (Tc) measured by a differential scanning calorimetry that is not measurable or is between 70°C and 130°C. When flakes obtained by crushing a polyethylene terephthalate (PET) container having the polyester film are heat-treated at a temperature of 210°C for 90 minutes, the clumping ratio is 10% or less.

[0010] Another embodiment of the method for producing a polyester film includes the steps of preparing a copolymerized polyester resin in which a diol and a dicarboxylic acid are copolymerized, melt-extruding the copolymerized polyester resin at a temperature of 250°C to 300°C to produce an unstretched sheet, stretching the unstretched sheet at a temperature of 70°C to 100°C, and then heat-setting the unstretched sheet at a temperature of 65°C to 90°C to produce a polyester film, wherein the crystallization temperature (Tc) of the polyester film measured by a differential scanning calorimeter is not measured or is 70°C to 130°C, and when flakes obtained by crushing a polyethylene terephthalate container provided with the polyester film are heat-treated at a temperature of 210°C for 90 minutes, the clumping fraction is 10% or less.

[0011] Another embodiment of a method for recycling polyethylene terephthalate containers includes the steps of preparing a polyethylene terephthalate container having the polyester film, crushing the polyethylene terephthalate container having the film to obtain flakes, and heat-treating the flakes to produce recycled polyester chips, wherein when the flakes are heat-treated at a temperature of 210°C for 90 minutes, the clumping fraction is 10% or less, and the flakes include first flakes obtained by crushing the polyethylene terephthalate container and second flakes obtained by crushing the polyester film. Effect of the Invention

[0012] The crystallization temperature (Tc) of the polyester film according to the embodiment is not measurable or satisfies 70°C to 130°C when measured by a differential scanning calorimeter, so that the crystallinity can be easily controlled. Therefore, during the recycling process, the occurrence of clumping is suppressed even during long-term high-temperature drying, so that the polyester film can be applied to the recycling process.

[0013] In addition, since the clumping fraction is very low, recyclability can be improved while preventing environmental pollution, and the quality, yield and productivity of recycled polyester chips produced by the method for recycling polyethylene terephthalate containers using the polyester film can be improved.

[0014] Moreover, the method for recycling polyethylene terephthalate containers according to the embodiment does not require a separate process for separating the container from the film, so time and cost are reduced and it is economical. [Brief description of the drawings]

[0015] [Figure 1] FIG. 1 shows the polyester film applied to the product before and after heat shrinking. [Diagram 2] FIG. 2 shows a method for measuring the clamping of a polyethylene terephthalate container provided with a polyester film in Experimental Example 2-1. [Diagram 3] FIG. 3 shows a method for measuring the heat shrinkage rate of the polyester film in Experimental Example 1-2. [Figure 4] FIG. 4 shows a method for measuring the solvent adhesion properties of polyester film. [Diagram 5] FIG. 5 shows a method for measuring the shrinkage stress of a polyester film. [Figure 6] FIG. 6 shows a method for measuring the skirt ratio of a polyester film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The present invention will be described in detail below with reference to examples. The examples are not limited to the contents of the following disclosure, and may be modified in various forms without departing from the spirit of the invention.

[0017] In this specification, when a part "comprises" a certain component, this does not mean that other components are excluded, but that other components may be further included, unless specifically stated to the contrary.

[0018] All numbers and expressions expressing quantities of components, reaction conditions, and the like described herein, unless otherwise specifically indicated, should be understood to be modified in all instances by the term "about."

[0019] In this specification, terms such as first, second, primary, secondary, etc. are used to describe various components, and the components are not limited by the terms. The terms are used only to distinguish one component from another.

[0020] Heat-shrinkable labels or packaging materials made of polyester film are difficult to recycle, even though they have excellent thermal properties and chemical resistance, and are almost always discarded after use. This is because when polyester film is used in the current recycling process, i.e., the regeneration process, the polyester film causes various process defects during the long, high-temperature process, which increases costs. Even if recycling is possible, there is a problem in that the high crystallinity of polyester film results in poor seaming properties when applying the Variable Sleeve Offset Printing (VSOP) method.

[0021] In addition, polyethylene terephthalate containers collected from general consumers have been washed and crushed, and then subjected to additional processes such as liquid specific gravity separation, dehydration drying and / or air specific gravity separation in order to remove a large amount of film contained in the crushed material, followed by pelletization to produce recycled polyester chips. However, even after the above processes, it is difficult to completely remove the film used as the label of the polyethylene terephthalate container, and the recycled polyester chips may be colored by the ink contained in the film. In addition, there is a problem that clumping occurs, in which the recycled polyester chips irregularly aggregate during the recycling process, especially the heat treatment process, due to the thermal properties of the film.

[0022] Therefore, a gravity separation method was proposed in which films of low specific gravity polymers such as polystyrene, polyethylene, and polypropylene are used as labels to facilitate gravity separation. However, the ink layer prevents effective low specific gravity, and it is still difficult to completely separate and remove the film. Furthermore, the problem of residual ink discoloring the recycled polyester chips could not be solved.

[0023] The polyester film according to the embodiment has controlled crystallinity, excellent shrinkage characteristics and seam characteristics in various printing methods, excellent recyclability, and almost no clumping occurs even during long-term high-temperature drying in the recycling process. Therefore, the quality, yield, and productivity of the recycled polyester chips manufactured by the polyester film or the method for recycling polyethylene terephthalate containers using the same can be improved.

[0024] [Polyester film] The polyester film according to one embodiment is a polyester film including a copolymer polyester resin in which a diol and a dicarboxylic acid are copolymerized, and has a crystallization temperature (Tc) measured by a differential scanning calorimetry that is not measurable or is between 70°C and 130°C. When flakes obtained by crushing a polyethylene terephthalate (PET) container having the polyester film thereon are heat-treated at a temperature of 210°C for 90 minutes, the clumping fraction is 10% or less.

[0025] The crystallization temperature (Tc) of the polyester film according to the embodiment measured by a differential scanning calorimeter is not measured or is 70°C to 130°C. For example, the crystallization temperature (Tc) of the film measured by a differential scanning calorimeter may be not measured or may be 80°C to 130°C, 85°C to 125°C, 90°C to 123°C, 96°C to 120°C, 98°C to 120°C, or 99.5°C to 118°C. By adjusting the crystallization temperature within the above range, the crystallinity of the polyester film is effectively controlled, and the clumping fraction during the regeneration process of the film or a polyethylene terephthalate container containing the film is very low, so that the recyclability can be improved while preventing environmental pollution.

[0026] The differential scanning calorimeter (DSC) may be specifically a modulated differential scanning calorimeter (MDSC), more specifically a temperature-modulated differential scanning calorimeter (TMDSC).

[0027] Specifically, the crystallization temperature can be measured by scanning at a heating rate of 10° C. / min using a differential scanning calorimeter (DSC) mode. In the measurement results, the first endothermic temperature is the glass transition temperature (Tg), the exothermic temperature measured after the Tg is the crystallization temperature (Tc), and the endothermic temperature measured after the Tc is the melting point (Tm). The heat of crystallization is calculated as an integral value at the Tc, and the larger the value of the heat of crystallization, the faster the crystallization speed and the higher the transition rate to the crystalline phase.

[0028] In addition, when flakes obtained by crushing a polyethylene terephthalate container provided with the polyester film are heat-treated for 90 minutes at a temperature of 210° C., the clumping fraction may be 10% or less. For example, the clumping fraction may be 8% or less, 6% or less, 5% or less, or 4% or less, and preferably 3% or less, 2% or less, 1.5% or less, 1% or less, 0.8% or less, or 0.5% or less.

[0029] The clumping refers to agglomerates that may be formed during the regeneration process, and the size of the agglomerates may be, for example, three times or more the size of the flakes before the heat treatment. The clumping fraction refers to the weight ratio of the agglomerates based on the total weight of the flakes before the heat treatment.

[0030] Specifically, in the recycling process of polyethylene terephthalate containers with a film as a label, the containers are crushed into flakes, which are passed through a sieve and then subjected to a heat treatment process. In this process, the flakes may stick together to form agglomerates, which are called clumping. The formed agglomerates are separated by filtering through a sieve again, and the weight is measured. The weight ratio of the agglomerates is calculated based on the total weight of the flakes before the heat treatment to obtain the clumping fraction. Therefore, the higher the clumping fraction, the lower the recyclability.

[0031] The polyester film according to the embodiment has effectively controlled crystallinity, so that when it is applied as a label for a polyethylene terephthalate container, wrinkles or distortion of the polyethylene terephthalate container do not occur. In addition, even if the flakes crushed together with the polyethylene terephthalate container are heat-treated during the recycling process after use, the clumping fraction is very low, so that the recyclability can be improved, and the quality, yield, and productivity of the recycled polyester chips produced by recycling can be improved.

[0032] When plastic flakes fuse together and form clumps during the recycling process, this can cause various problems, so the Association of Plastic Recyclers (APR) in the United States has established a guide (APR PET-S-08) for evaluating the clumping fraction (%). Specifically, the clumping fraction can be the ratio of the amount of the polyester film (3 parts by weight) and polyethylene terephthalate container (97 parts by weight) that cannot pass through a sieve with a mesh size of 11.2 mm (0.625'' sieve) after crushing them into particles of 9.5 mm or less and heat-treating them at a temperature of 210°C under a pressure of 8.7 kPa (a load of 2.5 kgf applied to a cylinder with a diameter of 6 cm) for 90 minutes.

[0033] The polyester film may have a melting point (Tm) of 170° C. or higher as measured by a differential scanning calorimeter. For example, the melting point may be 175° C. or higher, 180° C. or higher, or 190° C. or higher, and may be 170° C. to 240° C., 175° C. to 235° C., 180° C. to 235° C., 185° C. to 230° C., 190° C. to 225° C., or 195° C. to 225° C.

[0034] If the melting point of the polyester film exceeds the above range, the adhesive strength of the polyester film with a solvent decreases, making it difficult to use in a seam process. If the melting point is below the above range, the clumping fraction may be high.

[0035] Specifically, when the crystallization temperature of the polyester film is 96°C to 120°C and the melting point is 170°C or higher, more preferably when the crystallization temperature of the polyester film is 96°C to 120°C and the melting point is 190°C or higher, the effect of preventing the clumping phenomenon that may occur during the recycling process can be maximized.

[0036] In addition, the heat of crystallization of the film measured at the crystallization temperature (Tc) may be 0.01 J / g to 50 J / g. For example, the heat of crystallization of the film measured at the crystallization temperature (Tc) may be 0.01 J / g to 40 J / g, 0.05 J / g to 30 J / g, 0.1 J / g to 20 J / g, 0.1 J / g to 10 J / g, 0.1 J / g to 8 J / g, 0.2 J / g to 6 J / g, or 0.3 J / g to 5.7 J / g. When the heat of crystallization satisfies the above range, the crystallinity of the polyester film is effectively controlled, and the clumping fraction is very low during the regeneration process of the film or a polyethylene terephthalate container containing the film, so that the recyclability can be improved while preventing environmental pollution.

[0037] In addition, the polyester film according to the embodiment can be adjusted in shrinkage rate in the main shrinkage direction to a specific range for each temperature. For example, when the polyester film is heat-treated at a temperature of X° C. for 10 seconds, the shrinkage rate in the main shrinkage direction is adjusted to T X Then, T 70 , T 80 , T 90 , and T 100 The range of T can be adjusted. X Specifically, the heat treatment to obtain the above-mentioned polyester film may be performed by immersing the polyester film in hot water at X° C. for 10 seconds.

[0038] Specifically, when the film is heat-treated at a temperature of 70° C. for 10 seconds, the thermal shrinkage rate in the first direction (T 70 ) can be 0% to 50%. For example, T 70may be 0% or more, 5% or more, 10% or more, 15% or more, or 20% or more, and may be 50% or less, 40% or less, 35% or less, 30% or less, 25% or less, or 20% or less.

[0039] In this specification, the first direction may be a transverse direction (TD) or a machine direction (MD), and the second direction perpendicular to the first direction may be a machine direction (MD) or a transverse direction (TD). Specifically, the first direction may be a main shrinkage direction. More specifically, the first direction may be a transverse direction (TD) as a main shrinkage direction, and the second direction may be a machine direction (MD).

[0040] In addition, when the film is heat-treated at a temperature of 80° C. for 10 seconds, the thermal shrinkage rate in the first direction (T 80 ) can be 30% or more. For example, T 80 is 35% or more, 45% or more, 50% or more, or 55% or more, and may be 30% to 85%, 40% to 80%, 50% to 80%, 55% to 75%, or 58% to 71%. When heat-treated at a temperature of 80°C for 10 seconds, the heat shrinkage rate in the first direction satisfies the above range, so that labeling is easy when the film surrounds at least a part of a container. Specifically, when the film is applied to a label for a polyethylene terephthalate container, wrinkles and distortion of the polyethylene terephthalate container do not occur.

[0041] When the film is heat-treated at a temperature of 90° C. for 10 seconds, the thermal shrinkage rate in the first direction (T 90 ) can be 50% or more. For example, T 90 is 55% or more, 60% or more, or 65% or more, and may be 50% to 90%, 60% to 85%, 65% to 83%, or 69% to 80%. When heat-treated at a temperature of 90°C for 10 seconds, the heat shrinkage rate in the first direction satisfies the above range, so that labeling is easy when the film surrounds at least a part of a container. Specifically, when the film is applied to a label for a polyethylene terephthalate container, wrinkles and distortion of the polyethylene terephthalate container do not occur.

[0042] When the film is heat-treated at a temperature of 100° C. for 10 seconds, the thermal shrinkage rate in the first direction (T 100 ) can be 40% to 90%. For example, T 100 may be 40% or more, 50% or more, 60% or more, or 70% or more, and 90% or less, 85% or less, 80% or less, 75% or less, or 70% or less. That is, the polyester film may have a heat shrinkage rate in the first direction of 50% to 80% when heat-treated at a temperature of 100° C. for 10 seconds.

[0043] Meanwhile, the polyester film according to the embodiment can be adjusted in shrinkage rate in a first direction and a second direction perpendicular to the first direction within a specific range for each temperature. For example, when the polyester film is heat-treated at a temperature of X° C. for 10 seconds, the shrinkage rate in the second direction is adjusted to T X ', then T 70 ', T 75 ', T 80 ', T 90 ', and T 100 The range of T' can be adjusted within a specific range. X The heat treatment to obtain X° C. may be by immersing the polyester film in hot water at X° C. for 10 seconds.

[0044] The polyester film T 70 ', T 75 ', T 80 ', T 90 ', and T 100 Each of the T's may be independently -10% to 10%. For example, 70 ', T 75 ', T 80 ', T 90 ', and T 100 ' may be -10% or more, -8% or more, -6% or more, -4% or more, -2% or more, or 0% or more, and may be 10% or less, 8% or less, 6% or less, 4% or less, or 2% or less, respectively.

[0045] Polyester films according to implementations can have excellent solvent adhesion, i.e., seam properties.

[0046] For example, the polyester film may have a peel strength of 300 gf / in or more after adhesion with 1,3-dioxolane. Specifically, the peel strength of the polyester film after adhesion with 1,3-dioxolane may be 300 gf / in or more, 400 gf / in or more, 500 gf / in or more, 600 gf / in or more, or 700 gf / in or more, and 3000 gf / in or less, 2500 gf / in or less, 2000 gf / in or less, or 1500 gf / in or less. When the peel strength of the polyester film is adjusted within the above range, it may be suitable for use in a polyester film seaming process.

[0047] The peel strength can be measured under the following conditions: a solvent is applied onto the polyester film, another polyester film is laminated thereon, a pressure of 160 Pa is applied to the solvent-applied portion for 1 hour, and then the polyester film is peeled off at a speed of 300 mm / min and an angle of 180°.

[0048] 4 shows a method for measuring the adhesive properties of a polyester film using a solvent. For example, 1,3-dioxolane is applied to a first polyester film 100 in a strip shape having a width of 2 mm, and the adhesive portion 120 is formed to an area of ​​0.6 cm2. 2 A second polyester film 200 was attached on top of the polyester film, a 2 kg weight was placed on the adhesive portion 120, and the mixture was aged for 1 hour. The two polyester films were peeled at a speed of 300 mm / min at an angle of 180°, while measuring the maximum force. The polyester film was cut into a rectangle with dimensions (x, y) of 9 cm wide and 3 cm long.

[0049] The polyester film according to the embodiment may have a shrinkage stress in the main shrinkage direction adjusted within a specific range. For example, when the polyester film is heat-treated at 90° C. for 1 minute, the maximum stress in the main shrinkage direction may be 7.0 N or 6.0 N. Also, when the polyester film is heat-treated at 90° C. for 1 minute, the residual stress in the main shrinkage direction may be 6.0 N or 5.5 N.

[0050] Specifically, the heat treatment for obtaining the shrinkage stress may be performed by fixing the polyester film in the main shrinkage direction and immersing it in hot water at 90° C. for 1 minute. In addition, the stress at the highest point in the curve of the stress as a function of time obtained during the shrinkage process may be defined as the maximum stress, and the stress at the end of the shrinkage time may be defined as the residual stress.

[0051] FIG. 5 shows a method for measuring the shrinkage stress of a polyester film. For example, the first polyester film 100 was cut to have an initial dimension x of 110 mm in the direction to be measured, an excess dimension z of 5 mm at both ends, and a dimension y of 15 mm in the direction perpendicular thereto (FIG. 5(a)). The cut film was attached to a stress tester 2, and both ends of the film were fixed to jigs 21 spaced 100 mm apart (FIG. 5(b)). The stress tester 2 with the film attached was immersed in a water bath at 90° C. for 1 minute, and the maximum stress (S MAX ), and residual stress after shrinkage (S RES ) was measured by the load cell 22 (FIG. 5(c)).

[0052] The skirt ratio of the polyester film according to the embodiment may be adjusted within a specific range. Specifically, the skirt ratio may be calculated by fixing the polyester film in the main shrinkage direction, measuring the length of the polyester film before and after shrinkage in a direction perpendicular to the main shrinkage direction, and dividing the difference in the measured length before and after shrinkage by the length of the polyester film in the main shrinkage direction, as a ratio. More specifically, the skirt ratio measured under the condition of heat-treating the polyester film at a temperature of 90° C. for 10 seconds may be 17.4%.

[0053] Fig. 6 shows a method for measuring the skirt ratio of a polyester film. For example, the polyester film 100 was cut to an initial dimension x1 of 60 mm in the direction to be measured, and fixed to a heat fixing frame with a width y of 15 mm using a jig 21 (Fig. 6(a)). After immersing the film in a water bath at 90°C for 10 seconds, the reduced dimension x2 was measured (Fig. 6(b)). In this specification, the film was fixed in the width direction (TD), which is the main shrinkage direction, and the length after shrinkage in the machine direction (MD), which is perpendicular to the width direction (TD), was measured and calculated based on the following formula.

[0054] ΔSR(mm)=x1(mm)-x2(mm) SR%(%)=ΔSR(mm) / y(mm)×100 The glass transition temperature (Tg) of the film measured by a differential scanning calorimeter may be equal to or higher than 60° C. For example, the glass transition temperature (Tg) of the film measured by a differential scanning calorimeter may be equal to or higher than 60° C., equal to or higher than 65° C., equal to or higher than 70° C. and lower than 80° C., or equal to or higher than 70° C. and lower than 80° C., or from 70° C. to 75° C.

[0055] The film may have a light transmittance of 90% or more at a wavelength of 550 nm. Specifically, the light transmittance of the film measured at a wavelength of 550 nm before and after immersion in a 1% aqueous sodium hydroxide (NaOH) solution at a temperature of 85° C. may be 90.5% or more, 91% or more, 92% or more, or 93% or more, respectively.

[0056] The change in light transmittance of the film before and after immersion in a 1% aqueous sodium hydroxide (NaOH) solution at a temperature of 85° C. may be 0.7% or less. For example, the change in light transmittance of the film before and after the immersion may be 0.6% or less or 0.5% or less.

[0057] The change in light transmittance means the absolute value of the difference between the light transmittance of the film measured at a wavelength of 550 nm before the immersion and the light transmittance of the film measured at a wavelength of 550 nm after the immersion.

[0058] Furthermore, the change in Col-L (ΔL) before and after immersion of the film in a 1% aqueous sodium hydroxide (NaOH) solution at a temperature of 85° C. may be 0.7 or less, the change in Col-a (Δa) may be 0.5 or less, and the change in Col-b (Δb) may be 0.5 or less. For example, the change in Col-L (ΔL) before and after immersion may be 0.65 or less, 0.6 or less, 0.55 or less, or 0.5 or less, the change in Col-a (Δa) may be 0.3 or less, 0.1 or less, 0.08 or less, 0.06 or less, or 0.05 or less, and the change in Col-b (Δb) may be 0.3 or less, 0.1 or less, 0.08 or less, or 0.07 or less.

[0059] The change in Col-L (ΔL) means the absolute value of the difference between the Col-L value before immersion and the Col-L value after immersion, the change in Col-a (Δa) means the absolute value of the difference between the Col-a value before immersion and the Col-a value after immersion, and the change in Col-b (Δb) means the absolute value of the difference between the Col-a value before immersion and the Col-a value after immersion.

[0060] The Col-L, Col-a, and Col-b are color systems established by the International Commission on Illumination (CIE (Commission International d'Eclairage)), in which colors are expressed by L (lightness), a (complementary color of green to red), and b (complementary color of yellow to blue), and can be measured using an UltraScan PRO (HunterLab), but are not limited thereto.

[0061] The polyester film according to the embodiment includes a copolymerized polyester resin. Specifically, the copolymerized polyester resin may be a copolymer of two or more diols and dicarboxylic acids, and more specifically, may be a copolymerized polyethylene terephthalate (Co-PET) resin.

[0062] Specifically, the diol may include at least one selected from the group consisting of ethylene glycol, diethylene glycol, neopentyl glycol, alkyl group-substituted or unsubstituted propanediol, alkyl group-substituted or unsubstituted butanediol, alkyl group-substituted or unsubstituted pentanediol, alkyl group-substituted or unsubstituted hexanediol, alkyl group-substituted or unsubstituted octanediol, and combinations thereof.

[0063] For example, the diol may include one or more selected from the group consisting of ethylene glycol, diethylene glycol, neopentyl glycol, 1,3-propanediol, 1,2-octanediol, 1,3-octanediol, 2,3-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 2-butyl-2-ethyl-1,3-propanediol, 2,2-diethyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, 3-methyl-1,5-pentanediol, and 1,1-dimethyl-1,5-pentanediol.

[0064] The dicarboxylic acid may include an aromatic dicarboxylic acid, an aliphatic dicarboxylic acid, an alicyclic dicarboxylic acid, or an ester thereof.

[0065] For example, the dicarboxylic acid may be terephthalic acid, dimethyl terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, orthophthalic acid, adipic acid, azelaic acid, sebacic acid, decanedicarboxylic acid, esters thereof, or combinations thereof. Specifically, the dicarboxylic acid may include one or more selected from the group consisting of terephthalic acid, dimethyl terephthalate, naphthalenedicarboxylic acid, and orthophthalic acid.

[0066] According to an embodiment, the copolymer polyester resin may be a polymer of two or more diols and an aromatic dicarboxylic acid. Specifically, the copolymer polyester resin may be a polymer of ethylene glycol, a diol containing one or more comonomers, and an aromatic dicarboxylic acid.

[0067] The diol comprises ethylene glycol and may comprise one or more comonomers selected from the group consisting of neopentyl glycol and diethylene glycol.

[0068] Specifically, the diol may contain 50 mol % to 90 mol % of ethylene glycol based on the total number of moles of the diol. For example, the diol may contain 60 mol % to 90 mol %, 65 mol % to 88 mol %, 68 mol % to 85 mol %, 70 mol % to 83 mol %, or 71 mol % to 80 mol % of ethylene glycol based on the total number of moles of the diol.

[0069] In addition, the diol may contain at least one comonomer selected from the group consisting of neopentyl glycol and diethylene glycol at 15 mol% or more. For example, the diol may contain at least one comonomer selected from the group consisting of neopentyl glycol and diethylene glycol at 17 mol% or more, 19 mol% or more, 20 mol% or more, 15 mol% to 50 mol%, 15 mol% to 40 mol%, 17 mol% to 35 mol%, 19 mol% to 30 mol%, or 20 mol% to 29 mol% based on the total number of moles of the diol. When the content of the comonomer satisfies the above range, the heat shrinkage rate in the main shrinkage direction is excellent and the crystallinity can be controlled more effectively.

[0070] In addition, if the content of the comonomer is less than the above range, the heat shrinkage property of the polyester film may be deteriorated. Specifically, the heat shrinkage rate of the polyester film in the main shrinkage direction may be insufficient at a specific temperature, and the heat shrinkage rate of the polyester film in a direction perpendicular to the main shrinkage direction may be excessively high at a specific temperature.

[0071] Specifically, the diol may contain diethylene glycol as a comonomer. For example, the content of diethylene glycol in the diol may be 1 mol% to 10 mol%, 1 mol% to 8 mol%, 3 mol% to 6 mol%, or 3.5 mol% to 5.5 mol%.

[0072] The diol may contain neopentyl glycol as a comonomer. For example, the content of neopentyl glycol in the diol may be 5 mol% to 35 mol%, 7 mol% to 33 mol%, 10 mol% to 30 mol%, 13 mol% to 28 mol%, or 15 mol% to 25 mol%.

[0073] When the content of neopentyl glycol satisfies the above range, the heat shrinkage rate in a first direction or a second direction perpendicular to the first direction during heat shrinkage of the film can be easily adjusted, and wrinkles and deformation can be more effectively prevented when the film is applied to a container.

[0074] The polyester resin may further contain a monohydric alcohol other than the diol component. For example, the monohydric alcohol may be methanol, ethanol, isopropyl alcohol, allyl alcohol, or benzyl alcohol. Specifically, the polyester resin may contain the monohydric alcohol in an amount of 10 mol% to 30 mol%, 13 mol% to 25 mol%, or 15 mol% to 22 mol% based on the total number of moles of the diol component and the monohydric alcohol, but is not limited thereto.

[0075] The dicarboxylic acid may comprise an aromatic dicarboxylic acid. For example, the dicarboxylic acid may comprise 80 mol% or more, 90 mol% or more, 95 mol% or more, 99 mol% or more, or 100 mol% of terephthalic acid or dimethyl terephthalic acid, based on the total number of moles of the dicarboxylic acid.

[0076] The diol and the dicarboxylic acid may undergo a transesterification reaction and then be polymerized to form a copolymerized polyester resin.

[0077] Specifically, the transesterification catalyst may be one or more catalysts selected from the group consisting of manganese acetate tetrahydrate, calcium, and zinc. The content of the catalyst may be 0.02 to 0.2 parts by weight, 0.02 to 0.1 parts by weight, or 0.05 to 0.08 parts by weight based on the total weight of the dicarboxylic acid.

[0078] After the ester exchange reaction is completed, one or more additives selected from the group consisting of silica, potassium, and magnesium; a stabilizer such as trimethyl phosphate; and a polymerization catalyst such as antimony trioxide or tetrabutylene thiamine may be added as necessary.

[0079] The polyester film may have a thickness of 10 μm to 100 μm. For example, the base layer may have a thickness of 20 μm to 80 μm, 30 μm to 70 μm, 35 μm to 65 μm, 35 μm to 55 μm, 40 μm to 60 μm, or 35 μm to 45 μm.

[0080] [Manufacturing method of polyester film] Another embodiment of the method for producing a polyester film includes the steps of preparing a copolymerized polyester resin in which a diol and a dicarboxylic acid are copolymerized, melt-extruding the copolymerized polyester resin at a temperature of 250°C to 300°C to produce an unstretched sheet, stretching the unstretched sheet at a temperature of 70°C to 100°C, and then heat-setting the unstretched sheet at a temperature of 65°C to 90°C to produce a polyester film, wherein the crystallization temperature (Tc) of the polyester film measured by a differential scanning calorimeter is not measured or is 70°C to 130°C, and when flakes obtained by crushing a polyethylene terephthalate container provided with the polyester film are heat-treated at a temperature of 210°C for 90 minutes, the clumping fraction is 10% or less.

[0081] The composition and process conditions of the polyester film finally produced by the above method are adjusted so as to satisfy the above-mentioned characteristics (crystallization temperature, shrinkage characteristics, etc.) Specifically, in order for the final polyester film to satisfy the above-mentioned characteristics, the composition of the copolymerized polyester resin may be adjusted, and the extrusion temperature, casting temperature, preheating temperature during stretching, stretch ratio for each direction, stretching temperature, stretching speed, etc. may be adjusted, or the heat treatment temperature and relaxation rate may be adjusted while performing heat treatment and relaxation after stretching.

[0082] Each step will be described in more detail below. First, the copolymer polyester resin is prepared. The copolymer polyester resin is as described above.

[0083] Specifically, the polymerization of the copolymerized polyester resin may be carried out by a normal transesterification reaction and polycondensation reaction, and the diol and dicarboxylic acid components and their contents used in this reaction are as exemplified above.

[0084] Thereafter, the copolymer polyester resin is melt-extruded at a temperature of 250°C to 300°C or 260°C to 280°C, and then cooled to obtain an unstretched sheet. The unstretched sheet may be preheated while passing through a chamber while being transported at a speed of 10 m / min to 110 m / min, 25 m / min to 90 m / min, 40 m / min to 80 m / min, or 50 m / min to 60 m / min.

[0085] The preheating may be performed for 0.01 to 1 minute at 90° C. to 120° C. For example, the preheating temperature (T1) may be 95° C. to 115° C. or 97° C. to 113° C., and the preheating time may be 0.05 to 0.5 minutes, or 0.08 to 0.2 minutes.

[0086] Thereafter, the preheated unstretched sheet is stretched at a temperature of 70°C to 95°C.

[0087] Specifically, the stretching may be uniaxial stretching or biaxial stretching. Specifically, the stretching may be uniaxial stretching in the transverse direction (TD) or biaxial stretching in the machine direction (MD) followed by transverse direction (TD).

[0088] The stretching may be performed at a temperature lower than the preheating temperature (T1) by 10° C. to 20° C. For example, the stretching may be performed at 70° C. to 100° C., 75° C. to 100° C., 80° C. to 98° C., or 83° C. to 96° C.

[0089] When the stretching is uniaxial stretching, the stretching may be performed at a stretch ratio of 3.5 to 5 times, 3.5 to 4.8 times, or 3.8 to 4.6 times in the transverse direction (TD), and when the stretching is biaxial stretching, the stretching may be performed at a stretch ratio of 1.1 to 2 times or 1.1 to 1.5 times in the machine direction (MD), and then at a stretch ratio of 3.5 to 5 times, 3.5 to 4.8 times, or 3.8 to 4.6 times in the transverse direction (TD).

[0090] In addition, a coating process may be performed after the stretching. Specifically, a coating process may be performed before uniaxial stretching in the transverse direction (TD), or after stretching in the machine direction (MD) and before stretching in the transverse direction (TD). More specifically, a coating process may be performed to form an accelerating layer or the like that may impart functionality such as antistatic properties to the film. The coating process may be performed by spin coating or in-line coating, but is not limited thereto.

[0091] Thereafter, the stretched sheet is heat-set at a temperature of 65° C. to 90° C. to produce a polyester film.

[0092] The heat fixing may be annealing, and may be performed for 0.01 to 1 minute at a temperature of 65° C. to 90° C. For example, the heat fixing temperature (T2) may be 65° C. to 85° C. or 69° C. to 81° C., and the heat fixing time may be 0.05 to 0.5 minutes or 0.08 to 0.2 minutes.

[0093] [How to recycle polyethylene terephthalate containers] Another embodiment of a method for recycling polyethylene terephthalate containers includes the steps of preparing a polyethylene terephthalate container having the polyester film, crushing the polyethylene terephthalate container having the film to obtain flakes, and heat-treating the flakes to produce recycled polyester chips, wherein when the flakes are heat-treated at a temperature of 210°C for 90 minutes, the clumping fraction is 10% or less, and the flakes include first flakes obtained by crushing the polyethylene terephthalate container and second flakes obtained by crushing the polyester film.

[0094] To recycle a polyethylene terephthalate container according to one implementation, first provide a polyethylene terephthalate container at least partially surrounded by the polyester film.

[0095] Conventionally, collected waste products, which may contain a mixture of containers, metals, glass, plastics, etc., are washed and polyester containers are sorted, and a process is carried out to remove the films encasing the containers in order to improve the recyclability and quality of the containers. The removal process has been carried out by mechanically tearing or cutting the films, or by additional processes such as liquid specific gravity separation, dehydration drying, air specific gravity separation, or pelletization.

[0096] However, it is difficult to completely remove the film in the removal process, and in particular, it is difficult to improve the quality of the recycled polyester chips produced due to the ink residue formed on the film.

[0097] The polyester container recycling method according to the embodiment has the effect of reducing costs because recycled polyester chips can be produced without a separate process of removing the film surrounding the polyethylene terephthalate container.

[0098] The polyethylene terephthalate container has the polyester film on its outer surface. Specifically, after the polyester film surrounds the outer surface of the polyethylene terephthalate container, the film may be shrunk by steam or hot air to enclose at least a portion of the outer surface of the polyethylene terephthalate container. For example, the polyester film may be a heat-shrinkable film that serves as a label for the polyethylene terephthalate container, but is not limited thereto. The polyester film is as described above.

[0099] The polyethylene terephthalate container provided with the film is then crushed to obtain flakes.

[0100] Specifically, at least a portion of the outer surface of the polyethylene terephthalate container is surrounded by the film, and the container and the film are crushed together to obtain flakes without a separate process for separating the container and the film.

[0101] That is, the flakes include first flakes obtained by pulverizing the polyester container and second flakes obtained by pulverizing the film.

[0102] The particle size of the first flakes may be 0.1 mm to 25 mm, and the particle size of the second flakes may be 0.1 mm to 25 mm. For example, the particle size of the first flakes may be 0.3 mm to 23 mm, 0.5 mm to 20 mm, 1 mm to 20 mm, 0.5 mm to 15 mm, 0.5 mm to 13 mm, 1 mm to 18 mm, 1 mm to 15 mm, 1 mm to 13 mm, or 2 mm to 10 mm, and the particle size of the second flakes may be 0.3 mm to 23 mm, 0.5 mm to 20 mm, 1 mm to 20 mm, 0.5 mm to 15 mm, 0.5 mm to 13 mm, 1 mm to 18 mm, 1 mm to 15 mm, 1 mm to 13 mm, or 2 mm to 10 mm, but is not limited thereto.

[0103] Thereafter, before the heat treatment step, a step of washing the ground flakes can be further carried out. Specifically, the washing step can be carried out at a temperature of 85°C to 90°C with a washing solution containing water and / or 1 part by weight of aqueous sodium hydroxide solution.

[0104] For example, the crushed flakes may be washed with water, washed with the washing solution, and then washed with water for a third time. By carrying out the washing steps, impurities that may remain in the crushed flakes can be removed, and ink components can be effectively removed, thereby improving the quality and purity of the recycled polyester chips produced and maximizing recyclability.

[0105] In addition, after the washing step, a step of drying the washed flakes for 10 to 90 minutes at 60° C. to 175° C. can be further performed. For example, the drying step can be performed at 65° C. to 175° C., 70° C. to 170° C., 90° C. to 165° C., 100° C. to 165° C., 120° C. to 165° C., 140° C. to 165° C., or 150° C. to 165° C. for 10 to 85 minutes, 10 to 70 minutes, or 15 to 30 minutes.

[0106] The washing and drying steps may be repeated 1 to 5 times. For example, the washing and drying steps may be repeated 2 to 5 times or 3 to 5 times in order to effectively remove impurities remaining in the flakes.

[0107] Finally, the flakes are heat treated to produce recycled polyester chips.

[0108] Specifically, the flakes include first flakes obtained by pulverizing the polyethylene terephthalate container and second flakes obtained by pulverizing the polyester film.

[0109] The heat treatment may be performed for 60 to 120 minutes at 200° C. to 220° C. For example, the heat treatment may be performed for 70 to 120 minutes at 200° C. to 215° C. or 205° C. to 220° C., or for 80 to 120 minutes.

[0110] In addition, when the flakes are heat-treated at a temperature of 210°C for 90 minutes, the clumping fraction is 10% or less. Therefore, the clumping fraction that may occur when the first and second flakes stick to each other is low, and the recycled polyester chips produced are of excellent quality. Specifically, the flakes include second flakes obtained by pulverizing the polyester film according to the embodiment, and thus the quality of the recycled polyester chips produced can be improved by effectively reducing or preventing the formation of agglomerates.

[0111] After the heat treatment process, recycled polyester chips can be obtained. Specifically, after the heat treatment process, recycled polyester chips including the first flakes and the second flakes can be obtained. For example, the flakes can be melt-extruded and then cut to obtain recycled polyester chips, but the present invention is not limited thereto.

[0112] [Recycled polyester chips] In another embodiment, recycled polyester chips are produced by the method for recycling polyethylene terephthalate containers.

[0113] Specifically, the recycled polyester chips may include first flakes including polyethylene terephthalate and second flakes including polyester resin.

[0114] The intrinsic viscosity (IV) of the recycled polyester chips may be 0.55 dl / g or more. For example, the intrinsic viscosity of the recycled polyester chips may be 0.58 dl / g or more, or 0.59 dl / g or more, and may be 0.55 dl / g to 3.0 dl / g, 0.55 dl / g to 2.0 dl / g, 0.55 dl / g to 1.0 dl / g, 0.58 dl / g to 0.85 dl / g, or 0.58 dl / g to 0.7 dl / g.

[0115] The recycled polyester chips may contain 70% to 99% by weight of polyethylene terephthalate and 1% to 30% by weight of copolymer polyester resin, based on the total weight of the recycled polyester chips. For example, the recycled polyester chips may contain 80% to 99% by weight, 90% to 99% by weight, or 95% to 99% by weight of polyethylene terephthalate and 1% to 20% by weight, 1% to 10% by weight, or 1% to 5% by weight of copolymer polyester resin, based on the total weight of the recycled polyester chips.

[0116] (Example) The above contents will be described in more detail with reference to the following examples, however, the following examples are only for illustrating the present invention and the scope of the examples is not limited to these examples.

[0117] [Production of polyester film] (Example 1-1) (1) Preparation of copolymer polyester resin Terephthalic acid (TPA) as a dicarboxylic acid, ethylene glycol (EG) as a diol, and a comonomer were charged into an autoclave equipped with a stirrer and a distillation column, and manganese acetate was added as an ester exchange reaction catalyst in an amount of 0.07 parts by weight per 100 parts by weight of the dicarboxylic acid. The reaction was then carried out by removing the by-product methanol while increasing the temperature to 220°C.

[0118] When the transesterification reaction was completed, 0.07 parts by weight of silica with an average particle size of 0.28 μm was added per 100 parts by weight of dicarboxylic acid, and 0.4 parts by weight of trimethyl phosphate was added as a stabilizer. After 5 minutes, 0.035 parts by weight of antimony trioxide and 0.005 parts by weight of tetrabutyl titanate were added as polymerization catalysts and stirred for 10 minutes. Then, the reactants were transferred to a second reactor equipped with a vacuum device, and the pressure was gradually reduced while the temperature was raised to 285°C, and polymerization was carried out for about 210 minutes to obtain a copolymerized polyester resin.

[0119] (2) Film manufacturing The copolymer polyester resin prepared in step (1) was extruded at 270°C through a T-die and cooled to obtain an unstretched sheet. The unstretched sheet was then passed through a roll while being transported at a speed of 55 m / min to adjust its thickness. The unstretched sheet was preheated at 105°C for 0.1 minutes while being transported at a speed of 55 m / min, and stretched 4.3 times in the transverse direction (TD) at 83°C. The stretched sheet was then heat-set at a temperature of 69°C for 0.1 minutes to produce a polyester film having a thickness of 40 μm.

[0120] (Examples 1-2 to 1-6 and Comparative Example 1-1) A polyester film was prepared in the same manner as in Example 1-1, except that the composition, content and process conditions were changed as shown in Table 1 below.

[0121] [Table 1]

[0122] (Experimental Example 1-1: Tc, Tm and heat of crystallization) 4 mg of each sample of the polyester films of Examples 1-1 to 1-6 and Comparative Example 1-1 prepared above was placed in a differential scanning calorimeter (Q2000, TA Instruments) and scanned at a heating rate of 10° C. / min using a differential scanning calorimeter (DSC) mode.

[0123] In the measurement results, the first endothermic temperature was the glass transition temperature (Tg), the exothermic temperature measured after the Tg was the crystallization temperature (Tc), and the endothermic temperature measured after the Tc was the melting point (Tm). The integral value at the Tc was calculated as the heat of crystallization, and the larger the value of the heat of crystallization, the faster the crystallization speed and the higher the transition rate to the crystalline phase.

[0124] (Experimental Example 1-2: Heat shrinkage rate) Fig. 3 shows a method for measuring the heat shrinkage rate of a polyester film. Referring to Fig. 3, the polyester films 100 of Examples 1-1 to 1-6 and Comparative Example 1-1 prepared above were cut to 300 mm in the direction to be measured and 15 mm in the direction perpendicular thereto. At this time, the 300 mm is the first dimension x1 before shrinkage, and the 15 mm is the second dimension (Fig. 3(a)).

[0125] The cut polyester film 100 was immersed in a water bath heated to 80°C or 90°C for 10 seconds, and the shrink dimension of the polyester film 100a after shrinking, i.e., the first dimension x2 after shrinking, was measured (FIG. 3(b)) and calculated based on the following formula. The heat shrinkage rate (%) in this experimental example was obtained with respect to the main shrinkage direction (TD) of the film. Heat shrinkage rate (%) = (x1-x2) / x1×100

[0126] [Table 2]

[0127] As can be seen from Table 2 above, the polyester films of Examples 1-1 to 1-6 had heat shrinkage rates at each temperature in the main shrinkage direction (TD), crystallization temperatures (Tc), and the resulting heat of crystallization and melting points (Tm) all within the preferred ranges.

[0128] [Manufacturing of recycled polyester chips] (Example 2-1) (1) Manufacture of polyethylene terephthalate containers with polyester film A part of the outer surface of a polyethylene terephthalate container (PET container, 30 g) was wrapped with the polyester film of Example 1-1 prepared above. At this time, it was fixed using an acrylic adhesive. Thereafter, the polyester film of Example 1-1 was shrunk under a temperature of 90°C and hot air conditions to obtain a polyethylene terephthalate container provided with a polyester film.

[0129] (2) Polyethylene terephthalate container recycling process The container equipped with the polyester film produced in step (1) was crushed in a crusher to obtain flakes. The flakes were first washed with water. Then, they were second washed for 15 minutes with a cleaning solution (a mixture of 0.3 parts by weight of Triton X-100 solution and 1.0 parts by weight of NaOH solution) stirred in a water tank at 88°C and 880 rpm. Then, the second washed flakes were third washed with water at room temperature to remove the remaining cleaning solution, and dried at 160°C for 20 minutes.

[0130] Thereafter, the chips were heat-treated at 210° C. for 90 minutes to produce recycled polyester chips.

[0131] (Examples 2-2 to 2-8 and Comparative Example 2-1) Recycled polyester chips were produced in the same manner as in Example 2-1, except that the polyester films of Examples 1-2 to 1-6 and Comparative Example 1-1 were used instead of the polyester film of Example 1-1.

[0132] (Experimental Example 2-1: Clumping ratio) The clumping fraction (%) was measured according to the Association of American Plastic Recyclers (APR) procedure for Polyethylene Terephthalate Flake Clumping Evaluation (APR PET-S-08).

[0133] FIG. 2 illustrates a method for measuring the clamping of a polyethylene terephthalate container provided with a polyester film.

[0134] As shown in FIG. 2(a), a product 1 having a polyester film as a label 11a in a polyethylene terephthalate container 20 was crushed in a crusher 6 and passed through a first sieve with a mesh size of 9.5 mm (0.374″ sieve, not shown), to obtain mixed flakes consisting of 97 g of first flakes 20a in which the polyethylene terephthalate was crushed and 3 g of second flakes 10a in which the polyester film was crushed.

[0135] Then, as shown in Fig. 2(b), the mixed flakes were placed in a cylinder with a diameter of 6 cm and a height of 8 cm, and a weight of 2.5 kg was placed on top of the mixed flakes to apply a load. The cylinder with the weight placed on it was then heat-treated in a convection oven at 210°C for 90 minutes, and then cooled at room temperature.

[0136] Thereafter, as shown in FIG. 2(c), the cooled mixed flakes were placed on a second sieve 8 (0.625″ sieve) with a mesh size d of 11.2 mm and filtered, and the agglomerated mixed flakes 10b remaining on the second sieve 8 were collected and weighed. Clumping fraction (%) = weight of clumped mixed flakes / weight of initial mixed flakes x 100

[0137] (Experimental Example 2-2: Intrinsic Viscosity) The recycled polyester chips produced in Examples 2-1 to 2-6 and Comparative Example 2-1 were dissolved in ortho-chlorophenol at 100° C., and the drop time was measured using an Ostwald viscometer in a thermostatic bath at 35° C. to obtain the relative viscosity. The intrinsic viscosity IV of the value corresponding to the obtained relative viscosity was confirmed in Table 3 below and rounded off to two decimal places.

[0138] [Table 3] JPEG0007592014000004.jpg27156

[0139] [Table 4]

[0140] As shown in Table 4, the recycled polyester chips of Examples 2-1 to 2-6, which satisfy the specific crystallization temperature (Tc) range and specific melting point (Tm) range in Table 2, have a very low clumping fraction in a similar intrinsic viscosity range compared to Comparative Example 2-1, which is advantageous for long-term high-temperature drying during the recycling process and can improve recyclability. [Explanation of symbols]

[0141] d: mesh diameter x: 1st dimension x1: First dimension before shrinkage x2: First dimension after shrinkage y: second dimension z: the third dimension S MAX : Maximum stress S RES : Residual stress 1: Products with labels attached 2: Stress tester 6: Crusher 7: Weight 8: Sieve 10a: 2nd flake 10b: Agglomerated mixed flakes 11: Label (before shrinkage) 11a: Label after shrinkage 20:Product 20a: 1st flake 21: Jig 22: Load cell 100: (First before shrinkage) Polyester film 100a: Polyester film after shrinkage 120: Adhesive part 200: 2nd polyester film

Claims

1. A polyester film comprising a copolymerized polyester resin in which a diol and a dicarboxylic acid are copolymerized, The diols include ethylene glycol, neopentyl glycol, and diethylene glycol; The dicarboxylic acid includes terephthalic acid, The diol contains 50 mol % to 90 mol % of the ethylene glycol, 5 mol % to 35 mol % of the neopentyl glycol, and 1 mol % to 10 mol % of the diethylene glycol based on the total number of moles of the diol; The crystallization temperature (Tc) peak measured by a differential scanning calorimetry is not observed or the crystallization temperature (Tc) is 90°C to 130°C; A polyester film having a clumping ratio of 8% or less when flakes obtained by crushing a polyethylene terephthalate (PET) container having the polyester film thereon are heat-treated at a temperature of 210° C. for 90 minutes.

2. 2. The polyester film according to claim 1, wherein the crystallization temperature (Tc) measured by the differential scanning calorimeter is 96° C. to 120° C., and the melting point (Tm) measured by the differential scanning calorimeter is 170° C. or higher.

3. 2. The polyester film according to claim 1, wherein the clumping fraction is 5% or less.

4. 2. The polyester film according to claim 1, wherein the heat of crystallization measured at the crystallization temperature (Tc) is 0.01 J / g to 50 J / g.

5. The polyester film according to claim 1, which has a heat shrinkage rate of 30% or more in a first direction when heat-treated at a temperature of 80° C. for 10 seconds.

6. A step of preparing a copolymerized polyester resin in which a diol and a dicarboxylic acid are copolymerized; melt-extruding the copolymer polyester resin at a temperature of 250°C to 300°C to prepare an unstretched sheet; and preheating the unstretched sheet at a temperature of 90° C. to 120° C. for 0.01 to 1 minute, stretching the sheet at a temperature of 83° C. to 96° C., and then heat-setting the sheet at a temperature of 69° C. to 81° C. for 0.05 to 0.5 minutes to prepare a polyester film. The diols include ethylene glycol, neopentyl glycol, and diethylene glycol; The dicarboxylic acid includes terephthalic acid, The diol contains 50 mol % to 90 mol % of the ethylene glycol, 5 mol % to 35 mol % of the neopentyl glycol, and 1 mol % to 10 mol % of the diethylene glycol based on the total number of moles of the diol; When the polyester film is measured by a differential scanning calorimeter, no peak is observed in the crystallization temperature (Tc) or the crystallization temperature (Tc) is 90° C. to 130° C.; The method for producing a polyester film, wherein when flakes obtained by crushing a polyethylene terephthalate container provided with the polyester film are heat-treated at a temperature of 210° C. for 90 minutes, the clumping fraction is 8% or less.

7. Providing a polyethylene terephthalate container provided with the polyester film of claim 1; crushing the polyethylene terephthalate container provided with the film to obtain flakes; and heat treating the flakes to produce recycled polyester chips. When the flakes are heat-treated at a temperature of 210° C. for 90 minutes, the clumping fraction is 8% or less; The method for recycling polyethylene terephthalate containers, wherein the flakes include first flakes obtained by pulverizing the polyethylene terephthalate container and second flakes obtained by pulverizing the polyester film.

Citation Information

Patent Citations

  • Shrink film and preparation method thereof

    CN108908922A

  • Heat-shrinkable polyester film and label

    JP2002361741A

  • Heat-shrinkable polyester film

    JP2011184690A

  • Copolymerized polyester heat shrinkable film

    JP2013510919A

  • Polyester heat shrinkable film

    JP2017526557A