Chemical coolant for aerosol fire-extinguishing agent and preparation method therefor

By using organic acids, carbonates and other components in aerosol fire extinguishing agents for acid-base neutralization reactions, the corrosiveness and conductivity problems of aerosol fire extinguishing agents are solved, its application range is expanded, and efficient fire extinguishing performance is maintained .

WO2024212282A1PCT designated stage expired Publication Date: 2024-10-17HUBEI JIANDUN FIRE TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/092038
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-11
Filing Date
2023-05-04
Publication Date
2024-10-17

AI Technical Summary

Technical Problem

Existing aerosol fire extinguishing agents have corrosiveness and conductivity problems, which limit their application scope. It is also difficult to improve the fire extinguishing agent formula to maintain high insulation and low corrosion performance while ensuring fire extinguishing efficiency.

Method used

By using a combination of organic acids, carbonates or alkaline carbonates, binders and release agents, the principle of neutralization reaction is used to neutralize the strong alkaline substances sprayed by the aerosol fire extinguishing agent, thereby reducing the corrosiveness and improving the Insulation, chemical coolant for preparing an aerosol fire extinguishing agent.

Benefits of technology

While ensuring fire extinguishing efficiency, it reduces the corrosiveness and conductivity of aerosol fire extinguishing agents, expands its application range, and generates neutral potassium salt substances through acid-base neutralization reactions, reducing electrochemical corrosion on metal surfaces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023092038_17102024_PF_FP_ABST
    Figure CN2023092038_17102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present invention are a chemical coolant for an aerosol fire-extinguishing agent and a preparation method therefor. Under the principle of a neutralization reaction, a chemical coolant suitable for a K-type aerosol fire-extinguishing agent is prepared by mixing an organic acid, and a carbonate or a basic carbonate with a binder and a release agent, and a coolant suitable for an S-type aerosol fire-extinguishing agent is prepared by mixing an organic acid, a carbonate or a basic carbonate, an alkaline organic substance, a binder and a release agent. The coolant can effectively neutralize strongly alkaline substances generated during fire extinguishing via different types of aerosol fire-extinguishing agents and enable same to generate sylvites having neutral pH and weak hygroscopicity, such that the corrosivity of the aerosol fire-extinguishing agents is effectively reduced; and low-hygroscopicity sylvites cannot be ionized, thereby showing a very strong electrical insulating property. In the present invention, by using the coolant on the premise that raw material components and the fire extinguishing performance of an aerosol fire-extinguishing agent are unchanged, not only is the temperature of a nozzle of a fire-extinguishing device effectively reduced, but the effects of high insulation and low corrosion of sediments are also achieved, and the application range is widened.
Need to check novelty before this filing date? Find Prior Art

Description

Chemical coolant for aerosol fire extinguishing agent and preparation method thereof Technical Field

[0001] The invention belongs to the technical field of hot aerosol fire extinguishing coolants, and particularly relates to a chemical coolant for aerosol fire extinguishing agents and a preparation method thereof. Background Art

[0002] Aerosol fire extinguishing agents, a new type of fire extinguishing agent developed over the past four decades, are solid mixtures composed of an oxidizing agent, a reducing agent, a combustion rate control agent, and a binder. Currently, commonly used aerosol fire extinguishing agents are primarily divided into two categories: K-type and S-type. K-type aerosol fire extinguishing agents, also known as potassium salt fire extinguishing agents, represent the second stage of aerosol fire extinguishing agent technology development. They primarily utilize potassium nitrates, chlorates, and perchlorates as the primary oxidants. S-type aerosol fire extinguishing agents primarily utilize strontium salts as the primary oxidant, supplemented by potassium nitrate, a novel composite oxidant.

[0003] K-type aerosol fire extinguishing agent has the advantage of high spraying fire extinguishing efficiency. It mainly captures free radicals through potassium active particles. Potassium can easily react with free radicals such as HO·, H· and O· to ​​reduce the concentration of active free radicals in the fire scene. However, the fire extinguishing products it sprays mainly include CO2, N2, K2O and K2CO3. Among them, K2O has strong hygroscopicity and reacts with water to form strong base KOH; in addition, K2CO3 also has strong hygroscopicity. After absorbing moisture, KOH and K2CO3 will ionize to produce OH - 、CO3 2- and K + Plasma has strong electrical conductivity and corrosiveness. During use, firstly, the hot aerosol released by potassium salt as an oxidant has a strong electrical conductivity that can damage live equipment. Secondly, the strong corrosiveness of KOH and K2CO3 has a corrosive effect on metal parts, thereby damaging the insulation of the circuit boards of precision instruments and causing certain corrosion to cultural relics and paper documents. The application sites are greatly restricted and the market share is gradually decreasing. The substances sprayed by S-type aerosol fire extinguishing agents are mainly SrO, Sr(OH)2, SrCO3 and other products of the decomposition of strontium nitrate. The corrosiveness and electrical insulation of the released products are greatly improved compared to K-type aerosols, but the released products still have certain corrosiveness and conductivity. Therefore, there is an urgent need for a substance or method that can solve the corrosiveness and conductivity of aerosol fire extinguishing agents. The current idea is mainly to conduct high insulation and low corrosion research based on the aerosol fire extinguishing agent itself or the coolant used in conjunction with it.

[0004] Chinese patent CN114350326A discloses a coolant and its preparation method, a temperature-sensitive flocculent gel, and an aerosol fire extinguishing device. The coolant comprises an organic acid, an organic polyol, and a binder. The coolant absorbs heat during decomposition or sublimation, lowering the nozzle temperature of the aerosol fire extinguishing device. Furthermore, the coolant decomposes or sublimates upon heating to form a temperature-sensitive flocculent gel. When the temperature of the temperature-sensitive flocculent gel is below the temperature-sensitive response temperature, it coats the fire-extinguishing particles, preventing them from contacting water in the air and forming a strong electrolyte that could cause secondary damage to the protected object. When the temperature of the temperature-sensitive flocculent gel is above the temperature-sensitive response temperature, the fire-extinguishing particles are released to extinguish the fire. Chinese patent CN108992827A discloses a method for preparing an insulating anti-corrosion aerosol fire extinguishing agent. The insulating anti-corrosion aerosol fire extinguishing agent is prepared by reacting and mixing nanocellulose, sodium lignosulfonate, and ethylenediamine with potassium nitrate, strontium nitrate, and other substances. The aerosol fire extinguishing agent ensures high heat transfer efficiency between the aerosols while effectively reducing corrosion of metal equipment by the solid particles after extinguishing the fire. Chinese patent CN106621165B discloses a low-temperature S-type aerosol fire extinguishing agent, whose regulators use potassium oxalate, magnesium powder and hexamethylenetetramine to ensure that the mixed combustion product has low corrosiveness and excellent insulation properties.

[0005] However, when improving the formula of aerosol fire extinguishing agents to achieve high insulation and low corrosion properties, it is very difficult to ensure that their fire extinguishing efficiency remains unchanged. The use of the coating concept to treat aerosol fire extinguishing particles also needs to overcome the difficulty of not affecting the fire extinguishing efficiency. Therefore, how to prepare an agent independent of aerosol fire extinguishing agents and their spray products to help achieve the goals of high insulation and low corrosion and expand the application range of aerosol fire extinguishing agents has become an urgent problem to be solved in the field of aerosol fire extinguishing agents.

[0006] Summary of the Invention

[0007] In order to solve the above technical problems, the present invention provides a coolant for an aerosol fire extinguishing agent and a preparation method thereof. By combining the use of an organic acid, a carbonate or basic carbonate, a binder and a release agent, the neutralization reaction principle is utilized to neutralize the strongly alkaline substances sprayed by the aerosol fire extinguishing agent, thereby reducing corrosiveness and improving insulation while ensuring the cooling effect of the aerosol nozzle.

[0008] The technical solution adopted in the present invention is as follows:

[0009] The invention discloses a coolant chemical coolant for an aerosol fire extinguishing agent, which consists of 30%-70% of an organic acid, 30%-70% of a carbonate or a basic carbonate, 1%-10% of a binder and 1%-10% of a release agent.

[0010] Preferably, the chemical coolant further comprises 10%-20% alkaline organic matter.

[0011] More preferably, the alkaline organic substance is any one of dicyandiamide, melamine, o-phenylenediamine, m-phenylenediamine and p-phenylenediamine.

[0012] Preferably, the organic acid is any one of cinnamic acid, benzoic acid, terephthalic acid, phthalic acid, citric acid, oxalic acid, tartaric acid, ethylenediaminetetraacetic acid, lauric acid, salicylic acid, and sorbic acid.

[0013] Preferably, the carbonate is any one of copper carbonate, manganese carbonate, magnesium carbonate, zinc carbonate, calcium carbonate, strontium carbonate, and barium carbonate; and the basic carbonate is any one of basic copper carbonate, basic zinc carbonate, and basic magnesium carbonate.

[0014] Preferably, the binder is any one of ethyl cellulose, phenolic resin, epoxy resin, hydroxypropyl methylcellulose, polyvinyl alcohol, and dextrin.

[0015] Preferably, the release agent is any one of magnesium stearate, zinc stearate, molybdenum disulfide, tungsten disulfide, and graphite.

[0016] The present invention also provides a method for preparing a coolant for an aerosol fire extinguishing agent, which specifically comprises the following steps:

[0017] (1) (1) Weigh the various raw materials in claim 1 or 2 in proportion, sieve mix 2-5 times, and mix evenly to obtain a solid mixture;

[0018] (2) adding methanol to the solid mixture, mixing the wet materials, and granulating the wet materials through a mesh to obtain wet coolant particles;

[0019] (3) drying the wet coolant particles and then sieving them twice to obtain dry coolant particles;

[0020] (4) The dry coolant particles are pressed into sheets to obtain a finished coolant sheet (the coolant is cylindrical in shape with a diameter of 6 mm and a height of 5.5 mm).

[0021] Preferably, the mesh size of the sieve in step (1) is 100 mesh; the mesh size of the sieve in steps (2) and (3) is 20 mesh.

[0022] Preferably, the drying condition in step (3) is drying at 55-65° C. for 10-15 hours.

[0023] The beneficial effects of the present invention are as follows: based on the fact that the products released by aerosol fire extinguishing agents easily absorb moisture to form highly corrosive substances such as K2O and K2CO3, the present invention uses the principle of acid-base neutralization reaction to add a coolant containing an acidic substance into the outlet channel of the aerosol fire extinguishing agent to cause a chemical reaction with the released products to generate neutral potassium salt substances. These neutral metal potassium salts have very weak hygroscopicity and thus do not ionize, exhibiting strong electrical insulation. At the same time, the neutral potassium salts with very weak hygroscopicity are unlikely to cause electrochemical corrosion on metal surfaces, thereby reducing the corrosiveness of the aerosol fire extinguishing agent. The present invention only changes the type of potassium salt, without changing the potassium concentration or reducing the fire extinguishing ability of the aerosol. The additional coolant not only reduces the temperature of the fire extinguishing device nozzle, but also expands the application range of the aerosol fire extinguishing agent. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 shows copper plates with different degrees of corrosion, where A is a photo of a slightly corroded copper plate after the spraying experiment of the coolant prepared in Example 1, B is a photo of a moderately corroded copper plate after the spraying experiment of the coolant prepared in Comparative Example 2, and C is a photo of a severely corroded copper plate after the spraying experiment of the coolant prepared in Comparative Example 3. DETAILED DESCRIPTION

[0025] The technical solutions of the present invention are further explained below with reference to the accompanying drawings and specific embodiments. It is worth noting that the following embodiments are only preferred embodiments of the present invention and are not intended to further limit the present invention. The scope of protection of the present invention shall be subject to the contents of the claims. Any modification or equivalent substitution of the technical solutions of the present invention made by those skilled in the art without creative work shall fall within the scope of protection of the present invention.

[0026] Example 1 Coolant for K-type aerosol fire extinguishing agent

[0027] (1) 50% cinnamic acid, 41% basic copper carbonate, 4% magnesium stearate, and 5% phenolic resin were mixed, sieved three times through a 100-mesh sieve, and dry-mixed to obtain a solid mixture;

[0028] (2) adding 14% anhydrous methanol to the solid mixture obtained in step (1) to perform wet mixing, and granulating the mixed wet material through a 20-mesh sieve to obtain wet coolant particles;

[0029] (3) drying the obtained wet coolant particles at 60° C. for 12 h until the volatile content is less than 1%, and sieving them twice through a 20-mesh sieve to obtain dry coolant particles;

[0030] (4) Finally, the dry coolant granules were added to a tablet press and compressed at 10 MPa to obtain coolant tablets with a diameter of 6 mm and a thickness of 5.5 mm.

[0031] Example 2 Coolant for K-type aerosol fire extinguishing agent

[0032] (1) 50% salicylic acid, 41% basic magnesium carbonate, 4% zinc stearate, and 5% ethyl cellulose were mixed, sieved three times through a 100-mesh sieve, and dry-mixed to obtain a solid mixture;

[0033] (2) adding 14% anhydrous methanol to the solid mixture obtained in step (1) to perform wet mixing, and granulating the mixed wet material through a 20-mesh sieve to obtain wet coolant particles;

[0034] (3) drying the obtained wet coolant particles at 60° C. for 12 h until the volatile content is less than 1%, and sieving them twice through a 20-mesh sieve to obtain dry coolant particles;

[0035] (4) Finally, the dry coolant granules were added to a tablet press and compressed at 10 MPa to obtain coolant tablets with a diameter of 6 mm and a thickness of 5.5 mm.

[0036] Example 3 Coolant for K-type aerosol fire extinguishing agent

[0037] (1) 40% phthalic acid, 51% basic zinc carbonate, 4% molybdenum disulfide and 5% epoxy resin were mixed, sieved three times with a 100-mesh sieve, and dry-mixed to obtain a solid mixture;

[0038] (2) adding 14% anhydrous methanol to the solid mixture obtained in step (1) to perform wet mixing, and granulating the mixed wet material through a 20-mesh sieve to obtain wet coolant particles;

[0039] (3) drying the obtained wet coolant particles at 60° C. for 12 h until the volatile content is less than 1%, and sieving them twice through a 20-mesh sieve to obtain dry coolant particles;

[0040] (4) Finally, the dry coolant granules were added to a tablet press and compressed at 10 MPa to obtain coolant tablets with a diameter of 6 mm and a thickness of 5.5 mm.

[0041] Example 4 Coolant for K-type aerosol fire extinguishing agent

[0042] (1) 60% benzoic acid, 31% basic magnesium carbonate, 4% tungsten disulfide and 5% hydroxypropyl methylcellulose were mixed, sieved three times with a 100-mesh sieve, and dry-mixed to obtain a solid mixture;

[0043] (2) adding 14% anhydrous methanol to the solid mixture obtained in step (1) to perform wet mixing, and granulating the mixed wet material through a 20-mesh sieve to obtain wet coolant particles;

[0044] (3) drying the obtained wet coolant particles at 60° C. for 12 h until the volatile content is less than 1%, and sieving them twice through a 20-mesh sieve to obtain dry coolant particles (volatile content is less than 1%);

[0045] (4) Finally, the dry coolant granules were added to a tablet press and compressed at 10 MPa to obtain coolant tablets with a diameter of 6 mm and a thickness of 5.5 mm.

[0046] Example 5 Coolant for K-type aerosol fire extinguishing agent

[0047] (1) 60% citric acid, 31% manganese carbonate, 4% graphite and 5% polyvinyl alcohol were mixed, sieved three times with a 100-mesh sieve, and dry-mixed to obtain a solid mixture;

[0048] (2) adding 14% anhydrous methanol to the solid mixture obtained in step (1) to perform wet mixing, and granulating the mixed wet material through a 20-mesh sieve to obtain wet coolant particles;

[0049] (3) drying the obtained wet coolant particles at 60° C. for 12 h until the volatile content is less than 1%, and sieving them twice through a 20-mesh sieve to obtain dry coolant particles (volatile content is less than 1%);

[0050] (4) Finally, the dry coolant granules were added to a tablet press and compressed at 10 MPa to obtain coolant tablets with a diameter of 6 mm and a thickness of 5.5 mm.

[0051] Example 6 Coolant for S-type aerosol fire extinguishing agent

[0052] (1) 50% cinnamic acid, 31% basic copper carbonate, 10% dicyandiamide, 4% magnesium stearate and 5% phenolic resin were mixed, sieved three times with a 100-mesh sieve, and dry-mixed to obtain a solid mixture;

[0053] (2) adding 14% anhydrous methanol to the solid mixture obtained in step (1) to perform wet mixing, and granulating the mixed wet material through a 20-mesh sieve to obtain wet coolant particles;

[0054] (3) drying the obtained wet coolant particles at 60° C. for 12 h until the volatile content is less than 1%, and sieving them twice through a 20-mesh sieve to obtain dry coolant particles;

[0055] (4) Finally, the dry coolant granules were added to a tablet press and compressed at 10 MPa to obtain coolant tablets with a diameter of 6 mm and a thickness of 5.5 mm.

[0056] Example 7 Coolant for S-type aerosol fire extinguishing agent

[0057] (1) 35% phthalic acid, 46% basic zinc carbonate, 10% melamine, 4% magnesium stearate and 5% ethyl cellulose were mixed, sieved three times with a 100-mesh sieve, and dry-mixed to obtain a solid mixture;

[0058] (2) adding 14% anhydrous methanol to the solid mixture obtained in step (1) to perform wet mixing, and granulating the mixed wet material through a 20-mesh sieve to obtain wet coolant particles;

[0059] (3) drying the obtained wet coolant particles at 60° C. for 12 h until the volatile content is less than 1%, and sieving them twice through a 20-mesh sieve to obtain dry coolant particles;

[0060] (4) Finally, the dry coolant granules were added to a tablet press and compressed at 10 MPa to obtain coolant tablets with a diameter of 6 mm and a thickness of 5.5 mm.

[0061] Example 8 Coolant for S-type aerosol fire extinguishing agent

[0062] (1) 50% salicylic acid, 31% basic magnesium carbonate, 10% dicyandiamide, 4% magnesium stearate, and 5% ethyl cellulose were mixed, sieved three times with a 100-mesh sieve, and dry-mixed to obtain a solid mixture;

[0063] (2) adding 14% anhydrous methanol to the solid mixture obtained in step (1) to perform wet mixing, and granulating the mixed wet material through a 20-mesh sieve to obtain wet coolant particles;

[0064] (3) drying the obtained wet coolant particles at 60° C. for 12 h until the volatile content is less than 1%, and sieving them twice through a 20-mesh sieve to obtain dry coolant particles;

[0065] (4) Finally, the dry coolant granules were added to a tablet press and compressed at 10 MPa to obtain coolant tablets with a diameter of 6 mm and a thickness of 5.5 mm.

[0066] Example 9 Coolant for S-type aerosol fire extinguishing agent

[0067] (1) 45% ethylenediaminetetraacetic acid, 31% copper carbonate, 15% o-phenylenediamine, 4% zinc stearate, and 5% dextrin were mixed, sieved three times through a 100-mesh sieve, and dry-mixed to obtain a solid mixture;

[0068] (2) adding 14% anhydrous methanol to the solid mixture obtained in step (1) to perform wet mixing, and granulating the mixed wet material through a 20-mesh sieve to obtain wet coolant particles;

[0069] (3) drying the obtained wet coolant particles at 60° C. for 12 h until the volatile content is less than 1%, and sieving them twice through a 20-mesh sieve to obtain dry coolant particles;

[0070] (4) Finally, the dry coolant granules were added to a tablet press and compressed at 10 MPa to obtain coolant tablets with a diameter of 6 mm and a thickness of 5.5 mm.

[0071] Example 10 Coolant for S-type aerosol fire extinguishing agent

[0072] (1) 51% lauric acid, 30% strontium carbonate, 10% m-phenylenediamine, 4% molybdenum disulfide and 5% ethyl cellulose were mixed, sieved three times through a 100-mesh sieve, and dry-mixed to obtain a solid mixture;

[0073] (2) adding 14% anhydrous methanol to the solid mixture obtained in step (1) to perform wet mixing, and granulating the mixed wet material through a 20-mesh sieve to obtain wet coolant particles;

[0074] (3) drying the obtained wet coolant particles at 60° C. for 12 h until the volatile content is less than 1%, and sieving them twice through a 20-mesh sieve to obtain dry coolant particles;

[0075] (4) Finally, the dry coolant granules were added to a tablet press and compressed at 10 MPa to obtain coolant tablets with a diameter of 6 mm and a thickness of 5.5 mm.

[0076] Example 11 Coolant for S-type aerosol fire extinguishing agent

[0077] (1) 41% tartaric acid, 40% barium carbonate, 10% p-phenylenediamine, 4% tungsten disulfide and 5% ethyl cellulose were mixed, sieved three times through a 100-mesh sieve, and dry-mixed to obtain a solid mixture;

[0078] (2) adding 14% anhydrous methanol to the solid mixture obtained in step (1) to perform wet mixing, and granulating the mixed wet material through a 20-mesh sieve to obtain wet coolant particles;

[0079] (3) drying the obtained wet coolant particles at 60° C. for 12 h until the volatile content is less than 1%, and sieving them twice through a 20-mesh sieve to obtain dry coolant particles (volatile content is less than 1%);

[0080] (4) Finally, the dry coolant granules were added to a tablet press and compressed at 10 MPa to obtain coolant tablets (cylindrical granules) with a diameter of 6 mm and a thickness of 5.5 mm.

[0081] Comparative Example 1

[0082] (1) 91% salicylic acid, 4% magnesium stearate, and 5% ethyl cellulose were mixed, sieved three times through a 100-mesh sieve, and dry-mixed to obtain a solid mixture;

[0083] (2) adding 14% anhydrous methanol to the solid mixture obtained in step (1) to perform wet mixing, and granulating the mixed wet material through a 20-mesh sieve to obtain wet coolant particles;

[0084] (3) drying the obtained wet coolant particles at 60° C. for 12 h until the volatile content is less than 1%, and sieving them twice through a 20-mesh sieve to obtain dry coolant particles;

[0085] (4) Finally, the dry coolant granules were added to a tablet press and compressed at 10 MPa to obtain coolant tablets with a diameter of 6 mm and a thickness of 5.5 mm.

[0086] Comparative Example 2

[0087] (1) 91% dicyandiamide, 4% magnesium stearate, and 5% ethyl cellulose were sieved three times through a 100-mesh sieve and dry-mixed to obtain a solid mixture;

[0088] (2) adding 14% anhydrous methanol to the solid mixture obtained in step (1) to perform wet mixing, and granulating the mixed wet material through a 20-mesh sieve to obtain wet coolant particles;

[0089] (3) drying the obtained wet coolant particles at 60° C. for 12 h until the volatile content is less than 1%, and sieving them twice through a 20-mesh sieve to obtain dry coolant particles (volatile content is less than 1%);

[0090] (4) Finally, the dry coolant granules were added to a tablet press and compressed at 10 MPa to obtain coolant tablets (cylindrical granules) with a diameter of 6 mm and a thickness of 5.5 mm.

[0091] Comparative Example 3

[0092] (1) Mix 91% basic magnesium carbonate, 4% magnesium stearate, and 5% ethyl cellulose, sieve through a 100-mesh sieve three times, and dry-blend until uniformly mixed to obtain a solid mixture;

[0093] (2) adding 14% anhydrous methanol to the solid mixture obtained in step (1) to perform wet mixing, and granulating the mixed wet material through a 20-mesh sieve to obtain wet coolant particles;

[0094] (3) drying the obtained wet coolant particles at 60° C. for 12 h until the volatile content is less than 1%, and sieving them twice through a 20-mesh sieve to obtain dry coolant particles;

[0095] (4) Finally, the dry coolant granules were added to a tablet press and compressed at 10 MPa to obtain coolant tablets with a diameter of 6 mm and a thickness of 5.5 mm.

[0096] Comparative Example 4

[0097] (1) 71% salicylic acid, 20% dicyandiamide, 4% magnesium stearate, and 5% ethyl cellulose were sieved three times through a 100-mesh sieve and dry-mixed to obtain a solid mixture;

[0098] (2) adding 14% anhydrous methanol to the solid mixture obtained in step (1) to perform wet mixing, and granulating the mixed wet material through a 20-mesh sieve to obtain wet coolant particles;

[0099] (3) drying the obtained wet coolant particles at 60° C. for 12 h until the volatile content is less than 1%, and sieving them twice through a 20-mesh sieve to obtain dry coolant particles;

[0100] (4) Finally, the dry coolant granules were added to a tablet press and compressed at 10 MPa to obtain coolant tablets with a diameter of 6 mm and a thickness of 5.5 mm.

[0101] Comparative Example 5

[0102] Φ6 ceramic balls (purchased from Pingxiang Zhongtian Chemical Filling Material Co., Ltd.) were directly used as the physical coolant for the K-type aerosol fire extinguishing agent.

[0103] Comparative Example 6

[0104] Φ6 ceramic balls (purchased from Pingxiang Zhongtian Chemical Filling Material Co., Ltd.) were directly used as the physical coolant of the S-type aerosol fire extinguishing agent.

[0105] Comparative Example 6

[0106] Verification

[0107] 70 g of the coolant prepared in Examples 1-5, Comparative Example 1, Comparative Example 2, and Comparative Example 5 were respectively mixed with 50 g of a K-type aerosol (homemade, 73% KNO3 + 27% reducing agent) coated charge (diameter 32 mm, height) to form an aerosol fire extinguishing device. The dielectric strength of the solid precipitation was tested according to the 7.30 test in XF 499.1-2010, the pH of the aqueous solution of the aerosol fire extinguisher was tested according to the 7.31 test, and the corrosiveness of the solid precipitation was tested according to the 7.32 test method. The results are shown in Table 1.

[0108] 70 g of the coolants prepared in Examples 6-11, Comparative Example 2, Comparative Example 4 and Comparative Example 6 were respectively mixed with 50 g of S-type aerosol (homemade, 43% KNO3 + 30% Sr(NO3)2 + 27% reducing agent) coated powder columns to form an aerosol fire extinguishing device. The electrical insulation, corrosiveness and pH value were tested according to the above experimental methods. The results are shown in Table 1.

[0109] Table 1 Effects of different coolants on the electrical insulation, corrosiveness, pH value and spray temperature of aerosol fire extinguishing agents

[0110] As can be seen from the above table, the electrical insulation and corrosiveness of the products released by the K-type and S-type aerosols using ceramic balls as coolants in Comparative Examples 5 and 6 are not ideal. In particular, the K-type aerosol is highly corrosive and conductive, and its sediment solution is alkaline.

[0111] After the combination of K-type aerosol and organic acid coolant (Comparative Example 1), S-type aerosol and basic carbonate coolant (Comparative Example 2), the corrosiveness of the sediment is stronger, and the electrical insulation is relatively good. And after the use of organic acid-carbonate coolant and K-type aerosol combination (Examples 1-5) and organic acid-organic amine-carbonate and S-type aerosol combination (Examples 6-11), its release shows good electrical insulation and very weak corrosiveness, and the acidity and alkalinity of the sediment solution are close to neutral. It can be seen from the above results that coolant can solve the corrosiveness and electrical insulation of aerosol fire extinguishing agent. And the composition of the coolant can be adjusted according to the type of aerosol, to meet the low corrosion and high insulation performance of the sediment. In the K-type aerosol coolant, an amount of alkaline organic amine is added to weaken the acidity of the coolant, thereby being applicable to the S-type aerosol.

Claims

1. A chemical coolant for an aerosol fire extinguishing agent, Features: The chemical coolant consists of 30-70% of organic acid, 30-70% of carbonate or basic carbonate, 1-10% of binder and 1-10% of release agent.

2. A chemical coolant for an aerosol fire extinguishing agent according to claim 1, Features: The chemical coolant also includes 10-20% alkaline organic matter.

3. A chemical coolant for an aerosol fire extinguishing agent according to claim 2, Features: The alkaline organic substance is any one of dicyandiamide, melamine, o-phenylenediamine, m-phenylenediamine and p-phenylenediamine.

4. The chemical coolant for an aerosol fire extinguishing agent according to claim 1, Features: The organic acid is any one of cinnamic acid, benzoic acid, terephthalic acid, phthalic acid, citric acid, oxalic acid, tartaric acid, ethylenediaminetetraacetic acid, lauric acid, salicylic acid, and sorbic acid.

5. The chemical coolant for an aerosol fire extinguishing agent according to claim 1, Features: The carbonate is any one of copper carbonate, manganese carbonate, magnesium carbonate, zinc carbonate, calcium carbonate, strontium carbonate and barium carbonate; the basic carbonate is any one of basic copper carbonate, basic zinc carbonate and basic magnesium carbonate.

6. The chemical coolant for an aerosol fire extinguishing agent according to claim 1, Features: The binder is any one of ethyl cellulose, phenolic resin, epoxy resin, hydroxypropyl methyl cellulose, polyvinyl alcohol and dextrin.

7. The chemical coolant for an aerosol fire extinguishing agent according to claim 1, Features: The release agent is any one of magnesium stearate, zinc stearate, molybdenum disulfide, tungsten disulfide and graphite.

8. A method for preparing a chemical coolant for an aerosol fire extinguishing agent, Features: The following steps are involved: (1) Weigh various raw materials in claim 1 or 2 in proportion, mix with a sieve for 2-5 times, and mix evenly to obtain a solid mixture; (2) adding methanol to the solid mixture, mixing the wet materials, and granulating through a screen to obtain wet coolant particles; (3) drying the wet coolant particles and then sieving them twice to obtain dry coolant particles; (4) Pressing the dry coolant particles into sheets to obtain a finished coolant sheet.

9. The preparation method according to claim 8, Features: The mesh size of the sieve in step (1) is 100 mesh; the mesh size of the sieve in steps (2) and (3) is 20 mesh.

10. The preparation method according to claim 8, Features: The drying condition in step (3) is drying at 55-65° C. for 10-15 hours.

Citation Information

Patent Citations

  • Catalytic chemical coolant for hot aerosol and preparation method thereof

    CN101757760A

  • Coolant, preparation method thereof, temperature-sensitive flocculating gel and aerosol fire extinguishing device

    CN114350326A

  • Chemical coolant for aerosol fire extinguishing agent and preparation method of chemical coolant

    CN116515465A

  • Formula and preparation process of cooling antiflame agent

    CN1284390A

  • Composition for cooling fire-extinguishing aerosol and method of its production

    RU2120318C1