Insulating resin composition for electric power cables, and electric power cable
The insulating resin composition for power cables, featuring unmodified polyolefin resin, unsaturated organic acids, and ethylene copolymers, addresses water tree defects and dielectric loss issues, ensuring efficient power transport in humid conditions by suppressing water tree growth and maintaining low dielectric loss tangent.
Patent Information
- Application Number
- PCT/JP2024/012598
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Power cables in humid environments suffer from water tree defects and increased dielectric loss tangent due to the use of hydrophilic molecules like polyethylene glycol, which lead to reduced power transport efficiency.
An insulating resin composition comprising unmodified polyolefin resin, unsaturated organic acids or their derivatives, and ethylene copolymers with carboxylic acid esters, which suppress water tree growth and dielectric loss tangent without excessive water uptake.
The composition effectively inhibits water tree growth and maintains low dielectric loss tangent even in high-moisture environments, enhancing power cable efficiency and reliability.
Smart Images

Figure JP2024012598_03102024_PF_FP_ABST
Abstract
Description
Insulating resin composition for power cables and power cables
[0001] The present disclosure relates to an insulating resin composition for power cables and a power cable.
[0002] The insulating resin of power cables laid in moist environments such as underground or undersea is prone to developing dendritic defects called water trees, which arise from foreign matter or air bubbles (voids) in the resin.
[0003] Water trees are generated and grow when the water in the cable insulation resin concentrates on the interface of foreign matter or voids due to dielectrophoresis of water caused by the flow of electricity through the power cable. Because water trees can cause destruction of power cables, there is a need to suppress the growth of water trees.
[0004] To prevent water tree growth, cross-linked polyethylene (XLPE) resins are sometimes made by adding hydrophilic molecules to hydrophobic polyethylene, such as polyethylene glycol, or polyethylene glycol derivatives in which the terminals of polyethylene glycol are modified with olefin or acrylic to enhance compatibility with XLPE. By introducing a hydrophilic molecular structure such as polyethylene glycol, water is dispersed uniformly in the XLPE resin, preventing water from concentrating on the interfaces of foreign objects and voids, thereby preventing the initiation and growth of water trees.
[0005] Patent Document 1 discloses a polyolefin composition for electrical insulation containing a polyolefin or cross-linked polyolefin and a small amount of high-molecular-weight polyethylene glycol. It also discloses a technology that a low-hydrophilic or hydrophobic material such as polypropylene glycol does not prevent the formation of water trees in the insulator.
[0006] However, conventional water tree-suppressed XLPE resins obtained by adding polyethylene glycol or polyethylene glycol derivatives can contain far more water molecules than XLPE resins without the addition of polyethylene glycol or polyethylene glycol derivatives. Therefore, when a power cable using conventional water tree-suppressed XLPE resin as an insulator is operated for a long period of time in a humid environment, the large amount of water molecules that migrate from outside the cable into the XLPE resin increases the dielectric tangent (tan δ) of the XLPE resin, resulting in a decrease in the power transmission efficiency of the power cable.
[0007] The increase in the dielectric loss tangent due to the addition of such hydrophilic molecules is observed not only in XLPE resins but also in non-crosslinked polypropylene-based insulators. Therefore, water tree-suppressed XLPE resins that do not contain highly hydrophilic polyethylene glycol or polyethylene glycol derivatives are preferred.
[0008] U.S. Pat. No. 4,305,849
[0009] An object of the present disclosure is to provide an insulating resin composition for power cables, and a power cable, which can suppress the growth of water trees and suppress an increase in dielectric tangent even in a moisture-rich environment.
[0010] [1] An insulating resin composition for a power cable, comprising components (a), (b), and (c), wherein component (a) is an unmodified polyolefin resin, component (b) is a resin containing at least one compound selected from unsaturated organic acids and derivatives thereof as a constituent element, and component (c) is an ethylene-based copolymer containing a carboxylic acid ester. [2] The insulating resin composition for a power cable according to the above [1], wherein component (a) is unmodified polypropylene. [3] The insulating resin composition for a power cable according to the above [2], further comprising component (d), wherein component (d) is an olefin-based copolymer or a styrene-based copolymer. [4] The insulating resin composition for a power cable according to the above [1], wherein component (a) is unmodified polyethylene. [5] The insulating resin composition for a power cable according to the above [4], further comprising component (e), wherein component (e) is a crosslinking agent. [6] The insulating resin composition for a power cable according to the above [5], wherein the crosslinking agent is an organic peroxide. [7] The insulating resin composition for a power cable according to any one of [1] to [6] above, wherein the component (b) is at least one resin selected from a polyolefin grafted with at least one compound selected from maleic anhydride and its derivatives, and a maleic anhydride copolymer. [8] The insulating resin composition for a power cable according to any one of [1] to [7] above, wherein the component (c) is at least one ethylene copolymer selected from an ethylene-methacrylic acid ester copolymer, an ethylene-acrylic acid ester copolymer, and an ethylene-vinyl acetate copolymer. [9] A power cable comprising: a conductor; an inner semiconducting layer disposed outside the conductor and surrounding the conductor; an insulating layer disposed outside the inner semiconducting layer and surrounding the inner semiconducting layer, the inner semiconducting layer being formed from the insulating resin composition for a power cable according to any one of [1] to [8] above; and an outer semiconducting layer disposed outside the insulating layer and surrounding the insulating layer.
[0011] According to the present disclosure, it is possible to provide an insulating resin composition for power cables and a power cable that can suppress the growth of water trees and suppress an increase in the dielectric loss tangent even in a moisture-rich environment.
[0012] Fig. 1 is a cross-sectional view showing an example of a power cable to which an insulating resin composition for a power cable according to an embodiment of the present invention is applied, and Fig. 2 is a schematic diagram showing a water tree test.
[0013] Hereinafter, a detailed description will be given based on an embodiment.
[0014] The present inventors conducted extensive research into the suppression of water tree growth and the suppression of an increase in the dielectric loss tangent, and as a result, discovered the following. In insulating resin compositions, ethylene-based copolymers containing carboxylic acid esters can suppress water treeing while reducing water uptake compared to highly hydrophilic polyethylene glycols and polyethylene glycol derivatives. However, like polyethylene glycols traditionally used as water tree inhibitors, ethylene-based copolymers containing carboxylic acid esters also increase the dielectric loss tangent of insulating resin compositions. In response to this problem, the present inventors discovered that a resin containing at least one compound selected from unsaturated organic acids and their derivatives as a constituent can suppress the increase in the dielectric loss tangent of insulating resin compositions caused by the incorporation of ethylene-based copolymers containing carboxylic acid esters, excluding polyethylene glycols and polyethylene glycol derivatives. Furthermore, they found that the resin can suppress water tree growth in insulating resin compositions and also suppress the increase in the dielectric loss tangent even in a moisture-rich environment. The present disclosure was completed based on these findings.
[0015] An insulating resin composition for a power cable according to an embodiment includes component (a), component (b), and component (c), in which component (a) is an unmodified polyolefin resin, component (b) is a resin containing, as a constituent element, at least one compound selected from unsaturated organic acids and derivatives thereof, and component (c) is an ethylene-based copolymer containing a carboxylic acid ester.
[0016] The insulating resin composition for a power cable according to the embodiment includes, as constituent elements, the component (a), the component (b), and the component (c). The insulating resin composition is an insulator.
[0017] The component (a) contained in the insulating resin composition is an unmodified polyolefin resin, and in particular, unmodified polypropylene or unmodified polyethylene is preferred.
[0018] The unmodified polypropylene is preferably homopolypropylene, random polypropylene, or block polypropylene. The random polypropylene is preferably a random copolymer of ethylene or an α-olefin and propylene, and the propylene component is preferably 90 wt % or more. The block polypropylene is preferably a copolymer of homopolypropylene, ethylene, and an α-olefin. Here, the α-olefin is preferably an olefin having 3 to 8 carbon atoms. When component (a) is unmodified polypropylene, the insulating resin composition is recyclable.
[0019] The unmodified polyethylene may be produced by either a low-pressure process or a high-pressure process, but low-density polyethylene (LDPE) produced by a high-pressure process is preferred.
[0020] Component (b) contained in the insulating resin composition is a resin containing at least one compound selected from unsaturated organic acids and their derivatives as a constituent element, and is at least one of a resin in which the compound is grafted onto a polymer and a copolymer resin of the compound with another monomer. Component (b) suppresses an increase in the dielectric loss tangent of the insulating resin composition due to component (c), which is a water tree suppressing component. By including component (b) in the insulating resin composition, an increase in the dielectric loss tangent of the insulating resin composition can be suppressed even when the insulating resin composition is exposed to a moisture-rich environment. The amount of component (b) contained in the insulating resin composition is preferably 1.0 wt % or more and 20.0 wt % or less. If the amount of component (b) is less than 1.0 wt%, it will be insufficient to suppress the increase in the dielectric tangent, and if the amount of component (b) is more than 20.0 wt%, the resin will adhere to the wall surface inside the extruder during conductor coating by extrusion, generating a gel, and the gel mixed into the insulator will deteriorate the dielectric tangent of the power cable or become a starting point for water tree generation.
[0021] The unsaturated organic acid is an unsaturated dicarboxylic acid, an unsaturated dicarboxylic acid anhydride, or an unsaturated dicarboxylic acid derivative. The unsaturated dicarboxylic acid is preferably maleic acid, fumaric acid, or itaconic acid. The unsaturated dicarboxylic acid anhydride is preferably maleic anhydride (MAH) or itaconic anhydride. The unsaturated dicarboxylic acid derivative is preferably monomethyl maleate, monoethyl maleate, diethyl maleate, monomethyl fumarate, dimethyl fumarate, diethyl fumarate, maleic acid monoamide, maleimide, N-methylmaleimide, N-phenylmaleimide, N-cyclohexylmaleimide, or triallyl isocyanurate. These may be used alone or in combination of two or more. Of these, the unsaturated organic acid is preferably maleic anhydride, a five-membered cyclic acid anhydride.
[0022] Examples of polymers onto which unsaturated organic acids and derivatives thereof can be grafted include polyolefins such as polyethylene and polypropylene; olefin copolymers such as ethylene-methacrylate copolymer, ethylene-acrylate copolymer, and ethylene-vinyl acetate copolymer; and styrene copolymers such as styrene-butadiene block copolymer (SBR), styrene-butadiene-styrene block copolymer (SBS), styrene-isoprene-styrene block copolymer (SIS), styrene-ethylene-butylene-styrene block copolymer (SEBS), and styrene-ethylene-ethylene-propylene-styrene block copolymer (SEEPS).
[0023] From the viewpoint of resin compatibility, a particularly preferred polymer to be grafted with an unsaturated organic acid or a derivative thereof is polypropylene when the unmodified polyolefin resin of component (a) is unmodified polypropylene, and polyethylene when the unmodified polyolefin resin of component (a) is unmodified polyethylene.
[0024] The graft amount of the unsaturated organic acid and its derivative in component (b) is preferably 0.01 wt % or more and 2.00 wt % or less in the graft resin of component (b). By using a resin with unsaturated organic acids grafted in this range, the unsaturated organic acids are uniformly dispersed in the insulating resin composition, and the dielectric loss tangent in the system can be uniformly reduced.
[0025] Furthermore, when the unsaturated organic acid and its derivative are maleic anhydride, the content of maleic anhydride in the insulating resin composition is preferably 0.01 wt% or more but less than 0.50 wt%. When maleic anhydride is contained in the insulating resin composition within this range, the dielectric loss tangent within the system can be uniformly controlled. In particular, when maleic anhydride is contained in an amount exceeding 0.50 wt%, the maleic anhydride grafted resin may adhere to the metal inner walls of the kneading device or extrusion device, causing scorch. Furthermore, the adhesion of the maleic anhydride grafted resin may reduce the uniformity of the resin composition, resulting in ineffective suppression of water tree growth. Furthermore, when the content is 0.47 wt% or less, non-uniformity of the resin composition due to resin adhesion is less likely to occur.
[0026] The graft resin can be prepared, for example, by the method described in paragraph
[0098] of Japanese Patent No. 6205032, by mixing the raw materials, polymer resin, antioxidant, modified monomer, and organic peroxide in an extruder, heating, and reacting them. It is also possible to purchase and use commercially available maleic anhydride graft resins. Examples include Admer (registered trademark) manufactured by Mitsui Chemicals, Inc., Modic (registered trademark) manufactured by Mitsubishi Chemical Corporation, Umex (registered trademark) manufactured by Sanyo Chemical Industries, Ltd., Tuftec (registered trademark) M manufactured by Asahi Kasei Corporation, and OREVAC (registered trademark) manufactured by SK Functional Polymers.
[0027] Preferred monomers constituting the copolymer resin with an unsaturated organic acid or a derivative thereof are ethylene monomer, propylene monomer, butene monomer, olefin monomers having 5 or more carbon atoms, styrene monomer, methacrylic acid ester monomer, acrylic acid ester monomer, and vinyl acetate monomer.
[0028] Component (b) is preferably at least one resin selected from polyolefins grafted with at least one compound selected from maleic anhydride and its derivatives, and maleic anhydride copolymers. Furthermore, the graft resin of an unsaturated organic acid and its derivatives is preferably maleic anhydride-grafted polyethylene resin (MAH-g-PE) or maleic anhydride-grafted polypropylene resin (MAH-g-PP). The copolymer resin of an unsaturated organic acid and its derivatives is preferably ethylene-maleic anhydride copolymer (Et-MAH copolymer) resin.
[0029] Examples of styrene-maleic anhydride copolymers include XIRAN (registered trademark) manufactured by Polyscope and Arastar manufactured by Arakawa Chemical Industries, Ltd., examples of α-olefin and maleic anhydride copolymers include Diacarna (registered trademark) manufactured by Mitsubishi Chemical Corporation and Fusabond (registered trademark) manufactured by The Dow Chemical Company, etc. Furthermore, examples of ethylene-acrylic acid ester-maleic anhydride terpolymers include LOTADER (registered trademark) MAH manufactured by SK Functional Polymer, and examples of ethylene-vinyl acetate-maleic anhydride terpolymers include OREVAC (registered trademark) T manufactured by SK Functional Polymer, etc.
[0030] Component (c) contained in the insulating resin composition is an ethylene-based copolymer containing a carboxylic acid ester, and is a component that suppresses the growth of water trees. Of these, component (c) is preferably at least one ethylene-based copolymer selected from ethylene-methacrylic acid ester copolymer, ethylene-acrylic acid ester copolymer, and ethylene-vinyl acetate copolymer (EVA). Preferred ethylene-methacrylic acid ester copolymers are ethylene-methyl methacrylate copolymer (EMMA), ethylene-ethyl methacrylate copolymer, and ethylene-butyl methacrylate copolymer. Preferred ethylene-acrylic acid ester copolymers are ethylene-methyl acrylate copolymer, ethylene-ethyl acrylate copolymer (EEA), and ethylene-butyl acrylate copolymer.
[0031] Suitable examples of ethylene-methacrylic acid ester copolymers, ethylene-acrylic acid ester copolymers and ethylene-vinyl acetate copolymers include Acryft (registered trademark) manufactured by Sumitomo Chemical Co., Ltd., EEA resin and EVA resin manufactured by Eneos NUC Corporation, Rexpearl (registered trademark) EEA and Novatec (registered trademark) EVA manufactured by Japan Polyethylene Corporation, and Evaflex (registered trademark) manufactured by Dow Mitsui Polychemicals.
[0032] The lower limit of the content of component (c) in the insulating resin composition is preferably 1.0 wt% or more for efficient water tree suppression, and 2.0 wt% or more for uniform water tree suppression. The upper limit of the content of component (c) is preferably 40.0 wt% or less for suppressing the water absorption of the insulating resin composition, and 20.0 wt% or less for efficiently suppressing an increase in the dielectric loss tangent due to hydrophilic molecules.
[0033] In addition to the above components (a) to (c), the insulating resin composition may further contain an olefin copolymer or a styrene copolymer as an elastomer, which is component (d). The insulating resin composition preferably contains component (d) because the flexibility of the insulating resin composition is enhanced. In particular, when the unmodified polyolefin resin of component (a) is unmodified polypropylene, the incorporation of these copolymers is effective in improving the flexibility of the insulating resin composition.
[0034] The olefin copolymer is a copolymer of ethylene or propylene with an α-olefin. The α-olefin is preferably an α-olefin having 3 to 8 carbon atoms. The olefin copolymer is preferably an ethylene-propylene copolymer.
[0035] The olefin copolymer may be blended as an olefin thermoplastic elastomer, which will be described later. The polymerization catalyst for the olefin copolymer is preferably a Ziegler-Natta catalyst, a metallocene catalyst, or a constrained geometry catalyst, and the olefin copolymer may be produced using a gas phase, solution, or slurry polymer process.
[0036] The olefin-based thermoplastic elastomer is preferably a resin obtained by multistage gas phase polymerization. The resin obtained by multistage gas phase polymerization is a resin composition containing polypropylene and an olefin-based copolymer, specifically, polypropylene and ethylene-α-olefin copolymer rubber or propylene-α-olefin copolymer rubber, and improves impact strength (especially impact strength at low temperatures) while maintaining the rigidity and heat resistance of polypropylene. Resins obtained by multistage gas phase polymerization are generally called heterophasic copolymers, impact copolymers, reactor-made alloys, reactor-made thermoplastic elastomers, or reactor TPOs (thermoplastic alloys).
[0037] In multistage gas-phase polymerization, finely powdered resin components produced in each stage are blended in a reactor during polymerization. By melt-kneading this mixture, a resin with a microphase-separated structure is obtained, which has a sea of finer propylene polymer components such as polypropylene and islands of elastomer components (copolymer rubber components), compared to conventional methods of blending and melt-kneading pellets of polypropylene and elastomer. The average particle size of the elastomer components in the insulating resin composition is preferably 5 μm or less, more preferably 1 μm or less. Here, the average particle size is determined by the average major axis of the elastomer component islands, obtained by photographing a freeze-fracture surface of the resin using, for example, a transmission electron microscope (TEM).
[0038] Suitable commercially available olefin-based thermoplastic elastomers obtained by such multistage gas phase polymerization include a series of resins called Cattalloy process resins, such as Adflex, Hifax, Softell, and Adsyl (registered trademarks) (all manufactured by LyondellBasell). Other suitable products include Tafmer (registered trademark) PN (manufactured by Mitsui Chemicals, Inc.), Tafthren (registered trademark) (manufactured by Sumitomo Chemical Co., Ltd.), Newcon (registered trademark) (manufactured by Japan Polypropylene Corporation), and Prime TPO (registered trademark) (manufactured by Prime Polymer Co., Ltd.).
[0039] When the unmodified polyolefin resin of component (a) is unmodified polypropylene, the insulating resin composition is not preferably provided with a crosslinking agent of component (e), because the decomposition reaction of polypropylene becomes the main reaction rather than the crosslinking reaction. However, when the unmodified polyolefin resin of component (a) is unmodified polyethylene, the insulating resin composition is preferably provided with a crosslinking agent of component (e), because the polyethylene is crosslinked to obtain a crosslinked product of the insulating resin composition, thereby increasing the breakdown voltage of the insulating resin composition. The crosslinking agent is preferably an organic peroxide.
[0040] Among these, the crosslinking agent is preferably di-t-hexyl peroxide (Perhexyl D manufactured by NOF Corporation), dicumyl peroxide (Percumyl D manufactured by NOF Corporation), 2,5-dimethyl-2,5-di(t-butylperoxy)hexane (Perhexa 25B manufactured by NOF Corporation), α,α'-di(t-butylperoxy)diisopropylbenzene (Perbutyl P manufactured by NOF Corporation), t-butylcumyl peroxide (Perbutyl C manufactured by NOF Corporation), or di-t-butyl peroxide (Perbutyl D manufactured by NOF Corporation). These may be used alone or in combination of two or more. Dicumyl peroxide is particularly preferred.
[0041] The lower limit of the content of the crosslinking agent in the insulating resin composition is preferably 0.1 wt % or more, more preferably 0.5 wt % or more, and the upper limit is preferably 5.0 wt % or less, more preferably 3.0 wt % or less. When the content of the crosslinking agent is within the above range, when the insulating resin composition is extruded onto a conductor using an extruder at a temperature of 120° C. or more and 135° C. or less, an insulating layer can be formed without causing unnecessary gelation of the resin, and good crosslinking can be achieved in the crosslinking step after the formation of the insulating layer.
[0042] The insulating resin composition may contain an antioxidant in addition to the above components. The antioxidant is preferably a hindered phenol-based or semi-hindered phenol-based antioxidant primarily intended for radical scavenging, or a phosphorus-based or sulfur-based antioxidant primarily intended for peroxide decomposition. These may be used alone or in combination of two or more.
[0043] The lower limit of the content of the antioxidant in the insulating resin composition is preferably 0.01 wt % or more, more preferably 0.20 wt % or more, and the upper limit is preferably 1.00 wt % or less, more preferably 0.60 wt % or less. When the content of the antioxidant is within the above range, oxidation degradation of the cross-linked product of the insulating resin composition can be effectively suppressed.
[0044] In addition to the above components, the insulating resin composition may contain various substances as long as they do not inhibit the growth of water trees and reduce the dielectric loss tangent. Examples of such substances include stabilizers, lubricants, inorganic fillers, surface treatment agents, flame retardants, acid scavengers, and voltage stabilizers. However, the median diameter (D50) of the inorganic filler is preferably 10 μm or less and 10.0 wt % or less. If these values are exceeded, the inorganic filler may become a nucleus for water treeing. By holding the insulating resin composition at 600°C in a nitrogen atmosphere, the organic components are decomposed and volatilized, leaving the inorganic filler as a residue. The inorganic filler can then be measured using a laser diffraction scattering method.
[0045] The insulating resin composition can be obtained by melt-kneading raw materials such as component (a), component (b), and component (c). As the melt-kneading device, existing kneaders such as a single-screw or twin-screw extruder, a Banbury mixer, or a kneader can be used. In particular, it is preferable to extrude the resin using a single-screw or twin-screw extruder capable of continuous kneading, equipped with a metal mesh filter with a mesh size of 100 μm or less for the purpose of removing foreign matter from the resin. Furthermore, in the case of an insulating resin composition containing a crosslinking agent (component (e)), kneading is preferably carried out at a temperature of 120°C or higher and 135°C or lower to suppress crosslinking of the resin.
[0046] The specific gravity of the insulating resin composition is preferably 0.90 or more and 0.93 or less.
[0047] The insulating resin composition preferably has a dielectric loss tangent of 1.0% or less, more preferably 0.5% or less, when measured at 90°C and 30 kV / mm in accordance with the rubber and plastic insulated wire testing method of JIS C 3005. When the dielectric loss tangent of the insulating resin composition is within the above range, a power cable using an insulating layer made of the insulating resin composition has a small dielectric loss tangent, thereby reducing energy loss and improving power transmission efficiency.
[0048] Furthermore, in order to suppress the growth of water trees in the insulating resin composition, the moisture absorption rate of a 1 mm thick insulating resin composition after storing it in a thermo-hygrostat at a temperature of 70°C and a relative humidity of 90% for 24 hours is preferably 100 ppm or more, more preferably 150 ppm or more. By imparting moisture absorption properties to the insulating resin composition, moisture in the insulating resin composition is uniformly dispersed, thereby suppressing the growth of water trees in the insulating resin composition. Furthermore, from the viewpoint of suppressing an increase in the dielectric loss tangent, the moisture absorption rate of the insulating resin composition is preferably 800 ppm or less, more preferably 350 ppm or less.
[0049] Such an insulating resin composition is suitable for use as an insulating material for power cables laid in moist environments such as underground or on the seabed. A power cable having an insulating layer made of the insulating resin composition can suppress the growth of water trees in the insulating layer and can also suppress an increase in the dielectric loss tangent even in moist environments, allowing the power cable to transmit electricity efficiently even when used at high voltage or extra-high voltage.
[0050] FIG. 1 is a cross-sectional view showing an example of a power cable to which an insulating resin composition according to an embodiment of the present invention is applied.
[0051] As shown in FIG. 1 , power cable 1 includes conductor 2, internal semiconductive layer 3 disposed on the outside of conductor 2, insulating layer 4 disposed on the outside of internal semiconductive layer 3 and formed from the insulating resin composition, and external semiconductive layer 5 disposed on the outside of insulating layer 4. Internal semiconductive layer 3 surrounds conductor 2. Insulating layer 4 surrounds internal semiconductive layer 3. In insulating resin compositions in which component (a) is unmodified polypropylene, insulating layer 4 is a non-crosslinked product (non-crosslinkable resin) made of the insulating resin composition. In insulating resin compositions in which component (a) is unmodified polyethylene, insulating layer 4 is a crosslinked product (crosslinkable resin) made by crosslinking the insulating resin composition. External semiconductive layer 5 surrounds insulating layer 4. Thus, power cable 1 includes internal semiconductive layer 3, insulating layer 4, and external semiconductive layer 5 laminated in this order on conductor 2 made of a metal such as copper or aluminum.
[0052] The internal semiconductive layer 3 and the external semiconductive layer 5 contain, for example, an olefin-based elastomer and conductive carbon black in the case of a non-crosslinkable resin, or contain, for example, an ethylene-based copolymer such as an ethylene-ethyl acrylate copolymer, an ethylene-methyl acrylate copolymer, an ethylene-butyl acrylate copolymer, or an ethylene-vinyl acetate copolymer in the case of a crosslinkable resin, and conductive carbon black.
[0053] The power cable 1 may further include a metal shielding layer (not shown) that is arranged outside the outer semiconductive layer 5 and surrounds the outer semiconductive layer 5. The power cable 1 may further include a sheath (not shown) that is arranged outside the metal shielding layer and surrounds the metal shielding layer.
[0054] The conductor 2 is continuously fed to a resin extrusion port, where it is coated with an inner semiconductive layer 3, an insulating layer 4 (insulating resin composition layer), and an outer semiconductive layer 5. These three layers may be extruded simultaneously or sequentially. If the conductor is heated by heat transfer from the previously coated resin during coating, the cooling rate of the resin near the conductor will be slow. Therefore, it is preferable to adjust the temperature of the conductor by cooling to between 1°C and 100°C before feeding the conductor to the resin extrusion port.
[0055] The insulating resin composition is coated by extruding it onto the conductor 2 (onto the internal semiconducting layer 3) from the resin extrusion port of a resin extruder equipped with a metal mesh filter with a mesh size of 100 μm or less for the purpose of removing foreign matter. The temperature of the insulating resin composition during extrusion is preferably equal to or higher than the melting point of the insulating resin composition. In particular, when a crosslinkable resin is used, the temperature is preferably 110°C or higher, more preferably 120°C or higher, and is preferably 140°C or lower to prevent scorch. When a non-crosslinkable resin is used, the temperature is preferably 140°C or higher, more preferably 180°C or higher, and is preferably 300°C or lower to prevent thermal decomposition of polypropylene.
[0056] After the conductor 2 is thus coated with the insulating resin composition layer, if the resin is a crosslinkable resin, a crosslinking reaction of the insulating resin composition layer is caused by heating under pressure to crosslink the insulating resin composition, thereby forming the insulating layer 4. If the resin is a non-crosslinkable resin, the insulating resin composition layer is slowly cooled under normal pressure or pressure by air cooling at room temperature to 150°C to form the insulating layer 4. In this way, the power cable 1 is obtained. Thereafter, the power cable 1 is cooled in a cooling pipe or a cooling water tank, and a metal shielding layer or sheath (not shown) is formed by a normal method, if necessary.
[0057] From the viewpoint of insulating properties, the thickness of the insulating layer 4 is preferably 2 mm or more, more preferably 5 mm or more, and even more preferably 10 mm or more, and from the viewpoint of ease of installation, the thickness is preferably 50 mm or less, and more preferably 40 mm or less.
[0058] Furthermore, from the viewpoint of insulating properties, the thickness of the internal semiconductive layer 3 and the thickness of the external semiconductive layer 5 are preferably 0.1 mm or more, and more preferably 0.5 mm or more, and from the viewpoint of conductive properties, they are preferably 5.0 mm or less, more preferably 3.0 mm or less, and even more preferably 2.0 mm or less.
[0059] According to the embodiment described above, even if an ethylene-based copolymer containing a carboxylic acid ester (component (c)) is contained to suppress the growth of water trees, an increase in the dielectric loss tangent due to component (c) can be suppressed by containing a resin containing at least one compound selected from unsaturated organic acids and derivatives thereof (component (b)) as a constituent element. Furthermore, by applying an insulating resin composition capable of suppressing the growth of water trees and reducing the dielectric loss tangent to the insulating layer of a power cable, the power transmission efficiency of the power cable can be improved.
[0060] Although the embodiments have been described above, the present invention is not limited to the above embodiments, but includes all aspects encompassed by the concept and scope of the claims of the present disclosure, and can be modified in various ways within the scope of the present disclosure.
[0061] Next, examples and comparative examples will be described, but the present invention is not limited to these examples.
[0062] The raw materials used in the examples and comparative examples are as follows.
[0063] The component (a) is as follows: Component (a-1): Unmodified polypropylene (B241; random polypropylene manufactured by Prime Polymer Co., Ltd., MFR 0.5) Component (a-2): Unmodified polyethylene (CE1559; polyethylene manufactured by Sumitomo Chemical Co., Ltd., MFR 0.6)
[0064] The components (b) are as follows: Component (b-1): Maleic anhydride grafted PE resin (Modic L553; manufactured by Mitsubishi Chemical Corporation, PE resin grafted with 1.00 wt% maleic anhydride) Component (b-2): Maleic anhydride grafted PP resin (Admer QE800; manufactured by Mitsui Chemicals, Inc., PP resin grafted with 0.4 wt% maleic anhydride, MFR 9.1) Component (b-3): Ethylene-maleic anhydride copolymer (Fusabond M603; manufactured by Dow, 18 wt% maleic anhydride, MFR 25.0)
[0065] The components (c) are as follows: Component (c-1): Ethylene-acrylic acid ester copolymer (NUC-6520; EEA manufactured by Eneos NUC Corporation, acrylate content 24 wt%, MFR 1.6) Component (c-2): Ethylene-methyl methacrylate copolymer (Acryft WH102; EMMA manufactured by Sumitomo Chemical Co., Ltd., methyl methacrylate content 17 wt%, MFR 0.25) Component (c-3): Ethylene-vinyl acetate copolymer (NUC-3888; EVA manufactured by Eneos NUC Corporation, vinyl acetate content 21 wt%, MFR 1.8)
[0066] The components (d) are as follows: Component (d-1): Olefin-based elastomer (Catalloy Q100F; TPO manufactured by SunAllomer, a thermoplastic elastomer consisting of a propylene-α-olefin copolymer and polypropylene, MFR 0.6) Component (d-2): Ethylene-propylene copolymer (Esprene SPO P-4801; EPR manufactured by Sumitomo Chemical Co., Ltd.) Component (d-3): Styrenic elastomer (Septon 8066; SEBS manufactured by Kuraray Co., Ltd., a styrene content of 33 wt%, no MFR flowability)
[0067] Component (e) is as follows: Component (e-1): Crosslinking agent (Percumyl D; dicumyl peroxide manufactured by NOF Corporation)
[0068] The components other than those mentioned above are as follows: Antioxidant (Irganox 1010; manufactured by BASF, a hindered phenol-based antioxidant) Polyethylene glycol (PEG-20000; manufactured by Adeka Corporation, number-average molecular weight 20,000)
[0069] (Examples 1 to 14 and Comparative Examples 1 and 2) Using a Henschel mixer, the raw materials were dry-blended according to the formulations shown in Tables 1 and 3, and then extruded using a single-screw extruder (L / D=24, resin discharge temperature 200°C) equipped with a plain-woven mesh having an opening of 0.091 mm, to obtain pellet-shaped insulating resin compositions (hereinafter also referred to as resin pellets) having the compositions (parts by mass) shown in Tables 1 and 3.
[0070] Examples 21 to 31 and Comparative Examples 11 to 12 Resin pellets having the compositions (parts by mass) shown in Tables 2 and 4 were obtained in the same manner as in Example 1, except that the resin discharge temperature was changed to 120°C.
[0071] [Measurements and Evaluations] The insulating resin compositions obtained in the above Examples and Comparative Examples were subjected to the following measurements and evaluations. The results are shown in Tables 1 to 4.
[0072] [1] Moisture Absorption Rate Using resin pellets, sheet-like samples measuring 100 mm in length, 150 mm in width, and 1 mm in thickness were molded. For unmodified polypropylene-based Examples 1-14 and Comparative Examples 1-2, samples were obtained by pressure molding at 230°C. For unmodified polyethylene-based Examples 21-31 and Comparative Examples 11-12, samples were obtained by pressure molding at 120°C for 10 minutes and then crosslinking at 160°C for 30 minutes. The sheet-like samples thus obtained were divided into six test pieces. The test pieces were then stored in a constant temperature and humidity chamber at 70°C and 90% relative humidity for 24 hours, after which they were removed and their moisture content was measured using the Karl Fischer method, Method B (moisture evaporation method) of JIS K7251, to determine the moisture absorption rate.
[0073] [2] Water Tree Length First, a small power cable was manufactured. An insulating resin composition was extruded using a single-screw extruder (L / D = 24, full-flight screw) equipped with a 0.091 mm plain-woven mesh and loaded with resin pellets. At the same time, an inner and outer semiconductive layers were extruded using another single-screw extruder (L / D = 24, full-flight screw) equipped with a 0.091 mm plain-woven mesh and loaded with semiconductive resin. The inner semiconductive layer, insulating layer (insulating resin composition), and outer semiconductive layer were simultaneously coated on the copper conductor using a three-layer extrusion head. The inner semiconductive layer, insulating layer, and outer semiconductive layer were extruded at 200°C for the unmodified polypropylene-based Examples 1 to 14 and Comparative Examples 1 and 2, and at 120°C for the unmodified polyethylene-based Examples 21 to 31 and Comparative Examples 11 and 12.
[0074] The semiconductive resin used in Examples 1 to 14 and Comparative Examples 1 and 2 was a dry blend of 30 parts of EVA450 (ethylene-vinyl acetate copolymer resin manufactured by Mitsui Dow Polychemicals), 70 parts of Elastomer Q200F (TPO manufactured by SunAllomer Co., Ltd., MFR 0.8), 30 parts of Denka Black (carbon black manufactured by Denka Co., Ltd.), and 0.5 parts of an antioxidant (Nocrac 300, a hindered phenol-based antioxidant manufactured by Ouchi Shinko Chemical Co., Ltd.) in a Henschel mixer, extruded in a single-screw extruder (L / D = 24, 200°C), and pelletized. The semiconductive resin used in Examples 21 to 31 and Comparative Examples 11 and 12 was NUCV-9590 (an ethylene-ethyl acrylate copolymer-based semiconductive resin composition manufactured by Eneos NUC Corporation).
[0075] Next, the coated cables were air-cooled in Examples 1 to 14 and Comparative Examples 1 and 2, and then cooled in a water bath. In Examples 21 to 31 and Comparative Examples 11 and 12, they were subjected to thermal crosslinking through a pressurized crosslinking tube at 260°C and 0.5 MPa, and then cooled in a water bath. In this way, small power cables were obtained that included a copper conductor with an outer diameter of approximately 2 mm, an inner semiconductive layer with a thickness of approximately 0.5 mm, an insulating layer with a thickness of approximately 2 mm, and an outer semiconductive layer with a thickness of approximately 0.5 mm.
[0076] Next, the resulting small-sized power cable 1, as shown in Figure 2, was immersed in a 3.5 wt% NaCl aqueous solution, and a 4 kV, 1000 Hz AC voltage was applied between the conductor and the NaCl aqueous solution for 200 hours to perform a water tree test. After the test, the power cable was sliced into 1 mm thick slices, and the resulting 10 samples were observed under an optical microscope to measure the maximum length of water trees that had developed. Samples with a water tree length of less than 150 μm were deemed to have been successful in suppressing water tree growth and passed the test, while samples with a water tree length of 150 μm or more were deemed to have been unsuccessful in suppressing water tree growth and failed the test.
[0077] [3] Dielectric loss tangent (tan δ) Using the power cable manufactured as described above, the dielectric loss tangent before moisture absorption was measured at 90°C and 30 kV / mm in accordance with JIS C 3005, a test method for rubber and plastic insulated wires. The power cable was then stored for 24 hours in a thermo-hygrostat at 70°C and 90% relative humidity. After that, aluminum tape was wrapped around the surface of the outer semiconductive layer to prevent moisture evaporation due to heating during measurement. The dielectric loss tangent after moisture absorption was measured at 90°C and 30 kV / mm in accordance with JIS C 3005, a test method for rubber and plastic insulated wires, in the same manner as described above. The dielectric loss tangent measured at 90°C and 30 kV / mm both before and after moisture absorption is preferably 1.00% or less, more preferably 0.50% or less.
[0078]
[0079]
[0080]
[0081]
[0082] As shown in Table 1, in the above examples, the insulating resin compositions contained components (a), (b), and (c), which suppressed the growth of water trees and prevented an increase in the dielectric loss tangent even in a humid environment. On the other hand, in the above comparative examples, the insulating resin compositions did not contain at least one of components (a) to (c), so they were unable to suppress the growth of water trees and prevent an increase in the dielectric loss tangent even in a humid environment. In particular, in comparative examples 1 and 11, the insulating resin compositions did not contain component (b), so the dielectric loss tangent increased both before and after moisture absorption. In comparative examples 2 and 12, the insulating resin compositions contained polyethylene glycol, so the amount of moisture absorption was large, increasing the dielectric loss tangent before moisture absorption and significantly increasing the dielectric loss tangent after moisture absorption.
[0083] REFERENCE SIGNS LIST 1 Power cable 2 Conductor 3 Inner semiconductive layer 4 Insulating layer 5 Outer semiconductive layer
Claims
1. An insulating resin composition for power cables comprising components (a), (b) and (c), wherein the component (a) is an unmodified polyolefin resin, the component (b) is a resin containing, as a constituent element, at least one compound selected from unsaturated organic acids and derivatives thereof, and the component (c) is an ethylene-based copolymer containing a carboxylic acid ester.
2. The insulating resin composition for power cables according to claim 1, wherein the component (a) is an unmodified polypropylene.
3. The insulating resin composition for power cables according to claim 2, further comprising a component (d), said component (d) being an olefin-based copolymer or a styrene-based copolymer.
4. The insulating resin composition for power cables according to claim 1, wherein the component (a) is an unmodified polyethylene.
5. The insulating resin composition for power cables according to claim 4, further comprising a component (e), said component (e) being a crosslinking agent.
6. The insulating resin composition for power cables according to claim 5, wherein the crosslinking agent is an organic peroxide.
7. The insulating resin composition for power cables according to claim 1, wherein the component (b) is at least one resin selected from polyolefins grafted with at least one compound selected from maleic anhydride and its derivatives, and maleic anhydride copolymers.
8. The insulating resin composition for power cables according to claim 1, wherein the component (c) is at least one ethylene-based copolymer selected from the group consisting of ethylene-methacrylic acid ester copolymers, ethylene-acrylic acid ester copolymers, and ethylene-vinyl acetate copolymers.
9. A power cable comprising: a conductor; an inner semiconductive layer disposed on the outside of the conductor and surrounding the conductor; an insulating layer formed from the power cable insulating resin composition according to any one of claims 1 to 8, disposed on the outside of the inner semiconductive layer and surrounding the inner semiconductive layer; and an outer semiconductive layer disposed on the outside of the insulating layer and surrounding the insulating layer.
Citation Information
Patent Citations
Insulating resin composition for DC power cable, crosslinked resin, DC power cable, member for forming reinforcing insulating layer of DC power cable joint, and DC power cable joint
JP6205032B1
Polyolefin composition containing high molecular weight polyethylene glycol useful for electrical insulation
US4305849A
Crosslinkable flame-retardant composition with excellent heat resistance
JP1995062158A
Flame-retardant resin composition and wiring material using the same
JP2003160704A
Flexible flame-retardant resin material and electric wire / cable using the same
JP2005029604A
Cited By
Insulating layer for an electric cable, based on polypropylene and polar group-bearing polymers
EP4783199A1
INSULATING LAYER FOR ELECTRICAL CABLES, BASED ON POLYPROPYLENE AND POLYMERS CARRYING POLAR GROUPS
FR3171732A1