Lithium extraction method by extraction-stripping separation and purification

The extraction-reverse extraction separation and purification method using a composite extractant and industrial exhaust gases efficiently separates lithium from impurities, enhancing yield and purity while reducing costs and environmental impact.

JP7596374B2Active Publication Date: 2024-12-09INSTITUTE OF PROCESS ENGINEERING CHINESE ACADEMY OF SCIENCES +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2022525618
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-11-01
Filing Date
2020-10-29
Publication Date
2024-12-09
Estimated Expiration
2040-10-29

AI Technical Summary

Technical Problem

Existing lithium extraction methods suffer from low yield, high impurity levels, high water consumption, and complex processes, making them inefficient and costly for industrial applications.

Method used

A method involving extraction-reverse extraction separation and purification using a composite extractant under high pH conditions, combined with gas-liquid-liquid three-phase back extraction, utilizing industrial exhaust gases to achieve efficient lithium extraction and separation from impurities, with a multi-stage continuous countercurrent process.

Benefits of technology

The method achieves a lithium yield of over 83% with a purity of over 96%, reduces costs, and minimizes environmental impact by recycling liquids and gases, while simplifying the process flow and equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007596374000002
    Figure 0007596374000002
  • Figure 0007596374000003
    Figure 0007596374000003
  • Figure 0007596374000001
    Figure 0007596374000001
Patent Text Reader

Abstract

The present invention relates to a method for extracting lithium by extraction-stripping separation and purification. The method comprises the following steps: (1) using an extraction system containing a composite extractant to extract and separate a lithium-containing solution under conditions of pH 10-13 to obtain a lithium-loaded organic phase; (2) subjecting the lithium-loaded organic phase obtained in step (1) to gas-liquid-liquid three-phase stripping to obtain a lithium-loaded stripped solution; and (3) heat-treating and separating the stripped solution obtained in step (2) to obtain a mother liquor separated from the lithium product. The extraction-stripping separation and purification method provided by the present invention uses a composite extractant to efficiently separate lithium from impurity ions such as Na, K, and B. Furthermore, by using gas-liquid-liquid three-phase continuous stripping, the lithium stripping rate is over 90%, the total yield is over 83%, and the purity of the obtained lithium product is over 96%. This method has the advantages of large throughput, simple process and equipment, low investment, effective utilization of industrial exhaust gas, energy conservation, environmental protection, and continuous production.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims priority to a Chinese patent application bearing application number 201911061643.6, filed with the China Patent Office on November 1, 2019, for "Method for extracting lithium by extraction-stripping separation and purification," the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to the technical field of separation in the chemical industry, and more particularly to a method for extracting lithium by extraction-stripping separation and purification. [Background technology]

[0003] Lithium is the metal with the smallest density and is widely used in electronics, chemistry, new energy, pharmaceuticals, etc. Lithium resources are mainly supplied from salt lakes, minerals, and seawater. With the recent development of waste resource recycling, waste lithium batteries have also become an important supply source. The process of extracting lithium from these raw materials requires multiple purification steps. A typical process often involves evaporation and concentration, separation and removal of impurities, and deep removal of calcium ions and magnesium ions to obtain a high-purity lithium-containing solution, which is then precipitated to obtain lithium carbonate products.

[0004] CN108423696A discloses a method for extracting high-purity lithium salt from a lithium-containing solution, which includes the steps of: adding a pH value adjuster to the lithium-containing solution to adjust the pH value of the solution to be greater than 4; concentrating the lithium-containing solution into a lithium-rich solution with a lithium concentration of more than 2g / L; inserting an ultrasonic device into the lithium-rich solution, adding a precipitant, and subjecting it to ultrasonic vibration; filtering after ultrasonic treatment, and washing and drying the resulting solid phase to obtain a lithium salt. The method requires concentrating the lithium-containing solution and has a small processing capacity; at the same time, in the process of precipitating lithium, the lithium-rich solution contains a large amount of ions such as sodium and potassium, which results in a large amount of entrainment into the lithium salt, which affects its purity, and a large amount of fresh water washing is required to produce a lithium salt with a higher purity, resulting in a large amount of water consumption. In addition, since the lithium salt has a certain solubility in the aqueous phase, the mother liquor after precipitation still contains a large amount of lithium, which reduces the yield of lithium.

[0005] CN104884648A provides a method for extracting lithium from a lithium-containing solution, which includes the steps of: preparing a lithium-containing solution containing carbonate ions; concentrating the lithium-containing solution to a lithium concentration of 2.481 g / L or less to obtain a first precipitate; performing solid-liquid separation on the concentrated lithium-containing solution and the first precipitate; adding a phosphorus supplying material to the concentrated lithium-containing solution to precipitate the dissolved lithium as lithium phosphate; concentrating the precipitated lithium phosphate filtrate again to a lithium concentration of 2.481 g / L or less to obtain a second precipitate; performing solid-liquid separation on the reconcentrated filtrate and the second precipitate; and adding core particles to the reconcentrated filtrate to precipitate the dissolved lithium as lithium phosphate. This method requires multiple concentration and solid-liquid separation, which results in low lithium yield, long process flow, and large investment, making it unfavorable for industrial application.

[0006] From the above literature, it can be seen that a process with high lithium yield, high purity of lithium product, large processing capacity, short process, low investment and easy industrial production is currently an urgent problem to be solved. Summary of the Invention [Problem to be solved by the invention]

[0007] In view of the problems existing in the prior art, the present invention provides a method for extracting lithium by extraction-stripping separation and purification, which uses an extraction system containing a composite extractant to extract a lithium-containing solution under high pH conditions, thereby realizing efficient extraction of lithium and separation of many impurity elements such as Na, K, B, etc.; and uses industrial exhaust gas to carry out gas-liquid-liquid three-phase stripping through a multi-stage continuous countercurrent process to realize highly efficient stripping of lithium. The method provided by the present invention has a large processing capacity, a high total yield of lithium, and recycling of the liquid phase; the use of gas phase recycling achieves zero emissions and a high utilization rate; the use of industrial exhaust gas as the gas source for three-phase stripping can greatly reduce costs and protect the environment; and at the same time, the process flow is short, the equipment is simple, the investment is low, and it is easy to apply to industrial production. [Means for solving the problem]

[0008] To achieve this goal, the present invention uses the following technical solutions: The present invention provides a method for extracting lithium by extraction-stripping separation and purification, (1) using an extraction system containing a composite extractant to extract and separate a lithium-containing solution under a condition of pH=10-13 to obtain a lithium-loaded organic phase; Step (2) of subjecting the lithium-loaded organic phase obtained in step (1) to gas-liquid-liquid three-phase stripping to obtain a lithium-loaded stripped liquid; The method includes a step (3) of heat-treating and separating the stripped liquid obtained in the step (2) to obtain a lithium product and a mother liquor separated therefrom.

[0009] Preferably, the hybrid extractant in step (1) comprises a neutral extractant and a chelating extractant, and the extraction system comprises the hybrid extractant and a diluent.

[0010] Preferably, the neutral extractant comprises any one or a combination of at least two of the following: tributyl phosphate TBP, dimethylheptyl methyl phosphate P350, trioctyl phosphine oxide TOPO, trioctyl / hexyl phosphine oxide Cyanex 923, and N,N-di(1-methylheptyl)acetamide N503.

[0011] Preferably, the chelating extractant comprises any one or a combination of at least two of the extractants having the same functional group, namely 2-hydroxy-5-nonylacetophenone oxime LIX84, dodecylphenyl-methyl-β-diketone LIX54, 2-hydroxy-5-nonylbenzaldehyde oxime LIX860 and 2-hydroxy-5-nonylacetophenone oxime LIX84, dodecylphenyl-methyl-β-diketone LIX54, 2-hydroxy-5-nonylbenzaldehyde oxime LIX860.

[0012] Preferably, the volume ratio of the neutral extractant to the chelating extractant is 0.2:1 to 2:1.

[0013] Preferably, the extraction system further comprises a phase modifier.

[0014] Preferably, the extraction system includes a composite extractant, a phase modifier and a diluent; the volume fraction of the composite extractant in the extraction system is 5-30%, and the volume fraction of the phase modifier is 0-10%.

[0015] Preferably, the lithium-containing solution in step (1) comprises any one or a combination of at least two of lithium ore leachate, lithium precipitation mother liquor, lithium battery waste leachate, and salt lake brine.

[0016] Preferably, the lithium concentration in the lithium-containing solution is 0.25 to 5 g / L.

[0017] Preferably, the concentrations of the main impurity elements sodium, potassium and boron in the lithium-containing solution are independently 10 to 150 g / L, 0 to 50 g / L and 0 to 10 g / L, respectively.

[0018] Preferably, the lithium-containing solution further comprises metal ions such as rubidium, aluminum, magnesium, cesium and calcium.

[0019] Preferably, the volume ratio of the lithium-containing solution to the organic phase of the extraction system is 0.2:1 to 5:1.

[0020] Preferably, in step (1), the lithium concentration in the lithium-loaded organic phase is 0.5 to 3 g / L.

[0021] Preferably, step (1) further comprises washing the lithium-loaded organic phase.

[0022] Preferably, the cleaning liquid is water and / or a lithium containing solution.

[0023] Preferably, the gas-liquid-liquid three-phase back-extraction system in step (2) comprises a first liquid phase, a second liquid phase, and a gas phase.

[0024] Preferably, the gas in the gas phase comprises any one or a combination of at least two of SO2, SO3, CO2, or Cl2.

[0025] Preferably, the gas in the gas phase is SO2 and / or CO2.

[0026] Preferably, the first liquid phase comprises water.

[0027] Preferably, the second liquid phase comprises a lithium-loaded organic phase.

[0028] Preferably, the gas-liquid-liquid three-phase stripping is controlled to pH=6-9.

[0029] Preferably, the volume ratio of the first liquid phase to the second liquid phase is from 0.05:1 to 2:1.

[0030] Preferably, the gas-liquid-liquid three-phase stripping in step (2) uses a multi-stage continuous countercurrent operation.

[0031] Preferably, the gas-liquid-liquid three-phase stripping device includes any one of a continuous mixing settling tank, an extraction tower, or a centrifugal extractor; the number of stages of the gas-liquid-liquid three-phase stripping is adjustable between 1 and 10.

[0032] Preferably, the concentration of lithium in the stripping solution in step (2) is >5g / L.

[0033] Preferably, the heat treatment method in step (3) includes any one or a combination of at least two of oxidation, evaporative crystallization, or pyrolysis.

[0034] Preferably, the heat treatment temperature is 60 to 90°C.

[0035] Preferably, the heat treatment time is 0.5 to 2 hours.

[0036] Preferably, the oxidizing agent used in the oxidation is air, oxygen, and ozone gas.

[0037] Preferably, the evaporative crystallization uses MVR or multiple effect evaporation.

[0038] Preferably, the pyrolysis uses a closed or semi-closed vessel.

[0039] Preferably, the method of separating in step (3) comprises any one of filtration, suction filtration or centrifugation, or a combination of at least two of them.

[0040] Preferably, the lithium product is lithium sulfate, lithium chloride, or lithium carbonate, and the product purity is >96%.

[0041] Preferably, the mother liquor after separation in step (3) is returned to the first liquid phase in step (1) and / or step (2). Effect of the Invention

[0042] Compared with the prior art, the beneficial effects of the present invention are: (1) The method for extracting lithium by extraction-stripping separation and purification provided by the present invention uses a composite extractant to effectively separate lithium from impurity ions such as Na, K, B, etc., and achieves the lithium stripping rate of more than 90% through continuous gas-liquid-liquid three-phase stripping, thereby realizing the recycling of liquid and gas phases, with a total lithium yield of more than 83%, and the purity of the obtained lithium product being more than 96%; (2) The method provided by the present invention has a large throughput, simple process and equipment, low investment, low energy consumption, and can realize continuous production, and has relatively high application value. [Brief description of the drawings]

[0043] [Figure 1] FIG. 1 is a process flow diagram of lithium extraction by extraction-stripping separation and purification provided by the present invention. [Diagram 2] 2 is a schematic diagram of a gas-liquid-liquid three-phase extraction device provided by the present invention. In Fig. 2, 1 is an electric stirrer, 2 is a gas outlet, 3 is a light phase outlet, 4 is a stirring tower plate, 5 is the tower body of the extraction tower, 6 is a gas distributor, 7 is a gas inlet, 8 is a heavy phase outlet, 9 is a heavy phase inlet, 10 is a light phase inlet, and 11 is a pulse system. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0044] The present invention provides a method for extracting lithium by extraction-stripping separation and purification. (1) extracting and separating the lithium-containing solution using an extraction system containing a composite extractant under a condition of pH=10-13 to obtain a lithium-loaded organic phase; (2) subjecting the lithium-loaded organic phase obtained in step (1) to gas-liquid-liquid three-phase stripping to obtain a stripped liquid loaded with lithium; The method includes a step (3) of heat-treating and separating the stripped liquid obtained in the step (2) to obtain a lithium product and a mother liquor separated therefrom.

[0045] In the method provided by the present invention, an extraction system containing a composite extractant is used, and under the condition of a relatively high pH value, lithium is effectively extracted by the composite extractant and enters the loaded organic phase; then, the lithium-loaded organic phase is subjected to gas-liquid-liquid three-phase back extraction, using an acid gas as the gas phase, and the gas is dissolved in the liquid phase to produce a small amount of H + Provided, H + contacts with the lithium-loaded organic phase, and Li + In exchange for Li + is back-extracted into the aqueous solution, and the consumed H + is replenished by continuous gas reactions, and Li is back-extracted into the aqueous phase. + The lithium-ionized cation combines with the anions produced by the gas-liquid reaction to form a supported aqueous solution of lithium; a purer lithium product is then obtained by thermal treatment.

[0046] Preferably, in step (1), the composite extractant comprises a neutral extractant and a chelating extractant, and the extraction system comprises the composite extractant and a diluent. Under the condition of pH=10-13, lithium and the impurities of the neutral extractant are extracted by the chelating extractant, thereby realizing efficient extraction of lithium. The extraction reaction is shown in the following formula (1):

[0047] Li n L+nE N +nHE Ch+nOH - =nLi·E N E Ch +L n- +nH2O(1)

[0048] In formula (1), L is Cl - or SO4 2- and E N is a neutral extractant, and HE Ch is a chelating extractant.

[0049] Na, K and B plasmas are E N Since it does not form any impurities with Li, it is not extracted by the composite extractant, and Li is well separated from impurity elements such as Na, K and B.

[0050] In the present invention, the extraction process is carried out under strong alkaline conditions, pH=10-13, for example, it may be 10, 11, 12 or 13, etc. When pH<10, the extraction process can separate impurities formed by lithium and HE. Ch H generated by + cannot be effectively neutralized and lithium cannot be effectively extracted. When pH>13, large amounts of Na + and K. + HE Ch and NaE Ch or K.E. Ch , where lithium is not efficiently extracted and is not well separated from Na and K.

[0051] Preferably, the neutral extractant comprises any one or a combination of at least two of tributyl phosphate (TBP), dimethylheptyl methyl phosphate (P350), trioctyl phosphine oxide (TOPO), trioctyl / hexyl phosphine oxide (Cyanex 923), and N,N-di-(1-methylheptyl)acetamide (N503), among which typical but non-limiting combinations are P350 and N503, TBP and TOPO, TBP, P350 and Cyanex 923, P350, Cyanex 923 and N503.

[0052] Preferably, the chelating extractant comprises any one or at least two combinations of extractants having the same functional group, namely 2-hydroxy-5-nonylacetophenone oxime (LIX84), dodecylphenyl-methyl-β-diketone (LIX54), 2-hydroxy-5-nonylbenzaldehyde oxime (LIX860) and 2-hydroxy-5-nonylacetophenone oxime (LIX84), dodecylphenyl-methyl-β-diketone (LIX54), 2-hydroxy-5-nonylbenzaldehyde oxime (LIX860), among which typical but non-limiting combinations are LIX54 and LIX84I, LIX54 and LIX860, LIX54, LIX84I and LIX860.

[0053] Preferably, the volume ratio of the neutral extractant to the chelating extractant is 0.2:1 to 2:1, for example, 0.2:1, 0.3:1, 0.5:1, 0.8:1, 1:1, 1.2:1, 1.5:1, 1.8:1 or 2:1.

[0054] Preferably, the extraction system further comprises a phase modifier.

[0055] Preferably, the extraction system includes a composite extractant, a phase modifier and a diluent, where the volume fractions of the composite extractant and the phase modifier are independently 5-30% and 0-10%, respectively. For example, the volume fraction of the composite extractant can be 5%, 10%, 15%, 20%, 25%, or 30%, etc.; the volume fraction of the phase modifier can be 0%, 0.5%, 1%, 3%, 5%, 8%, 9%, or 10%, etc., and the phase modifier is added or not and the volume ratio of addition is determined according to whether the "emulsion" problem occurs in the extraction system.

[0056] In the present invention, the specific type of diluent and phase modifier is not particularly limited, and any type commonly used by those skilled in the art is applicable to the present invention. In a specific embodiment of the present invention, the diluent is n-dodecane or sulfonated kerosene, and the phase modifier is dodecanol.

[0057] Preferably, the lithium-containing solution in step (1) comprises any one or a combination of at least two of lithium ore leachate, precipitated lithium mother liquor, lithium battery waste leachate and salt lake brine, where typical but non-limiting combinations are: lithium ore leachate and lithium precipitation mother liquor, salt lake brine, salt lake brine and lithium precipitation mother liquor, lithium battery waste leachate, lithium battery waste leachate and lithium precipitation mother liquor, etc.

[0058] Preferably, the concentration of lithium in the lithium-containing solution is 0.25 to 5 g / L, and may be, for example, 0.25 g / L, 0.3 g / L, 0.5 g / L, 0.8 g / L, 1 g / L, 1.5 g / L, 2 g / L, 2.5 g / L, 3 g / L, 3.5 g / L, 4 g / L, 4.5 g / L, 4.8 g / L, or 5 g / L.

[0059] Preferably, the concentrations of sodium, potassium and boron, which are the main impurity elements in the lithium-containing solution, are independently 10 to 150 g / L, 0 to 50 g / L and 0 to 10 g / L, respectively. For example, the sodium concentration is 10 g / L, 15 g / L, 20 g / L, 30 g / L, 50 g / L, 80 g / L, 90 g / L, 95 g / L, 100 g / L, 120 g / L, 1 the concentration of potassium can be 0 g / L, 1 g / L, 5 g / L, 10 g / L, 15 g / L, 20 g / L, 30 g / L, 40 g / L, 45 g / L or 50 g / L, etc.; the concentration of boron can be 0 g / L, 1 g / L, 2 g / L, 3 g / L, 5 g / L, 7 g / L, 9 g / L, or 10 g / L / L, etc.

[0060] Preferably, the lithium-containing solution further comprises metal ions such as rubidium, aluminum, magnesium, cesium and calcium.

[0061] Preferably, the volume ratio of the lithium-containing solution to the organic phase is 0.2:1 to 5:1, such as 0.2:1, 0.3:1, 0.5:1, 0.8:1, 1:1, 1.2:1, 1.5:1, 1.8:1, 2:1, 2.5:1, 3:1, 4:1 or 5:1. If the volume ratio is less than 0.2:1, lithium cannot be effectively extracted and Li cannot be sufficiently separated from Na and K; if the volume ratio is more than 5:1, the effect of single-stage extraction of lithium is reduced and the extraction yield of lithium is reduced.

[0062] Preferably, the lithium concentration in the lithium-loaded organic phase described in step (1) may be 0.5 to 3 g / L, for example, 0.5 g / L, 0.8 g / L, 1 g / L, 1.2 g / L, 1.5 g / L, 1.8 g / L, 2 g / L, 2.2 g / L, 2.6 g / L, 2.8 g / L, or 3 g / L.

[0063] Preferably, the lithium-loaded organic phase is washed. Although Na, K, B, etc. are not extracted in the organic extraction system, the extraction process causes phase entrainment, and small amounts of impurities such as Na, K, and B enter the loaded organic phase with the entrained water, so it is necessary to wash the impurities into the aqueous phase and further purify the lithium.

[0064] Preferably, the cleaning liquid is water and / or a lithium containing solution.

[0065] Preferably, the gas-liquid-liquid three-phase back-extraction system in step (2) comprises a first liquid phase, a second liquid phase, and a gas phase.

[0066] Preferably, the gas in the gas phase comprises any one of SO2, SO3, CO2 or Cl2, or a combination of at least two of them, preferably SO2 and / or CO2.

[0067] In the gas used for stripping in the present invention, SO2 and SO3 are mainly exhaust gases produced by high-temperature treatment of sulfide ores in metallurgical processes, and are used in industry to prepare sulfuric acid by-products. SO2 is oxidized and converted to SO3 using a catalyst, and then absorbed to prepare sulfuric acid, which makes the process complicated and the preparation cost high. CO2 is mainly exhaust gases from power plants and high-temperature boilers, and a large amount of CO2 exhaust is also generated in the lime combustion step, but it is currently discharged after purification treatment, which generates greenhouse gases. Cl2 is a by-product of the chlorine-alkali industry, and is currently used in the production of hydrochloric acid, disinfectants, and chlorine-based plastics industries, but there is a large excess of Cl2 by-products in China. The present invention uses industrially produced exhaust gases or greenhouse gases emitted to realize highly efficient stripping of lithium, greatly reducing the implementation cost and reducing environmental pollution at the same time.

[0068] Preferably, the first liquid phase comprises water.

[0069] Preferably, the second liquid phase comprises a lithium-loaded organic phase.

[0070] In the present invention, the gas used for stripping dissolves in the first liquid phase and releases a small amount of H + Provided, H + contacts the lithium-loaded organic phase, and Li + In exchange for Li + is back-extracted into the aqueous solution, and the consumed H + is replenished by continuous gas reactions, and Li is back-extracted into the aqueous phase. + The lithium-loaded aqueous solution is formed by combining with the anions produced by the gas-liquid reaction. The lithium stripping is shown in the following equation (2).

[0071] nLi·E N E Ch +G+1 / 2nH2O=Li n G(O) 1 / 2n +nE N +nHE Ch (2)

[0072] In equation (2), G is the gas used for stripping.

[0073] Preferably, the gas-liquid-liquid three-phase stripping is controlled to pH=6-9, for example, 6, 7, 8 or 9. Lithium stripping is achieved by a gas-liquid-liquid continuous three-phase reaction, and Li n G(O) 1 / 2n is generated, the pH is neutral or close to alkaline, and the back-extraction process system is automatically maintained at a pH between 6 and 9, which is close to neutral or alkaline, and there is no need to add other reagents for pH adjustment.

[0074] Preferably, the volume ratio of the first liquid phase to the second liquid phase is 0.05:1 to 2:1, for example, 0.05:1, 0.1:1, 0.5:1, 1:1, 1.5:1, 2:1, etc. When the volume ratio is less than 0.05:1, the lithium stripping effect is low; when the volume ratio is more than 2:1, the lithium concentration in the stripping aqueous solution is low, and the lithium recovery rate is low.

[0075] Preferably, the gas-liquid-liquid three-phase stripping in step (2) uses a multi-stage continuous countercurrent operation.

[0076] Preferably, the device used for the gas-liquid-liquid three-phase stripping includes a continuous mixing settling tank, an extraction tower, or a centrifugal extractor, and the number of stages of the gas-liquid-liquid three-phase stripping can be adjusted between 1 and 10. The gas-liquid-liquid three-phase stripping device is more preferably an extraction tower, and the size and number of stages of the extraction tower can be adjusted according to the needs of the actual production process.

[0077] In the present invention, the gas-liquid-liquid three-phase stripping apparatus can achieve a lithium stripping rate of more than 90% by adjusting the number of apparatuses and / or process parameters.

[0078] Preferably, the lithium concentration in the stripping solution described in step (2) is >5 g / L, and may be, for example, 5.1 g / L, 5.2 g / L, 5.5 g / L, 5.8 g / L, 6.0 g / L, 6.5 g / L, 7.0 g / L, 9.0 g / L or 10 g / L.

[0079] Preferably, the heat treatment method in step (3) includes any one or a combination of at least two of oxidation, evaporative crystallization, and pyrolysis, among which typical but non-limiting combinations are pyrolysis and evaporative crystallization, and oxidation and evaporative crystallization.

[0080] Preferably, the heat treatment temperature described in step (3) is 60-90°C, such as 60°C, 65°C, 70°C, 75°C, 80°C, 85°C or 90°C, etc., when the temperature is lower than 60°C, the yield of lithium products will be low, and when the temperature is higher than 90°C, the energy consumption of the heat treatment section will be increased.

[0081] Preferably, the heat treatment time is 0.5 to 2 hours, and may be, for example, 0.5 hours, 1 hour, 1.5 hours, or 2 hours.

[0082] In the present invention, the heat treatment is adjusted according to the type of gas used in the stripping. When SO2 gas is used for stripping, Li2SO3 solution is obtained, Li2SO4 is formed after heating and oxidation, and then evaporated and crystallized by heating to obtain Li2SO4 product; when SO3 is used for stripping, Li2SO4 is obtained, and Li2SO4 product is obtained by direct evaporation and crystallization; when CO2 gas is used for stripping, Li2CO3 product is obtained by heating; when Cl2 is used for stripping, LiCl product is obtained.

[0083] Preferably, the oxidizing agent used in the oxidation is air, oxygen, and ozone gas.

[0084] Preferably, the evaporative crystallization uses MVR or multiple effect evaporation.

[0085] Preferably, a closed or semi-closed vessel is used for the pyrolysis.

[0086] Preferably, the separation method includes any one of filtration, vacuum filtration, and centrifugation, or a combination of at least two of them, among which typical but non-limiting combinations are centrifugation and filtration, and centrifugation and vacuum filtration.

[0087] Preferably, the lithium product is lithium sulphate, lithium chloride or lithium carbonate and the product purity is >96%, such as 96.5%, 97%, 98% or 99%.

[0088] Preferably, the mother liquor after separation in step (3) is returned to the lithium-containing solution in step (1) and / or returned to the first liquid phase in step (2) to improve the overall yield of lithium and achieve zero discharge of wastewater.

[0089] Preferably, the method provided by the present invention comprises the following steps:

[0090] (1) Mix the neutral extractant and the chelating extractant to form a composite extractant, and control the volume ratio of the neutral extractant and the chelating extractant to be 0.2:1-2:1. Then add and mix a diluent and a phase modifier to form an extraction system, and control the volume fractions of the composite extractant and the phase modifier to be 5-30% and 0-10% respectively independently. Under the condition of pH=10-13, extract with a solution with a lithium concentration of 0.25-5g / L, and control the volume ratio of the lithium-containing solution to the organic phase to be 0.2:1-5:1, and then separate to obtain a lithium-loaded organic phase with a lithium concentration of 0.5-3g / L; The neutral extractant includes any one or a combination of at least two of tributyl phosphate (TBP), dimethylheptyl methyl phosphate (P350), trioctyl phosphine oxide (TOPO), trioctyl / hexyl phosphine oxide (Cyanex 923), and N,N-di(1-methylheptyl)acetamide (N503); The chelating extractant includes any one or a combination of at least two of the extractants having the same functional group, namely 2-hydroxy-5-nonylacetophenone oxime (LIX84), dodecylphenyl-methyl-β-diketone (LIX54), 2-hydroxy-5-nonylbenzaldehyde oxime (LIX860) and 2-hydroxy-5-nonylacetophenone oxime (LIX84), dodecylphenyl-methyl-β-diketone (LIX54), 2-hydroxy-5-nonylbenzaldehyde oxime (LIX860); (2) The lithium-loaded organic phase obtained in step (1) is washed, and then subjected to gas-liquid-liquid three-phase back extraction in a continuous countercurrent extraction column, and the back extraction system is controlled at pH=6-9 to obtain a back-extracted solution with a lithium concentration of >5g / L; The gas in the gas-liquid-liquid three-phase stripping system comprises any one or a combination of at least two of SO2, SO3, CO2, or Cl2; (3) The stripped liquid obtained in step (2) is separated by heat treatment at 60-90°C for 0.5-2 hours to obtain the lithium product and the mother liquor.

[0091] The technical solution of the present invention is further described below through specific embodiments with reference to the drawings. Those skilled in the art should understand that the embodiments are only for helping to understand the present invention, and should not be regarded as specific limitations of the present invention.

[0092] The process flow of lithium extraction by extraction-stripping separation and purification provided by the present invention is as shown in Figure 1. In this process, lithium is extracted from a lithium-containing solution under conditions of pH = 10-13, the extract is then washed to remove impurities such as Na, K and B, and the extract is continuously stripped by gas-liquid-liquid three-phase to obtain lithium stripped solution, which is then subjected to heat treatment and separation to obtain lithium products. The separated mother liquor is recycled back to the Li extraction step according to cycle method 1 and / or back to the Li stripping step according to cycle 2 for recycling.

[0093] The schematic diagram of the gas-liquid-liquid three-phase stripping device provided by the present invention is as shown in FIG. 2. This is an extraction tower, in which the gas phase enters the extraction tower through the gas inlet 7 at the bottom of the tower, enters the tower body 5 of the extraction tower through the gas distributor 6, and reacts with the liquid, and the unreacted gas is discharged from the gas outlet 2 at the top of the tower; the first liquid phase enters the extraction tower through the light phase inlet 10 at the bottom of the tower and is stripped by the tower body, and the stripped liquid containing lithium is discharged from the light phase outlet 3; the second liquid phase enters the tower through the heavy phase inlet 9 at the top of the tower, stripping occurs, and the reacted solution is discharged through the heavy phase outlet 8. According to the actual production needs, the plate of the tower body is adjusted to realize the adjustment of the number of stages. The electric agitator 1 and the stirring tower plate 4 make the gas-liquid-liquid three phases fully contact, and the pulse system 11 supplies power to the counterflow of the first liquid phase.

[0094] Example 1 This embodiment provides a method for extracting lithium by extraction-stripping separation and purification, which includes the following steps: (1) Mix TBP and LIX84 to form a composite extractant, control the volume ratio of TBP to LIX84 at 0.2:1, use sulfonated kerosene as a diluent, the volume fraction of the composite extractant is 20%, and add 5% volume fraction of dodecanol as a phase adjuster. Under the condition of pH=10, extract the solution obtained by purifying high valent metal ions from the leachate of lithium battery waste with a lithium concentration of 0.5g / L and a sodium concentration of 10g / L, control the volume ratio of the solution obtained by purifying high valent metal ions from the leachate of lithium battery waste to the organic phase at 2.2:1, and then separate to obtain the loaded organic phase with a lithium concentration of 1g / L; (2) The loaded organic phase obtained in step (1) is washed with water three times, and then gas-liquid-liquid three-phase stripping is carried out in a continuous countercurrent extraction tower, the number of stages of the extraction tower is three, CO2 is used as the gas phase, water is the first liquid phase of stripping, the volume ratio of water to the loaded organic phase is controlled at 0.15:1, and the pH of the stripping system is controlled at 8, and the stripped liquid has a lithium concentration of 6.5g / L; (3) The stripped liquor obtained in step (2) is heat-treated at 60°C for 2 hours and suction-filtered to obtain lithium carbonate product, and the mother liquor after precipitation of lithium carbonate is returned to the stripping segment of step (2).

[0095] Example 2 This embodiment provides a method for extracting lithium by extraction-stripping separation and purification, which includes the following steps: (1) Mix TOPO and LIX860 to form a composite extractant, control the volume ratio of TOPO and LIX860 to 1:1, take n-dodecane as diluent, the volume fraction of the composite extractant is 25%, and extract the precipitated lithium mother liquor with lithium concentration of 2g / L, sodium concentration of 50g / L, potassium concentration of 25g / L, and boron concentration of 10g / L under the condition of pH=12, control the volume ratio of the precipitated lithium mother liquor to the organic phase to 1:1, and then separate to obtain the loaded organic phase with lithium concentration of 2g / L; (2) The loaded organic phase obtained in step (1) is washed with water three times, and then gas-liquid-liquid three-phase stripping is carried out in a continuous countercurrent extraction tower, the number of stages of the extraction tower is three, SO2 is used as the gas phase, water is the stripping liquid phase, the volume ratio of water to the loaded organic phase is 0.1:1, and the pH of the stripping system is controlled at 6. The stripping liquid has a lithium concentration of 19.5g / L; (3) The stripped solution obtained in step (2) is oxidized with air at 80°C for 1 hour, and then the MVR is evaporated to obtain the lithium sulfate product.

[0096] Example 3 This embodiment provides a method for extracting lithium by extraction-stripping separation and purification, which includes the following steps: (1) Mix Cyanex923 and LIX54 to form a composite extractant, control the volume ratio of Cyanex923 and LIX54 at 2:1, take sulfonated kerosene as diluent, the volume fraction of the composite extractant is 15%, and extract salt lake brine concentrate with lithium concentration of 5g / L, sodium concentration of 100g / L, potassium concentration of 50g / L and boron concentration of 5g / L under the condition of pH=13, control the volume ratio of salt lake brine concentrate to organic phase at 0.2:1, and then separate to obtain the loaded organic phase with lithium concentration of 2.4g / L; (2) The loaded organic phase obtained in step (1) is washed with water four times, and then gas-liquid-liquid three-phase stripping is carried out in a continuous countercurrent extraction tower, the number of stages of the extraction tower is three, CO2 is used as the gas phase, water is the first liquid phase of stripping, the volume ratio of water to the loaded organic phase is controlled at 0.25:1, and the pH of the stripping system is controlled at 9, and a stripped liquid with a lithium concentration of 9.3 g / L is obtained; (3) The stripped liquid obtained in step (2) is heat treated at 80°C for 0.5h and filtered to obtain the lithium carbonate product, and the mother liquor is returned to the extraction segment in step (1).

[0097] Example 4 Compared with Example 1, the only difference is that the solution obtained by purifying high valent metal ions from the leachate of lithium battery waste in step (1) is replaced with a mixed solution of lithium ore leachate and precipitated lithium mother liquor, in which the concentration of Li is 1.0 g / L, the concentration of Na is 20 g / L, and small amounts of other impurities are also contained; the volume ratio of the organic phase to the lithium-containing solution is increased to 1:1, and the lithium in the supported organic phase is 0.99 g / L.

[0098] Example 5 Compared with Example 1, the only difference is that the concentration of the solution obtained by purifying high valent metal ions from the leachate of lithium battery waste in step (1) is changed to 0.25 g / L, the volume ratio of the solution obtained by purifying high valent metal ions from the leachate of extracted lithium battery waste to the organic phase is changed to 5:1, and the lithium concentration in the loaded organic phase is 1.18 g / L.

[0099] Example 6 Compared with Example 1, the only difference is that the volume ratio of the solution obtained by purifying high valent metal ions from the leachate of lithium battery waste in step (1) to the organic phase is changed to 5:1, the pH is increased to 13, and the lithium concentration in the loaded organic phase is 2.48 g / L.

[0100] Example 7 Compared with Example 1, the only difference is that the volume ratio of water to the supported organic phase in step (2) is changed to 0.05:1.

[0101] Example 8 Compared with Example 1, the only difference is that the volume ratio of TBP and LIX84 in step (1) is changed to 2:1.

[0102] Example 9 Compared with Example 1, the only difference is that the volume ratio of the solution obtained by purifying high valent metal ions from the leachate of lithium battery waste in step (1) to the organic phase is changed to 5:1.

[0103] Example 10 Compared with Example 2, the only difference is that the volume ratio of water to the supported organic phase in step (2) is changed to 2:1.

[0104] Comparative Example 1 Compared with Example 1, the only difference is that the composite extractant formed by TBP and LIX84 in step (1) was replaced by single TBP or LIX84, and the extraction rate of Li was both less than 10%.

[0105] Comparative Example 2 Compared with Example 1, the only difference is that the gas in the gas-liquid-liquid three-phase stripping in step (2) is replaced with air, the pH after stripping is 11.2, and the stripping rate of Li is <20%.

[0106] Comparative Example 3 Compared to Example 1, the only difference is that the pH=10 in step (1) is changed to pH=9, resulting in a Li extraction rate of 35.3%, making it uneconomical for industrial implementation.

[0107] Comparative Example 4 Compared to Example 1, the only difference is that the pH in step (1) is changed from 10 to 14, resulting in a Li extraction rate of 75.5%. This is thought to be due to the competitive extraction of impurity elements Na and K, which reduces the Li extraction rate, and at the same time increases the pH value and alkali consumption, making it less economical for practical use.

[0108] Evaluation of lithium extraction by extraction-stripping separation and purification: The amounts of lithium extracted, stripped and the total yield of lithium in the methods of Examples 1 to 8 and Comparative Examples 1 to 4 were calculated and evaluated. The evaluation results are shown in Table 1.

[0109] Lithium extraction rate, back extraction rate and total lithium yield in Examples 1 to 8 and Comparative Examples 1 to 4 [Table 1]

[0110] In the present invention, the method for calculating the lithium single recovery rate is as follows.

[0111] R0=R l ×R2

[0112] Where, R0 - lithium single recovery rate, %; R1 - lithium single extraction rate, %; R2 - lithium single back extraction rate, %.

[0113] Through the analysis of the examples and comparative examples, it is found that the method provided by the present invention realizes efficient extraction and purification of lithium by using a composite extractant, the extraction rate of lithium is more than 92%, and through gas-liquid-liquid three-phase continuous stripping, the stripping rate of lithium is more than 90%, the total yield is more than 83%, and the purity of the obtained lithium product is more than 96%. This method has high efficiency and strong industrial applicability.

[0114] The applicant declares that the present invention is illustrated by the above-mentioned embodiments, but does not mean that the present invention is not limited to the above-mentioned features, i.e., the present invention must be relied upon to be implemented. Improvements of the present invention, equivalent replacements of the methods selected for the present invention, as well as the addition of auxiliary methods, selection of specific methods, etc., will be obvious to those skilled in the art and fall within the scope of protection and disclosure of the present invention.

Claims

1. A method for extracting lithium by extraction-stripping separation and purification, comprising the steps of: (1) using an extraction system containing a composite extractant to extract and separate a lithium-containing solution under a condition of pH=10-13 to obtain a lithium-loaded organic phase; Step (2) of subjecting the lithium-loaded organic phase obtained in step (1) to gas-liquid-liquid three-phase stripping to obtain a stripped solution loaded with lithium; The method includes a step (3) of heat-treating and separating the stripped liquid obtained in the step (2) to obtain a mother liquor separated from the lithium product, The method, wherein the gas-liquid-liquid three-phase back-extraction system in step (2) comprises a first liquid phase, a second liquid phase, and a gas phase.

2. 2. The method of claim 1, wherein the composite extractant in step (1) comprises a neutral extractant and a chelating extractant, and the extraction system comprises the composite extractant and a diluent.

3. The neutral extractant includes any one or a combination of at least two of tributyl phosphate TBP, dimethylheptyl methyl phosphate P350, trioctyl phosphine oxide TOPO, trioctyl / hexyl phosphine oxide Cyanex 923, and N,N-di(1-methylheptyl)acetamide N503; The chelating extractant includes any one or at least two combinations of extractants having the same functional group, namely 2-hydroxy-5-nonylacetophenone oxime (LIX84), dodecylphenyl-methyl-β-diketone (LIX54), 2-hydroxy-5-nonylbenzaldehyde oxime (LIX860) and 2-hydroxy-5-nonylacetophenone oxime (LIX84), dodecylphenyl-methyl-β-diketone (LIX54), 2-hydroxy-5-nonylbenzaldehyde oxime (LIX860); 3. The method according to claim 2, wherein the volume ratio of the neutral extractant to the chelating extractant is 0.2:1 to 2:

1.

4. The extraction system also includes dodecanol; 2. The method according to claim 1, wherein the extraction system comprises a composite extractant, dodecanol and a diluent; the volume fraction of the composite extractant in the extraction system is 5-30%, and the volume fraction of dodecanol is 0-10%.

5. The lithium-containing solution in step (1) includes any one or a combination of at least two of lithium ore leachate, precipitated lithium mother liquor, lithium battery waste leachate, and salt lake brine; The concentration of lithium in the lithium-containing solution is 0.25 to 5 g / L; the concentrations of the major impurity elements sodium, potassium and boron in the lithium-containing solution are independently 10-150 g / L, 0-50 g / L, and 0-10 g / L, respectively; The lithium-containing solution further includes metal ions such as rubidium, aluminum, magnesium, cesium, and calcium; the volume ratio of said lithium-containing solution to the organic phase of the extraction system is 0.2:1 to 5:1; 2. The method according to claim 1, wherein in step (1), the concentration of lithium in the lithium-loaded organic phase is 0.5 to 3 g / L.

6. Step (1) further includes washing the lithium-loaded organic phase; 2. The method according to claim 1, wherein the cleaning solution for cleaning is water and / or a lithium-containing solution.

7. the gas phase is an acid gas; The gas in the gas phase is SO 2 , S.O. 3 , CO 2 Or Cl 2 the lithium product is lithium sulfate, lithium chloride, or lithium carbonate, and the product purity is >96%; the first liquid phase comprises water; the second liquid phase comprises a lithium-loaded organic phase; The pH of the gas-liquid-liquid three-phase back extraction system is 6-9; 2. The method of claim 1, wherein the volume ratio of the first liquid phase to the second liquid phase is from 0.05:1 to 2:

1.

8. The gas-liquid-liquid three-phase stripping in step (2) uses a multi-stage continuous countercurrent operation; The gas-liquid-liquid three-phase stripping device includes any one of a continuous mixing settling tank, an extraction tower, or a centrifugal extractor; the number of stages of the gas-liquid-liquid three-phase stripping is adjustable between 1 and 10; 2. The method of claim 1, wherein the concentration of lithium in the stripping solution in step (2) is >5 g / L.

9. The heat treatment method in step (3) includes any one or a combination of at least two of oxidation, evaporative crystallization, or pyrolysis; The temperature of the heat treatment is 60 to 90° C.; The heat treatment time is 0.5 to 2 hours; 2. The method of claim 1, wherein the oxidizing agent used in the oxidation is air, oxygen, and ozone gas.

10. The evaporative crystallization uses MVR or multiple effect evaporation; The pyrolysis uses a closed or semi-closed vessel; 10. The method of claim 9, wherein the separating method in step (3) includes any one or a combination of at least two of filtration, suction filtration, or centrifugation.

Citation Information

Patent Citations

  • Technology for extracting lithium from lithium-containing alkaline brine based on mixer settlers

    CN107937734A

  • Lithium carbonate preparation method

    CN110240183A